Heat aging resistant polyamide molding composition

By using a combination of polyethyleneimine homopolymer and secondary aromatic amine condensation products in polyamide molding compositions, the problems of insufficient heat aging resistance of polyamide molding compositions at high temperatures and corrosion of copper compounds are solved, achieving It provides high heat resistance and improved mechanical properties without metal halide.

CN115335456BActive Publication Date: 2024-10-29BASF SE
View PDF 52 Cites 0 Cited by

Patent Information

Application Number
CN202180023897.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-23
Publication Date
2024-10-29
Estimated Expiration
2041-03-23

AI Technical Summary

Technical Problem

Existing polyamide molding compositions have insufficient thermal aging resistance at high temperatures, and the use of copper compounds or metal halide stabilizers poses a risk of corrosion, making it difficult to meet electrification and connectivity requirements.

Method used

Use a combination of polyamide, polyethyleneimine homopolymer or copolymer with secondary aromatic amines and their condensation products as heat stabilizers to replace traditional copper compounds or metal halides to form metal halide-free thermoplastic molding combinations things.

Benefits of technology

Significantly improves the thermal aging resistance of polyamide molding compositions, prevents thermal oxidative degradation, avoids the risk of corrosion of copper compounds, is suitable for electrically friendly applications, and maintains high mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003861423450000121
    Figure BDA0003861423450000121
  • Figure BDA0003861423450000131
    Figure BDA0003861423450000131
  • Figure BDA0003861423450000141
    Figure BDA0003861423450000141
Patent Text Reader

Abstract

A thermoplastic molding composition comprises: a) 30-99.8 wt% of at least one thermoplastic polyamide as component A; b) 0.001-5 wt% of at least one polyethyleneimine homopolymer or copolymer as component B; c) 0.1-2.0 wt% of at least one secondary aromatic amine and / or at least one condensation product of a secondary aromatic amine with an aliphatic aldehyde, an aliphatic ketone or a mixture thereof as component C; d) 0-3 wt% of at least one lubricant as component D; e) 0-50 wt% of at least one fibrous filler and / or particulate filler as component E; f) 0-25 wt% of other additives as component F, wherein the total weight % of components A to F is 100 wt%.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to thermoplastic molding compositions comprising polyamides which have improved heat aging resistance.

[0002] The invention further relates to the use of the molding compositions according to the invention for producing fibers, foils and moldings of any type, and to the fibers, foils and moldings obtained.

[0003] Furthermore, the invention relates to a mixture which comprises a specific combination of heat-aging-resistant additives for polyamide molding compositions.

[0004] Thermoplastic polyamides, such as PA6 and PA66, are often used in the form of glass-fiber-reinforced molding compositions as materials in the design of components that are exposed to high temperatures and / or humidity during their service life and undergo thermo-oxidative degradation.

[0005] Different heat aging additives that counteract or delay thermo-oxidative degradation are used in polyamide molding compositions, such as copper-containing stabilizers, organic HALS (hindered amine light stabilizer) compounds or combinations of hindered phenols or polyhydric alcohols. It is highly desirable to improve the heat aging resistance (HAR) of polyamides, since this can achieve a longer life of components that are subject to thermal stress or can reduce the risk of failure of these components. In addition, improved HAR can also allow the use of these components at higher temperatures.

[0006] EP1851265B1 discloses a thermoplastic molding composition comprising a thermoplastic polyamide, a polyethyleneimine homopolymer or copolymer, a lubricant and a copper-containing stabilizer. The molding material is said to have improved HAR, good flowability and good mechanical properties.

[0007] EP2356174B1 discloses a thermoplastic molding composition comprising a thermoplastic polyamide, a specific branched polyethyleneimine polymer having a primary amine / secondary amine / tertiary amine ratio of 1 / 0.7-1.4 / 0.3-1.11 / 0.8-1.3 / 0.5-0.9, a lubricant, a copper-containing stabilizer, a fiber or particle filler and a melanin. The molding made from the molding composition should have improved weld strength and increased thermal stability.

[0008] EP2379644B1 relates to a thermoplastic molding composition comprising polyamide, a polyethyleneimine homopolymer having a primary amino group, a secondary amino group and a tertiary amino group in a ratio of 1 / 0.91 / 0.64 and an average molecular weight MW of 1300, and iron powder. The molding composition should have improved HAR, good flowability and good mechanical properties.

[0009] EP0463512A1 discloses a stabilizer combination and its use for preparing a stabilized impact-modified polyamide. The stabilizer combination comprises a Cu(I) halide, a triarylphosphine, an alkali halide and an amine, preferably an aromatic amine. The condensation product of diphenylamine and acetone is disclosed.

[0010] DE1152252 discloses a method for stabilizing polycaprolactam, wherein the stabilizer is a condensation product of diarylamine and ketone.

[0011] DE 1123103 relates to a process for stabilizing high molecular weight linear polycondensates containing amide groups. Condensation products of N,N'-diphenyl-p-phenylenediamine and formaldehyde are described therein.

[0012] US 2011 / 021687 A1 relates to a thermoplastic polyamide composition comprising: A) at least one thermoplastic polyamide, B) at least one hyperbranched polyethyleneimine, C) at least one amorphous oxide and / or hydrated oxide of at least one metal or semimetal having a primary particle number average diameter of 0.5 to 20 nm.

[0013] DE 1152252 B discloses the stabilization of polycaprolactam with amino compounds. The amino compounds are water-insoluble diarylamine-ketone condensation products. Optionally, other amino compounds are used in addition.

[0014] DE1123103B discloses the stabilization of polyamides with secondary aromatic amine derivatives. The secondary aromatic amine derivatives are condensation products of aliphatic aldehydes and secondary aromatic amines.

[0015] The heat aging resistance of the known molding compositions is still unsatisfactory, in particular in the case of prolonged exposure to heat. Moreover, due to increasing electrification, more and more applications require materials that do not contain any halide-based stabilizer systems (e.g. copper iodide) because of the risk of corrosion and corresponding failures. Therefore, none of the compositions disclosed in the cited documents has good thermal stability while avoiding the use of widely used metal halide stabilizers.

[0016] It is therefore an object of the present invention to provide thermoplastic molding compositions comprising polyamides which have an improved HAR and which retain good mechanical properties after heat aging without requiring the use of copper compounds or metal halides.

[0017] This object is achieved by a thermoplastic molding composition comprising:

[0018] a) 30-99.8 wt % of at least one thermoplastic polyamide as component A;

[0019] b) 0.001 to 5 wt% of at least one polyethyleneimine homopolymer or copolymer as component B;

[0020] c) 0.1 to 2.0 wt % of at least one secondary aromatic amine and / or at least one condensation product of a secondary aromatic amine with an aliphatic aldehyde, an aliphatic ketone or a mixture thereof as component C;

[0021] d) 0-3 wt% of at least one lubricant as component D;

[0022] e) 0-50 wt% of at least one fibrous filler and / or particulate filler as component E;

[0023] f) 0-25 wt% of other additives as component F;

[0024] The total wt% of components A to F is 100 wt%.

[0025] The above object is also achieved by a mixture, which comprises or consists of the following components:

[0026] b) 0.001 to 5 parts by weight of at least one polyethyleneimine homopolymer or copolymer as component B;

[0027] c) as component C, 0.1 to 2.0 parts by weight of at least one secondary aromatic amine and / or at least one condensation product of a secondary aromatic amine with an aliphatic aldehyde, an aliphatic ketone or a mixture thereof.

[0028] In this mixture, the amounts of component B and component C listed below in wt % may be used as parts by weight (eg, 0.5 wt % becomes 0.5 parts by weight).

[0029] The abovementioned objects are also achieved by the use of the mixture for improving the HAR of polyamides, in particular after heat ageing.

[0030] The abovementioned object is also achieved by a process for producing a thermoplastic molding composition by mixing components A to F as described above.

[0031] The objects mentioned above are also achieved by the use of the thermoplastic molding composition for producing fibers, foils and moldings of any type, and by fibers, foils and moldings made from the thermoplastic molding composition as defined above.

[0032] According to the present invention, it has been found that a specific combination of at least one polyethyleneimine homopolymer or copolymer and at least one secondary aromatic amine and / or at least one condensation product of a secondary aromatic amine and an aliphatic aldehyde, an aliphatic ketone or a mixture thereof acts as a heat stabilizer in thermoplastic polyamide molding compositions and significantly improves heat aging resistance in the case of prolonged exposure to heat. By including this specific combination in a thermoplastic molding composition comprising at least one thermoplastic polyamide, thermooxidative degradation of the molding composition can be prevented or delayed.

[0033] By using the specific combination as a heat stabilizer to improve heat aging resistance and prevent thermo-oxidative degradation, it is not necessary to use copper compounds or metal halides as stabilizers in the molding composition.

[0034] Copper compounds (such as copper halides) and metal halides can cause corrosion due to ion migration. Therefore, the mixture according to the invention can be used to prepare a thermoplastic molding composition that is copper-free and metal-halide-free and is therefore electrically friendly or electrically neutral. Therefore, the molding composition according to the invention can be used for electrically friendly applications, including electromigration, electrification and connectivity.

[0035] Thus, the thermoplastic molding composition can be free of metal halides, particularly copper halides and alkali metal halides, and still achieve a high HAR.

[0036] During production, at the molding temperature and during the life of the molded part at elevated use temperatures, components B and C do not migrate from the thermoplastic molding composition. This effect is most pronounced in thermoplastic molding compositions based on polyamide as the main component.

[0037] Number average molecular weight and weight average molecular weight (Mn, Mw) and polydispersity data can be obtained using gel permeation chromatography (GPC) in hexafluoroisopropanol as solvent with PMMA calibration.

[0038] This molecular weight determination can be applied to all components of the thermoplastic molding compositions of the present invention.

[0039] The molding compositions of the invention comprise, as component A, 30 to 99.8% by weight, preferably 35 to 99.7% by weight, particularly preferably 45 to 99.7% by weight, of at least one thermoplastic polyamide.

[0040] If component D, component E or component F or a combination thereof is present in the thermoplastic molding composition, the maximum content of component A is reduced by the minimum content of each of component D, component E or component F or a combination thereof.

[0041] The polyamide of the molding composition of the invention generally has an intrinsic viscosity of 90 to 350 ml / g, preferably 110 to 240 ml / g, determined in accordance with ISO 307 at 25° C. in a 0.5% strength by weight solution in 96% strength by weight sulfuric acid.

[0042] Preferred are semicrystalline or amorphous resins having a molecular weight (weight average) of at least 5000, such as those described by way of example in the following U.S. Patents: 2,071,250; 2,071,251; 2,130,523; 2,130,948; 2,241,322; 2,312,966; 2,512,606; and 3,393,210.

[0043] Examples of these are: polyamides derived from lactams having 7 to 13 ring members, such as polycaprolactam, polycaprolactamine and polylauramide, and polyamides obtained by reacting dicarboxylic acids with diamines.

[0044] Dicarboxylic acids which can be used are alkanedicarboxylic acids and aromatic dicarboxylic acids having 6 to 12, in particular 6 to 10, carbon atoms. Merely by way of example, those which may be mentioned here are adipic acid, azelaic acid, sebacic acid, dodecanedioic acid and terephthalic acid and / or isophthalic acid.

[0045] Particularly suitable diamines are: alkanediamines having 6 to 12 carbon atoms, in particular 6 to 8 carbon atoms, and also m-dimethylenediamine, bis(4-aminophenyl)methane, bis(4-aminocyclohexyl)methane, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-aminocyclohexyl)propane and 1,5-diamino-2-methylpentane.

[0046] Preferred polyamides are: polyhexamethylene adipamide, polyhexamethylene sebacamide and polycaprolactam, and nylon-6 / 6,6 copolyamides, in particular with a proportion of caprolactam units of 5 to 95 wt % (e.g., Polyamides from BASF SE). C31).

[0047] Other suitable polyamides are obtainable from ω-aminoalkylnitriles, such as aminocapronitrile (PA 6), and adiponitrile with hexamethylenediamine (PA 66) in the presence of water by known direct polymerization, as described, for example, in DE-A 10313681, EP-A 1198491 and EP 922065.

[0048] Mention may also be made of polyamides obtainable, for example, by condensation of 1,4-diaminobutane with adipic acid at elevated temperatures (nylon-4,6). The preparation of polyamides of this structure is described by way of example in EP-A 38094, EP-A 38582 and EP-A 39524.

[0049] Other suitable examples are polyamides obtainable by copolymerization of two or more of the above-mentioned monomers, and mixtures of two or more polyamides in any desired proportions. Particular preference is given to mixtures of nylon-6,6 with other polyamides, in particular mixtures of nylon-6 and nylon-66, as well as nylon-6 / 6,6 copolyamides and nylon-6,6 / 6 copolyamides.

[0050] Other copolyamides which have proven particularly advantageous are semiaromatic copolyamides such as PA 6 / 6T and PA 66 / 6T, in which the triamine content is less than 0.5 wt %, preferably less than 0.3 wt % (see EP-A 299 444). Other high temperature resistant polyamides are known from EP-A 1 994 075 (PA 6T / 6I / MXD6).

[0051] The processes described in EP-A 129 195 and 129 196 can be used for preparing the abovementioned preferred semiaromatic copolyamides having a low triamine content.

[0052] The following list is not exhaustive and includes the polyamides A) mentioned and other polyamides A) for the purposes of the present invention, as well as the monomers included:

[0053] AB polymer:

[0054] PA 4 Pyrrolidone

[0055] PA 6 ε-caprolactam

[0056] PA 7 Hydrolactam

[0057] PA 8 Octyl Caprolactam

[0058] PA 9 9-aminoaspartic acid

[0059] PA 11 11-Aminoundecanoic acid

[0060] PA 12 Lauryl Lactam

[0061] AA / BB polymer:

[0062] PA 46 Tetramethylenediamine, Adipic Acid

[0063] PA 66 Hexamethylenediamine, Adipic Acid

[0064] PA 69 Hexamethylenediamine, Azelaic acid

[0065] PA 610 Hexamethylenediamine, Sebacic acid

[0066] PA 612 Hexamethylenediamine, decanedicarboxylic acid

[0067] PA 613 Hexamethylenediamine, Undecanedicarboxylic Acid

[0068] PA1212 1,12-dodecanediamine, decanedicarboxylic acid

[0069] PA 1313 1,13-Diaminotridecane, undecanedicarboxylic acid

[0070] PA 6T Hexamethylenediamine, terephthalic acid

[0071] PA MXD6 m-xylene diamine, adipic acid

[0072] AA / BB polymer:

[0073] PA 6I Hexamethylenediamine, Isophthalic acid

[0074] PA 6-3-T Trimethylhexamethylenediamine, terephthalic acid

[0075] PA 6 / 6T (see PA6 and PA 6T)

[0076] PA 6 / 66 (see PA 6 and PA 66)

[0077] PA 6 / 12 (see PA 6 and PA 12)

[0078] PA 66 / 6 / 610 (see PA66, PA 6 and PA 610)

[0079] PA 6I / 6T (see PA 6I and PA 6T)

[0080] PA PACM 12 Diaminodicyclohexylmethane, laurolactam

[0081] PA 6I / 6T / PACM is PA 6I / 6T+diaminodicyclohexylmethane

[0082] PA 12 / MACMI laurolactam, dimethyldiaminodicyclohexylmethane, isophthalic acid

[0083] PA 12 / MACMT laurolactam, dimethyldiaminodicyclohexylmethane, terephthalic acid

[0084] PA PDA-T Phenylenediamine, terephthalic acid

[0085] Most preferred are PA 6, PA 66, PA 6 / 66 and PA 66 / 6.

[0086] Suitable copolyamides consist of:

[0087] A1) 20.0 to 90.0 wt. % of units derived from terephthalic acid and hexamethylenediamine,

[0088] A2) 0 to 50.0 wt. % of units derived from ε-caprolactam,

[0089] A3) 0-80.0 wt% of units derived from adipic acid and hexamethylenediamine,

[0090] A4) 0-40.0 wt% of other polyamide-forming monomers,

[0091] The proportion of component A2) or component A3) or component A4) or a mixture thereof is at least 10.0% by weight.

[0092] Component A1) comprises from 20.0 to 90.0% by weight of units derived from terephthalic acid and hexamethylenediamine.

[0093] Besides the units derived from terephthalic acid and hexamethylenediamine, the copolyamide optionally also comprises units derived from ε-caprolactam and / or units derived from adipic acid and hexamethylenediamine and / or units derived from other polyamide-forming monomers.

[0094] The aromatic dicarboxylic acids A4) contain 8 to 16 carbon atoms. Suitable aromatic dicarboxylic acids include, for example, isophthalic acid, substituted terephthalic acids and isophthalic acids, for example 3-tert-butylisophthalic acid, polycyclic dicarboxylic acids, for example 4,4′-diphenyldicarboxylic acid and 3,3′-diphenyldicarboxylic acid, 4,4′-diphenylmethanedicarboxylic acid and 3,3′-diphenylmethanedicarboxylic acid, 4,4′-sulfodiphenylcarboxylic acid and 3,3′-sulfodiphenylcarboxylic acid, 1,4-naphthalenedicarboxylic acid or 2,6-naphthalenedicarboxylic acid, phenoxyterephthalic acid, particularly preferably isophthalic acid.

[0095] Further polyamide-forming monomers A4) can be derived from dicarboxylic acids having 4 to 16 carbon atoms and aliphatic or cycloaliphatic diamines having 4 to 16 carbon atoms, and also from aminocarboxylic acids / corresponding lactams having 7 to 12 carbon atoms. Examples of suitable monomers of these types are mentioned: linoleic acid, azelaic acid and sebacic acid as representatives of aliphatic dicarboxylic acids, 1,4-butanediamine, 1,5-pentanediamine, piperazine, 4,4′-diaminodicyclohexylmethane, 2,2-(4,4′-diaminodicyclohexyl)propane and 3,3′-dimethyl-4,4′diaminodicyclohexylmethane or m-dimethyldiamine as representatives of lactams / aminocarboxylic acids, caprolactam, enantholactam, ω-aminoundecanoic acid and laurolactam.

[0096] Suitable copolyamides of this type are described in more detail in DE-A-10 2009011668.

[0097] The amount of component B is 0.001-5 wt %, preferably 0.01-1.5 wt %, particularly preferably 0.1-1.0 wt %, such as 0.15-0.35 wt %.

[0098] Component B is at least one polyethyleneimine homopolymer or copolymer.

[0099] In the context of the present invention, polyethyleneimines are understood to mean homopolymers and copolymers which are obtainable, for example, by the process disclosed in the electronic version of the Encyclopedia of Industrial Chemistry by ULLMANN under the keyword "aziridines" or in accordance with WO-A 94 / 12560.

[0100] Homopolymers are usually obtained by polymerizing ethyleneimine (aziridine) in aqueous or organic solution in the presence of an acid-scavenging compound, an acid or a Lewis acid. Such homopolymers are branched polymers which usually contain primary, secondary and tertiary amino groups in a ratio of about 30%:40%:30%. The distribution of the amino groups can usually be determined by 13 C NMR spectroscopy.

[0101] The comonomer used is preferably a compound having at least two amino functional groups. Examples of suitable comonomers include alkylenediamines having 2 to 10 carbon atoms in the alkylene group, preferably ethylenediamine and propylenediamine. Other suitable comonomers are diethylenetriamine, triethylenetetramine, tetraethylenepentamine, dipropylenetriamine, tripropylenetetramine, dihexamethylenetriamine, aminopropylethylenediamine and bisaminopropylethylenediamine.

[0102] The polyethyleneimines generally have an average molecular weight (weight average) of 100 to 3,000,000, preferably 800 to 2,000,000 (determined by light scattering).

[0103] Also suitable are crosslinked polyethyleneimines, which can be obtained by reacting polyethyleneimines with difunctional or polyfunctional crosslinking agents which have at least one halohydrin, glycidyl, aziridine or isocyanate unit or a halogen atom as a functional group. Examples include: epichlorohydrin or dichlorohydrin ethers of polyalkylene glycols having 2 to 100 ethylene oxide and / or propylene oxide units, and the compounds listed in DE-A 19931720 and U.S. Pat. No. 4,144,123. Methods for preparing crosslinked polyethyleneimines are known from the above-mentioned documents as well as from EP-A 895,521 and EP-A 25,515.

[0104] Preferred polyethyleneimine homo- or copolymers are further disclosed in EP 2356174 B1, paragraphs

[0026] to

[0035] and EP 1851265 B1, paragraphs

[0022] to

[0025] and EP 2379644 B1, paragraphs

[0023] to

[0025] .

[0105] Grafted polyethyleneimines are also suitable, where the grafting agents used may be all compounds which are capable of reacting with the amino or imino groups of the polyethyleneimines. Suitable grafting agents and processes for preparing grafted polyethyleneimines can be obtained, for example, from EP-A 675914.

[0106] Likewise suitable polyethyleneimines in the context of the present invention are amidated polymers which are generally obtainable by reacting polyethyleneimines with carboxylic acids, their esters or anhydrides, carboxamides or carbonyl halides. Depending on the proportion of amidated nitrogen atoms in the polyethyleneimine chain, the amidated polymers can subsequently be crosslinked with the crosslinking agents mentioned. Preference is given to amidating up to 30% of the amino functions so that sufficient primary and / or secondary nitrogen atoms are still available for the subsequent crosslinking reaction.

[0107] Also suitable are alkoxylated polyethyleneimines, which are obtainable, for example, by reacting polyethyleneimine with ethylene oxide and / or propylene oxide. Such alkoxylated polymers are subsequently also crosslinkable.

[0108] Other suitable polyethyleneimines include hydroxyl-containing polyethyleneimines and amphoteric polyethyleneimines (introducing anionic groups), and lipophilic polyethyleneimines, which are usually obtained by introducing long-chain hydrocarbon groups into the polymer chain. The method for preparing such polyethyleneimines is known to those skilled in the art, and therefore further details on this topic are not required.

[0109] The polyethyleneimine may be linear, substantially linear or branched.

[0110] In one embodiment of the present invention, the polyethyleneimine is selected from highly branched polyethyleneimines. Highly branched polyethyleneimines are characterized by their high degree of branching (DB). The degree of branching can be determined, for example, by 13 C-NMR spectroscopy, preferably at D 2 O and is defined as follows:

[0111] DB=D+T / D+T+L

[0112] Among them, D (dendritic) corresponds to the tertiary amino moiety, L (linear) corresponds to the secondary amino moiety, and T (terminal) corresponds to the primary amino moiety.

[0113] In the context of the present invention, highly branched polyethyleneimines are polyethyleneimines having a DB in the range from 0.25 to 0.90.

[0114] In one embodiment of the present invention, the polyethyleneimines are selected from highly branched polyethyleneimines (homopolymers) having an average molecular weight Mw in the range of 600 to 75000 g / mol, preferably in the range of 800 to 25000 g / mol.

[0115] In another embodiment of the present invention, the polyethyleneimine is selected from copolymers of ethyleneimine, such as ethyleneimine and at least one other compound other than ethyleneimine having two NH 2A copolymer of a diamine (e.g., propylene imine) containing a diamine group, or a copolymer of a diamine having three NH 2 Copolymers of compounds containing amine groups (such as melamine).

[0116] Preferably, component B is selected from:

[0117] - homopolymers of ethyleneimine,

[0118] - a copolymer of ethyleneimine and an amine having at least two amino groups,

[0119] - cross-linked polyethyleneimine,

[0120] - grafted polyethyleneimine,

[0121] - amidated polymers obtainable by reaction of polyethylene imine with carboxylic acids or carboxylic esters, carboxylic anhydrides, carboxamides or carbonyl halides,

[0122] - alkoxylated polyethyleneimine,

[0123] - hydroxyl-containing polyethyleneimine,

[0124] - an amphoteric polyethyleneimine, and

[0125] - Lipophilic polyethyleneimine.

[0126] As component C, 0.1-2.0 wt %, preferably 0.2-1.6 wt %, more preferably 0.2-0.9 wt % of secondary aromatic amine and / or at least one condensation product of secondary aromatic amine with aliphatic aldehyde, aliphatic ketone or a mixture thereof is used.

[0127] Thus, secondary aromatic amines can be used as component C. Furthermore, at least one condensation product of a secondary aromatic amine with an aliphatic aldehyde, an aliphatic ketone or a mixture of an aliphatic aldehyde or an aliphatic ketone can be used. Most preferably, a combination of a secondary aromatic amine and a condensation product is used.

[0128] In another embodiment, as component C, 0.1-2.0 wt %, preferably 0.2-1.6 wt %, more preferably 0.0-0.9 wt % of at least one condensation product of a secondary aromatic amine with an aliphatic aldehyde, an aliphatic ketone or a mixture thereof and at least one secondary aromatic amine are used.

[0129] Preferably, the weight ratio of the secondary aromatic amine to the condensation product is from 0.5:20 to 20:0.5, more preferably from 1:10 to 10:1, most preferably from 1:5 to 5:1.

[0130] More preferably, component C comprises or is at least one condensation product of a diarylamine with formaldehyde and / or acetone. Preferably, component C comprises, in addition to the condensation product, at least one secondary aromatic amine.

[0131] Secondary arylamines are amine compounds containing two carbon groups chemically bonded to a nitrogen atom, wherein at least one, preferably both, carbon groups are aromatic. An example is diphenylamine. Preferably, at least one aromatic group, such as a phenyl, naphthyl or heteroaromatic group, is substituted with at least one substituent, preferably containing 1 to 20 carbon atoms. Examples of suitable secondary arylamines include: 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, which can be used as 445 is commercially available from Uniroyal Chemical Company; the secondary aromatic amine condensation product of diphenylamine and acetone is commercially available from Uniroyal Chemical Company at Commercially available; and p-(p-toluenesulfonylamino)diphenylamine, also available as SA is available from Uniroll Chemicals. Other suitable secondary aromatic amines include N,N'-di-(2-naphthyl)-p-phenylenediamine, available from ICI Rubber Chemicals, Kolkata, India. Other suitable secondary aromatic amines include 4,4'-bis(α,α'-tert-trioctyl)diphenylamine, 4,4'-bis(α-methylbenzyl)diphenylamine and others mentioned in EP 0509282 B1.

[0132] Suitable condensation products of carbonyl compounds (such as formaldehyde, acetaldehyde or acetone) and optionally substituted diphenylamines are described in EP 0 463 512 A1, DE-AS 1 123 103 and DE-AS 1 152 252.

[0133] Preferred amines may be amines of formula I disclosed in EP 0463512 A1, page 3, line 37 to page 5, line 29. The condensation products of diarylamines and ketones may be as disclosed in DE-AS 115252. Specifically, the reference discloses condensates of diphenylamine and phenylnaphthylamine with acetone. For the condensation of diarylamines with aliphatic ketones, further reference may be made to US 1906935 and US 1975167.

[0134] Condensation products of aliphatic aldehydes with secondary aromatic amines which can be used according to the invention are disclosed in DE-AS 1123103, see in particular column 1, lines 29 to 50. Secondary aromatic amines contain an aromatic radical and a further radical which may be aromatic, aliphatic or cycloaliphatic.

[0135] Suitable secondary aromatic amines are shown in formula (I) in column 1, line 29 to column 3, line 22. Suitable secondary amines are, for example, N,N'-diphenyl-p-phenylenediamine and N,N'-di-β-naphthyl-p-phenylenediamine or N,N'-dicyclohexyl-p-phenylenediamine. For more examples, see this reference.

[0136] Suitable secondary arylamines are disclosed in EP 2307480 B1, see in particular paragraphs

[0046] to

[0048] .

[0137] Aliphatic aldehydes in the sense of the present invention are: for example, monoaldehydes such as formaldehyde, acetaldehyde, propionaldehyde, butyraldehyde, isobutyraldehyde and 2-ethylhexanal, and dialdehydes such as dioxane, malondialdehyde and succinaldehyde.

[0138] The amine and the aldehyde (or ketone) may be used in equimolar amounts.

[0139] The preferred aliphatic ketone is acetone.

[0140] In the most preferred embodiment of the present invention, component C comprises at least one condensation product (condensation product or polycondensation product) of diarylamine with formaldehyde and acetone. In the condensation product, preferably equimolar amounts of diarylamine on the one hand and formaldehyde and acetone on the other hand are used. In addition, component C preferably further comprises at least one secondary aromatic amine. A mixture of condensation product and secondary aromatic amine is most preferred.

[0141] Suitable component C is available from OKA Tec GmbH, Germany, under the name

[0142] At least one lubricant may be used as component D. The amount of component D is 0-3 wt%, preferably 0-1.5 wt%, more preferably 0-1.0 wt%.

[0143] If present, component D is present in an amount of 0.05-3 wt%, preferably 0.1-1.5 wt%, more preferably 0.0-1.0 wt%.

[0144] If component D is present, the maximum amount of component A is reduced by the minimum amount of component D. Thus, it is reduced by 0.05 wt%, preferably 0.1 wt%.

[0145] The polyamide molding composition according to the invention does not need to contain component D. Therefore, according to a first embodiment, component D is not contained in the thermoplastic molding composition. However, by additionally using component D, the fluidity of the thermoplastic molding composition can be further increased. Therefore, according to a second embodiment of the invention, the thermoplastic molding composition contains 0.05-3 wt %, preferably 0.1-1.5 wt %, more preferably 0.0-1.0 wt % of component D. According to the invention, molding compositions containing these amounts of component D are particularly preferred.

[0146] Preference is given to aluminum salts, alkali metal salts or alkaline earth metal salts, or esters or amides of fatty acids having 10 to 44 carbon atoms, preferably having 12 to 44 carbon atoms.

[0147] The metal ions are preferably alkaline earth metals and aluminum, particularly preferably calcium or magnesium.

[0148] Preferred metal salts are calcium stearate and calcium monate and aluminum stearate.

[0149] It is also possible to use mixtures of the various salts in any desired mixing ratio.

[0150] The carboxylic acids may be monobasic or dibasic. Examples which may be mentioned are polyaspartic acid, palmitic acid, lauric acid, artificial fatty acids, dodecanedioic acid, pecanic acid, particular preference being given to stearic acid, capric acid and montanoic acid (mixture of fatty acids having 30 to 40 carbon atoms).

[0151] The ester-forming aliphatic alcohol may be monohydric to tetrahydric. Examples of alcohols are n-butanol, n-octanol, stearyl alcohol, ethylene glycol, propylene glycol, neopentyl glycol, pentaerythritol, preferably glycerol and pentaerythritol.

[0152] The aliphatic amines forming the amides can be monobasic to tribasic. Examples of these are stearamide, ethylenediamine, propylenediamine, hexamethylenediamine, di(6-aminohexyl)amine, particularly preferably ethylenediamine and hexamethylenediamine. Preferred esters or amides are, respectively, glyceryl distearate, glyceryl tristearate, ethylenediamine distearate, glyceryl monopalmitate, glyceryl trilaurate, glyceryl monosorbate and pentaerythritol tetrastearate.

[0153] It is also possible to use mixtures of various esters or amides, or combinations of esters and amides in any desired mixing ratio.

[0154] As component E, the thermoplastic molding composition comprises 0 to 50% by weight, preferably 0 to 45% by weight, more preferably 0 to 40% by weight, of at least one fibrous filler and / or particulate filler.

[0155] Preferably, component E comprises glass fibers and is present in an amount of 10-50 wt%, more preferably 15-45 wt%, most preferably 20-40 wt%.

[0156] If component E is present, the maximum amount of component A is reduced by the minimum amount of component E so that the total amount of components A to F is still 100 wt%.

[0157] Fibrous or particulate fillers E which may be mentioned are carbon fibers, glass fibers, glass beads, amorphous silica, calcium silicate, calcium metasilicate, magnesium carbonate, kaolin, chalk, powdered quartz, mica, barium sulfate and feldspar.

[0158] Preferred fibrous fillers which may be mentioned are carbon fibers, aramid fibers and potassium titanate fibers, particular preference being given to glass fibers in the form of E glass. These can be used as rovings or in the form of commercially available chopped glass.

[0159] Fibrous fillers can be surface pretreated with silane compounds to improve compatibility with thermoplastics.

[0160] Suitable silane compounds have the general formula:

[0161] (X-(CH 2 ) n ) k -Si-(OC m H 2m+1 ) 4-k

[0162] The substituents are defined as follows:

[0163]

[0164] n is an integer from 2 to 10, preferably from 3 to 4,

[0165] m is an integer of 1 to 5, preferably 1 to 2, and

[0166] k is an integer from 1 to 3, preferably 1.

[0167] Preferred silane compounds are aminopropyltrimethoxysilane, aminobutyltrimethoxysilane, aminopropyltriethoxysilane and aminobutyltriethoxysilane, and the corresponding silanes which comprise a glycidyl group as replacement for X.

[0168] The amount of the silane compound generally used for the surface coating is 0.01 to 2 wt %, preferably 0.025 to 1.0 wt %, in particular 0.05 to 0.5 wt % (based on component E).

[0169] Acicular mineral fillers are also suitable.

[0170] For the purposes of the present invention, an acidic mineral filler is a mineral filler having a strongly acidic character. For example, needle-shaped wollastonite. The L / D (aspect ratio) of the mineral is preferably from 8:1 to 35:1, preferably from 8:1 to 11:1. The mineral filler may optionally be treated with the above-mentioned silane compound, but pretreatment is not necessary.

[0171] Other fillers that can be mentioned are kaolin, calcined kaolin, wollastonite, talcum and chalk, and lamellar or acidic nano fillers, and the amount of these fillers is preferably 0.1-10%. Preferred complexes for this purpose are boehmite, bentonite, montmorillonite, vermiculite, hectorite and lithophore. By prior art methods, the lamellar nano filler is organically modified so that it has good compatibility with organic binders. Adding lamellar or needle-shaped nano fillers to nanocomposite materials of the present invention further improves mechanical strength.

[0172] As component F, the molding compositions of the invention may contain 0 to 25% by weight, preferably 0 to 20% by weight, more preferably 0 to 15% by weight, of further additives.

[0173] If other additives are used, the minimum amount is preferably 0.1 wt%, more preferably 0.25 wt%, most preferably 0.5 wt%.

[0174] The thermoplastic molding composition of the present invention may contain, as component F, conventional processing aids, other stabilizers, oxidation retarders, agents for resisting thermal and UV decomposition, mold release agents, colorants (such as dyes and pigments), nucleating agents, plasticizers, etc.

[0175] As component F, 0.05 to 3% by weight, preferably 0.1 to 2% by weight, in particular 0.1 to 1% by weight, of at least one sterically hindered phenol antioxidant may be used.

[0176] Its molecular weight is preferably greater than 500 g / mol, more preferably greater than 1000 g / mol. In addition, component C should preferably show high thermal stability, for example, in a TGA (thermogravimetric analysis) experiment (40° C. to 120° C., 10° C. / min, isothermal for 15 minutes, then at 120° C. to 600° C., 20° C. / min), a maximum weight loss of 5%, more preferably a maximum weight loss of 2%, is measured at 300° C. under nitrogen conditions.

[0177] It preferably has at least one, more preferably at least two, branched chains C 3-12 The alkyl-substituted phenol group acts as a steric hindering group and is covalently linked to the structure of component C.

[0178] Suitable sterically hindered phenols are in principle all compounds which have a phenolic structure and which have at least one substituent on the phenolic ring. The substituent is, for example, a branched C 3-12 Alkyl, preferably branched C 3-6 Alkyl, more preferably isopropyl or tert-butyl.

[0179] Preferably, a compound of the formula,

[0180]

[0181] in:

[0182] R 1 and R 2 is alkyl, substituted alkyl or substituted triazolyl, wherein the group R 1 and R 2 can be the same or different, and R 3 is an alkyl group, a substituted alkyl group, an alkoxy group or a substituted amino group. The alkyl and alkoxy residues preferably have 1 to 12 carbon atoms, more preferably 1 to 6 carbon atoms. The substituents are preferably C 1-12 Alkyl, more preferably C 1-6 Alkyl, most preferably C 1-4 Alkyl. 1 To R3 At least one of is preferably a substituent as defined above.

[0183] Antioxidants of the aforementioned type are described, for example, in DE-A 2702661 (US Pat. No. 4,360,617).

[0184] Another group of preferred sterically hindered phenols is provided by those derived from substituted phenylcarboxylic acids, in particular from substituted phenylpropionic acids, which preferably have at least one substituent on the phenyl group. They contain in their structure at least one, preferably two, covalently linked substituted phenylcarboxylic acid units, which preferably have at least one substituent on the phenyl group.

[0185] The preferred phenyl carboxylic acid is phenyl-C 1-12 -carboxylic acid, more preferably phenyl-C 2-6 -carboxylic acid. The phenyl group is preferably a phenol group having at least one substituent on the phenol ring as described above. Therefore, the above sterically hindered phenol is preferably combined with C 1-12 Alkane carboxylic acid is covalently linked, preferably a linear C 2-6 Alkane carboxylic acids.

[0186] Particularly preferred compounds of this type are those of the formula:

[0187]

[0188] Where R 4 , R 5 , R 7 and R 8 Independent of each other, it is C that can be substituted by itself 1 -C 8 alkyl (at least one of these groups is a substituent), and R 6 It is a divalent aliphatic group having 1 to 10 carbon atoms, and its main chain may also have a CO bond. 4 To R 8 At least one of is a substituent as defined above.

[0189] Preferred compounds corresponding to these formulae are:

[0190]

[0191] (manufactured by BASF SE 245)

[0192]

[0193] (manufactured by BASF SE 259)

[0194] As examples of sterically hindered phenols, all of the following should be mentioned:

[0195] 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl]propionate (Irgan from BASF SE 1010), 3,5-di-tert-butyl-4-hydroxybenzylphosphonic acid distearyl ester, 2,6,7-trioxy-1-phosphobicyclo[2.2.2]octa-4-ylmethyl-3,5-di-tert-butyl-4-hydroxyindole acid butyl ester, 3,5-di-tert-butyl-4-hydroxyphenyl-3,5-distearylthiotriazoleamine, 2-(2'-hydroxy-3'-hydroxy-3',5'-di-tert-butyl)-5-chlorobenzotriazole, 2,6-di-tert-butyl-4-hydroxymethylphenol, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 4,4'-methylenebis(2,6-di-tert-butylphenol), 3,5-di-tert-butyl-4-hydroxybenzyldimethylamine.

[0196] Compounds which have proven to be particularly effective and which are therefore preferably used are 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 1,6-hexanediol bis(3,5-di-tert-butyl-4-hydroxyphenyl) propionate ( 259), pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and N,N'-hexamethylenebis-3,5-di-tert-butyl-4-hydroxyhydrocinnamamide ( 1098), and the products of the above-mentioned BASF SE 245 and 1010, they have particularly good applicability.

[0197] In some cases, sterically hindered phenols having not more than one sterically hindering group in the ortho position relative to the phenolic hydroxyl group have proven to be particularly advantageous; in particular when assessing color fastness to prolonged storage under diffuse light.

[0198] According to a preferred embodiment of the invention, the molding composition is free of copper, in particular free of copper stabilizers, such as, for example, Cu / (I) halides and combinations of Cu(I) halides with alkali metal halides.

[0199] More preferably, the thermoplastic molding composition of the present invention is free of metal halides.Metal halide-free systems, so-called electro-friendly systems, are of great interest because electromigration, electrification and connectivity are a growing trend in almost all industries.

[0200] The thermoplastic molding composition is therefore preferably free of metal halides, in particular copper halides and alkali metal halides.

[0201] If, however, no electro-friendly applications are envisaged, the molding compositions of the invention may comprise 0.05 to 3 wt %, preferably 0.1 to 1.5 wt %, in particular 0.1 to 1 wt % of a copper stabilizer, preferably a copper(I) halide, in particular as a mixture with an alkali metal halide, preferably KI, in particular in a ratio of 1:4, or a sterically hindered phenol, or a mixture thereof.

[0202] Preferred salts of monovalent copper used are cuprous acetate, cuprous chloride, cuprous amide and cuprous iodide. The material comprises these in an amount of 5 to 500 ppm of copper, preferably 10 to 250 ppm, based on the polyamide.

[0203] Good properties are particularly achieved if the copper is present in the polyamide in molecular distribution. This is achieved by adding a concentrate comprising the polyamide, the monovalent copper salt and the alkali metal halide in the form of a solid homogeneous solution to the molding composition. For example, a typical concentrate consists of 79 to 95% by weight of polyamide and 21 to 5% by weight of a mixture of copper iodide or copper bromide and potassium iodide. The copper concentration in the solid homogeneous solution is preferably 0.3 to 3% by weight, in particular 0.5 to 2% by weight, based on the total weight of the solution, and the molar ratio of cuprous iodide to potassium iodide is 1 to 11.5, preferably 1 to 5.

[0204] Suitable polyamides for the concentrate are homopolyamides and copolyamides, in particular nylon-6.

[0205] The molding compositions of the invention may contain 0.001 to 10% by weight, preferably 0.05 to 5% by weight, in particular 0.1 to 2.5% by weight of particles having a particle size of up to 10 μm (d 50 The iron powder may be obtained by thermal decomposition of ferroboron pentacarbon.

[0206] Iron exists in many isotopes:

[0207] 1. α-Fe (ferrite) forms a space-centered cubic lattice, can be magnetized, dissolves a small amount of carbon, and exists in pure iron up to 928°C. At 770°C (Curie temperature), it loses its ferromagnetic properties and becomes paramagnetic; iron in the temperature range of 770 to 928°C is also called β-Fe. At room temperature and a pressure of at least 13000MPa, α-Fe becomes so-called ε-iron, with a volume reduction of about 0.20cm 3 / mol, the density increased from 7.85 to 9.1 (at 20000MPa);

[0208] 2.γ-Fe (austenite) forms a face-centered cubic lattice, is non-magnetic, dissolves a large amount of carbon, and is only seen in the temperature range of 928 to 1398°C;

[0209] 3. Delta-iron, centered in space, exists with a melting point between 1398°C and 1539°C.

[0210] Metallic iron is generally silvery white, with a density of 7.874 (heavy metal), a melting point of 1539°C, a boiling point of 2880°C, and a specific heat (18 to 100°C) of about 0.5g. -1 K -1 , tensile strength is 220 to 280N / mm 2 . This value applies to chemically pure iron.

[0211] The industrial production of iron uses the smelting of iron ore, slag, calcined pyrite or blast furnace dust, and the remelting of scrap and alloys.

[0212] The iron powder of the invention is prepared by thermal decomposition of iron pentacarbonyl, preferably at a temperature of 150° C. to 350° C. The particles thus obtained have a preferably spherical shape, thus being spherical or almost spherical (another term is spheroidal).

[0213] Preferred iron powders have the following particle size distribution; the particle size distribution here is determined by laser scattering in very dilute aqueous suspension (eg using Beckman LS13320). The particle sizes (and distributions) described below may optionally be obtained by grinding and / or sieving.

[0214] Here dxx means that XX% of the total volume of the particles is less than a specified value.

[0215] d 50 Value: up to 10 μm, preferably 1.6 to 8 μm, in particular 2.9 to 7.5 μm, very particularly 3.4 to 5.2 μm

[0216] d 10 Value: preferably 1 to 5 μm, in particular 1 to 3 μm, very particularly 1.4 to 2.7 μm

[0217] d 90 Values: preferably 3 to 35 μm, in particular 3 to 12 μm, very particularly 6.4 to 9.2 μm.

[0218] The iron content of the iron powder is preferably 97-99.8 g / 100 g, preferably 97.5-99.6 g / 100 g. The content of other metals is preferably less than 1000 ppm, in particular less than 100 ppm, very particularly less than 10 ppm.

[0219] Iron content is usually determined by infrared spectroscopy.

[0220] The carbon content is preferably 0.01-1.2 g / 100 g, preferably 0.05-1.1 g / 100 g, in particular 0.4-1.1 g / 100 g. Preferably, the carbon content of the iron powder corresponds to the carbon content of the powder after the thermal decomposition process without hydrogen reduction.

[0221] Carbon content is usually determined by burning the sample in an oxygen stream and then detecting the generated CO using IR using a method based on ASTM E1019. 2 Gas (via Leco CS230 or CS mat6250 from Juwe).

[0222] The nitrogen content is preferably at most 1.5 g / 100 g, preferably 0.01 to 1.2 g / 100 g.

[0223] The oxygen content is preferably at most 1.3 g / 100 g, preferably 0.3 to 0.65 g / 100 g.

[0224] N and O are determined by heating the sample to about 2100°C in a graphite furnace. The oxygen obtained from the sample is converted into CO and measured by an IR detector. The N released from the N-containing compound under reaction conditions is released by the carrier gas and detected and recorded by a TCD (thermal conductivity detector) (both methods are based on ASTM E1019).

[0225] The tap density is preferably 2.5-5 g / cm 3 , especially 2.7-4.4g / cm 2 This usually means the density of the powder when it is, for example, filled into a container and compacted by vibration. Further preferred iron powders can be made of iron phosphate, iron phosphite or SiO 2 Surface coating.

[0226] The BET surface area according to DIN ISO 9277 is preferably in the range of 0.1 to 10 m 2 / g, especially 0.1-5m 2 / g, preferably 0.2-1m 2 / g, especially 0.4-1m 2 / g.

[0227] In order to achieve a particularly good dispersion of the iron particles, a masterbatch comprising a polymer can be used. Suitable polymers for this purpose are polyolefins, polyesters or polyamides, whereby the masterbatch polymer is preferably identical to component A. The mass fraction of iron in the polymer is generally 15-80 wt%, preferably 20-40 wt%.

[0228] Examples of further customary additives F are up to 25 wt %, preferably up to 20 wt %, of elastomeric polymers (also often referred to as impact modifiers, elastomers or rubbers).

[0229] The elastomeric polymer is different from component B.

[0230] These are generally copolymers, preferably composed of at least two of the following monomers: ethylene, propylene, butadiene, isobutylene, isoprene, chloroprene, vinyl acetate, styrene, acrylonitrile and acrylic esters and / or methacrylic esters having 1 to 18 carbon atoms in the alcohol component.

[0231] Such polymers are described in Houben Weyl, Methoden der organischen Chemie, Vol. 14 / 1 (Georg Thieme Verlag, Stuttgart, Germany, 1961), pp. 392-406, and in CB Bucknall's monograph "Toughened Plastics" (Applied Science Publishers, London, UK, 1977).

[0232] Some preferred types of such elastomers are described below.

[0233] Preferred types of such elastomers are those known as ethylene propylene (EPM) rubber and ethylene propylene diene (EPDM) rubber.

[0234] EPM rubbers generally have virtually no residual double bonds, whereas EPDM rubbers may have from 1 to 20 double bonds per 100 carbon atoms.

[0235] Examples of the diene monomers for EPDM rubbers that may be mentioned are conjugated dienes such as isoprene and butadiene, non-conjugated dienes having 5 to 25 carbon atoms such as 1,4-pentadiene, 1,4-hexadiene, 2,5-dimethyl-1,5-hexadiene and 1,4-octadiene, cyclodienes such as cyclopentadiene, cyclohexadiene, cyclooctadiene and dicyclopentadiene, and alkenyl norbornenes such as 5-ethylidene-2-norbornene, 5-butene-2-norbornene, 2-methallyl-5-norbornene and 2-isopropenyl-5-norbornene, and tricyclic dienes such as 3-methyltricyclo[5-[[[[[[[[[[[[[[[[[[[[[[[[[[[[[[ 2,6 ]-3,8-decadiene, and mixtures thereof. Preferred are 1,5-hexadiene, 5-ethylidene norbornene and dicyclopentadiene. The diene content of the EPDM rubber is preferably 0.5-50 wt%, especially 1-8 wt%, based on the total weight of the rubber.

[0236] EPM rubbers and EPDM rubbers may also preferably be grafted with reactive carboxylic acids or derivatives thereof Examples of these are acrylic acid, methacrylic acid and derivatives thereof, such as glycidyl (meth)acrylate, and maleic anhydride.

[0237] Copolymers of ethylene with acrylic acid and / or methacrylic acid and / or with esters of these acids are another group of preferred rubbers. The rubber may also comprise dicarboxylic acids, such as maleic acid and fumaric acid, or derivatives of these acids, such as esters and anhydrides, and / or monomers containing epoxy groups. These dicarboxylic acid derivatives or monomers containing epoxy groups are preferably incorporated into the rubber by adding monomers containing dicarboxylic acid groups and / or epoxy groups and having the general formula I or II or III or IV to the monomer mixture.

[0238] R 1 C(COOR 2 )=C(COOR 3 )R 4 (I)

[0239]

[0240]

[0241]

[0242] Where R 1 To R 9 is hydrogen or an alkyl group having 1 to 6 carbon atoms, m is an integer from 0 to 20, g is an integer from 0 to 10, and p is an integer from 0 to 5.

[0243] Group R 1 To R 9 Preferred is hydrogen, wherein m is 0 or 1 and g is 1. Corresponding compounds are maleic acid, fumaric acid, maleic anhydride, allyl glycidyl ether and vinyl glycidyl ether.

[0244] Preferred compounds of formula I, II and IV are maleic acid, maleic anhydride and (meth)acrylates containing epoxy groups, such as glycidyl acrylate and glycidyl methacrylate, and esters with tertiary alcohols, such as tert-butyl acrylate. Although the latter has no free carboxyl groups, its behavior is close to that of free acids and is therefore referred to as monomers with latent carboxyl groups.

[0245] The copolymer is advantageously composed of 50-98 wt % of ethylene, 0.1-20 wt % of monomers comprising epoxy groups and / or methacrylic acid and / or monomers comprising anhydride groups, the remainder being (meth)acrylate.

[0246] Particular preference is given to copolymers consisting of:

[0247] - 50-98 wt%, in particular 55-95 wt%, of ethylene,

[0248] 0.1 to 40 wt %, in particular 0.3 to 20 wt %, of glycidyl acrylate and / or glycidyl methacrylate, (meth)acrylic acid and / or maleic anhydride, and

[0249] 1 to 45% by weight, in particular 5 to 40% by weight, of n-butyl acrylate and / or 2-ethylhexyl acrylate.

[0250] Other preferred (meth)acrylates are the methyl, ethyl, propyl, isobutyl and tert-butyl esters.

[0251] Comonomers that can be used with these are vinyl esters and vinyl ethers.

[0252] The above-mentioned ethylene copolymers can be prepared by processes known per se, preferably by random copolymerization at high pressure and temperature. Suitable processes are well known.

[0253] Other preferred elastomers are emulsion polymers, the preparation of which is described, for example, by Blackley in the monograph “Emulsion Polymerization”. The emulsifiers and catalysts which can be used are known per se.

[0254] In principle, it is possible to use homogeneously structured elastomers or elastomers with a shell structure. The shell structure is determined by the order in which the individual monomers are added. The morphology of the polymer is also influenced by this order of addition.

[0255] Monomers mentioned here merely as examples for the preparation of the rubber part of the elastomer are acrylic acid esters, such as n-butyl acrylate and 2-ethylhexyl acrylate, the corresponding methacrylic acid esters, butadiene and isoprene, and mixtures thereof. These monomers can be copolymerized with other monomers, such as styrene, acrylonitrile, vinyl ether, and with other acrylic acid esters or methacrylic acid esters, such as methyl methacrylate, methyl acrylate, ethyl acrylate or propyl acrylate.

[0256] The soft or rubber phase (glass transition temperature below 0°C) of the elastomer can be the core, outer shell or intermediate shell (if the structure of the elastomer has more than two shells). Elastomers with more than one shell can also have more than one shell consisting of a rubber phase.

[0257] If, in addition to the rubber phase, one or more hard components (glass transition temperature above 20° C.) are involved in the structure of the elastomer, it is usually prepared by polymerizing styrene, acrylonitrile, methacrylonitrile, α-methylstyrene, p-methylstyrene, or acrylates or methacrylates (such as methyl acrylate, ethyl acrylate or methyl methacrylate) as the main monomers. In addition, relatively small proportions of other comonomers can also be used.

[0258] It has proven advantageous in certain cases to use emulsion polymers which have reactive groups on their surface. Examples of such groups include epoxy, carboxyl, latent carboxyl, amino and amide groups, as well as functional groups which can be introduced by the simultaneous use of monomers of the general formula,

[0259]

[0260] The substituents can be defined as follows:

[0261] R 10 is hydrogen or C 1 -C 4 alkyl,

[0262] R 11 It is hydrogen, C 1 -C 8 alkyl or aryl, especially phenyl,

[0263] R 12 It is hydrogen, C 1 -C 10 Alkyl, C 6 -C 12 Aryl or -OR 13 ,

[0264] R 13 It is C 1 -C 8 Alkyl or C 6 -C 12 an aryl group, optionally having a substituent which is an O-containing group or an N-containing group,

[0265] X is a chemical bond, C 1 -C 10 Alkylene or C 6 -C 12 Arylene, or

[0266]

[0267] Y is OZ or NH-Z, and

[0268] Z is for C 1 -C 10 Alkylene or C 6 -C 12 Arylene.

[0269] The grafting monomers described in EP-A 208 187 are also suitable for introducing reactive groups on the surface.

[0270] Other examples which may be mentioned are acrylamide, methacrylamide and substituted acrylates or methacrylates, for example (N-tert-butylamino)ethyl methacrylate, (N,N-dimethylamino)ethyl acrylate, (N,N-dimethylamino)methyl acrylate and (N,N-diethylamino)ethyl acrylate.

[0271] The particles of the rubber phase may also have been crosslinked. Examples of crosslinking monomers are 1,3-butadiene, divinylbenzene, diallyl phthalate and dihydrodicyclopentadienyl acrylate and the compounds described in EP-A 50265.

[0272] Monomers referred to as grafted monomers can also be used, i.e. monomers with two or more polymerizable double bonds reacting at different rates during polymerization. Preferably, this type of compound is used, wherein at least one reactive group polymerizes at a rate approximately the same as other monomers, and other reactive groups (or multiple reactive groups) are for example significantly more slowly polymerized. Different polymerization rates produce a certain proportion of unsaturated double bonds in rubber. If another phase is subsequently grafted onto this type of rubber, at least some double bonds present in the rubber react with the grafted monomer to form a chemical bond, i.e. the grafted phase has at least a certain degree of chemical bond with the grafted base.

[0273] Examples of such graft-linked monomers are monomers containing an allyl group, in particular allyl esters of ethylenically unsaturated carboxylic acids, such as allyl acrylate, allyl methacrylate, diallyl maleate, diallyl fumarate and diallyl itaconate, and the corresponding monoallyl compounds of these dicarboxylic acids. In addition, there are also a variety of other suitable graft-linked monomers. For further details, reference may be made here to, for example, U.S. Patent No. 4,148,846.

[0274] The proportion of these crosslinking monomers in the impact-modifying polymer is generally up to 5% by weight, preferably not more than 3% by weight, based on the impact-modifying polymer.

[0275] Some preferred emulsion polymers are listed below. Here we can first mention graft polymers having a core and at least one shell, which have the following structure:

[0276]

[0277] Instead of graft polymers whose structure has more than one shell, homogeneous (i.e. single-shell) elastomers composed of 1,3-butadiene, isoprene and n-butyl acrylate or copolymers thereof can also be used. These products can also be prepared by the simultaneous use of crosslinking monomers or monomers with reactive groups.

[0278] Examples of preferred emulsion polymers are: n-butyl acrylate-(meth)acrylic acid copolymers, n-butyl acrylate / glycidyl acrylate or n-butyl acrylate / glycidyl methacrylate copolymers, graft polymers having a core consisting of n-butyl acrylate or based on butadiene and having a shell consisting of the above copolymers, and copolymers of ethylene with comonomers providing reactive groups.

[0279] The elastomers can also be prepared by other conventional methods, for example by suspension polymerization.

[0280] Preference is also given to silicone rubbers, as described in DE-A 3725576, EP-A 235690, DE-A 380003 and EP-A 319 290.

[0281] Of course, mixtures of the aforementioned rubber types may also be used.

[0282] UV stabilizers which may be mentioned are various substituted resorcinols, salicylates, diphenyltriazoles and benzophenones, which are generally used in amounts of up to 2% by weight, based on the molding composition.

[0283] Materials that can be added as colorants are inorganic pigments such as titanium dioxide, ultramarine, iron oxide and carbon black, and organic pigments such as phthalocyanine, quinacridone, and dyes such as anthraquinones.

[0284] The molding compositions of the invention can comprise, as component F, 0.05 to 5% by weight, preferably 0.1 to 2% by weight, in particular 0.25 to 1.5% by weight of melanin.

[0285] Melanin is a group of phenazine dyes (azine dyes) related to phenazine blue, usually black or gray, in various forms (water-soluble, oil-soluble, alcohol-soluble), used for wool dyeing and wool printing, black dyeing of silk and coloring of leather, shoe creams, varnishes, plastics, paints, inks, etc., and also used as a microscope dye.

[0286] In industry, nitrobenzene, aniline and aniline hydrochloride are reacted with metallic iron and FeCl 3 Melanin (the name comes from the Latin niger = black) is obtained by heating.

[0287] Component C5) can be used in the form of the free base or in the form of a salt (eg hydrochloride).

[0288] More details about melanin can be found in the encyclopedia Romp Chemical Dictionary ( ChemieLexikon), Thieme Verlag Stuttgart, 1995, keyword “melanin”.

[0289] Materials that can be used as nucleating agents are sodium phenylphosphonate, alumina, silica, and preferably talc.

[0290] The thermoplastic molding compositions may also contain, as component F, flame retardants.

[0291] As component F, the thermoplastic molding material can comprise 1.0 to 10.0% by weight, preferably 2.0 to 6.0% by weight, in particular 3.0 to 5.0% by weight, of at least one phosphazene of the general formula (IX) or (X) as flame retardant.

[0292] The minimum amount of component F is at least 1.0 wt %, preferably at least 2.0 wt %, particularly preferably at least 3.0 wt %.

[0293] The maximum amount of component F is 10.0 wt %, preferably 6.0 wt %, particularly preferably 5.0 wt %.

[0294] "Phosphazene" is understood to mean a cyclic phosphazene of the general formula (IX) or a linear phosphazene of the general formula (X),

[0295]

[0296] Where m is an integer between 3 and 25, R 4 and R 4′ Same or different, and indicates C 1 -C 20 Alkyl, C 6 -C 30 Aryl, C 6 -C 30 Arylalkyl or C 6 -C 30 Alkyl substituted aryl,

[0297]

[0298] Wherein, n represents 3 to 1000, and X represents -N=P(OPh) 3 Or -N=P(O)OPh, Y represents -P(OPh) 4 or -P(O)(OPh) 2 .

[0299] The production of such phosphazenes is described in EP-A 0945478 .

[0300] Particularly preferred is formula (XI): 3 N 3 C 36 Cyclophenoxyphosphazene,

[0301]

[0302] or a linear phenoxyphosphazene according to formula (XII),

[0303]

[0304] The phenyl group may be optionally substituted. Phosphazenes in the context of the present application are described in Mark, JE, Allcock, HR, West, R., Inorganic Polymers, Prentice Hall, 1992, pp. 61-141.

[0305] Preference is given to using cyclic phenoxyphosphazenes having at least three phenoxyphosphazene units as component F. The corresponding phenoxyphosphazenes are described, for example, in paragraphs

[0051] to

[0053] of US 2010 / 0261818. Reference may be made in particular to formula (I) therein. The corresponding cyclic phenoxyphosphazenes are further described in EP-A-2100919, in particular paragraphs

[0034] to

[0038] therein. The production may be carried out as described in paragraph

[0041] of EP-A-2100919. In one embodiment of the invention, the phenyl group in the cyclic phenoxyphosphazene may be C 1-4 Alkyl substitution is preferred when pure phenyl groups are involved.

[0306] For further description of cyclophosphazene, see Chemie Lexikon, 9th edition, keyword "phosphazene". For example, by 5 and NH 4 The cyclophosphazene is produced by reacting phenol with phenoxy groups.

[0307] Cyclophenoxyphosphazene compounds can be prepared, for example, as described in Allcock, HR, Phosphorus and Nitrogen Compounds (Academic Press, 1972) and Mark, JE, Allcock HR, West, R., Inorganic Polymers (Prentice Hall, 1992).

[0308] Component F is preferably a mixture of cyclic phenoxyphosphazenes having three and four phenoxyphosphazene units. The weight ratio of rings comprising three phenoxyphosphazene units to rings comprising four phenoxyphosphazene units is preferably about 80:20. Larger rings of phenoxyphosphazene units may also be present, but in smaller quantities. Suitable cyclic phenoxyphosphazenes are available from Fushimi Pharmaceutical Co., Ltd. under the name FP-100. This is a matt white / yellowish solid with a melting point of 110°C, a phosphorus content of 13.4% and a nitrogen content of 6.0%. The proportion of rings containing three phenoxyphosphazene units is at least 80.0 wt%.

[0309] The thermoplastic molding material preferably comprises 1.0 to 6.0% by weight, preferably 2.5 to 5.5% by weight, in particular 3.0 to 5.0% by weight, of at least one aliphatic or aromatic phosphoric acid ester or polyphosphoric acid as flame retardant.

[0310] Therefore, solid non-migrating phosphates with a melting point between 70°C and 150°C are particularly preferred. This results in products that are easy to meter and show significantly less migration in the molding material. Particularly preferred examples are the commercially available phosphate ester PX-200 (CAS: 139189-30-3) from Daihachi or Sol DP from ICL-IP. When this allows the preferred melting range to be achieved, other phosphates with appropriately substituted phenyl groups can be envisioned. Depending on the substitution pattern in the ortho or para position on the aromatic ring, the general structural formula is as follows:

[0311]

[0312]

[0313] in,

[0314] R 1 = hydrogen, methyl, ethyl or isopropyl, but preferably hydrogen.

[0315] n=between 0 and 7, but preferably 0.

[0316] R 2-6 = hydrogen, methyl, ethyl or isopropyl, but preferably methyl. 6 Preferably, it is the same as R4 and R5.

[0317] m=can be, but needs to be different, and is between 1, 2, 3, 4 and 5, but preferably 2.

[0318] R" may be hydrogen, methyl, ethyl or cyclopropyl, but is preferably methyl and hydrogen.

[0319] The PX-200 is a specific example:

[0320]

[0321] Particular preference is given to using at least one aromatic ester of polyphosphoric acid. Such aromatic polyphosphates are available, for example, from Daihachi Chemical under the name PX-200.

[0322] As component F, the thermoplastic molding material according to the invention can comprise 5.0-30.0 wt %, preferably 10.0-25.0 wt %, in particular 12.0-20.0 wt %, for example about 16.0 wt %, of at least one metal phosphite or phosphinate as described below as a flame retardant.

[0323] The minimum amount of component F is 5.0 wt%, preferably 10.0 wt%, especially 12.0 wt%.

[0324] The maximum amount of component F is 30.0 wt %, preferably 25.0 wt %, particularly preferably 20.0 wt %.

[0325] Examples of preferred flame retardants of component F are metal phosphites derived from hypophosphorous acid. For example, metal salts of hypophosphorous acid with Mg, Ca, Al or Zn as metal can be used. Aluminum hypophosphite is particularly preferred here.

[0326] Also suitable are phosphinates of the formula (I) and / or diphosphonates of the formula (II) or polymers thereof,

[0327]

[0328] in,

[0329] R 1 , R 2 same or different and represent hydrogen, C 1 -C 6 Alkyl, linear or branched and / or aromatic;

[0330] R 3 Represents C 1 -C 10 Alkylene, straight or branched chain, C 6 -C 10 -arylene, -alkylenearylene or -arylenealkylene;

[0331] M represents Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, K and / or a protonated nitrogen group;

[0332] m=1 to 4; n=1 to 4; x=1 to 4, preferably m=3, x=3.

[0333] Preferably, R 1 , R 2 are the same or different and represent hydrogen, methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-pentyl and / or phenyl.

[0334] Preferably, R 3 represents methylene, ethylene, n-propylene, isopropylene, n-butylene, tert-butylene, n-pentylene, n-octylene or n-dodecylene, phenylene or naphthylene; methylphenylene, ethylphenylene, tert-butylphenylene, methylnaphthylene, ethylnaphthylene or tert-butylnaphthylene; phenylmethylene, phenylethylene, phenylpropylene or phenylbutylene.

[0335] Particularly preferably, R 1 , R 2 is hydrogen, methyl, ethyl, and M is Al, particularly preferably aluminum hypophosphite.

[0336] The production of phosphites is preferably achieved by precipitation of the corresponding metal salt from aqueous solution. However, the phosphites can also be prepared on suitable inorganic metal oxides or sulfides as support materials (white pigments, e.g. TiO 2 SnO 2 、ZnO、ZnS、SiO 2 ). This thus provides surface modified pigments which can be used as laser markable flame retardants for thermoplastic polyesters.

[0337] Preferably, when using metal salts of substituted phosphorous acids, in which, compared to hypophosphorous acid, one or two hydrogen atoms have been replaced by phenyl, methyl, ethyl, propyl, isobutyl, isooctyl, or the group R'-CH-OH has been replaced by R'-H, phenyl, tolyl. The metal is preferably Mg, Ca, Al, Zn, Ti, Fe. Particularly preferred is diethylaluminum phosphite (DEPAL).

[0338] For a description of phosphites or bisphosphonates, reference is made to DE-A 19960671, also to DE-A 4430932 and DE-A 199933901.

[0339] Further flame retardants are, for example, halogen-containing flame retardants.

[0340] Suitable halogen-containing flame retardants are preferably brominated compounds, such as brominated diphenyl ether, brominated trimethylphenylindane (FR 1808 from DSB), tetrabromobisphenol A and hexabromocyclododecane.

[0341] Suitable flame retardants are preferably brominated compounds, such as brominated oligocarbonates (BC 52 or BC 58 from Great Lake), having the structural formula:

[0342]

[0343] Particularly suitable are polypentabromobenzyl acrylates where n>4 (eg FR 1025 from ICL-IP has the formula:

[0344]

[0345] Preferred brominated compounds also include oligomeric reaction products (n>3) of tetrabromobisphenol A with epoxides (such as FR2300 and 2400 from DSB) having the formula:

[0346]

[0347] The brominated oligostyrenes preferably used as flame retardants have an average degree of polymerization (number average) between 3 and 90, preferably between 5 and 60, measured by vapor pressure osmometry in toluene. The same applies to cyclic oligomers. In a preferred embodiment of the invention, the brominated oligostyrenes have the formula I shown below, wherein R represents hydrogen or an aliphatic group, in particular an alkyl group, such as CH 2 or C 2 H 5 , and n represents the number of repeating chain building blocks. 1 This can be hydrogen or bromine or a fragment of a conventional free radical former:

[0348]

[0349] The value of n can be from 1 to 88, preferably from 3 to 58. The brominated oligostyrene contains 40.0-80.0 wt %, preferably 55.0-70.0 wt % of bromine. Preference is given to products consisting mainly of polydibromostyrene. These substances are meltable without decomposition and are, for example, soluble in tetrahydrofuran. The substances can be produced by ring bromination - optionally aliphatic hydrogenation - of styrene oligomers, for example obtained by thermal polymerization of styrene (according to DT-OS 2537385) or by free radical oligomers of appropriately brominated styrene. The production of flame retardants can also be achieved by ionic oligomerization of styrene and subsequent bromination. The amount of brominated oligostyrene required to impart flame retardant properties to the polyamide depends on the bromine content. The bromine content in the molding material of the invention is 2.0-30.0 wt %, preferably 5.0-12.0 wt %.

[0350] The brominated polystyrene according to the invention is generally obtained by the process described in EP-A 047549:

[0351]

[0352] The brominated polystyrenes obtainable and commercially available by this process are predominantly ring-substituted tribrominated products. n' (see III) generally has a value of 125 to 1500, which corresponds to a molecular weight of 42500 to 235000, preferably 130000 to 135000.

[0353] The bromine content (based on the content of ring-substituted bromine) is generally at least 50.0 wt %, preferably at least 60.0 wt %, particularly preferably 65.0 wt %.

[0354] The glass transition temperature of commercially available powdered products is generally between 160°C and 200°C. For example, they are available from Albemarle under the name HP-7010 and Ferro Company under the name PB 68 obtained.

[0355] Mixtures of brominated oligostyrenes and brominated polystyrenes can also be used in the molding materials of the invention, the mixing ratio being freely selectable.

[0356] Also suitable are chlorine-containing flame retardants, preferably Decoran from OxyChem

[0357] Suitable halogen-containing flame retardants are preferably ring-brominated polystyrene, brominated polybenzyl acrylate, brominated bisphenol A epoxy oligomer or brominated bisphenol A polycarbonate.

[0358] In one embodiment of the invention, no halogen-containing flame retardants are used in the thermoplastic molding materials according to the invention.

[0359] In the context of the present invention, flame-retardant melamine compounds suitable as component F are melamine compounds which, when added to glass-fiber-filled polyamide molding materials, reduce the flammability and influence the fire behavior in a flame-retardant manner, resulting in improved performance in the UL 94 test and the heating wire test.

[0360] The melamine compound is, for example, selected from melamine borate, melamine phosphate, melamine sulfate, melamine pyrophosphate, melam, melem, melon or melamine cyanurate or a mixture thereof.

[0361] Melamine cyanurates which are preferably suitable according to the invention are reaction products of preferably equimolar amounts of melamine (formula I) and cyanuric acid / isocyanuric acid (formulas Ia and Ib).

[0362]

[0363] For example, it is obtained by reacting an aqueous solution of the starting compound at 90°C to 100°C. The commercially available product is a white powder with an average particle size of d 50 1.5-7μm, d 99 The value is less than 50μm.

[0364] Other suitable compounds (also generally described as salts or adducts) are melamine sulfates, melamine, melamine borates, oxalates, primary phosphates, secondary phosphates and secondary pyrophosphates, melamine neopentyl glycol borate. According to the invention, the molding material preferably does not contain polymeric melamine phosphates (CAS No. 56386-64-2 or 218768-84-4).

[0365] This is understood to mean melamine polyphosphates of 1,3,5-triazine compounds, whose average degree of condensation n is between 20 and 200 and whose 1,3,5-triazine content is from 1.1 to 2.0 mol of 1,3,5-triazine compounds per mole of phosphorus atom, the 1,3,5-triazine compound being selected from melamine, melam, melem, melon, ammeline, melamine monoamide, 2-ureidomelamine, acetoguanamine, benzoguanamine and diaminophenyltriazine. Preferably, the n value of such salts is generally between 40 and 150, and the ratio of 1,3,5-triazine compounds per mole of phosphorus atom is preferably between 1.2 and 1.8. Furthermore, the pH of a 10 wt.% aqueous slurry of the salt prepared according to EP-B1 095 030 is generally greater than 4.5, preferably at least 5.0. The pH value is usually determined by adding 25 g of salt and 225 g of clean water at 25°C to a 300 ml beaker, stirring the resulting aqueous slurry for 30 minutes, and then measuring the pH value. The above n value, i.e., the number average degree of condensation, can be determined by 31P solid-state NMR. JR van Wazer, CF Callis, J. Shoolery and R. Jones, J. Am. Chem. Soc., 78, 5715, 1956 disclosed that the number of adjacent phosphate groups gives a unique chemical shift, which allows a clear distinction between orthophosphate, pyrophosphate and polyphosphate.

[0366] Suitable guanidine salts are:

[0367]

[0368] In the context of the present invention, "compounds" are to be understood as meaning not only, for example, benzoguanidine itself and its adducts / salts, but also nitrogen-substituted derivatives and their addition products / salts.

[0369] Also suitable is ammonium polyphosphate (NH 4 PO 3 ) n , wherein n is about 200 to 1000, preferably 600 to 800, and tris(hydroxyethyl)isocyanurate (THEIC) of formula IV,

[0370]

[0371] or reaction products thereof with aromatic carboxylic acids Ar(COOH)m, which may optionally be present in a mixture with one another, wherein Ar represents a monocyclic, bicyclic or tricyclic aromatic six-membered ring system and m is 2, 3 or 4.

[0372] Examples of suitable carboxylic acids include phthalic acid, isophthalic acid, terephthalic acid, 1,3,5-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, pyromellitic acid, methylbenzoic acid, nitrous acid, 1-naphthoic acid, 2-naphthalenedicarboxylic acid, naphthalene dicarboxylic acid, and diphthalic acid.

[0373] According to the process of EP-A 584567, production is carried out by reaction of tris(hydroxyethyl)isocyanurate with an acid, its alkyl ester or its halide.

[0374] The reaction products are mixtures of monomeric esters and oligomeric esters, which may also be crosslinked. The degree of oligomerization is generally between 2 and about 100, preferably between 2 and 20. Preference is given to using mixtures of THEIC and / or its reaction products with phosphorus-nitrogen-containing compounds, in particular (NH 4 PO 3 ) n or melamine pyrophosphate or polymerized melamine phosphate. For example, (NH 4 PO 3 ) n The mixing ratio with THEIC is preferably 90.0-50.0:10.0-50.0, in particular 80.0-50.0:50.0-20.0, based on the wt % of the mixture of these compounds.

[0375] Likewise suitable flame retardants are benzoguanidine compounds of the formula V, in particular adducts thereof with phosphoric acid, boric acid and / or pyrophosphoric acid,

[0376]

[0377] Therein R, R' denotes a straight-chain or branched alkyl group having 1 to 10 carbon atoms, preferably hydrogen, and in particular adducts thereof with phosphoric acid, boric acid and / or pyrophosphoric acid.

[0378] Also preferred are allantoin compounds of the formula VI, and their salts with phosphoric acid, boric acid and / or pyrophosphoric acid, and glycolurils of the formula VII or their salts with the above-mentioned acids,

[0379]

[0380] Wherein R and R′ are as defined in Formula V,

[0381]

[0382] wherein R is as defined in Formula V.

[0383] Suitable products are commercially available or obtainable according to DE-A 196 14 424.

[0384] The cyanoguanidine (formula VIII) which can be used according to the invention can be obtained, for example, by reacting calcium cyanoamide with carbonic acid, the cyanoamide dimerizing at pH 9 to pH 10 to provide the cyanoguanidine group.

[0385]

[0386] The commercially available product is a white powder with a melting point of 209°C to 211°C.

[0387] Particular preference is given to using melamine cyanurate (e.g. MC25).

[0388] It is also possible to use isolated metal oxides such as antimony trioxide, antimony pentoxide and sodium antimonate and similar metal oxides. However, it is best to avoid the use of such metal oxides because they are already present in component F. For a description of pentabromophenyl acrylate and antimony trioxide or antimony pentoxide, reference is made to EP-A 0 624 626.

[0389] Phosphorus, such as red phosphorus, can also be used as a flame retardant. Red phosphorus can be used, for example, in the form of a masterbatch.

[0390] Also considered are dicarboxylic acids of the formula,

[0391]

[0392] in,

[0393] R 1 To R 4 independently of one another represent halogen or hydrogen, provided that at least one radical R 1 To R 4 represents halogen,

[0394] x = 1 to 3, preferably 1, 2,

[0395] m=1 to 9, preferably 1 to 3, 6, 9, especially 1 to 3,

[0396] n=2 to 3,

[0397] M = alkaline earth metals, nickel, cerium, iron, indium, gallium, aluminum, lead, yttrium, zinc, mercury.

[0398] Preferred dicarboxylates include, independently of one another, Cl or Br or H as radical R 1 To R 4 , particularly preferably all radicals R 1 To R 4 It is Cl and / or Br.

[0399] As the metal M, Be, Mg, Ca, Sr, Ba, Al, Zn and Fe are preferred.

[0400] Such dicarboxylates are commercially available or can be produced according to the method described in US Pat. No. 3,354,191.

[0401] Functional polymers can also be used as component F. These can be, for example, flame retardant polymers. Such polymers are described, for example, in US 8314202 and contain 1,2-bis[4-(2-hydroxyethoxy)phenyl]ethanone repeating units. Another suitable functional polymer for increasing the amount of carbon residues is poly(2,6-dimethyl-1,4-phenoxy) (PPPO).

[0402] The thermoplastic molding compositions of the invention can be produced by methods known per se, by mixing the starting components in conventional mixing equipment (e.g. screw-based extruders, Brabender mixers or Banbury mixers) and then extruding them. After extrusion, the extrudate can be cooled and pelletized. It is also possible to premix the individual components and then add the remaining raw materials individually and / or in the form of a mixture. The mixing temperature is generally 230 to 320° C.

[0403] These materials are suitable for producing any type of fibers, foils and moldings. Some examples are: cylinder head covers, motorcycle covers, intake manifolds, charge air cooler covers, plug connectors, gears, cooling fan wheels and cooling water tanks.

[0404] In the electrical and electronic fields, the improved flow polyamide can be used to produce plugs, plug parts, plug connectors, membrane switches, printed circuit board modules, microelectronic components, coils, I / O plug connectors, printed circuit substrate (PCB) plugs, flexible printed circuit (FPC) plugs, flexible integrated circuit (FFC) plugs, high-speed plug connections, terminal blocks, connector plugs, device connectors, cable harness assemblies, circuit mounts, circuit mount assemblies, three-dimensional injection molded circuit mounts, electrical connection components and electromechanical components.

[0405] Possible uses inside the car are instrument panels, steering column switches, seat components, headrests, center consoles, transmission components and door modules, while possible uses outside the car include door handles, exterior mirror components, windshield wiper components, windshield wiper guards, grilles, roof rails, sunroof frames, engine hoods, cylinder head covers, air intake ducts (especially intake manifolds), windshield wipers and external body parts.

[0406] The combination of components B and C produces an effective system that stabilizes polyamides at temperatures of 180°C and above while remaining a completely metal halide-free system.

[0407] In a preferred embodiment, the thermoplastic molding compositions are completely free of halides, so that they also contain no halogen-containing flame retardants.

[0408] In particular, the combination of polyethyleneimine homopolymers or copolymers with secondary aromatic amines and / or condensation products of secondary aromatic amines with aliphatic aldehydes, aliphatic ketones or mixtures thereof has proven to be an effective system for stabilizing polyamides. Even under moisture absorption or electrical tension, the additives do not float to the surface. Thus, contamination and corrosion of electrical components can be avoided. Example

[0409] The following components were used:

[0410] PA1: polyamide-66, viscosity 150 ml / g, measured according to ISO 307 at 25° C. in a 0.5 wt % solution in 96 wt % sulfuric acid, melting point 260° C. (from BASF SE A27)

[0411] PA2: Polyamide 6, viscosity 150 ml / g, measured according to ISO 307 at 25° C. in a 0.5 wt % solution in 96 wt % sulfuric acid, melting point 220° C. (from BASF SE B27)

[0412] GF: Standard E-glass fiber, NEG T249H

[0413] Lubricant: Ethylene bisstearamide (EBS) from Lonza Cologne GmbH

[0414] Stabilizer 1: Cuprous iodide (CAS: 7681-65-4)

[0415] Stabilizer 2: Potassium iodide (CAS: 7681-11-0)

[0416] Stabilizer 3: OKAFLEX from OKA Tec GmbH TM EM

[0417] Stabilizer 4: Polyethyleneimine (CAS: 9002-98-6), from BASF SE WF

[0418] Colorant: Solvent Black 7 (CAS: 8005-02-5)

[0419] Preparation of particles

[0420] The natural colored polyamide pellets were previously dried in a drying oven at 100°C for 4 hours to a moisture content below 0.1%, while all other ingredients were premixed in a rotary mixer for 10 minutes. In the next step, the dried polyamide pellets were melt-extruded together with the dry blended ingredients and pelletized using a twin-screw extruder with a diameter of 25 mm and an L / D ratio of 44 at a cylinder temperature of 300°C for PA66 and 280°C for PA6. The resulting pellets were injection molded on an injection molding machine at a melt temperature of 300°C (PA66) and a melt temperature of 280°C (PA6) onto various samples for adjacent characterization.

[0421] The composition and mechanical data of the invention (INV) and comparative examples (COMP) are listed in Table 1 below.

[0422] The tensile modulus of elasticity, tensile stress at break and tensile strain at break are determined according to ISO 527. The Charpy (notched) impact strength is determined according to ISO 179-2 / 1eU and ISO 179-2 / 1eAf, respectively. The melting point and crystallization temperature are determined using differential scanning calorimetry (DSC) according to ISO 11357. All specifications refer to the versions valid in 2020.

[0423] Heat aging experiments were conducted in a standard laboratory oven at elevated temperature and air as shown in the table below. The retention of tensile strength and elongation at break after heat aging was compared to the original specimens, with the non-heat aged control specimens considered to be 100%.

[0424] Table 1

[0425]

[0426] The above examples illustrate that by using a combination of stabilizer 4 (polyethyleneimine according to component B) and stabilizer 3 (according to component C), polyamide molding compositions can be obtained that exhibit high retention of tensile strength after long-term heat treatment. High retention of tensile strength can be achieved without using CuI and KI.

[0427] Compared to a stabilizer system formed of CuI / KI, superior results were obtained. When compared to a stabilizer system comprising CuI, KI and polyethyleneimine, the stabilized system according to the invention produced similar tensile strengths after heat aging at 180°C and improved tensile strengths after heat aging at 150°C. The compositions "Invention 1" and "Invention 2" according to the invention did not require the presence of CuI / KI to achieve this effect.

[0428] Similar results were obtained when polyamide 6 was used instead of polyamide 66 as the thermoplastic polymer, see Example "Invention 2".

[0429] The above examples illustrate that the retention of tensile strength can be significantly improved, especially at an aging temperature of 150°C, by using a polyethyleneimine homopolymer or copolymer in combination with an aromatic amine co-stabilizer selected from secondary aromatic amine compounds and / or condensation products of secondary aromatic amines, aliphatic aldehydes and aliphatic ketones.

Claims

1. A thermoplastic molding composition comprising: a) 30-99.8 wt % of at least one thermoplastic polyamide as component A; b) 0.001 to 5 wt% of at least one polyethyleneimine homopolymer or copolymer as component B; c) 0.1 to 2.0 wt % of at least one condensation product of a secondary aromatic amine with an aliphatic aldehyde, an aliphatic ketone or a mixture thereof, or a combination of at least one secondary aromatic amine and said at least one condensation product, as component C; d) 0-3 wt% of at least one lubricant as component D; e) 0-50 wt% of at least one fibrous filler and / or particulate filler as component E; f) 0-25 wt% of other additives as component F, Wherein, the total weight % of components A to F is 100wt%, It does not contain copper.

2. The thermoplastic molding composition according to claim 1, wherein component B is selected from: - homopolymers of ethyleneimine, - copolymers of ethyleneimine and of amines having at least two amino groups, - cross-linked polyethyleneimine, - grafted polyethyleneimine, - amidated polymers obtainable by reaction of polyethylene imine with carboxylic acids or carboxylic esters, carboxylic anhydrides, carboxamides or carbonyl halides, - alkoxylated polyethyleneimine, - hydroxyl-containing polyethyleneimine, - amphoteric polyethyleneimine, and - Lipophilic polyethyleneimine.

3. The thermoplastic molding composition according to claim 1 or 2, wherein the weight average molecular weight Mw of component B is 100 to 3000000 g / mol.

4. The thermoplastic molding composition according to claim 3, wherein the weight average molecular weight Mw of component B is 500 to 2000000 g / mol.

5. The thermoplastic molding composition according to claim 4, wherein the weight average molecular weight Mw of component B is greater than 700 to 150000 g / mol.

6. The thermoplastic molding composition according to claim 1 or 2, wherein component B is a polyethyleneimine homopolymer having a weight average molecular weight Mw of 10000 to 50000 g / mol.

7. The thermoplastic molding composition according to claim 1 or 2, wherein component D is selected from the group consisting of aluminum salts, alkali metal salts, alkaline earth metal salts, esters or amides of fatty acids having 10 to 44 carbon atoms.

8. The thermoplastic molding composition according to claim 1 or 2, which is free of metal halides.

9. The thermoplastic molding composition according to claim 1 or 2, wherein component C comprises at least one condensation product of a diaromatic amine with formaldehyde and / or acetone.

10. The thermoplastic molding composition according to claim 1 or 2, wherein component C is at least one condensation product of a diaromatic amine with formaldehyde and / or acetone.

11. The thermoplastic molding composition according to claim 9, wherein component C further comprises at least one secondary aromatic amine.

12. The thermoplastic molding composition according to claim 1 or 2, wherein component D is present in an amount of 0.05 to 3 wt%.

13. The thermoplastic molding composition according to claim 12, wherein component D is present in an amount of 0.1 to 1.5 wt%.

14. The thermoplastic molding composition according to claim 13, wherein component D is present in an amount of 0.1 wt% to 1.0 wt%.

15. The thermoplastic molding composition according to claim 1 or 2, wherein component E comprises glass fibers and is present in an amount of 10 to 50 wt%.

16. The thermoplastic molding composition of claim 15, wherein component E comprises glass fibers and is present in an amount of 15-45 wt%.

17. The thermoplastic molding composition according to claim 16, wherein component E comprises glass fibers and is present in an amount of 20-40 wt%.

18. Process for producing the thermoplastic molding composition according to claim 1, by mixing components A to F.

19. Use of the thermoplastic molding composition according to any of claims 1 to 17 for producing fibers, foils and moldings of any type.

20. Fibers, foils or moldings made from the thermoplastic molding composition according to any one of claims 1 to 17.

Citation Information

Patent Citations

  • Thermoplastic molded mass, useful for the preparation of fibers, molded bodies or foil, comprises a thermoplastic polyamide, a high- or hyper- branched polyester in an acid or alcohol component containing aromatic core, and an additive

    DE102009011668A1

  • process for the production of polyamides

    DE10313681A1

  • Process for stabilizing high-molecular, linear polycondensates containing amide groups

    DE1123103A

  • Process for Stabilizing Polycaprolactam

    DE1152252B

  • synergistic flame retardant combination for polymers

    DE19614424A1