Polyarylene sulfide and method for producing the same

By optimizing the manufacturing method of polyarylene sulfides, and combining distillation, water washing, and organic solvent washing with inactive gas flow heating, the problems of mold contamination and poor melt flowability of polyarylene sulfides were solved, achieving low-cost, high-efficiency molding processability and coupling agent reactivity.

CN115335435BActive Publication Date: 2024-11-05TORAY INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180022344.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-11-05
Filing Date
2021-03-22
Publication Date
2024-11-05
Estimated Expiration
2041-03-22

AI Technical Summary

Technical Problem

Existing technologies for preparing polyarylene sulfides suffer from problems such as severe mold contamination, poor melt flowability, and low reactivity with coupling agents. In particular, oligomer components tend to adhere to the mold at high temperatures, leading to decreased molding processability and higher costs.

Method used

A method for manufacturing polyarylene sulfides includes heating a sulfiding agent, a dihaloaromatic compound, and an organic polar solvent to react, followed by distillation, water washing, and organic solvent washing, combined with heating through inactive gas flow. The process parameters are controlled to reduce oligomer content, optimize molecular weight distribution and particle shape, and improve melt flowability and coupling agent reactivity.

Benefits of technology

This technology enables the low-cost preparation of polyarylene sulfides with minimal mold contamination, excellent melt flowability, and high reactivity with coupling agents. It reduces the frequency of mold maintenance and gas generation during molding and improves processability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003851517770000051
    Figure BDA0003851517770000051
  • Figure BDA0003851517770000061
    Figure BDA0003851517770000061
  • Figure BDA0003851517770000062
    Figure BDA0003851517770000062
Patent Text Reader

Abstract

A method for producing polyarylene sulfide is a method for producing polyarylene sulfide by heating a mixture containing at least a sulfiding agent, a dihalogenated aromatic compound, and an organic polar solvent to react, wherein the following steps 1, 2, 3, and 4 are performed after the reaction to produce polyarylene sulfide is completed. Step 1: a step of distilling off the organic polar solvent from the reaction mixture obtained at the end of the reaction to obtain a solid component containing polyarylene sulfide. Step 2: a step of washing the solid component containing polyarylene sulfide with water after step 1. Step 3: a step of washing the polyarylene sulfide with an organic solvent after step 2 to reduce the amount of chloroform extractable components in the polyarylene sulfide to 1.7% by weight or less. Step 4: a step of distilling off the organic solvent used in step 3 while heating while flowing an inert gas at a flow rate of 0.2 L / min or more per 1 kg of polyarylene sulfide after step 3. Provided are polyarylene sulfide which has little mold contamination during molding, excellent melt fluidity, and high reactivity with a coupling agent, and a method for producing the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention provides a polyarylene sulfide which has little mold contamination during molding, excellent melt fluidity and high reactivity with a coupling agent, and a method for producing the same. Background Art

[0002] Polyarylene sulfide (hereinafter sometimes abbreviated as PAS) represented by polyphenylene sulfide is an engineering plastic having excellent heat resistance, chemical resistance, flame retardancy, electrical properties, and mechanical properties, and is widely used for fibers, films, injection molding, and extrusion molding.

[0003] The polyarylene sulfide resin is a resin having excellent properties as described above, but it is known that when it is heated and melted during molding, it generates gas due to oligomer components. Among them, oligomer components with relatively low volatility (high boiling point) are observed to adhere to the mold and accumulate after being vaporized by heating, and become mold dirt. Due to this influence, it is pointed out that regular mold maintenance is required, and in applications such as projectors and car headlight reflectors used at high temperatures, lens parts existing around them are blurred. Therefore, in order to solve this problem, technical development for reducing the amount of gas generated during heating by removing oligomer components in polyarylene sulfide resin has been carried out for many years.

[0004] As a method for reducing the gasification of PAS, for example, a method is known in which a dihalogenated aromatic compound and an alkali metal sulfide are reacted in an organic polar solvent, the reaction mixture is separated into solid and liquid, and the recovered solid component is subjected to solvent washing to obtain PAS. (See, for example, Patent Document 1.) According to this method, the oligomer component dissolved in the solvent can be efficiently removed, and PAS with a reduced gas amount can be obtained.

[0005] In addition, it is known that after a dihalogenated aromatic compound and an alkali metal sulfide react in an organic polar solvent, water is injected into the system before the PAS particles are precipitated, and then the system is slowly cooled to greatly increase the PAS particle size, and the PAS is sieved with a sieve having a mesh size of about 100 to 200 μm, and the obtained PAS is washed in the order of an organic solvent and water and dried to obtain PAS (quenching method). (See, for example, Patent Document 2.) By this method, the oligomer component dissolved in the solvent can also be efficiently removed, and PAS with a reduced amount of gas can be obtained.

[0006] In addition, it is known that after a dihalogenated aromatic compound and an alkali metal sulfide are reacted in an organic polar solvent, the reaction system in a high temperature state is flashed into a container under normal pressure or reduced pressure to recover PAS, and the PAS is washed with water and dried (flash method). Once PAS is obtained, the obtained PAS is heated to 220° C. in an inert gas atmosphere to obtain PAS with a reduced gas amount (aging method) (see, for example, Patent Document 3).

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 62-232437 (Patent Claims)

[0010] Patent Document 2: Japanese Patent Application Laid-Open No. 61-255933 (Patent Claims)

[0011] Patent Document 3: Japanese Patent Application Laid-Open No. 7-233256 (Patent Claims) Summary of the invention

[0012] Problems to be solved by the invention

[0013] However, the method of Patent Document 1 has the following characteristics: although it can remove the oligomer components with relatively low volatility (high boiling point) and reduce mold contamination, it is necessary to wash with water after solvent washing in order to remove the water-soluble substances by-products generated by the reaction, and the filtrate generated in the washing process contains all water, water-soluble substances and organic polar solvents with large latent heat of evaporation. Whether the filtrate is discarded or the organic polar solvent is recovered, it costs a lot, so there is a problem of excessive cost in industrial production of PAS.

[0014] In addition, the method of Patent Document 2 can achieve the same reduction of mold contamination as the method of Patent Document 1, and can remove water-soluble substances and oligomer components without using water when screening with a sieve, so it is a method that can reduce the recovery cost of organic polar solvents compared with the method of Patent Document 1, but the manufacturing cost of PAS is still relatively high, and further cost reduction is required. Further, for the method of Patent Document 2, it can be observed that the obtained PAS particles become porous, and there is a tendency that even the oligomer components that do not correspond to the cause of mold contamination are excessively washed and removed. There is also a problem that due to this influence, it is easy to obtain PAS with low melt fluidity and reduced molding processability, and improvement is required.

[0015] In addition, the method of Patent Document 3 is a method for producing PAS at low cost because the organic polar solvent can be recovered during the flash evaporation operation of the polymerization reactant. Therefore, the solvent recovery cost is low. However, since the treatment for low gasification is a heat treatment in an inert gas atmosphere, although highly volatile oligomer components can be removed, relatively low volatile (high boiling point) oligomer components that adhere / accumulate on the mold during the molding process of PAS cannot be removed. The resulting PAS becomes a substance that causes much mold contamination, and improvement is required.

[0016] Therefore, an object of the present invention is to improve such a conventional art and to produce PAS at low cost which has little mold contamination during molding, is excellent in melt fluidity, and has high reactivity with a coupling agent.

[0017] Methods for solving problems

[0018] In order to solve the above problems, the method for producing PAS of the present invention has the following structure. That is,

[0019] A method for producing polyarylene sulfide is a method for producing polyarylene sulfide by heating a mixture containing at least a sulfiding agent, a dihalogenated aromatic compound, and an organic polar solvent to react, wherein the following steps 1, 2, 3, and 4 are performed after the reaction to produce polyarylene sulfide is completed.

[0020] Step 1: A step of distilling off the organic polar solvent from the reaction mixture obtained at the end of the reaction to obtain a solid component containing polyarylene sulfide.

[0021] Step 2: After step 1, a step of washing the solid content containing polyarylene sulfide with water.

[0022] Step 3: After step 2, a step of washing the polyarylene sulfide with an organic solvent to reduce the amount of chloroform extractable components in the polyarylene sulfide to 1.7% by weight or less.

[0023] Step 4: After step 3, a step of distilling off the organic solvent used in step 3 while heating the mixture while flowing an inert gas at a flow rate of 0.2 L / min or more per 1 kg of polyarylene sulfide.

[0024] The PAS of the present invention has the following structure. That is,

[0025] A polyarylene sulfide, wherein the cumulative integral value of a molecular weight of 4,000 is 48 or more and 53 or less when the cumulative integral value of a molecular weight of 100 to 10,000 in a molecular weight distribution curve is 100, and when the melt flow rate of the polyarylene sulfide is MFR1 and the melt flow rate after the polyarylene sulfide and an epoxy silane coupling agent are mixed at a weight ratio of 100:1 and heated at 315.5°C for 5 minutes is MFR2, the rate of change represented by MFR2 / MFR1 is 0.085 or less.

[0026] In the method for producing PAS of the present invention, it is preferred that in step 1, the temperature for distilling off the organic polar solvent is 200° C. or higher and 250° C. or lower.

[0027] In the method for producing PAS of the present invention, it is preferred that in step 3, the water content of the polyarylene sulfide before washing with the organic solvent is 30% by weight or less.

[0028] In the method for producing PAS of the present invention, it is preferred that in step 3, the specific surface area of ​​the polyarylene sulfide before washing with the organic solvent is 5 m 2 / g or more and 50m 2 / g or less.

[0029] In the method for producing PAS of the present invention, it is preferred that in step 4, the temperature for distilling off the organic solvent is 70° C. or higher and 250° C. or lower.

[0030] In the method for producing PAS of the present invention, it is preferred that in step 4, the time for distilling off the organic solvent is 0.1 hours to 50 hours.

[0031] In the PAS of the present invention, the polyarylene sulfide preferably has a particle shape, and the median particle size D50 of the polyarylene sulfide particles is 1 μm or more and 400 μm or less.

[0032] Effects of the Invention

[0033] According to the method of the present invention, PAS having less mold contamination during resin molding, excellent melt fluidity, and high reactivity with a coupling agent can be produced by a method that is inexpensive in production cost and capable of mass production. DETAILED DESCRIPTION

[0034] Embodiments of the present invention are described below.

[0035] (1) Polyarylene sulfide

[0036] The polyarylene sulfide in the present invention is a homopolymer or copolymer having a repeating unit of the formula -(Ar-S)- as a main constituent unit. Ar includes units represented by the following formulas (A) to (L), and the formula (A) is particularly preferred.

[0037]

[0038] (R1 and R2 are substituents selected from hydrogen atom, alkyl group, alkoxy group and halogen group, and R1 and R2 may be the same or different). As long as the repeating unit is used as the main constituent unit, a small amount of branched units or crosslinked units shown in the following formula (M) to formula (P) may be included. The copolymerization amount of these branched units or crosslinked units is preferably in the range of 0 mol% to 1 mol% per 1 mol of -(Ar-S)- units.

[0039]

[0040] In addition, the PAS in the present invention can be a random copolymer, a block copolymer and a mixture thereof containing the above-mentioned repeating unit. As representative substances thereof, polyphenylene sulfide, polyphenylene sulfide sulfone, polyphenylene sulfide ketone, random copolymers thereof, block copolymers and mixtures thereof, etc. can be cited. As particularly preferred PAS, polyphenylene sulfide, polyphenylene sulfide sulfone and polyphenylene sulfide ketone containing 90 mol% or more of the p-phenylene unit represented by the following formula as the main constituent unit of the polymer can be cited.

[0041]

[0042] There is no particular limitation on the molecular weight of these PAS, but as a general weight average molecular weight Mw of PAS, 5,000 to 1,000,000 can be exemplified, preferably 7,500 to 500,000 can be exemplified, and more preferably 10,000 to 100,000 can be exemplified. In addition, the molecular weight determination of PAS in the present invention is implemented by gel permeation chromatography (GPC) as a type of size exclusion chromatography (SEC). In addition, regarding the melt viscosity known to be related to the weight average molecular weight Mw, according to the above-mentioned preferred Mw, the range of 0.1 to 1,000 Pa·s (300°C, shear rate 1,000 / sec) can be exemplified, and the range of 0.1 to 500 Pa·s can be exemplified. PAS having a molecular weight and a melt viscosity in the above-mentioned preferred range has excellent molding processability and tends to be preferably used in a large number of applications.

[0043] (2) Chloroform Extract

[0044] The chloroform extract component in the present invention is mainly an oligomer component contained in PAS, and is a component containing cyclic PAS and linear PAS oligomers. In addition, the ratio of these components is not particularly limited.

[0045] Here, the cyclic PAS is a cyclic compound having a repeating unit of the formula -(Ar-S)- as a main constituent unit, and is preferably a compound of the following general formula (Q) containing 80 mol % or more of the repeating unit.

[0046]

[0047] Here, as Ar, similarly to the case of the above-mentioned PAS, units represented by the above-mentioned formulae (A) to (L) etc. can be exemplified, among which the formula (A) is particularly preferred.

[0048] In addition, the above-mentioned repeating units of formula (A) to formula (L) may be randomly included in the cyclic PAS, may be included in blocks, or may be any of their mixtures. As their representative substances, cyclic polyphenylene sulfide, cyclic polyphenylene sulfide sulfone, cyclic polyphenylene sulfide ketone, cyclic random copolymers containing them, cyclic block copolymers and mixtures thereof, etc. can be exemplified. As a particularly preferred cyclic PAS, a cyclic polyphenylene sulfide (hereinafter, sometimes abbreviated as cyclic PPS) containing 80 mol% or more, especially 90 mol% or more of the p-phenylene sulfide unit represented by the following formula as the main constituent unit can be cited.

[0049]

[0050] The repetition number m in the above formula (Q) of the cyclic PAS is not particularly limited, but can be exemplified as a preferred range of 2 to 50, can be exemplified as a more preferred range of 3 to 40, and can be exemplified as a further preferred range of 4 to 30. In addition, the cyclic PAS may be either a single compound having a single repetition number or a mixture of cyclic PAS having different repetition numbers, but a mixture of cyclic PAS having different repetition numbers is often obtained.

[0051] The so-called linear PAS oligomer is a straight-chain oligomer having a repeating unit of the formula -(Ar-S)- as a main constituent unit, wherein Ar has the same structure as that shown in the above-mentioned (1) polyarylene sulfide. There is no limitation on the number of repetitions of the main constituent unit of the linear PAS oligomer, but as a component extracted by chloroform, a repeating number of 2 to 20 can be exemplified as a preferred range, and a repeating number of 2 to 10 can be exemplified as a more preferred range. The linear PAS oligomer may be a single compound having a single repeating number or a mixture of linear PAS oligomers having different repeating numbers, and a mixture of linear PAS oligomers having different repeating numbers is often obtained.

[0052] In the present invention, by reducing the oligomer component of low volatility (high boiling point) attached to / deposited on the mold during molding, it is the purpose to obtain PAS with less mold pollution, but it is confirmed that such oligomer component is almost equal to chloroform extraction component. Therefore, it is important to remove and reduce the chloroform extraction component in PAS in the present invention. The less the chloroform extraction component in this PAS is, the more the mold pollution during molding is reduced, if the chloroform extraction component amount in PAS is reduced to below 1.7 weight %, it is confirmed that the mold pollution during molding has an improvement tendency. Therefore, in the present invention, in the operation 3 described later, it is necessary to wash PAS with an organic solvent, and the chloroform extraction component amount in PAS is reduced to below 1.7 weight %. In addition, as the lower limit of the chloroform extraction component amount in PAS, it is more preferred to consider less from the viewpoint of reducing mold pollution, so it is most preferably 0 weight % that the chloroform extraction component is not included in PAS completely. On the other hand, as the upper limit, it is preferably below 1.2 weight %, more preferably below 1.0 weight %. When the amount of the chloroform extractable component in PAS is within the above-described preferred range, mold contamination during molding of PAS tends to be more clearly improved.

[0053] Here, regarding the amount of chloroform extractable components in PAS in the present invention, 10 g of PAS was weighed and subjected to Soxhlet extraction with 100 g of chloroform for 3 hours, and the weight of the component obtained by distilling off chloroform from the extract was measured and calculated as a ratio to the weight of the charged polymer.

[0054] In addition, in the present invention, although it is described that the less the amount of chloroform extract in PAS, the better from the viewpoint of reducing mold contamination during PAS molding, it is known that the chloroform extract in PAS exists in various resins to show a good fluidization effect of reducing the melt viscosity during melting, so in the case of attaching importance to this effect, sometimes a certain amount of chloroform extract is allowed to be included in PAS. In addition, regarding cyclic PAS, it is known that the application of high-functional materials and functional materials based on the characteristics generated by the ring shape is possible, for example, as a compound with inclusion ability, various effective utilization methods are known as an effective monomer for synthesizing high molecular weight linear polymers. The chloroform extract removed / recovered from PAS by the present invention can not only be discarded as waste, but also can be separated and recovered as needed cyclic PAS and effectively used in other uses, so in this respect, the present invention can be said to be an industrially preferred method.

[0055] (3) Vulcanizing agent

[0056] The so-called sulfiding agent used in the present invention may be any substance that can introduce a sulfur bond into a dihalogenated aromatic compound, and examples thereof include alkali metal sulfides and alkali metal hydrosulfides. Specific examples of alkali metal sulfides include sodium sulfide, potassium sulfide, lithium sulfide, rubidium sulfide, cesium sulfide, etc., among which sodium sulfide is preferably used. These alkali metal sulfides may be used in the form of hydrates or aqueous mixtures, or in the form of anhydrous substances.

[0057] Specific examples of the alkali metal hydrosulfide include sodium hydrosulfide, potassium hydrosulfide, lithium hydrosulfide, rubidium hydrosulfide, cesium hydrosulfide, etc. Among them, sodium hydrosulfide is preferably used. These alkali metal hydrosulfides can be used in the form of a hydrate or an aqueous mixture, or in the form of an anhydrous substance.

[0058] An alkali metal hydroxide and / or an alkaline earth metal hydroxide may also be used together with the sulfiding agent. Specific examples of the alkali metal hydroxide include sodium hydroxide, potassium hydroxide, lithium hydroxide, rubidium hydroxide, cesium hydroxide, etc., and specific examples of the alkaline earth metal hydroxide include calcium hydroxide, strontium hydroxide, barium hydroxide, etc., among which sodium hydroxide is preferably used.

[0059] When an alkali metal hydrosulfide is used as the sulfiding agent, it is particularly preferred to use an alkali metal hydroxide simultaneously, but the amount used can be 0.95 mol or more and 1.20 mol or less, 1.00 mol or more and 1.15 mol or less, and 1.005 mol or more and 1.100 mol or less, relative to 1 mol of the alkali metal hydrosulfide, as a preferred range, as a more preferred range, and as a further preferred range. The sulfiding agent may be introduced into the system at any time, but it is preferably introduced before the dehydration operation described later.

[0060] (4) Dihalogenated aromatic compounds

[0061] The dihalogenated aromatic compound used in the present invention is a compound having an aromatic ring, two halogen atoms in one molecule, and a molecular weight of 1,000 or less. Specific examples include dihalogenated benzenes such as p-dichlorobenzene, m-dichlorobenzene, o-dichlorobenzene, p-dibromobenzene, m-dibromobenzene, o-dibromobenzene, 1-bromo-4-chlorobenzene, and 1-bromo-3-chlorobenzene; dihalogenated benzenes including substituents other than halogen such as 1-methoxy-2,5-dichlorobenzene, 1-methyl-2,5-dichlorobenzene, 1,4-dimethyl-2,5-dichlorobenzene, 1,3-dimethyl-2,5-dichlorobenzene, and 3,5-dichlorobenzoic acid; and dihalogenated aromatic compounds such as 1,4-dichloronaphthalene, 1,5-dichloronaphthalene, 4,4'-dichlorobiphenyl, 4,4'-dichlorodiphenyl ether, 4,4'-dichlorodiphenyl sulfone, and 4,4'-dichlorodiphenyl ketone. Among them, dihalogenated aromatic compounds having p-dihalogenated benzenes represented by p-dichlorobenzene as the main component are preferred. Particularly preferred is one containing 80 to 100 mol % of p-dichlorobenzene, and more preferred is one containing 90 to 100 mol % of p-dichlorobenzene. In order to produce a PAS copolymer, two or more dihalogenated aromatic compounds may be used in combination.

[0062] The usage of the dihalogenated aromatic compound can be exemplified as preferably 0.1 mol or more and 3 mol or less, more preferably 0.5 mol or more and 2 mol or less, and further preferably 0.9 mol or more and 1.2 mol or less per 1 mol of sulfur in the sulfidizing agent. If the usage of the dihalogenated aromatic compound is within the above-mentioned preferred range, it is easy to control the molecular weight of PAS within the preferred region of the present invention, and PAS having a small amount of chloroform extractable components in PAS can be obtained.

[0063] In addition, the dihalogenated aromatic compound can be introduced into the system at any time without any problem, but it is preferably introduced after the dehydration operation described below. In addition, as the adding method, not only the method of adding the entire amount at once but also the method of introducing in stages can be adopted.

[0064] (5) Organic polar solvents

[0065] In the present invention, an organic polar solvent is used as a reaction solvent, wherein an organic amide solvent having high reaction stability is preferably used. As specific examples, N-alkylpyrrolidones such as N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, caprolactams such as N-methyl-ε-caprolactam, 1,3-dimethyl-2-imidazolidinone, N,N-dimethylacetamide, N,N-dimethylformamide, hexamethylphosphoric triamide, dimethyl sulfone, tetramethylene sulfoxide, etc., can be cited as aprotic organic solvents represented by the following, and further, mixtures thereof can also be used, wherein N-methyl-2-pyrrolidone is preferably used.

[0066] About the usage amount of the organic polar solvent in the present invention, the organic polar solvent amount of the reaction system can be exemplified as a preferred range of 0.5 mole or more and 10 moles or less relative to each 1 mole of sulfur of the vulcanizing agent, and can be exemplified as a more preferred range of 2 moles or more and 8 moles or less. If the organic polar solvent amount is the above-mentioned preferred range, it has a tendency that unpreferable reactions are difficult to occur and the degree of polymerization is easy to increase. Here, the organic polar solvent amount of the reaction system is the amount obtained by deducting the amount of organic polar solvent removed from the reaction system from the amount of organic polar solvent introduced into the reaction system. In addition, there is no problem in introducing the organic polar solvent into the system at any time, but in the case of carrying out the dehydration operation described later, there is a tendency that a part of the organic polar solvent is scattered outside the system, so it is preferred to adopt a method of introducing the minimum amount required for dehydration in advance before the dehydration operation, and introducing it by adding it in a manner to become the above-mentioned preferred usage amount after the dehydration operation is completed.

[0067] (6) Water

[0068] The water in the present invention refers to water directly added when the raw materials are added, water introduced incidentally by the added sulfiding agent, dihalogenated aromatic compound, organic polar solvent, water generated in the process of the reaction, etc. The amount of water present in the system at the start of the reaction is defined as the amount of water obtained by subtracting the water distilled out of the system by dehydration from the above total. The presence of water in the present invention has the effect of increasing the solubility of the sulfiding agent in the organic polar solvent and contributing to the promotion of the reaction. On the other hand, the excess water has the effect of reducing the nucleophilicity of the sulfiding agent and delaying the reaction, or increasing the pressure in the system, so it is important to control the amount of water present in the system within a preferred range.

[0069] Regarding the preferred range of the amount of water present in the system at the start of the reaction, as a lower limit, the closer to 0 mole relative to each 1 mole of sulfur of the vulcanizing agent, the more preferred, but as a substantial lower limit for implementing the present invention, it can be illustrated that each 1 mole of sulfur relative to the vulcanizing agent is 0.01 mole or more. In addition, as an upper limit, it can be illustrated that it is preferably 2.5 moles or less, and more preferably 2.0 moles or less. If the amount of water at the start of the reaction is the above-mentioned preferred range, there is a tendency that the reaction speed is fast and by-products can be suppressed. There is further a tendency that the pressure rise in the system can be suppressed and the cost related to the introduction of high-pressure equipment can also be reduced.

[0070] In the present invention, when the water content at the start of the reaction exceeds the above-mentioned preferred water content, an operation of reducing the water content in the reaction system by dehydration operation can be performed to adjust the water content. There is no particular limitation on the method of performing the dehydration operation. Regarding the raw materials added, a method of pre-dehydrating; a method of dehydrating a mixture in a state where no sulfiding agent, dihalogenated aromatic compound, or two or more components are added; a method of dehydrating after modulating a mixture containing a sulfiding agent, a dihalogenated aromatic compound, and an organic polar solvent, etc., can be used. However, from the perspective of precisely controlling the amount of dihalogenated aromatic compound used, which is easy to disperse by heating, it is preferred to use a method of dehydrating a mixture in a state where no dihalogenated aromatic compound is added. At this time, the temperature at which the mixture is heated also varies according to the combination of the sulfiding agent and the organic polar solvent used, and the ratio with water, etc., so it cannot be clearly specified, but as a lower limit, it can be exemplified as 150°C or more, preferably 160°C or more, and more preferably 170°C or more. In addition, as an upper limit, 250°C or less can be exemplified, and 230°C or less can be exemplified as being preferred. If the heating temperature during dehydration is in the preferred range described above, the added sulfidizing agent can be suppressed from scattering outside the system as hydrogen sulfide, and dehydration can be performed efficiently. In addition, there is no particular restriction on the pressure conditions during dehydration, and any of normal pressure, reduced pressure, and pressurized conditions can be adopted, but in order to distill and remove water more efficiently, it is preferably under normal pressure or reduced pressure. The so-called normal pressure here refers to the pressure near the standard state of the atmosphere, which is an atmospheric pressure condition near 101kPa in absolute pressure at a temperature near about 25°C. In addition, the atmosphere in the system is expected to be a non-oxidizing condition, preferably an inert gas atmosphere such as nitrogen, helium, and argon, and in particular, from the viewpoint of economy and ease of operation, it is more preferably under a nitrogen atmosphere.

[0071] (7) Method for producing polyarylene sulfide

[0072] In the present invention, a mixture containing at least a sulfiding agent, a dihalogenated aromatic compound, and an organic polar solvent is heated to react to produce PAS, and after the reaction to produce PAS is completed, the following steps 1, 2, 3, and 4 are performed to obtain PAS.

[0073] Step 1: A step of distilling off the organic polar solvent from the reaction mixture obtained at the end of the reaction to obtain a solid component containing PAS.

[0074] Step 2: After step 1, a step of washing the solid content including PAS with water.

[0075] Step 3: After step 2, a step of washing PAS with an organic solvent to reduce the amount of chloroform extractable components in PAS to 1.7% by weight or less.

[0076] Step 4: After step 3, a step of distilling off the organic solvent used in step 3 while heating the mixture while flowing an inert gas at a flow rate of 0.2 L / min or more per 1 kg of PAS.

[0077] The following describes their details.

[0078] (7-1) Generation of PAS

[0079] In the present invention, a mixture containing at least a sulfiding agent, a dihalogenated aromatic compound, and an organic polar solvent is heated to react to produce PAS.

[0080] In the present invention, the temperature at which the mixture is heated to react cannot be generally specified because it depends on the type and amount of the raw materials used, but as the lower limit, 120°C or more can be exemplified, preferably 180°C or more can be exemplified, more preferably 220°C or more, and further preferably 240°C or more can be exemplified. On the other hand, as the upper limit, 350°C or less can be exemplified, preferably a range of 320°C or less can be exemplified, more preferably a range of 310°C or less, and further preferably a range of 300°C or less can be exemplified. If the temperature at which the mixture is heated to react is within the above preferred range, PAS showing normal physical properties can be obtained more efficiently.

[0081] Here, when the mixture is heated to react at a temperature exceeding the reflux temperature of the mixture at normal pressure, as a method of heating at such a temperature, for example, a method of heating the mixture at a pressure exceeding normal pressure; a method of adding the mixture to a pressure-resistant container, sealing and heating. In addition, the so-called normal pressure is a pressure near the standard state of the atmosphere, and the so-called standard state of the atmosphere is an atmospheric pressure condition near 101 kPa in absolute pressure at a temperature of about 25°C. In addition, the so-called reflux temperature is a temperature in which the liquid component of the mixture repeatedly boils and condenses. In addition, the reaction in the present invention can be any of a reaction carried out at a certain temperature, a multi-stage reaction in which the temperature is raised in stages, or a reaction in which the temperature is continuously changed.

[0082] In addition, the time of heating the mixture to react also depends on the type, amount or reaction temperature of the raw material used, so it can not be generally specified, but as the lower limit, it can be exemplified to be preferably more than 0.5 hour, more preferably more than 1 hour. In addition, as the upper limit, it can be exemplified to be preferably within 20 hours, more preferably within 10 hours. If the time of heating the mixture to react is the above-mentioned preferred scope, then the raw material can be fully reacted and consumed, and the manufacture of PAS can be carried out efficiently in a shorter time.

[0083] In addition, the pressure in the reaction system varies according to the raw materials, composition, reaction temperature, and the degree of progress of the reaction constituting the mixture, so it cannot be uniquely specified, but in the preferred mode implemented by the present invention, about the pressure at the reaction temperature of the present invention, as the lower limit, it can be exemplified as preferably 0.25MPa or more, more preferably 0.3MPa or more in gauge pressure. In addition, as the upper limit, it can be exemplified as preferably 5MPa or less, more preferably 3MPa or less, and further preferably 2MPa or less. If the pressure in the reaction system is the above-mentioned preferred range, there is a tendency that the sulfiding agent as a raw material and the dihalogenated aromatic compound react and consume rapidly, and in addition, there is a tendency to easily avoid the use of expensive pressure-resistant equipment. Here, in order to make the pressure in the reaction system the above-mentioned preferred range, it can be pressurized in the reaction system by an inert gas at any stage before the reaction starts, in the reaction, and preferably before the reaction starts. In addition, the so-called gauge pressure here is a relative pressure based on atmospheric pressure, which has the same meaning as the pressure difference obtained by subtracting atmospheric pressure from absolute pressure.

[0084] In the present invention, in order to generate PAS, a mixture containing at least a sulfiding agent, a dihalogenated aromatic compound, and an organic polar solvent is heated to react, and after the reaction is completed, step 1 is then implemented. The so-called "reaction completion" in the present invention refers to the state in which the reaction is carried out until the conversion rate of the added dihalogenated aromatic compound becomes 97% or more. By reacting the dihalogenated aromatic compound until such a conversion rate, and then implementing the later-described step 1, the amount of chloroform extractable components in the obtained PAS can be reduced. In addition, in the present invention, the reaction is considered to be completed at the moment when the conversion rate of the dihalogenated aromatic compound becomes 97% or more, but it is also preferred to adopt a method of further continuing the reaction to further increase the conversion rate of the dihalogenated aromatic compound. In this case, as a more preferred range of the conversion rate of the dihalogenated aromatic compound in the reaction, as a lower limit, it can be exemplified as more preferably 98% or more, and more preferably 98.5% or more. On the other hand, about the upper limit, for the convenience of the following calculation formula, sometimes also exceeds 100%, because it changes according to the amount of the dihalogenated aromatic compound used, and therefore cannot be generally stipulated, but the conversion rate under the situation that the dihalogenated aromatic compound used is completely converted can be said to be the preferred upper limit. When the conversion rate of dihalogenated aromatic compound is in the above-mentioned preferred range, there is a tendency that the amount of chloroform extraction components in the obtained PAS is further reduced. In addition, in the present invention, the residual amount of dihalogenated aromatic compound in the reaction solution is estimated by gas chromatography, and the conversion rate of dihalogenated aromatic compound is calculated by the ratio with the amount of the added sulfidizing agent or the added dihalogenated aromatic compound. The calculation formula is as follows.

[0085] (a) When the dihalogenated aromatic compound is used in excess of the sulfidizing agent in terms of molar ratio

[0086] Conversion rate of dihalogenated aromatic compound (%) = [amount of dihalogenated aromatic compound added (mol) - residual amount of dihalogenated aromatic compound (mol)] / amount of sulfiding agent added (mol) × 100

[0087] (b) Other than the above (a)

[0088] Conversion rate of dihalogenated aromatic compound (%) = [amount of dihalogenated aromatic compound added (mol) - residual amount of dihalogenated aromatic compound (mol)] / amount of dihalogenated aromatic compound added (mol) × 100

[0089] Here, the amount of the added sulfiding agent refers to the amount of the sulfiding agent present in the system at the start of the reaction. When a part of the sulfiding agent is removed to the outside of the system as hydrogen sulfide by a dehydration operation before the start of the reaction, the amount of the sulfiding agent present in the system at the start of the reaction is estimated based on the number of moles of hydrogen sulfide dispersed.

[0090] In addition, the amount of dihalogenated aromatic compound added refers to the amount of dihalogenated aromatic compound present in the system at the start of the reaction. When a part of the dihalogenated aromatic compound is removed to the outside of the system by dehydration operation before the start of the reaction, the amount of dihalogenated aromatic compound present in the system at the start of the reaction is estimated based on the number of moles scattered.

[0091] (7-2) Process 1

[0092] Step 1 in the present invention is a step of distilling off the organic polar solvent from the reaction mixture obtained by the reaction for producing PAS, thereby obtaining a solid component containing PAS. The solid material obtained by this operation contains not only PAS but also water-soluble substances such as by-product salts and unreacted sulfiding agents. This operation has a tendency to easily recover the organic polar solvent and to reduce the cost of producing PAS.

[0093] There is no particular limitation on the method for distilling off the organic polar solvent from the reaction mixture to obtain a solid component containing PAS, and examples thereof include a method of distilling off the organic polar solvent by heating the obtained reaction mixture to a temperature above the boiling point of the organic polar solvent; a method of heating the reaction mixture in a closed state using a pressure-resistant reactor having a take-out port at the bottom of the container, opening the take-out port at the bottom of the container from a state where the reaction mixture is heated to a temperature above the boiling point at normal pressure, and taking out the reaction mixture in a normal pressure or reduced pressure atmosphere, thereby instantaneously vaporizing the organic polar solvent and distilling it off (flash evaporation method), etc.

[0094] The temperature for distilling off the organic polar solvent in step 1 is not particularly limited as long as it is above the boiling point of the organic polar solvent used, but as the lower limit, it can be exemplified as preferably 200°C or more, more preferably 220°C or more, and further preferably a temperature exceeding 220°C. On the other hand, as the upper limit, it can be exemplified as preferably 250°C or less, more preferably 240°C or less. If the temperature for distilling off the organic polar solvent in step 1 is within the above-mentioned preferred range, the distillation of the organic polar solvent is completed in a relatively short time, and in addition, it is possible to prevent the particles of the generated PAS from fusing with each other, and the solid component obtained after flash evaporation does not become a large mass, but tends to be easy to handle. In addition, there is a tendency for the specific surface area of ​​the obtained PAS particles to increase, and by this effect, when the PAS is washed with an organic solvent in the later-described step 3, there is a tendency to make the amount of chloroform extractable components in the PAS easier to reduce. Here, the temperature for distilling off the organic polar solvent in step 1 does not refer to the temperature of the container, but to the internal temperature.

[0095] The pressure conditions when distilling off the organic polar solvent by heating the reaction mixture to a temperature higher than the boiling point of the organic polar solvent may be any of normal pressure, reduced pressure, and increased pressure, but reduced pressure is preferred. Under such preferred pressure conditions, the distillation rate of the organic polar solvent can be accelerated, and there is a tendency to obtain an additional effect of removing oligomer components and other volatile impurities together with the organic polar solvent.

[0096] In the case of adopting the flash method, the conditions are not particularly limited, but preferred conditions include, for example, a reaction mixture in a high temperature and high pressure state of usually 250° C. or higher and 0.8 MPa or higher is passed through a liquid having a flow rate adjusted to about 290° C. and 5 kg / cm3 at a flow rate of 50 kg / hr or higher and 5,000 kg / hr or lower. 2 Above and 20kg / cm 2 The method of releasing the reaction mixture into a gas stream of high-temperature and high-pressure steam as follows. The feed rate of the reaction mixture at this time is preferably in the range of 0.5 kg / hr or more and 5,000 kg / hr or less. Such a preferred method tends to efficiently remove oligomer components and other volatile impurities along with steam, and also tends to make the solid component obtained after flash evaporation not bulky but easy to handle in a powdery granular form.

[0097] In addition, the temperature of the container for taking out the reaction mixture in the flash method is not particularly limited as long as it is above the boiling point of the organic polar solvent used at normal pressure, but as the lower limit, it can be exemplified as preferably above 200°C, more preferably above 220°C. On the other hand, as the upper limit, it can be exemplified as preferably below 250°C, more preferably below 240°C. If the temperature of the container for taking out the reaction mixture in the flash method is in the above-mentioned preferred range, the distillation and removal of the organic polar solvent is completed in a relatively short time, and in addition, it has the tendency that the particles of the generated PAS can be prevented from fusing with each other, and the solid component obtained after the flash evaporation does not become a large mass, but tends to be easy to become a powdery granular form that is easy to handle. Furthermore, there is a tendency that the specific surface area of ​​the obtained PAS particles increases, and by this effect, when the PAS is washed with an organic solvent in the later-described step 3, there is a tendency that the amount of chloroform extractable components in the PAS is easily reduced.

[0098] As described above, the solid component containing PAS is obtained by distilling off the organic polar solvent from the reaction mixture obtained by the reaction in step 1, but as an advantage of this operation, the recovery of the organic polar solvent can be implemented at low cost. In the resulting reaction mixture, not only PAS but also water-soluble substances such as by-product salts and unreacted sulfiding agents are contained, so it is very necessary to implement water washing during the recovery of PAS, but the filtrate produced in this process is often mixed with water, water-soluble substances and organic polar solvents. In the case of recovering the organic polar solvent from such a filtrate by distillation operation, water is a substance with a large latent heat of evaporation, so it costs a lot of money, and as a result, there is a tendency that the manufacturing cost of PAS increases significantly. In the present invention, the above situation can be avoided by initially recovering the organic polar solvent, so PAS can be manufactured at low cost.

[0099] (7-3) Process 2

[0100] Step 2 in the present invention is a step of washing the solid content containing PAS with water to remove water-soluble substances after step 1. The solid content obtained after distilling off the organic polar solvent in step 1 contains not only PAS but also water-soluble substances such as by-product salts and unreacted sulfiding agent, so these water-soluble substances are removed by washing with water in the next step 2.

[0101] There is no particular limitation on the method of washing the solid component containing PAS with water to remove water-soluble substances. Examples thereof include a method of adding water to the solid component containing PAS to form a slurry, and then performing solid-liquid separation by filtering, centrifuging, etc., to separate and recover PAS as a solid component, thereby removing water-soluble substances to the filtrate side; a method of spreading PAS on a filter material and washing it with water from above, etc. In addition, in the above-mentioned slurrying operation, stirring is preferably performed from the viewpoint of efficiently removing water-soluble substances.

[0102] When the solid component comprising PAS is washed with water and water-soluble substances are removed, there is no particular restriction on the bath ratio (weight bath ratio) of the amount of water relative to the amount of PAS, but as the lower limit, in terms of the bath ratio relative to the weight of PAS, more than 1 can be exemplified, preferably more than 2 can be exemplified, and more preferably more than 3 can be exemplified. On the other hand, as the upper limit, less than 100 can be exemplified in terms of the bath ratio relative to the weight of PAS, preferably less than 50 can be exemplified, and more preferably less than 20 can be exemplified. If the bath ratio when the solid component comprising PAS is washed with water and water-soluble substances is removed is the above-mentioned preferred range, there is a tendency to efficiently remove water-soluble substances. In addition, in the case of carrying out solid-liquid separation by operations such as filtration and centrifugation after slurrying, there is a tendency to be able to process in a short time.

[0103] There is no particular restriction on the temperature (slurry temperature) when the solid component containing PAS is washed with water to remove the water-soluble substance. As the lower limit, 0°C or more can be exemplified, preferably 100°C or more can be exemplified, more preferably 150°C or more, further preferably 170°C or more, and further preferably 180°C or more can be exemplified. On the other hand, as the upper limit, 250°C or less can be exemplified, preferably 220°C or less can be exemplified, and more preferably 200°C or less can be exemplified. If the temperature when PAS is washed with water to remove the water-soluble substance is in the above-mentioned preferred range, there is a tendency that the water-soluble substance enclosed in the particles of PAS can also be efficiently extracted without excessively increasing the internal pressure of the device. In addition, there is no particular restriction on the method of raising the temperature to above the boiling point of water, and an example can be given, for example, a method of adding PAS and water to a pressure-resistant container for slurrying, sealing and heating.

[0104] In addition, the stirring time when the solid component containing PAS is washed with water and the water-soluble substance is removed is not particularly limited, and as the lower limit, more than 0.1 minute can be exemplified, preferably more than 1 minute. In addition, as the upper limit, less than 3 hours can be exemplified, preferably less than 1 hour. If the stirring time when PAS is washed with water and the water-soluble substance is removed is the above-mentioned preferred range, then there is a tendency that the water-soluble substance contained in PAS can be efficiently extracted.

[0105] In addition, there is no particular limitation on the temperature in the solid-liquid separation device when the solid component containing PAS is slurried with water and then subjected to solid-liquid separation by filtration, centrifugation, or the like. As a lower limit, 0° C. or higher, preferably 20° C. or higher, and more preferably 50° C. or higher can be exemplified. On the other hand, as an upper limit, 100° C. or lower can be exemplified. If the temperature in the solid-liquid separation device is within the above-mentioned preferred range, the solid-liquid separation operation can be performed using a simple device without being affected by the boiling point and melting point of water under normal pressure.

[0106] In addition, there is no particular limitation on the number of times the solid component containing PAS is washed with water to remove water-soluble substances. When the number of times of the operation is one, there is a tendency that water-soluble substances tend to remain in the mother liquor in the solid component obtained after separation, so it is preferred to perform the washing operation two or more times. By performing the washing operation multiple times, water-soluble substances can be further removed.

[0107] In addition, the atmosphere when the solid component containing PAS is washed with water to remove water-soluble substances is implemented under the atmosphere without any problem, but from the viewpoint of preventing the decomposition and oxidation of the terminal group, it is preferably carried out under non-oxidizing conditions. In this case, it is preferably an inert gas atmosphere such as nitrogen, helium, and argon, and in particular, from the viewpoint of economy and ease of operation, it is more preferably under a nitrogen atmosphere.

[0108] In addition, when the solid component containing PAS is washed with water, the method of adding acid to the water used for washing also has a tendency to reduce the metal content contained in PAS, and is preferably adopted. As long as the added acid is a substance that does not show the effect of oxidizing / decomposing / degrading PAS, there is no special restriction, and both inorganic acid and organic acid can be used. At this time, it is preferred to carry out acid washing under the condition that the slurry pH in the acid washing is less than 7, and the type and addition amount of the acid selected from the inorganic acid and organic acid are adjusted and controlled. As the acid added, examples such as acetic acid, hydrochloric acid, dilute sulfuric acid, phosphoric acid, silicic acid, carbonic acid and propyl acid (propil acid) can be exemplified, and these acids can be used alone or in combination. Among them, from the viewpoint of cost, acetic acid and hydrochloric acid are preferably used. In addition, it is preferred that after adding acid and washing with water, washing with water is usually carried out at least once by adding and implementing so that the added acid does not remain in PAS.

[0109] Furthermore, in order to suppress the decomposition and oxidation of the terminal groups of PAS, it is desirable that the atmosphere when washing PAS with water by adding an acid be an inert atmosphere.

[0110] In step 2, PAS is wetted by washing with water, but PAS can be dried afterwards. Since water is a poor solvent for the chloroform extract component in PAS, PAS is dried in advance in step 2, and when PAS is washed with an organic solvent in the next step 3, there is a tendency that the washing effect is easy to increase. In addition, when the organic solvent used in step 3 is water-insoluble, there is a tendency that the washing effect of PAS does not change whether it is in a dry state or a wet state, so it is not necessarily necessary to dry PAS in step 2.

[0111] In the case where PAS is washed with water and then dried in step 2, if the drying temperature is too high, the PAS particles are fused to each other and the specific surface area becomes smaller, and a sufficient washing effect cannot be exerted in the later step 3. Therefore, as the lower limit of the drying temperature, it can be exemplified that it is preferably 70°C or more, more preferably 100°C or more, and further preferably 120°C or more. In addition, as the upper limit, it can be exemplified that it is preferably 170°C or less, and more preferably 150°C or less. If the drying temperature of PAS is in the above-mentioned preferred range, the specific surface area of ​​the dried PAS becomes larger, and it is easy to fully wash and remove the extracting components in the chloroform in the PAS in the later step 3. In addition, there is a tendency to be able to dry efficiently in a short time. In addition, the atmosphere during drying is preferably a non-oxidizing condition, preferably an inert gas atmosphere such as nitrogen, helium, and argon, and in particular, from the viewpoint of economy and ease of operation, it is more preferably a nitrogen atmosphere. By drying PAS in such an atmosphere, there is a tendency to prevent the modification caused by oxidation of PAS.

[0112] In addition, when PAS is washed with water and dried in operation 2, the time is not particularly limited, but as the lower limit, more than 0.5 hours can be exemplified, and preferably more than 1 hour can be exemplified. In addition, as the upper limit, less than 50 hours can be exemplified, preferably less than 20 hours can be exemplified, and more preferably less than 10 hours. If the drying time of PAS is the above-mentioned preferred range, PAS can be efficiently manufactured industrially.

[0113] Here, when the PAS is washed with water and then dried in step 2, there is no particular limitation on the dryer used, and a general vacuum dryer, hot air dryer, a rotary or stirring blade heating device, a fluidized bed dryer, etc. can be used. In addition, from the viewpoint of efficiently and uniformly drying the PAS, it is preferred to use a rotary or stirring blade heating device for drying.

[0114] (7-4) Process 3

[0115] Step 3 in the present invention is a step of washing PAS with an organic solvent after step 2 to make the amount of chloroform extractable components in PAS less than 1.7 wt %. When PAS is manufactured by the preferred method of the present invention (particularly, there is a tendency to be affected by the amount of organic polar solvent used during the reaction), the amount of chloroform extractable components in PAS is often 2.0 wt % or more and 5.0 wt % or less at the time of finishing step 2. As described above, since the chloroform extractable components in the PAS are confirmed to be the main cause of mold contamination during the molding of PAS, the content of the chloroform extractable components in the PAS is reduced by implementing step 3, thereby reducing mold contamination during molding.

[0116] In operation 3, it is necessary to wash PAS with an organic solvent so that the chloroform extraction component amount in PAS is below 1.7 % by weight. When the chloroform extraction component amount in PAS exceeds 1.7 % by weight, the mold pollution during the PAS molding process is not clearly improved, and the effect of the present invention cannot be obtained. In addition, as the lower limit of the chloroform extraction component amount in PAS, the less the more preferred from the viewpoint of reducing mold pollution, the 0 % by weight that the chloroform extraction component does not include in PAS at all is the most preferred. On the other hand, as the upper limit, it is more preferably below 1.2 % by weight, and further preferably below 0.9 % by weight. If the chloroform extraction component amount in PAS is the above-mentioned preferred scope, the mold pollution during the PAS molding process is more clearly improved.

[0117] The organic solvent used for washing PAS in step 3 is not particularly limited as long as it has high solubility in the chloroform extract component in PAS and low solubility in PAS and does not oxidize / decompose / degrade PAS. Examples thereof include amide-based polar solvents such as N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, and dimethylimidazolidinone; sulfoxide / sulfone-based solvents such as dimethyl sulfoxide and dimethyl sulfone; ketone-based solvents such as acetone, methyl ethyl ketone, diethyl ketone, and acetophenone; ether-based solvents such as dimethyl ether, diethyl ether, dipropyl ether, tetrahydrofuran, and diphenyl ether; ester-based solvents such as methyl acetate, ethyl acetate, and butyl acetate; nitrile-based solvents such as acetonitrile; chloroform, dichloromethane, and the like. Halogen solvents such as alkane, trichloroethylene, dichloroethylene, 1,2-dichloroethane, tetrachloroethane, chlorobenzene, 1-chloronaphthalene, etc., alcohol / phenol solvents such as methanol, ethanol, propanol, isopropanol, butanol, amyl alcohol, ethylene glycol, propylene glycol, phenol, cresol, polyethylene glycol, etc., aliphatic / aromatic hydrocarbon solvents such as n-hexane, cyclohexane, benzene, toluene, p-xylene, etc., among which N-methyl-2-pyrrolidone, dimethylformamide, tetrahydrofuran, chloroform, 1-chloronaphthalene, toluene, p-xylene can be preferably used because they have a tendency to have high solubility in the chloroform extraction component in PAS, and further, from the viewpoint of easy availability, N-methyl-2-pyrrolidone, which is often used as a polymerization solvent for PAS, is particularly preferably used. In addition, these organic solvents can be used alone, but can also be used as a mixed solvent of two or more.

[0118] Here, the amount of chloroform extractable components in PAS in the present invention is measured by the following method. First, 10 g of PAS is weighed and Soxhlet extraction is performed with 100 g of chloroform for 3 hours. The weight after chloroform is distilled off from the extract is measured, and the ratio relative to the weight of the charged polymer is obtained as the amount of chloroform extractable components.

[0119] In addition, step 4 in the present invention is a step of distilling off the organic solvent used in step 3 by heating while flowing an inert gas, but when step 4 is performed under the preferred conditions of the present invention, there is almost no change in the amount of chloroform-extractable components in PAS before and after the performance of step 4. Therefore, the amount of chloroform-extractable components in PAS after the performance of step 3 in the present invention was evaluated by the amount of chloroform-extractable components in PAS after the performance of step 4.

[0120] In addition, in process 3, the water content of PAS before washing with an organic solvent is preferably 30% by weight or less. Since water is a poor solvent for the chloroform extraction component in PAS, it is preferred to reduce the water content of PAS in advance so that the chloroform extraction component is easier to reduce when PAS is washed with an organic solvent. In addition, when the organic solvent used for washing PAS in process 3 is a water-insoluble organic solvent such as chloroform and toluene, it is possible to obtain a stable washing effect regardless of the water content of PAS, so it is not necessary to make the water content of PAS less than 30% by weight, but if N-methyl-2-pyrrolidone, which is a particularly preferred washing solvent from the viewpoint of ease of acquisition, is a water-soluble organic solvent, it can be said that reducing the water content in PAS in advance is a more preferred method. Here, as the lower limit of the water content of PAS before washing with an organic solvent, the less the better in order to improve the washing effect, and 0% by weight, which does not contain any water at all in PAS, is the most preferred. On the other hand, as the upper limit, it is more preferably 10 wt % or less, further preferably 5 wt % or less, and further preferably 1 wt % or less can be exemplified. In operation 3, if the moisture content of PAS before washing with an organic solvent is within the above-mentioned preferred range, when a water-soluble organic solvent is used for washing PAS, there is a tendency to make the chloroform extractable component amount in PAS more easily reduced. In addition, as a method for making the moisture content below 30 wt %, a method for drying PAS after washing with water in operation 2 as described above can be cited.

[0121] Here, the water content of PAS in the present invention is measured in accordance with Japanese Industrial Standard JIS K 7251 using the Karl Fischer method.

[0122] Generally, it is known that in the operation of washing particles with a solvent, the larger the specific surface area of ​​the particles, the higher the washing efficiency tends to be, and the washing in step 3 of the present invention also has such a tendency. Specifically, in step 3, the specific surface area of ​​PAS before washing with an organic solvent can be exemplified as preferably 5 m 2 / g or more, more preferably 8m 2 / g or more, more preferably 10m 2 On the other hand, as the upper limit, preferably 50 m 2 In step 3, if the specific surface area of ​​PAS before washing with an organic solvent is within the above preferred range, when PAS is washed with an organic solvent, the amount of chloroform extractable components in PAS tends to be more easily reduced.

[0123] In addition, as described above, the specific surface area of ​​PAS before washing with an organic solvent in step 3 can be adjusted by the temperature at which the organic polar solvent is distilled off from the reaction mixture in step 1, the drying temperature when drying after washing PAS with water in step 2, and the like. As the lower limit of the temperature at which the organic polar solvent is distilled off from the reaction mixture in step 1, it is preferably 200° C. or higher, and more preferably 220° C. or higher. On the other hand, as the upper limit, it is preferably 250° C. or lower, and more preferably 240° C. or lower. If the temperature at which the organic polar solvent is distilled off from the reaction mixture in step 1 is within the above-mentioned preferred range, there is a tendency that the particles of PAS can be prevented from fusing with each other, and the specific surface area of ​​PAS before washing with an organic solvent in step 3 can be adjusted to the above-mentioned preferred range. In addition, as described in step 2 (7-3), the drying temperature when drying after washing PAS with water is preferably 70° C. or higher and 170° C. or lower. When the drying temperature is within the above-mentioned preferred range after washing PAS with water in step 2 and then drying it, the particles of PAS can be prevented from fusing with each other, and the specific surface area of ​​PAS before washing with an organic solvent in step 3 tends to be easily adjusted to the above-mentioned preferred range.

[0124] Here, the specific surface area of ​​PAS in the present invention is determined by measuring PAS in a 0.2 g glass cell, degassing under reduced pressure at room temperature for 5 hours, measuring by krypton gas adsorption method, and analyzing by BET multipoint method.

[0125] There is no particular limitation on the method of removing the chloroform extract component in PAS by washing PAS with an organic solvent. Examples thereof include a method of removing the chloroform extract component in PAS to the filtrate side by adding an organic solvent to PAS to form a slurry, performing solid-liquid separation by filtering, centrifuging, etc., separating and recovering PAS as a solid component; and a method of spreading PAS on a filter material and washing it by pouring an organic solvent from above. In addition, in the above-mentioned slurrying operation, stirring is preferably performed from the viewpoint of efficiently removing the chloroform extract component in PAS.

[0126] When PAS is washed with an organic solvent to remove the chloroform extraction component in PAS, there is no particular restriction on the bath ratio (weight bath ratio) of the amount of organic solvent relative to the amount of PAS, but as a lower limit, it can be exemplified as 1 or more, preferably 2 or more, and more preferably 3 or more, in terms of the bath ratio relative to the weight of PAS. On the other hand, as an upper limit, it can be exemplified as 100 or less, preferably 50 or less, and more preferably 20 or less, in terms of the bath ratio relative to the weight of PAS. If the bath ratio when PAS is washed with an organic solvent to remove the chloroform extraction component in PAS is the above-mentioned preferred range, there is a tendency that the chloroform extraction component in PAS can be efficiently removed. In addition, when solid-liquid separation is performed by filtering, centrifugal separation, etc. after slurrying, there is a tendency that it can be processed in a short time.

[0127] There is no particular restriction on the temperature (slurry temperature) when PAS is washed with an organic solvent to remove the chloroform extraction component in PAS, but as a lower limit, it can be exemplified as 0°C or above, preferably 20°C or above, and more preferably 60°C or above. On the other hand, as an upper limit, it can be exemplified as 300°C or below, preferably 250°C or below, more preferably 200°C or below, and further preferably 150°C or below. If the temperature when PAS is washed with an organic solvent to remove the chloroform extraction component in PAS is in the above-mentioned preferred range, there is a tendency that the chloroform extraction component in PAS can be efficiently extracted without excessively increasing the pressure. In addition, when PAS is slurried with an organic solvent and solid-liquid separation is performed by filtration, centrifugation, etc., there is a tendency that the solid-liquid separation rate is increased and can be efficiently processed. In addition, there is no particular restriction on the method of raising the temperature to above the boiling point of the organic solvent, and an example can be given, for example, a method in which PAS and an organic solvent are added to a pressure-resistant container to slurry, sealed and heated.

[0128] In addition, the stirring time when the chloroform extraction component in PAS is removed by washing with an organic solvent is not particularly limited, but as the lower limit, more than 0.1 minute can be exemplified, preferably more than 1 minute, and more preferably more than 5 minutes. In addition, as the upper limit, less than 3 hours can be exemplified, preferably less than 1 hour, and more preferably less than 30 minutes. If the stirring time when the chloroform extraction component in PAS is removed by washing with an organic solvent is the above-mentioned preferred range, there is a tendency that the chloroform extraction component can be efficiently extracted.

[0129] In addition, there is no particular restriction on the temperature in the solid-liquid separation device when the solid-liquid separation is performed by filtering, centrifugation and other operations after the PAS is slurried with an organic solvent, but as a lower limit, 0°C or more can be exemplified, preferably 20°C or more can be exemplified, and more preferably 60°C or more. On the other hand, as an upper limit, 300°C or less can be exemplified, preferably 250°C or less can be exemplified, more preferably 200°C or less, and further preferably 150°C or less can be exemplified. If the temperature in the solid-liquid separation device is in the above-mentioned preferred range, it is possible to use a simple device to perform the solid-liquid separation operation without using expensive pressure-resistant equipment. In addition, there is a tendency that the solid-liquid separation speed is increased and can be processed efficiently.

[0130] Here, as a specific operation of solid-liquid separation, operations such as filtration and centrifugation can be cited, but in order to reduce the amount of mother liquor contained in the solid component obtained after solid-liquid separation, a method of pressurizing the solid component after solid-liquid separation is also preferably adopted. By additionally performing such an operation, there is a tendency that the amount of mother liquor contained in the solid component is reduced, and the chloroform extract component in PAS contained in PAS tends to be more easily reduced.

[0131] In addition, there is no particular limitation on the number of times the chloroform extract component in PAS is removed by washing PAS with an organic solvent, but when the number of times of the operation is one, there is a tendency that the chloroform extract component in PAS is likely to remain due to the mother liquor in the solid component obtained after separation, so it is preferred to perform the washing operation two or more times. By performing the washing operation multiple times in this way, the chloroform extract component can be further removed.

[0132] In addition, the atmosphere when washing PAS with an organic solvent to remove the chloroform extraction component in PAS can be implemented under the atmosphere without any problem, but from the viewpoint of preventing the decomposition and oxidation of the terminal group, it is preferably carried out under non-oxidizing conditions. In this case, it is preferably an inert gas atmosphere such as nitrogen, helium, and argon, and in particular, from the viewpoint of economy and ease of operation, it is more preferably under a nitrogen atmosphere.

[0133] (7-5) Process 4

[0134] Step 4 in the present invention is a step of heating after step 3 while flowing an inert gas at a flow rate of 0.2 L / min or more per 1 kg of PAS, thereby distilling off the organic solvent used in step 3. By performing step 4, PAS with less mold contamination during molding, excellent melt fluidity, and high reactivity with a coupling agent can be obtained.

[0135] In process 4, when the organic solvent used in process 3 is distilled off by heating under the condition that the flow rate of the inert gas is less than 0.2L / min per 1kgPAS, there is a tendency that PAS is easily thermally modified, and the reactivity of PAS with the coupling agent is reduced, and the hydrolysis resistance of the composite obtained by melt-mixing with other resins and inorganic fillers is not easy to increase. Here, as the lower limit of the flow rate of the inert gas when the organic solvent is distilled off in process 4, it can be exemplified as preferably 0.4L / min or more, and more preferably 0.8L / min or more. In addition, as an upper limit, it can be exemplified as preferably 50L / min or less, and more preferably 25L / min or less. If the flow rate of the inert gas when the organic solvent is distilled off in process 4 is the above-mentioned preferred range, the thermal modification of PAS can be further suppressed, and there is a tendency that the hydrolysis resistance of the composite obtained by melt-mixing with other resins and inorganic fillers is further improved. In addition, the hydrolysis resistance of PAS in the present invention is evaluated by first performing extrusion molding (cylinder temperature 320°C, adding: PAS: 60 parts by weight, chopped glass fiber (T-760H manufactured by Nippon Denki Glass Co., Ltd.): 40 parts by weight, epoxy silane coupling agent 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (KBM-303 manufactured by Shin-Etsu Silicone Co., Ltd.)) to produce pellets. Then, the obtained pellets are used to perform injection molding in accordance with ASTM standard (D-638), and the tensile strength of the obtained test piece is measured. Then, the test piece is immersed in a liquid X composed of 54% water, 45% ethylene glycol, 0.5% dipotassium phosphate, and 0.5% diethylene glycol at 150°C for 168 hours. For the test piece after immersion for 168 hours, the tensile strength is measured and the strength retention rate of the tensile strength is calculated. This strength retention rate is used as the hydrolysis resistance of PAS for evaluation.

[0136] Here, the so-called inert gas is a stable gas that does not undergo chemical reaction. It is preferred to use nitrogen, helium, argon, but particularly from the viewpoint of economy and ease of operation, it is more preferred to use nitrogen. In addition, about the oxygen concentration in the device for distilling off the organic solvent in operation 4, owing to making the inert gas flow, there is a tendency to inevitably become low concentration, but as the lower limit of the oxygen concentration in the device, the lower the more preferred in order to prevent the oxidation of PAS, 0 volume % that does not contain oxygen at all in the device is the most preferred. On the other hand, as the upper limit, it can be exemplified as preferably less than 1 volume %, more preferably less than 0.1 volume %, and further preferably less than 0.01 volume %. If the oxygen concentration in the device for distilling off the organic solvent in operation 4 is the above-mentioned preferred range, there is a tendency to prevent the modification caused by the oxidation of PAS.

[0137] In addition, there is no particular limitation on the pressure in the device for distilling off the organic solvent in step 4, and any of normal pressure, reduced pressure, and pressurized conditions may be used. However, since it is necessary to introduce expensive equipment that can withstand the pressure environment in order to adopt reduced pressure or pressurized conditions, it is preferably normal pressure from the perspective of more economical production of PAS. The so-called normal pressure here refers to a pressure near the standard state of the atmosphere, which is an atmospheric pressure condition near 101 kPa in absolute pressure at a temperature near about 25°C.

[0138] In step 4, the temperature for distilling off the organic solvent is not particularly limited, but the lower limit may be 70° C. or higher, preferably 100° C. or higher, and more preferably 120° C. or higher. The upper limit may be 250° C. or lower, and more preferably 230° C. or lower. When the drying temperature of PAS is within the above preferred range, there is a tendency that PAS can be dried efficiently in a short time without fusing.

[0139] In addition, the time for distilling off the organic solvent in step 4 is not particularly limited, but as the lower limit, it can be exemplified as more than 0.1 hours, and it can be exemplified as preferably more than 1 hour. In addition, as the upper limit, it can be exemplified as less than 50 hours, and it can be exemplified as preferably less than 20 hours, and more preferably less than 10 hours. If the drying time of PAS is the above-mentioned preferred range, the thermal modification of PAS can be suppressed, and it can be manufactured efficiently in industry.

[0140] Here, the dryer used for distilling and removing the organic solvent in step 4 is not particularly limited, and a general vacuum dryer, hot air dryer, a rotary or stirring blade heating device, a fluidized bed dryer, etc. can be used. In addition, from the viewpoint of efficiently and uniformly drying PAS, it is preferred to use a rotary or stirring blade heating device for drying.

[0141] In addition, when the boiling point of the organic solvent used for washing in step 3 is high, the treatment of distilling and removing the organic solvent in step 4 tends to be high temperature and long time. Therefore, in order to reduce this tendency, it is also preferred to adopt a method in which the organic solvent contained in PAS is replaced with other solvents with lower boiling points before performing step 4 and then dried. Here, the solvent for replacement is not particularly limited as long as it is a solvent mixed with the solvent used for washing, but water and acetone are often preferred from the viewpoint of being cheaply available and having a lower boiling point. As a method for replacing the organic solvent contained in PAS with other solvents with lower boiling points, there can be exemplified a method in which a solvent for replacement is added to PAS and slurried, and then solid-liquid separation is performed by filtering, centrifugal separation, etc.; a method in which PAS is spread on the filter material and the solvent for replacement is poured from above for washing, etc. This operation can be effective even if it is performed only once, but by performing it more than twice, the solvent replacement is further promoted, so that it is easier to make the drying process low temperature and short time.

[0142] In addition, step 4 in the present invention is a step of distilling off the organic solvent used in step 3 by heating while flowing an inert gas, but when step 4 is performed under the preferred conditions of the present invention, there is almost no change in the amount of chloroform-extractable components in PAS before and after the performance of step 4. Therefore, the amount of chloroform-extractable components in PAS after the performance of step 3 in the present invention can be evaluated by the amount of chloroform-extractable components in PAS after the performance of step 4.

[0143] (8) Other post-processing

[0144] The PAS obtained in this way has sufficiently little mold contamination during molding. However, in order to further reduce mold contamination, a method (aging method) of additionally subjecting the PAS obtained after the step 4 to heat treatment may be preferably adopted.

[0145] The temperature at which the PAS obtained after the implementation of step 4 is subjected to additional heat treatment is not particularly limited, but as a lower limit, 150° C. or more can be exemplified, and preferably 160° C. or more can be exemplified. In addition, as an upper limit, 270° C. or less can be exemplified, and preferably 260° C. or less can be exemplified. If the temperature at which the PAS is subjected to heat treatment is within the above-mentioned preferred range, there is a tendency that mold contamination generated during the molding of the PAS can be further reduced without excessively thermally modifying the PAS. In addition, there is a tendency that the PAS can be easily subjected to uniform heat treatment without fusing it.

[0146] In addition, the time for heat treatment of the PAS obtained after the operation 4 is implemented is not particularly limited, but as the lower limit, more than 0.2 hours can be exemplified, and preferably more than 0.3 hours can be exemplified. In addition, as the upper limit, less than 50 hours can be exemplified, preferably less than 10 hours can be exemplified, and more preferably less than 6 hours. If the time for heat treatment of PAS is the above-mentioned preferred range, there is a tendency to further reduce the mold contamination generated during the molding of PAS without excessive thermal modification of PAS.

[0147] Here, in the case of heat treatment of the PAS obtained after the implementation of operation 4, there is no particular restriction on the device used, and a general vacuum dryer, hot air dryer, a rotary or stirring blade heating device, a fluidized bed dryer, etc. can be used. In addition, from the viewpoint of making PAS efficiently and uniformly heat-treated, it is preferred to use a rotary or stirring blade heating device for heat treatment. In addition, from the viewpoint of preventing the decomposition and oxidation of the terminal group, the atmosphere when the PAS obtained after the implementation of operation 4 is heat-treated is preferably heat-treated under non-oxidizing conditions, and the heat treatment is sometimes carried out for the purpose of improving the melt viscosity of PAS, and in this case, it is sometimes heat-treated under an atmosphere containing a certain degree of oxygen. As the oxygen concentration in this case, as the lower limit, more than 0.5 volume % can be exemplified, and preferably more than 1 volume % can be exemplified. On the other hand, as the upper limit, less than 50 volume % can be exemplified, less than 25 volume % can be exemplified, and more preferably less than 15 volume % can be exemplified. If the oxygen concentration in the atmosphere when carrying out the heat treatment of PAS is the above-mentioned preferred scope, then there is a tendency that the melt viscosity of PAS is easily controlled to the desired viscosity when PAS is not excessively thermally modified. In addition, from the viewpoint of efficiently carrying out heat treatment, the airflow when the PAS obtained after the operation 4 is implemented is additionally heat treated preferably flows through the airflow with a certain degree of flow velocity. As this flow velocity, as the lower limit, it can be illustrated that it is more than 0.1L / minute relative to resin 1kg. On the other hand, as the upper limit, it can be illustrated that it is less than 50L / minute relative to resin 1kg, it can be illustrated that it is preferably less than 30L / minute, more preferably less than 15L / minute. If the flow velocity of the airflow when carrying out the heat treatment of PAS is the above-mentioned preferred scope, then there is a tendency that PAS can be efficiently heat treated.

[0148] (9) Characteristics of PAS obtained in the present invention

[0149] The PAS obtained by the method of the present invention has the characteristic of less mold pollution because the oligomer components with relatively low volatility (high boiling point) that adhere to / accumulate on the mold during the molding process are reduced. As a result, the maintenance frequency of the mold used in the PAS molding process can be reduced, and the productivity of the PAS molding process can be expected to be improved. In addition, the PAS obtained by the method of the present invention does not cause the problem of blurring the lens parts present in the surroundings when used in applications such as car headlight reflectors and projector peripheries at high temperatures, so it can be preferably used for these applications. Here, regarding the evaluation of mold contamination of PAS in the present invention, first, extrusion molding (cylinder temperature 320°C, adding: PAS: 60 parts by weight, chopped glass fiber (T-760H manufactured by Nippon Denki Glass Co., Ltd.): 40 parts by weight) was performed to produce pellets, and then the obtained pellets were supplied to an injection molding machine (SE-30D) manufactured by Sumitomo Heavy Industries, Ltd. at a cylinder temperature of 325°C, and a mold for gas evaluation with molded product dimensions: maximum length 55 mm, width 20 mm, thickness 2 mm, gate dimensions: width 2 mm, thickness 1 mm (side gate), gas venting part maximum length 20 mm, width 10 mm, depth 5 μm was heated to 130°C and allowed to stand, and continuous molding was performed 1,000 times. Then, the attached matter on the gas venting part was recovered and weighed for evaluation.

[0150] In addition, the PAS obtained by the method of the present invention has a tendency that the relatively volatile oligomer components that are not attached / deposited on the mold during the molding process are also reduced, and the amount of gas generated during heating is also reduced. Specifically, there is a tendency that the amount of gas captured when the PAS is heated at 320°C for 2 hours is more than 0.10% by weight and less than 0.75% by weight relative to the weight of the added PAS. Since the gas generated when the PAS is heated is a substance that causes bad odor, it is preferred that the amount of gas of the PAS obtained in the present invention is reduced to the above range, thereby also obtaining the effect of improving the working environment during the PAS molding process. Here, the gas generation of the PAS in the present invention is measured as follows: First, 3g of PAS is added to a glass ampoule with a belly of 100mm×25mmφ, a neck of 255mm×12mmφ, and a wall thickness of 1mm for vacuum sealing. Next, the body of the ampoule was inserted into an ARF-30K ceramic electric heating tube furnace manufactured by Asahika Seisakusho Co., Ltd., and heated at 320°C for 2 hours with the neck of the ampoule protruding out of the tube furnace. The ampoule was then taken out, and the neck of the ampoule to which the gas component adhered was cut off with a file to measure the weight. Furthermore, the cut neck was washed with chloroform, and the weight was measured again after drying. The value obtained by dividing the weight difference of the cut neck before and after chloroform washing by the original weight of PAS was used as the gas generation amount for evaluation.

[0151] If the molecular weight of the PAS obtained by the method of the present invention is measured by gel permeation chromatography (GPC), which is a type of size exclusion chromatography (SEC), it is known that the molecular weight distribution shows a characteristic shape that cannot be observed in the existing PAS. Specifically, it shows a shape of molecular weight distribution in which the cumulative integral value of the molecular weight of 4,000 is 48 or more and 53 or less when the cumulative integral value of the molecular weight of 100 to 10,000 in the molecular weight distribution curve is set to 100. For example, the method for manufacturing PAS using the quenching method as shown in Patent Document 2 performs the following operation: by slowly cooling after injecting water into the system after polymerizing PAS and before the PAS particles precipitate, the PAS particle size is greatly grown, but if such a treatment is performed, the PAS particles are easily porous, and by washing with an organic solvent, there is a tendency that even the oligomer components that are not the cause of mold contamination are excessively washed and removed. The PAS obtained by the quenching method shows a molecular weight distribution shape in which the cumulative integral value of the molecular weight 4,000 is less than 48 when the cumulative integral value of the molecular weight 100 to 10,000 in the molecular weight distribution curve is set to 100, and has a tendency to become a material with low melt fluidity and low molding processability although there is little mold contamination during molding. On the other hand, the method for producing PAS using the flash distillation method as shown in Patent Document 3 flashes the reaction system in a high temperature state into a container under normal pressure or reduced pressure after polymerizing PAS to distill off the polymerization solvent, but it is widely recognized that the biggest advantage of this method is that PAS can be produced cheaply, and the idea of ​​using an organic solvent for washing is not considered to be incurring additional costs. The PAS obtained by the flash distillation method shows a molecular weight distribution shape in which the cumulative integral value of the molecular weight 4,000 is greater than 53 when the cumulative integral value of the molecular weight 100 to 10,000 in the molecular weight distribution curve is set to 100, and has a tendency to become a material with high melt fluidity but high mold contamination during molding. Compared with the above-mentioned conventional PAS, the PAS obtained by the method of the present invention is a material that has both less mold contamination during molding and high melt fluidity, and can be said to be a material with better molding processability. Here, the melt fluidity of the PAS in the present invention is evaluated by measuring the melt flow rate (resin discharge per 10 minutes) according to ASTM-D1238-70 and comparing the values.

[0152] In addition, regarding the PAS obtained by the method of the present invention, when the melt flow rate of PAS is set to MFR1, and the melt flow rate after mixing PAS with an epoxy silane coupling agent at a weight ratio of 100:1 and heating at 315.5°C for 5 minutes is set to MFR2, the rate of change represented by MFR2 / MFR1 becomes less than 0.085. This means that the melt viscosity increases due to the reaction of PAS with the epoxy silane coupling agent, and the smaller the rate of change, the greater the melt viscosity. In the case where the rate of change represented by MFR2 / MFR1 exceeds 0.085, there is a problem of poor hydrolysis resistance when melt-kneading with other resins and inorganic fillers to form a composite. In order to obtain such a PAS, it is necessary to heat while causing an inert gas to flow at a flow rate of more than 0.2L / min per 1kg of PAS in step 4 of the present invention, thereby distilling off the organic solvent used in step 3. In this way, PAS, which reacts with epoxy silane coupling agent and greatly increases melt viscosity, has a tendency to improve hydrolysis resistance when melt-kneading with other resins and inorganic fillers to form a composite, and can be preferably used in applications requiring hydrolysis resistance. Here, there is no particular restriction on the lower limit of the rate of change represented by MFR2 / MFR1, but it can be exemplified as more than 0.0001, preferably more than 0.001, and more preferably more than 0.002. In addition, as an upper limit, it can be exemplified as less than 0.085 as described above, preferably less than 0.070, and more preferably less than 0.060. If the rate of change represented by MFR2 / MFR1 is the above-mentioned preferred range, then when PAS is melt-kneaded with other resins and inorganic fillers to form a composite, it has a tendency to further improve hydrolysis resistance, and can be particularly preferably used in applications requiring hydrolysis resistance. Here, the rate of change represented by MFR2 / MFR1 in the present invention is obtained by first measuring the melt flow rate of PAS according to ASTM-D1238-70 to obtain MFR1, then measuring the melt flow rate of a mixture of 1 g of PAS and 0.01 g of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (KBM-303 manufactured by Shin-Etsu Silicone) using a mortar and pestle to obtain MFR2, and calculating MFR2 / MFR1.

[0153] In addition, the PAS obtained by the method of the present invention preferably has a particle shape, and the median particle size D50 of the PAS particles is more than 1 μm and less than 400 μm. In order to achieve such a particle size, if polymerization is performed by flash evaporation, the particles are generated instantaneously, and crystal growth will not be fully carried out, so the median particle size D50 of the particles can be easily controlled within the above-mentioned preferred range. After the process 1 (flash evaporation) of the present invention is performed, the median particle size D50 is determined by several changes such as agglomeration and fusion of the particles during processes 2, 3, and 4. The PAS obtained in the present invention has a small particle size compared with the existing PAS manufactured by the quenching method, but such PAS has a tendency to melt more quickly and be easy to homogenize when melt-kneading with other resins and inorganic fillers.

[0154] Here, the median particle size D50 of PAS in the present invention is measured using a laser particle size distribution analyzer using N-methyl-2-pyrrolidone as a dispersion solvent.

[0155] In addition, the PAS obtained by the method of the present invention has a tendency to have a cooling crystallization temperature of 210°C or more and 250°C or less. The PAS obtained by the method of the present invention has a tendency to have high crystallinity compared to general PAS, so it can be particularly preferably used in the injection molding of resins. In general, for injection molding, it is known that the slower the cooling rate in the cooling crystallization temperature zone during cooling / solidification from a molten state, the more crystallization is promoted. In order not to speed up the cooling rate, the mold temperature of resins with low crystallinity is often set high, but the PAS obtained by the method of the present invention has a tendency to have high crystallinity, so crystallization is also fully carried out at a relatively low mold temperature, and PAS can be efficiently molded. The cooling crystallization temperature of the PAS obtained by the preferred method of the present invention varies according to the polymerization conditions and washing conditions, but as a lower limit, it has a tendency to be above 210°C, and a tendency to be above 220°C is greater. In addition, as an upper limit, it has a tendency to be below 250°C, and a tendency to be below 240°C is greater.

[0156] In addition, the PAS obtained by the method of the present invention has a tendency to have a high crystallinity in the powder state before the molding process, so it can also be preferably used in the use of PAS directly in the powder state, such as fillers, adsorbents, and coatings. In general, as a post-treatment method to improve the crystallinity of PAS, it is known that a method of annealing at a temperature slightly higher than the glass transition temperature is performed, but if PAS is washed with an organic solvent in step 3 of the present invention, it is observed that the solvent penetrates into the interior of the PAS particles and the solvent crystallization proceeds, and the tendency of the crystallinity of PAS increases. Therefore, the PAS obtained in the present invention has a high crystallinity even if the annealing treatment is not performed, so it can be preferably used as a powdery resin material with excellent heat resistance, chemical resistance, and mechanical properties.

[0157] In addition, the PAS obtained by the method of the present invention can be used not only for injection molding of resins, but also can be widely used as resin extrusion molding, fiber, sheet, film and tube molded products. The PAS obtained by the method of the present invention also plays an effect of reducing contamination of the die and punch die when molding fibers, sheets, films and tube shapes.

[0158] The PAS obtained by the method of the present invention can be used alone, or inorganic fillers such as glass fiber, carbon fiber, titanium oxide, calcium carbonate, antioxidants, heat stabilizers, ultraviolet absorbers, colorants, etc. can be added as desired, and other resins such as polyamide, polysulfone, polyphenylene, polycarbonate, polyethersulfone, polyethylene terephthalate, polybutylene terephthalate, polyethylene, polypropylene, polytetrafluoroethylene, olefin copolymers with functional groups such as epoxy, carboxyl, carboxylate, anhydride, polyolefin elastomers, polyether ester elastomers, polyether amide elastomers, polyamide-imide, polyacetal, polyimide, etc. can be used. By mixing these materials, there is a tendency that the material properties such as heat resistance and mechanical strength are improved.

[0159] Example

[0160] The present invention will be described in detail below with reference to Examples. These examples are for illustrative purposes only and are not intended to limit the present invention.

[0161] <Determination of the amount of dihalogenated aromatic compounds>

[0162] The amount of the dihalogenated aromatic compound in the reaction liquid (for example, the quantitative determination of p-dichlorobenzene) was carried out using gas chromatography (GC) under the following conditions.

[0163] Equipment: GC-2010 manufactured by Shimadzu Corporation

[0164] Column: DB-5 0.32 mm × 30 m (0.25 μm) manufactured by J&W Scientific

[0165] Carrier gas: Helium

[0166] Detector: Flame ionization detector (FID).

[0167] <Specific surface area measurement>

[0168] The specific surface area of ​​PAS (m 2 The measurement of PAS was carried out by adding PAS to 0.2 g of a glass cell and degassing under reduced pressure at room temperature for 5 hours, and then by a krypton gas adsorption method under the following conditions.

[0169] Device: BELSORP-max manufactured by Nippon Hiro Co., Ltd.

[0170] Adsorbate: Kr

[0171] Measuring temperature: 77k (liquid nitrogen temperature)

[0172] Determination mode: Isothermal adsorption process

[0173] Analytical method: BET multi-point method.

[0174] <Measurement of moisture content>

[0175] The water content (weight %) of PAS was measured in accordance with Japanese Industrial Standard JIS K 7251 using the Karl Fischer method.

[0176] <Molecular weight measurement and molecular weight distribution shape evaluation method>

[0177] The molecular weight of PAS was determined by gel permeation chromatography (GPC), which is a type of size exclusion chromatography (SEC). The sample was dissolved by adding 5 g of 1-chloronaphthalene to 5 mg of PAS and heating to 250°C. The solution was cooled to room temperature to form a slurry, and filtered with a membrane filter (pore size 0.1 μm). The modulated sample was subjected to GPC measurement under the following conditions, and the number average molecular weight (Mn) and weight average molecular weight (Mw) were calculated in terms of polystyrene.

[0178] Device: (SSC-7110 manufactured by Seman Science Co., Ltd.

[0179] Column name: Shodex UT806M×2

[0180] Eluent: 1-Chloronaphthalene

[0181] Detector: Differential refractive index detector

[0182] Column temperature: 210°C

[0183] Pre-thermostatic bath temperature: 250°C

[0184] Pump thermostat temperature: 50°C

[0185] Detector temperature: 210°C

[0186] Flow rate: 1.0mL / min

[0187] Sample injection volume: 300 μL.

[0188] Regarding the evaluation of the molecular weight distribution shape of PAS, the concentration fractions of the chromatogram obtained by the above-mentioned GPC measurement are sequentially accumulated, the molecular weight (logarithmic value) is plotted on the horizontal axis, and the cumulative value of the concentration fraction is plotted on the vertical axis. First, an integrated molecular weight distribution curve is prepared, and the molecular weight value of the horizontal axis of the integrated molecular weight distribution curve is cut out to be in the range of 100 to 10,000. The cumulative integral value of the molecular weight of 100 to 4,000 is calculated when the cumulative integral value of the molecular weight of 100 to 10,000 is set to 100, and this value is set as the molecular weight distribution shape.

[0189] <Determination of the amount of chloroform extract>

[0190] The amount of chloroform extractable components in PAS was calculated as follows: 10 g of PAS was weighed and subjected to Soxhlet extraction with 100 g of chloroform for 3 hours, the weight of the component obtained by distilling off chloroform from the extract was measured, and the weight was calculated as a ratio to the weight of the charged polymer (wt %).

[0191] In addition, step 4 in the present invention is a step of distilling off the organic solvent used in step 3 by heating while flowing an inert gas. However, when step 4 is carried out under the preferred conditions of the present invention, the amount of chloroform extractable components in PAS before and after the implementation of step 4 is almost unchanged. Therefore, the amount of chloroform extractable components in PAS after the implementation of step 3 in the present invention is evaluated by the amount of chloroform extractable components in PAS after the implementation of step 4.

[0192] <Gas generation measurement>

[0193] The gas generation amount of PAS is measured by first adding 3g of PAS into a glass ampoule with a belly of 100mm×25mmφ, a neck of 255mm×12mmφ, and a wall thickness of 1mm for vacuum sealing. Then, the body of the ampoule is inserted into the ceramic electric heating tube furnace ARF-30K manufactured by Asahika Seisakusho Co., Ltd., and heated at 320°C for 2 hours with the neck of the ampoule protruding out of the tube furnace. Then, the ampoule is taken out, and the neck of the ampoule with the gas component attached is cut off with a file and the weight is measured. Furthermore, the cut neck is washed with chloroform, and the weight is measured again after drying. The value obtained by dividing the weight difference before and after the chloroform washing of the cut neck by the original weight of PAS is used as the gas generation amount (weight %) for evaluation.

[0194] <Evaluation of mold contamination>

[0195] Regarding the evaluation of mold contamination of PAS, first, extrusion molding (cylinder temperature 320°C, adding: PAS: 60 parts by weight, chopped glass fiber (T-760H manufactured by Nippon Denki Glass Co., Ltd.): 40 parts by weight) was performed to produce pellets, and then the obtained pellets were supplied to an injection molding machine (SE-30D) manufactured by Sumitomo Heavy Industries, Ltd. at a cylinder temperature of 325°C. The mold for gas evaluation with molded product dimensions: maximum length 55 mm, width 20 mm, thickness 2 mm, gate dimensions: width 2 mm, thickness 1 mm (side gate), gas venting part maximum length 20 mm, width 10 mm, depth 5 μm was heated to 130°C and allowed to stand, and continuous molding was performed 1,000 times. Then, the attached matter in the gas venting part was recovered and the weight was measured to evaluate (mg / 1,000 times).

[0196] <Evaluation of melt flowability>

[0197] The melt fluidity of PAS was evaluated by measuring the melt flow rate (resin discharge amount per 10 minutes: g / 10 min) according to ASTM-D1238-70 and comparing the values.

[0198] Apparatus: Melt indexer manufactured by Toyo Seiki Seisaku-sho Co., Ltd. (using an orifice with a length of 8.0 mm and a hole diameter of 2.095 mm)

[0199] Load: 5,000g

[0200] Sample size: 7g

[0201] Temperature: 315.5°C (melting time 5 minutes)

[0202] <Evaluation of hydrolysis resistance>

[0203] The hydrolysis resistance of PAS was evaluated by first performing extrusion molding (cylinder temperature 320°C, adding: PAS: 60 parts by weight, chopped glass fiber (T-760H manufactured by Nippon Denki Glass Co., Ltd.): 40 parts by weight, epoxy silane coupling agent 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (KBM-303 manufactured by Shin-Etsu Chemical Co., Ltd.)) to produce pellets, then using the obtained pellets, injection molding was performed in accordance with ASTM standard (D-638), and the tensile strength of the obtained test piece was measured. Then, the test piece was immersed in a liquid composed of 54% water, 45% ethylene glycol, 0.5% dipotassium phosphate, and 0.5% diethylene glycol at 150°C for 168 hours. The tensile strength of the test piece after immersion for 168 hours was measured to calculate the strength retention rate of the tensile strength, and the strength retention rate was used as the evaluation of the hydrolysis resistance of PAS.

[0204] <Rate of change expressed by MFR2 / MFR1>

[0205] When the melt flow rate of PAS is defined as MFR1, and the melt flow rate after mixing PAS and an epoxy silane coupling agent at a weight ratio of 100:1 and heating at 315.5°C for 5 minutes is defined as MFR2, the rate of change represented by MFR2 / MFR1 is first determined by measuring the melt flow rate of PAS in accordance with ASTM-D1238-70 to obtain MFR1, and then measuring the melt flow rate of a mixture of 1 g of PAS and 0.01 g of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (KBM-303 manufactured by Shin-Etsu Chemical Co., Ltd.) mixed using a mortar and pestle, and heated at 315.5°C for 5 minutes to obtain MFR2, and then calculating MFR2 / MFR1.

[0206] <Measurement of median particle size D50>

[0207] The median particle size D50 (μm) of the particulate PAS obtained in the present invention was measured using the following apparatus under wet conditions using N-methyl-2-pyrrolidone as a dispersion solvent.

[0208] Equipment: SALD-2000 laser particle size distribution meter manufactured by Shimadzu Corporation

[0209] <Determination of the cooling crystallization temperature Tmc>

[0210] The temperature drop crystallization temperature Tmc (° C.) of PAS was measured using a differential scanning calorimeter under the following conditions.

[0211] Device: Q20 made by TAインスツルメンツ Corporation

[0212] Measurement atmosphere: Nitrogen flow

[0213] Sample weight: about 10 mg

[0214] Determination conditions:

[0215] (a) Maintain at 50°C for 1 minute

[0216] (b) Raise the temperature from 50°C to 340°C at a rate of 20°C / min

[0217] (c) Maintain at 340°C for 1 minute

[0218] (d) Cooling from 340°C to 100°C at a rate of 20°C / min

[0219] (e) Maintain at 100°C for 1 minute

[0220] (f) The temperature was increased from 100°C to 340°C at a rate of 20°C / min.

[0221] [Example 1]

[0222] The distillation apparatus and alkali trap were connected to an autoclave equipped with a stirrer and a take-out valve at the bottom, 11.6 kg (100 mol) of 48.3% aqueous sodium hydrosulfide solution, 8.25 kg (101 mol) of 48.9% aqueous sodium hydroxide solution, 16.4 kg (165 mol) of N-methyl-2-pyrrolidone, and 1.56 kg (19.0 mol) of sodium acetate were added, and the reaction container was fully purged with nitrogen.

[0223] Nitrogen was introduced into the autoclave while stirring at 60 rpm and slowly heated to 237°C for 3 hours to remove liquid, and 12 kg of distillate was obtained. The distillate was analyzed by gas chromatography, and the composition of the distillate was 10.2 kg of water and 1.8 kg of N-methyl-2-pyrrolidone. At this stage, 20 g (1 mol) of water and 14.6 kg of N-methyl-2-pyrrolidone remained in the reaction system. In addition, 0.675 mol of hydrogen sulfide was scattered from the reaction system by the dehydration operation.

[0224] Next, after cooling the autoclave to 170°C or less, 15 kg (101.8 mol) of p-dichlorobenzene and 14.6 kg (147 mol) of N-methyl-2-pyrrolidone were added, and the reaction vessel was fully purged with nitrogen again and sealed. Thus, the amount of the dihalogenated aromatic compound used in the mixture was 102.5 mol per 1 mol of sulfur in the sulfiding agent. In addition, the internal temperature dropped to 130°C by the addition operation.

[0225] Next, the temperature in the reaction vessel was raised from 130° C. to 275° C. over about 2 hours while stirring at 250 rpm, and the temperature was further maintained at 275° C. for 70 minutes to allow the reaction to proceed. The pressure in the system was 1.10 MPa.

[0226] (Process 1)

[0227] After the reaction was completed, the take-out valve at the bottom of the autoclave was opened, and the reaction solution at 1.10 MPa and 275° C. was flashed over 15 minutes into a container (equipped with a distillation device) at normal pressure and equipped with a stirrer and heated to 220° C. Then, the container was maintained at 240° C. while stirring to distill off N-methyl-2-pyrrolidone, and then the heating was stopped and the container was cooled to recover the solid content in the container.

[0228] (Process 2)

[0229] The solid substance obtained in step 1 was placed in another container equipped with a stirrer, 108 kg of ion exchange water was added, and the mixture was stirred at 70° C. for 30 minutes, and then filtered with a pressure filter to obtain a filter cake.

[0230] The filter cake obtained above was placed in a pressure-resistant container equipped with a stirrer, 128 kg of ion exchange water was added for nitrogen substitution, and the temperature was raised to 192° C. and stirred for 30 minutes. The container was then cooled, the slurry was taken out, and filtered with a pressure filter to obtain a filter cake.

[0231] The filter cake obtained above was again placed in a container equipped with a stirrer, 108 kg of ion exchange water was added, and the mixture was stirred at 70° C. for 30 minutes, and then filtered with a pressure filter to obtain a filter cake. This process was repeated three times.

[0232] The obtained wet cake was dried at 120° C. for 3 hours under a nitrogen gas stream to obtain dry polyphenylene sulfide (PPS). The water content of the obtained dry PPS was measured by the Karl Fischer method according to JIS K 7251 and was 0.1% by weight.

[0233] (Process 3)

[0234] The dried PPS obtained in step 2 was placed in a container equipped with a stirrer, and 54 kg of N-methyl-2-pyrrolidone (weight bath ratio to PPS: 5) was added, followed by stirring at 30° C. for 20 minutes and filtering with a pressure filter to obtain a filter cake.

[0235] (Process 4)

[0236] The wet cake obtained in step 3 (containing 10.8 kg of PPS) was heated at 200° C. for 20 hours while nitrogen gas flowed at a flow rate of 4 L / min (0.4 L / min per 1 kg of polyarylene sulfide) to distill off NMP, thereby obtaining dry PPS.

[0237] In step 3, the specific surface area of ​​PPS before washing with an organic solvent was measured and found to be 11 m 2 / g, and the water content was 0.1 wt%. In addition, the reaction to produce PPS was carried out in the same manner as in Example 1, and the reaction liquid was cooled and taken out before carrying out the step 1. The DCB conversion was analyzed and found to be 98.6%.

[0238] The PPS obtained in Example 1 was analyzed, and the weight average molecular weight Mw was 40,000. The cumulative integral value of the molecular weights from 100 to 4,000 when the cumulative integral value of the molecular weights from 100 to 10,000 was calculated to be 52. In addition, since the amount of chloroform extractable components in the PPS after the implementation of step 4 was 0.8% by weight, the amount of chloroform extractable components in the PPS after the implementation of step 3 in the present invention can also be considered to be 0.8% by weight. Furthermore, the median particle size D50 was 300 μm, the gas generation amount was 0.67% by weight, the cooling crystallization temperature Tmc was 222°C, MFR1 was 637 g / 10 minutes, MFR2 was 32 g / 10 minutes, and the change rate represented by MFR2 / MFR1 was 0.050.

[0239] The PPS obtained in Example 1 was used for injection molding. As a result, the melt fluidity was high, the appearance of the molded product was not poor, and the mold contamination after 1,000 moldings was as little as 0.5 mg. In addition, the hydrolysis resistance of the obtained composite was evaluated. As a result, the tensile strength before the test was 194 MPa, the tensile strength after the test was 170 MPa, and the strength retention rate was 88%, which was a composite with high hydrolysis resistance.

[0240] [Example 2]

[0241] PPS was produced in the same manner as in Example 1 except that the temperature for distilling off the organic polar solvent in step 1 was changed to 250° C. The specific surface area of ​​PPS before washing with the organic solvent in step 3 was 4.5 m 2 / g, and the moisture content is 0.1 wt%.

[0242] The PPS obtained in Example 2 was analyzed, and the weight average molecular weight Mw was 40,000. The cumulative integral value of the molecular weights from 100 to 4,000 was calculated when the cumulative integral value of the molecular weights from 100 to 10,000 was 100, and the result was 51. In addition, since the amount of chloroform extractable components in the PPS after the implementation of step 4 was 1.6% by weight, the amount of chloroform extractable components in the PPS after the implementation of step 3 in the present invention can also be considered to be 1.6% by weight. Furthermore, the median particle size D50 was 320 μm, MFR1 was 640 g / 10 minutes, MFR2 was 32 g / 10 minutes, and the rate of change represented by MFR2 / MFR1 was 0.050.

[0243] Injection molding was performed using the PPS obtained in Example 2. As a result, the melt fluidity was high, the appearance of the molded product was not poor, and the mold contamination after 1,000 moldings was as little as 0.7 mg. In addition, the hydrolysis resistance of the obtained composite was evaluated. As a result, the tensile strength before the test was 190 MPa, the tensile strength after the test was 166 MPa, and the strength retention rate was 87%, which was a composite with high hydrolysis resistance.

[0244] [Example 3]

[0245] PPS was produced in the same manner as in Example 1 except that the organic solvent used in step 3 was changed to toluene.

[0246] The PPS obtained in Example 3 was analyzed, and the weight average molecular weight Mw was 40,000. The cumulative integral value of the molecular weights from 100 to 4,000 was calculated when the cumulative integral value of the molecular weights from 100 to 10,000 was 100, and the result was 51. In addition, since the amount of chloroform extractable components in the PPS after the implementation of step 4 was 0.9 wt%, the amount of chloroform extractable components in the PPS after the implementation of step 3 in the present invention can also be considered to be 0.9 wt%. Furthermore, the median particle size D50 was 300 μm.

[0247] Injection molding was performed using the PPS obtained in Example 3. As a result, the melt fluidity was high, and the appearance of the molded product was not defective. The amount of mold contamination after 1,000 cycles of molding was as low as 0.6 mg.

[0248] [Example 4]

[0249] PPS was produced in the same manner as in Example 3 except that the wet cake obtained in step 2 was not dried so that the water content of PPS before washing with the organic solvent in step 3 was 45% by weight.

[0250] The PPS obtained in Example 4 was analyzed, and the weight average molecular weight Mw was 40,000. The cumulative integral value of the molecular weights from 100 to 4,000 was calculated when the cumulative integral value of the molecular weights from 100 to 10,000 was 100, and the result was 51. In addition, since the amount of chloroform extractable components in the PPS after the implementation of step 4 was 0.9 wt%, the amount of chloroform extractable components in the PPS after the implementation of step 3 in the present invention can also be considered to be 0.9 wt%. Furthermore, the median particle size D50 was 300 μm.

[0251] Injection molding was performed using the PPS obtained in Example 4. As a result, the melt fluidity was high, and the appearance of the molded product was not defective. The amount of mold contamination after 1,000 cycles of molding was as low as 0.6 mg.

[0252] As described above, in Example 4, toluene was used as the washing solvent and the water content of PPS before washing with the organic solvent in step 3 was 45 wt %. The same operation as in Example 3 was carried out, but the quality of the obtained PPS was almost unchanged.

[0253] [Comparative Example 1]

[0254] PPS was produced in the same manner as in Example 1 except that step 3 was not performed. The weight average molecular weight Mw of the obtained PPS was 39,000, and the cumulative integral value of the molecular weights from 100 to 4,000 was calculated to be 54 when the cumulative integral value of the molecular weights from 100 to 10,000 was 100. In addition, since the amount of chloroform extractable components in the PPS after step 4 was 2.9% by weight, the amount of chloroform extractable components in the PPS after step 3 in the present invention can also be considered to be 2.9% by weight. Furthermore, the median particle size D50 was 300 μm, the gas generation amount was 0.81% by weight, the cooling crystallization temperature Tmc was 200° C., MFR1 was 657 g / 10 minutes, MFR2 was 41 g / 10 minutes, and the rate of change represented by MFR2 / MFR1 was 0.062.

[0255] Injection molding was performed using the PPS obtained in Comparative Example 1. As a result, mold contamination deposits amounted to 1.5 mg after 1,000 cycles of molding. On the other hand, the hydrolysis resistance of the obtained composite was evaluated. The tensile strength before the test was 192 MPa, and the tensile strength after the test was 162 MPa. The strength retention rate was 84%, indicating that the composite had high hydrolysis resistance.

[0256] [Comparative Example 2]

[0257] After the reaction was completed, step 1 was not performed, and step 3 of Example 1 was repeated 3 times, and then step 2 of Example 1 was performed to produce PPS. As a result, the weight average molecular weight Mw of the obtained PPS was 42,000, and the cumulative integral value of the molecular weight 100 to 4,000 when the cumulative integral value of the molecular weight 100 to 10,000 was calculated to be 42. In addition, since the amount of chloroform extractable components in PPS after step 4 was 0.5% by weight, the amount of chloroform extractable components in PPS after step 3 in the present invention can also be considered to be 0.5% by weight. Furthermore, the median particle size D50 was 450 μm, the cooling crystallization temperature Tmc was 205°C, MFR1 was 580 g / 10 minutes, MFR2 was 72 g / 10 minutes, and the rate of change represented by MFR2 / MFR1 was 0.124.

[0258] Injection molding was performed using the PPS obtained in Comparative Example 2. As a result, although the mold contamination attachment after 1,000 moldings was as little as 0.4 mg, the melt fluidity was low, and a molded product with poor appearance was slightly produced. In addition, the hydrolysis resistance of the obtained composite was evaluated. The tensile strength before the test was 185 MPa, the tensile strength after the test was 102 MPa, and the strength retention rate was 55%, which was a composite with low hydrolysis resistance. In addition, water, water-soluble substances and organic polar solvents were mixed in the filtrate obtained by washing, and the recovery of the organic polar solvent was difficult. Therefore, it is difficult to produce PPS at a low cost using the method of Comparative Example 2.

[0259] [Comparative Example 3]

[0260] PPS was produced in the same manner as in Example 1 except that the flow rate of nitrogen gas was changed to 1 L / min (0.1 L / min per 1 kg of polyarylene sulfide) in step 4.

[0261] The PPS obtained in Comparative Example 3 was analyzed, and the weight average molecular weight Mw was 40,000. The cumulative integral value of the molecular weight of 100 to 4,000 was calculated when the cumulative integral value of the molecular weight of 100 to 10,000 was set to 100, and the result was 52. In addition, since the amount of chloroform extractable components in the PPS after the implementation of step 4 was 0.8% by weight, the amount of chloroform extractable components in the PPS after the implementation of step 3 in the present invention can also be considered to be 0.8% by weight. Furthermore, the median particle size D50 was 300μm, MFR1 was 630g / 10min, MFR2 was 57g / 10min, and the rate of change represented by MFR2 / MFR1 was 0.090. The PPS obtained in Comparative Example 3 was used for injection molding, and the melt flowability was high, and the appearance of the molded product was not observed to be poor, and the mold contamination attachment after 1,000 moldings was as little as 0.5mg. However, the hydrolysis resistance of the obtained composite was evaluated. As a result, the tensile strength before the test was 194 MPa, and the tensile strength after the test was 131 MPa. The strength retention rate was 68%, indicating that the composite had low hydrolysis resistance.

[0262] Table 1

[0263]

Claims

1. A method for producing polyarylene sulfide, comprising heating a mixture containing at least a sulfiding agent, a dihalogenated aromatic compound, and an organic polar solvent to react to produce polyarylene sulfide, wherein: After the reaction to produce polyarylene sulfide is completed, the following steps 1, 2, 3 and 4 are performed. Step 1: a step of distilling off the organic polar solvent from the reaction mixture obtained at the end of the reaction to obtain a solid component containing polyarylene sulfide, Step 2: After step 1, a step of washing the solid content containing polyarylene sulfide with water, Step 3: After step 2, a step of washing the polyarylene sulfide with an organic solvent to reduce the amount of chloroform extract in the polyarylene sulfide to 1.7 wt % or less, Step 4: After step 3, a step of distilling off the organic solvent used in step 3 while heating the mixture while flowing an inert gas at a flow rate of 0.2 L / min or more per 1 kg of polyarylene sulfide. 2 . The method for producing polyarylene sulfide according to claim 1 , wherein in step 1, the temperature for distilling off the organic polar solvent is 200° C. or higher and 250° C. or lower. 3 . The method for producing polyarylene sulfide according to claim 1 , wherein in step 3, the water content of the polyarylene sulfide before washing with the organic solvent is 30% by weight or less.

4. The method for producing polyarylene sulfide according to claim 1 or 2, wherein in step 3, the specific surface area of ​​the polyarylene sulfide before washing with the organic solvent is 5 m 2 / g or more and 50m 2 / g or less. 5 . The method for producing polyarylene sulfide according to claim 1 , wherein in step 4, the temperature for distilling off the organic solvent is 70° C. or higher and 250° C. or lower. 6 . The method for producing polyarylene sulfide according to claim 1 , wherein in step 4, the time for distilling off the organic solvent is 0.1 hours to 50 hours.

7. A polyarylene sulfide produced by the production method according to claim 1, wherein the cumulative integral value of a molecular weight of 4,000 is 48 or more and 53 or less when the cumulative integral value of a molecular weight of 100 to 10,000 in a molecular weight distribution curve is 100, and when the melt flow rate of the polyarylene sulfide is MFR1 and the melt flow rate after the polyarylene sulfide and an epoxy silane coupling agent are mixed at a weight ratio of 100:1 and heated at 315.5°C for 5 minutes is MFR2, the change rate represented by MFR2 / MFR1 is 0.085 or less, Furthermore, the amount of chloroform extractable components in the polyarylene sulfide is 1.7% by weight or less. The polyarylene sulfide according to claim 7, wherein the polyarylene sulfide has a particle shape, and a median particle size D50 of the polyarylene sulfide particles is 1 μm or more and 400 μm or less.