Polyorganosiloxane hybrid pressure-sensitive adhesive and preparation and use methods thereof
The existing solution is solved by using functionalized polyorganosiloxane and polyorganosilate resins with poly(meth)acrylate groups in a polyorganosiloxane mixed pressure sensitive adhesive, combined with peroxide catalysts In the technology, the problem of low crosslinking and grafting efficiency during polymerization process is prepared, and the performance of the adhesive is improved.
Patent Information
- Application Number
- CN202180022663.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-15
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-03-15
AI Technical Summary
In the prior art, thiol-functionalized polydimethylsiloxane may be crosslinked due to the reaction of aliphatic unsaturated groups during radical polymerization, and the grafting efficiency is limited by the level of thiol-functionalization, making it difficult to effectively manufacture. Polyorganosiloxanes with high molecular weight poly(meth)acrylate grafted.
Using a polyorganosiloxane mixed pressure sensitive adhesive composition, including functionalized polyorganosiloxane having poly(meth)acrylate groups, polyorganosilate resins and peroxide catalysts, by A specific reaction step and catalyst combination are used to prepare high molecular weight poly(meth)acrylate grafted polyorganosiloxanes for use in free radical reaction curable mixed pressure sensitive adhesives.
The molecular weight and grafting efficiency of poly(meth)acrylate grafted polyorganosiloxane are improved, crosslinking is avoided, and the performance and stability of the adhesive are enhanced.
Smart Images

Figure BDA0003853873330000062 
Figure BDA0003853873330000082 
Figure BDA0003853873330000091
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of U.S. Provisional Patent Application Serial No. 63 / 012,293, filed on April 20, 2020, under 35 U.S.C. § 119(e). U.S. Provisional Patent Application Serial No. 63 / 012,293 is hereby incorporated by reference. Technical Field
[0003] Polyorganosiloxanes having silicon-bonded poly(meth)acrylate groups (hereinafter referred to as "poly(meth)acrylate grafted polyorganosiloxanes") can be used in free radical reaction curable polyorganosiloxane hybrid pressure sensitive adhesive (hybrid PSA) compositions. Also disclosed are methods for preparing and using the hybrid PSA from the above-mentioned compositions. Background Art
[0004] Polyorganosiloxanes and acrylates have been used as bases for pressure sensitive adhesives. There is a need in the industry to provide pressure sensitive adhesives that have the properties of both polyorganosiloxanes and acrylates.
[0005] By polymerizing in the presence of a mercapto-functionalized polydimethylsiloxane, free radical polymerization can be used to bind acrylic chains to the polydimethylsiloxane backbone. The mercapto groups will act as chain transfer agents and enable acrylic chains to be grafted onto the polydimethylsiloxane chains as side groups and / or end groups. However, if the mercapto-functionalized polydimethylsiloxane also contains vinyl or other aliphatic unsaturated monovalent hydrocarbon functional groups, the system may become saturated or crosslinked due to the reaction of the aliphatic unsaturated groups during free radical polymerization. In addition, since chain transfer is a kinetically controlled process, the grafting efficiency may be low due to the low level of mercapto-functionalization. Therefore, an improved method for making poly(meth)acrylate grafted polyorganosiloxanes is desired. Summary of the invention
[0006] A polyorganosiloxane hybrid pressure-sensitive adhesive (hybrid PSA) composition comprising:
[0007] (I) a pressure-sensitive adhesive matrix comprising sufficient to provide 15 wt % to 40 wt % of
[0008] % by weight of the starting material (IA) and 5 to 60 wt % of the starting material (IB), a physical mixture of the starting materials (IA) and (IB), a reaction product of the starting materials (IA) and (IB), or a combination of the physical mixture and the reaction product; wherein
[0009] The starting material (IA) is a functionalized polyorganosiloxane having poly(meth)acrylate groups, wherein the functionalized polyorganosiloxane has the following unit formula:
[0010] [R 3 w (R 5 -SR”)(OR 4 ) (2-w) Si-O 1 / 2 ] p [R 3 v (R 5 -SR”)(OR 4 ) (1-v) Si-O 2 / 2 ] q [(R 5 -SR”)Si-O 3 / 2 ] k (R 6 R 7 2SiO 1 / 2 ) r (R 7 2SiO 2 / 2 ) s (R 6 R 7 SiO 2 / 2 ) t (R 7 3SiO 1 / 2 ) u , where each subscript w is independently 0, 1, or 2, each subscript v is independently 0 or 1, and each R 3 is an independently selected monovalent hydrocarbon group; each R 4 is an independently selected alkyl group; each R 5 is an independently selected divalent hydrocarbon group, each R" is independently a (meth)acrylate polymer or copolymer, each R 6 Selected from the group consisting of hydroxyl groups and aliphatic unsaturated monovalent hydrocarbon groups, each R 7 is an independently selected monovalent hydrocarbon group free of aliphatic unsaturation, subscript p ≥ 0, subscript q ≥ 0, subscript k ≥ 0, the amount (p+q+k) ≥ 1, subscript r ≥ 0, subscript s ≥ 0, subscript t ≥ 0, subscript u ≥ 0, the amount (r+t) ≥ 1, and the amount (p+q+k+r+s+t+u) is sufficient to provide the polyorganosiloxane with a molecular weight of at least 50 kDa; and
[0011] The starting material (IB) is a polyorganosilicate resin having a unit formula (R 15 2R 16 SiO 1 / 2 )x (R 15 3SiO 1 / 2 ) y (SiO 4 / 2 ) z , where R 15 is an alkyl group, an aryl group or an aralkyl group, such as methyl and phenyl; and R 16 is an alkenyl group having 2 to 18 carbon atoms, such as vinyl, allyl or hexenyl; subscripts x, y and z are mole fractions; subscript x≥0, subscript y≥0, subscript z>0, amount (x+y)>0, amount (x+y+z)≤1, subscripts x, y and z have values such that 0.9≤(x+y) / z≤1.3; the polyorganosilicate resin further comprises a hydroxyl group content of up to 5 wt % based on the weight of the polyorganosilicate resin; and the polyorganosilicate resin has a number average molecular weight of>1,500 Da as measured by gel permeation chromatography;
[0012] (II) a peroxide catalyst, wherein each R in the starting material (A) 6 When each R in the starting material (A) is hydroxyl, the peroxide catalyst is present in an amount of 2 to 4 wt %. 6 When the aliphatically unsaturated monovalent hydrocarbon group, the peroxide catalyst is present in an amount of 3 wt % to 4 wt %; and
[0013] 0 wt % to 70 wt % of (III) solvent; wherein all percentages are by weight based on the combined weight of all starting materials in the polyorganosiloxane hybrid pressure-sensitive adhesive composition.
[0014] The above-described mixed PSA composition can be used to prepare an adhesive article in a method comprising the steps of:
[0015] 1) coating the mixed PSA composition on the surface of a substrate, and
[0016] 2) Curing the hybrid PSA composition to form a hybrid PSA on the surface of the substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 shows a representative example of Scheme 1, where a (meth)acrylate polymer grows away from a thiol functional group after a hydrogen atom is abstracted from a free radical initiator fragment or a growing chain. The (meth)acrylate oligomer is then terminated / endcapped with a hydrogen atom from a different thiol molecule to form an alkoxysilyl functionalized (meth)acrylate macromonomer. This is described in Reference Example A below.
[0018] Figure 2A representative example of Scheme 2 for preparing the bisvinyl terminated poly(meth)acrylate grafted polyorganosiloxane described in Reference Example D below is shown. Figure 2 In the process, a bis-vinyl terminated polydimethylsiloxane, a bis-hydroxy terminated polydimethylsiloxane and an alkoxysilyl functionalized (meth)acrylate macromonomer prepared in Scheme 1 of FIG. 1 are reacted in the presence of a phosphazene catalyst and a solvent (toluene) to form a bis-vinyl terminated poly(meth)acrylate grafted polyorganosiloxane having the unit formula shown in the figure.
[0019] Figure 3 A representative example of Scheme 3 for preparing the bishydroxy-terminated poly(meth)acrylate-grafted polyorganosiloxane described in Reference Example C below is shown. Figure 3 In the embodiment of the present invention, a bishydroxy-terminated polydimethylsiloxane and an alkoxysilyl-functionalized (meth)acrylate macromonomer prepared in Scheme 1 of FIG. 1 are reacted in the presence of a phosphazene catalyst and a solvent (toluene) to form a bishydroxy-functionalized grafted poly(meth)acrylate-grafted polyorganosiloxane having a unit formula shown in the figure. DETAILED DESCRIPTION
[0020] The present invention discloses a method for preparing a product containing poly(meth)acrylate grafted polyorganosiloxane. The method comprises:
[0021] I) will include the following starting material combination:
[0022] A) an alkoxysilyl-functional (meth)acrylate macromonomer;
[0023] B) a polydiorganosiloxane selected from the group consisting of:
[0024] B1) an unsaturated polydiorganosiloxane having at least one silicon-bonded aliphatically unsaturated group per molecule;
[0025] B2) a hydroxy-functional polydiorganosiloxane having at least two silicon-bonded hydroxyl groups per molecule, and
[0026] B3) A combination of B1) and B2);
[0027] C) a condensation reaction catalyst;
[0028] Optionally, D) a polydialkylsiloxane; and
[0029] Optionally, E) a solvent; thereby preparing a product comprising a poly(meth)acrylate-grafted polyorganosiloxane and byproducts;
[0030] II) removing all or part of the by-products during and / or after step I);
[0031] Optionally, III) neutralizing the product; and
[0032] Optionally IV) recovering the poly(meth)acrylate-grafted polyorganosiloxane.
[0033] Step I) in the method may be performed by any convenient means, such as mixing. Step I) may be performed under inert conditions, such as nitrogen or other inert gases.
[0034] Combining the starting materials can be carried out at an elevated temperature, such as heating at 80° C. to 120° C. A solvent may optionally be added, for example, to facilitate combining the starting materials. Combining the starting materials may be carried out in any order of addition, such as combining A) alkoxysilyl functionalized (meth) acrylate macromonomers, B) polydiorganosiloxanes (e.g., either or both of B1) unsaturated polydiorganosiloxanes and B2) hydroxyl functionalized polydiorganosiloxanes) and / or D) polydialkylsiloxanes. The resulting mixture may then be heated, and C) a condensation reaction catalyst may then be added, optionally dissolved in E) a solvent. Without wishing to be bound by theory, it is believed that adding E) a solvent may facilitate the preparation of poly(meth) acrylate grafted polyorganosiloxanes having a high MW. When the starting materials react, byproducts are produced. The byproducts may include water and / or alcohols (such as methanol). All or a portion of the byproducts may be removed during and / or after step I). Without wishing to be bound by theory, it is believed that removal of by-products may drive the reaction to completion and / or facilitate increasing MW. The by-products may be removed by any convenient means such as stripping.
[0035] Step III) of the method is to neutralize the product. Neutralization can be carried out by adding F) a neutralizing agent to the product during and / or after step II). Neutralization can be carried out at ambient temperature or at an elevated temperature. Step IV) of the method is to recover the poly(meth)acrylate grafted polyorganosiloxane. Recovery of the poly(meth)acrylate grafted polyorganosiloxane can be carried out in any convenient manner, such as filtering, stripping and / or distillation. The starting materials used in the above method are as follows.
[0036] The starting material A) alkoxysilyl-functional (meth)acrylate macromonomer used in the above method may have the formula A-1): Each R 3 is an independently selected monovalent hydrocarbon group; each R 4 is an independently selected alkyl group; R 5is a divalent hydrocarbon group; R" is a (meth)acrylate polymer or copolymer, and subscript a is 0, 1 or 2. R" may have a DP of 1 to 1,000, and alternatively 5 to 600. Alternatively, the alkoxysilyl functional (meth)acrylate macromonomer may have formula A-2): Each R 1 are independently selected from the group consisting of hydrogen and alkyl groups; R 2 are independently selected from the group consisting of hydrogen, an alkyl group, an aryl group, and an aralkyl group; subscript n is 1 to 1,000; and R 3 , R 4 and R 5 As mentioned above.
[0037] Alternatively, in formula A-2), the subscript n may be 5 to 600. 1 The alkyl group of may be an alkyl group having 1 to 4 carbon atoms; or a methyl group or an ethyl group. 1 Methyl may be used. 2 The alkyl group of may have 1 to 18 carbon atoms, or 1 to 8 carbon atoms. 2 The alkyl groups of R include methyl, ethyl, propyl and butyl. 2 The aryl group has 6 to 18 carbon atoms and includes phenyl, and is suitable for R 2 The aralkyl group has 6 to 18 carbon atoms and includes a styryl group. Alternatively, in formula A-2), each R 2 It may be an independently selected alkyl group having 1 to 18 carbon atoms or 1 to 8 carbon atoms.
[0038] Alternatively, in formulas A-1) and A-2), subscript a may be 1 or 2, or 1, and or 2. Each R 3 may be independently selected monovalent hydrocarbon groups having 1 to 18 carbon atoms. 3 The monovalent hydrocarbon groups of include alkyl groups (e.g., methyl, ethyl, propyl, and butyl) and alkenyl groups (e.g., vinyl, allyl, and hexenyl), aryl groups (such as phenyl), and aralkyl groups (such as benzyl, tolyl, xylyl, and phenethyl). Alternatively, each R 3 may be independently selected from the group consisting of alkyl and alkenyl. 3 may be an alkyl group having 1 to 8 carbon atoms. 3 It may be selected from the group consisting of methyl and vinyl.
[0039] Each R 4 It may be an independently selected alkyl group having 1 to 6 carbon atoms. 4The alkyl group includes methyl, ethyl, propyl and butyl; or methyl.
[0040] Each R 5 It may be a divalent hydrocarbon group having 1 to 18 carbon atoms.
[0041] Applicable to R 5 The divalent hydrocarbon group includes an alkylene group such as ethylene (-CH2-CH2-), propylene (such as -CH2-CH2-CH2- or -CH(CH3)CH2-), butylene or hexylene; an arylene group such as phenylene, or an alkylarylene group such as:
[0042] Alternatively, R 5 It may be an alkylene group of 2 to 6 carbon atoms, such as propylene.
[0043] The starting material (A) alkoxysilyl functional (meth)acrylate macromonomer may have a glass transition temperature (Tg) greater than -52°C as calculated using the Fox equation.
[0044]
[0045] Where T g,Fox is the glass transition of the copolymer, T g,x is the glass transition of the homopolymer x, and w x is the weight fraction of x in the copolymer.
[0046] The amount of starting material A) used in the process for preparing the above-mentioned product comprising poly(meth)acrylate grafted polyorganosiloxane depends on various factors, however, starting material A) can be used in an amount of 4% to 11% based on the combined weight of starting materials A) and B) in the process. Alternatively, based on the same basis, the amount of starting material A) can be 1% to 50%, or 5% to 10%, or 5% to 9%.
[0047] Alkoxysilyl functional (meth) acrylate monomers suitable for use as starting material A) can be prepared by known methods, such as those disclosed in U.S. Pat. No. 6,733,884 to Brown. Alternatively, the alkoxysilyl functional (meth) acrylate can be prepared by a process comprising the steps of:
[0048] 1) The starting materials are combined as follows:
[0049] i) Formula (meth)acrylate monomer, wherein R 1 and R 2 As mentioned above;
[0050] ii) Formula A mercapto-functional alkoxysilane, wherein R 3 , R 4 , R 5 and subscript a as described above;
[0051] Optionally, iii) a free radical initiator; and
[0052] Optionally, iv) a solvent; thereby preparing a product comprising an alkoxysilyl-functional (meth)acrylate macromer; and
[0053] Optionally 2) recovering A) the alkoxysilyl-functional (meth)acrylate macromonomer.
[0054] In this method, i) (meth) acrylate monomers may be combined with iv) solvent (when present) before step 1). The solvent may optionally be dried before combining with starting material i) and / or any other starting material. Alternatively, i) (meth) acrylate monomers, ii) mercapto-functionalized alkoxysilanes and iv) solvent (when present) may be combined before step 1). The resulting combination may be heated in a reactor to, for example, 50° C. to 150° C. The reaction of starting materials i) and ii) may be carried out under sufficient heating to produce free radicals. Alternatively, iii) a free radical initiator, optionally dissolved in iv) solvent, may be added to the reaction vessel. Step 1) may be carried out under inert conditions, for example by purging the reactor with nitrogen. The starting materials in step 1) may be mixed, heated, or a combination of both. For example, mixing and heating can be performed by mixing while heating the starting materials from 50°C to reflux temperature, or 50°C to 150°C, or 50°C to 110°C; or 50°C to 100°C; or 75°C to 85°C for 1 to 6 hours. The starting materials can be added in any order, however, iii) the free radical initiator can be dissolved in iv) the solvent and optionally combined with i) the (meth) acrylate monomer, and the resulting combination can then be added to the reactor containing ii) the mercapto-functional alkoxysilane. Alternatively, i) the (meth) acrylate monomer and ii) the mercapto-functional alkoxysilane can be combined to form a mixture, and then iii) the free radical initiator can be added to the mixture. Without wishing to be bound by theory, it is believed that the resulting alkoxysilyl-functional (meth) acrylate macromonomer (prepared in this order of addition) will have a different molecular weight distribution than when a different order of addition is used.
[0055] Step 2), recovery of the alkoxysilyl functionalized (meth) acrylate macromonomer can be carried out in any convenient manner, such as cooling the reaction product prepared in step 1) to room temperature, and precipitation in a non-solvent (such as an alkane such as hexane, or an alcohol such as methanol), which will precipitate the alkoxysilyl functionalized (meth) acrylate macromonomer. Recovery can also optionally include drying the precipitate, such as by heating with heat at ambient pressure or reduced pressure, for example from 80° C. to 100° C., to remove residual monomers, solvents, or both.
[0056] In the process for preparing alkoxysilyl-functional (meth)acrylate macromonomers, the starting material i) is a (meth)acrylate monomer. Suitable (meth)acrylate monomers have the formula i-1): Where R 1 and R 2 As described above. Suitable (meth)acrylate monomers are known in the art and are commercially available, and some examples are shown in Table 1. The amount of starting material i) may be 20% to 99.8%, or 30% to 90%, and or 70% to 75%, based on the combined weight of starting materials i), ii), iii) and iv).
[0057] Table 1. Exemplary (meth)acrylate monomers
[0058]
[0059]
[0060] a Tg from Polymer Properties Database (polymerdatabase.com).
[0061] In the method for preparing an alkoxysilyl-functional (meth)acrylate macromer, the starting material ii) is a mercapto-functional alkoxysilane. The mercapto-functional alkoxysilane may have the formula ii-1): The subscripts a and R 3 , R 4 and R 5As mentioned above. Suitable mercapto-functionalized alkoxysilanes are known in the art and are commercially available. These include 3-mercaptopropyl trimethoxysilane, 3-mercaptopropyl triethoxysilane, 11-mercapto undecyl trimethoxysilane, (mercaptomethyl) methyl diethoxysilane, 3-mercaptopropyl methyl dimethoxysilane, all of which are commercially available from Gelest, Inc. (Morrisville, Pennsylvania, USA). Alternatively, mercapto-functionalized alkoxysilanes such as those described above and mercapto-functionalized monoalkoxysilanes, such as 3-mercaptopropyl dimethylmethoxysilane and 3-mercaptopropyl dimethylethoxysilane, can be synthesized by known methods, such as those disclosed in U.S. Patent Application 2005 / 0124821 and Agina, EV, ACS Applied Materials & Interfaces, 2015, Vol. 22, pp. 11755-11764. The amount of starting material ii) may be 0.1% to 50%, alternatively 1% to 10%, and alternatively 1% to 8%, based on the combined weight of starting materials i), ii), iii), and iv).
[0062] The starting material iii) for preparing the alkoxysilyl functionalized (meth) acrylate macromonomer is a free radical initiator. The free radical initiator can be selected from the group consisting of: iii-1) azo compounds, iii-2) peroxides (e.g., hydroxy peroxides, peracids and peresters, such as tert-alkyl peroxypivalate) and iii-3) their combinations. Suitable free radical initiators are known in the art, see, for example, U.S. Patent 8,258,243 (column 2, lines 9-34). Alternatively, suitable free radical initiators are commercially available. For example, tert-alkyl peroxypivalate can be commercially available from Akzo Nobel, for example, tert-amyl peroxypivalate is obtained as Trigonox 125-C75, and tert-butyl peroxypivalate is obtained as Trigonox 25-C75. The amount of starting material iii) may be 0 to 5%, alternatively 0.1% to 2%, alternatively 1% to 2%, based on the combined weight of starting materials i), ii), iii) and iv).
[0063] Solvents can be used in the above method. One or more of the starting materials used in the preparation of the alkoxysilyl functionalized (meth) acrylate macromonomer can be dissolved in iv) solvent before combining with other starting materials. For example, the free radical initiator can be dissolved in solvent oil. Alternatively, the solvent can be selected from the group consisting of: iv-1) hydrocarbons with a boiling point higher than 100°C (e.g., aromatic hydrocarbons, such as toluene or xylene), iv-2) polar solvents (such as acetone, methyl ethyl ketone, methyl acetate, ethyl acetate, acetonitrile, methanol, isopropanol or tert-butyl alcohol), iv-3) silicone oil (e.g., silicone oil can be polydialkylsiloxane, as described below), and iv-4) a combination of two or more thereof. Alternatively, the solvent can be toluene, for example, to facilitate the combination of starting material A) with other starting materials to prepare poly(meth) acrylate grafted polyorganosiloxane. When the polydialkylsiloxane is used as a solvent, the polydialkylsiloxane may serve as a starting material in the process for preparing a product comprising a poly(meth)acrylate grafted polyorganosiloxane. When toluene is used, solvent exchange may not be included in the process for preparing a product comprising a poly(meth)acrylate grafted polyorganosiloxane. The amount of the starting material iv) may be 0 to 70%, or 0 to 25%, based on the combined weight of the starting materials i), ii), iii) and iv).
[0064] In the process for preparing a product comprising poly(meth)acrylate grafted polyorganosiloxanes, the starting material B) is a polydiorganosiloxane. The polydiorganosiloxane is selected from the group consisting of: B1) unsaturated polydiorganosiloxanes having at least one silicon-bonded aliphatic unsaturated group per molecule, B2) hydroxy-functional polydiorganosiloxanes having at least two silicon-bonded hydroxyl groups per molecule, and B3) a combination of both B1) and B2). When starting material B1) is used, the poly(meth)acrylate grafted polyorganosiloxane has both silicon-bonded aliphatic unsaturated groups and silicon-bonded poly(meth)acrylate groups.
[0065] The starting material B1) is an unsaturated polydiorganosiloxane having at least one silicon-bonded aliphatically unsaturated group per molecule. The aliphatically unsaturated group may be in terminal position, pendant position or both terminal and pendant position.
[0066] The starting material B1) unsaturated polydiorganosiloxane may have the unit formula B1-1): (R 6 R 7 2SiO 1 / 2 ) b (R 7 2SiO 2 / 2 ) c (R 6 R 7 SiO 2 / 2) d (R 7 3SiO 1 / 2 ) e (R'OR 7 2SiO 1 / 2 ) f (R'OR 7 SiO 2 / 2 ) g , where each R 6 is an independently selected aliphatic unsaturated hydrocarbon group, each R 7 is an independently selected monovalent hydrocarbon group free of aliphatic unsaturation, each R' being independently selected from H and R 7 The group consisting of subscript b is 0, 1 or 2, subscript c ≥ 1, subscript d ≥ 0, subscript e is 0, 1 or 2, subscript f is 0, 1 or 2, and subscript g ≥ 0, provided that the amount (b+d) ≥ 1, the amount (b+e+f) = 2, and the amount (b+c+d+e+f+g) is at least 3, or 3 to 250.
[0067] R 6 The aliphatic unsaturated hydrocarbon group may have 2 to 18 carbon atoms and is exemplified by alkenyl such as vinyl, allyl or hexenyl; and alkynyl such as propynyl, butynyl or hexynyl. Alternatively, each R 6 Alternatively, each R 6 It may be a vinyl group.
[0068] R 7 The monovalent hydrocarbon group free of aliphatic unsaturated groups may have 1 to 18 carbon atoms and may be alkyl, aryl and aralkyl; or alkyl and aryl groups. Suitable alkyl groups include methyl, ethyl and propyl; or methyl. Suitable aryl groups include phenyl. Alternatively, each R 7 It may be an alkyl group such as methyl.
[0069] Alternatively, in unit formula B1-1), subscript b may be 0 or 2, subscript e may be 0 or 2, and subscript g may be 0. Alternatively, subscript c may be 1 to 250, subscript d may be 0 to 1, subscript g may be 0 to 1, and the amount (c+d+g) may be 1 to 250. Alternatively, the amount (b+e) may be 2. Alternatively, subscript c may be 1 to 100, or 10 to 75, or 25 to 75, and or 30 to 60. Alternatively, subscript d may be 0 to 50, or 0 to 25, or 0 to 10, or 0 to 5. Alternatively, subscript g may be 0 to 50, or 0 to 25, or 0 to 10, or 0 to 5. Subscript b is 0 to 2, alternatively, subscript b may be 0, and alternatively, subscript b may be 2. Subscript e is 0 to 2, alternatively, subscript e may be 0, and alternatively, subscript e may be 2. Subscript f is 0 to 2, alternatively, subscript f may be 0, and alternatively, subscript f may be 2.
[0070] The starting material B1) may contain both silicon-bonded aliphatic unsaturated hydrocarbon groups and silicon-bonded hydroxyl groups. Examples of starting materials B1) containing both silicon-bonded aliphatic unsaturated groups and silicon-bonded hydroxyl groups include OH-terminated polymethylvinylsiloxane and OH-terminated poly(dimethyl / methylvinyl)siloxane copolymers, which are commercially available from Gelest. See, for example, "Gelest Reactive Silicones: Forging New Polymer Links", 2016, https: / / www.gelest.com / wp-content / uploads / Reactive-SIlicones-No-Price-2016.pdf page 11. Alternatively, the starting material B1) may have silicon-bonded aliphatic unsaturated hydrocarbon groups, silicon-bonded hydroxyl groups, and silicon-bonded alkoxy groups. Examples of such materials include DOWSIL TM 4-7042, which is a mixture of hydroxyl-terminated poly(dimethyl, methylvinylsiloxane) and α-hydroxyl-terminated, ω-methoxy-terminated poly(dimethyl, methylvinylsiloxane), is commercially available from Dow Silicones Corporation, Midland, Michigan, USA. When the starting material B1) contains both silicon-bonded aliphatically unsaturated hydrocarbon groups and sufficient silicon-bonded hydroxyl groups, the starting material B2) hydroxyl-functional polydiorganosiloxane is optional.
[0071] Alternatively, in the above unit formula B1-1), the amount (f+g) may be less than 2 (so that the starting material B1) may have less than 2 silicon-bonded hydroxyl groups per molecule). Examples of suitable unsaturated polydiorganosiloxanes include:
[0072] Bi) dimethylvinylsiloxy terminated polydimethylsiloxane,
[0073] B-ii) dimethylvinylsiloxy-terminated poly(dimethylsiloxane / methylvinylsiloxane),
[0074] B-iii) dimethylvinylsiloxy-terminated polymethylvinylsiloxane,
[0075] B-iv) trimethylsiloxy-terminated poly(dimethylsiloxane / methylvinylsiloxane),
[0076] Bv) trimethylsiloxy-terminated polymethylvinylsiloxane,
[0077] B-vi) dimethylvinylsiloxy-terminated poly(dimethylsiloxane / methylvinylsiloxane),
[0078] B-vii) dimethylvinylsiloxy-terminated poly(dimethylsiloxane / methylphenylsiloxane),
[0079] B-viii) dimethylvinylsiloxy-terminated poly(dimethylsiloxane / diphenylsiloxane),
[0080] B-ix) phenyl, methyl, vinyl-siloxy-terminated polydimethylsiloxane,
[0081] Bx) dimethylhexenylsiloxy-terminated polydimethylsiloxane,
[0082] B-xi) dimethylhexenylsiloxy-terminated poly(dimethylsiloxane / methylhexenylsiloxane),
[0083] B-xii) dimethylhexenylsiloxy-terminated polymethylhexenylsiloxane,
[0084] B-xiii) trimethylsiloxy-terminated poly(dimethylsiloxane / methylhexenylsiloxane),
[0085] B-xiv) trimethylsiloxy-terminated polymethylhexenylsiloxane,
[0086] B-xv) dimethylhexenylsiloxy-terminated poly(dimethylsiloxane / methylhexenylsiloxane),
[0087] B-xvi) dimethylvinylsiloxy-terminated poly(dimethylsiloxane / methylhexenylsiloxane),
[0088] B-xvii) their combination. Vinyl functionalized polydiorganosiloxanes are available, see, for example, "Gelest Reactive Silicones: Forging New Polymer Links", 2016, https: / / www.gelest.com / wp-content / uploads / Reactive-SIlicones-No-Price-2016.pdf pages 8-11 and 15-16. When the starting material B1) does not contain enough silicon-bonded hydroxyl groups, the starting material B2) is used in the above method. The amount of the starting material B1) used in the method depends on various factors, including whether B1) has a terminal, a side group, or both a terminal and a side group of aliphatic unsaturated groups. However, the amount of the starting material B1) is sufficient to provide 0.1% to 10%, alternatively 0.1% to 2% of aliphatic unsaturated groups to all the starting materials in step I) of the method for preparing a product comprising poly(meth)acrylate grafted polyorganosiloxanes. Alternatively, the amount of starting material B1) may be 0.5% to 5%, alternatively 1% to 4%, and alternatively 1% to 3%, based on the combined weight of starting materials A) and B).
[0089] Alternatively, when starting material B1) has a hydroxyl function and starting material B2) is not used, B1) may be present in higher amounts, for example up to 90%.
[0090] In the process for preparing a product comprising poly(meth)acrylate grafted polyorganosiloxanes, the starting material B2) is a hydroxyl-functional polydiorganosiloxane having at least two silicon-bonded hydroxyl groups per molecule. The hydroxyl groups may be in terminal position, pendant position or both. The starting material B2) may have the unit formula B2-1): (R 8 2SiO 2 / 2 ) h (R 8 3SiO 1 / 2 ) i (HOR 8 2SiO 1 / 2 ) j , where each R 8 is an independently selected monovalent hydrocarbon group free of aliphatic unsaturation, subscript j is 1 or 2, subscript i is 0 or 1, the amount (j+i)=2, subscript h≥1, and the amount (h+i+j) is at least 3, or 3 to 250, and or 3 to 100. Alternatively, subscript h may be 1 to 250 or 1 to 100. Alternatively, i may be 0 and j may be 2. R 8The monovalent hydrocarbon group of includes alkyl groups, aryl groups and aralkyl groups; or alkyl groups and aryl groups. Suitable alkyl groups include methyl, ethyl and propyl; or methyl. Suitable aryl groups include phenyl. Alternatively, each R 8 Can be an alkyl group, such as methyl. Examples of starting material B2) include hydroxy-terminated polydimethylsiloxane, hydroxy-terminated poly (dimethyl / diphenyl) siloxane copolymer, hydroxy-terminated poly (dimethyl / methylphenyl) siloxane copolymer. Alternatively, suitable dihydroxy-terminated polydimethylsiloxanes are commercially available from Dow Silicones Corporation, Midland, Michigan, USA. Exemplary hydroxy-functionalized polydiorganosiloxanes are commercially available, including "Gelest Reactive Silicones: Forging New Polymer Links", 2016, https: / / www.gelest.com / wp-content / uploads / Reactive-SIlicones-No-Price-2016.pdf pages 22 and 24-25 of silanol functionalized polymers. Starting material B2) may be used in an amount of 80% to 95%, alternatively 85% to 95%, based on the combined weight of starting materials A) and B); alternatively 87% to 94%, and alternatively 89% to 94%, based on the same basis.
[0091] In the process for preparing a product comprising a poly(meth)acrylate grafted polyorganosiloxane, the starting material C) is a phosphazene condensation reaction catalyst, such as a phosphazene halide. Without wishing to be bound by theory, it is believed that when a phosphazene condensation reaction catalyst is used in the process, the formation of cyclic siloxane byproducts (such as octamethylcyclotetrasiloxane) can be minimized.
[0092] Phosphazene condensation reaction catalysts are exemplified by those disclosed in U.S. Pat. No. 9,051,428. Exemplary phosphazene condensation reaction catalysts may contain at least one -(N=P<)- unit per molecule, and may be oligomers having up to 10 such phosphazene units, for example having an average of 1.5 to 5 phosphazene units. The phosphazene condensation reaction catalyst may be, for example, a halogenated phosphazene, such as chlorophosphazene (phosphazene chloride), an oxygen-containing halogenated phosphazene, or an ionic derivative of a phosphazene, such as a phosphazene salt, such as an ionic derivative of a phosphazene halide, for example a perchlorooligomeric phosphazene salt.
[0093] One suitable type of phosphazene condensation reaction catalyst is an oxygen-containing halophosphazene, such as an oxygen-containing chlorophosphazene. Such an oxygen-containing chlorophosphazene may, for example, have the formula C-1):
[0094] C-2): In formula C-1) and C-2), the subscript p may have an average value of 1 to 10 or 1 to 5. The catalyst may also include tautomers of the catalyst having formula C-2). Another type of suitable oxygen-containing chlorophosphazene has formula C-3): Where R 9 represents an organosilicon moiety bonded to phosphorus via oxygen, for example, formula C-4): A phosphazene catalyst, wherein each R 10 represents a monovalent hydrocarbon group having 1 to 18 carbon atoms or a monovalent halogenated hydrocarbon group having 1 to 18 carbon atoms, and the subscript q has an average value of 1 to 10 or 1 to 5. The catalyst may also include condensation products of such organosilicon-containing phosphazenes. All or some of the chlorine atoms in any of the above oxygen-containing phosphazenes may be replaced by a group Q, wherein Q represents a moiety selected from the group consisting of a hydroxyl group, a monovalent organic group (such as an alkoxy group or an aryloxy group), a halogen atom other than chlorine, an organosilicon group, and a phosphorus-containing group.
[0095] Another suitable type of phosphazene catalyst is of formula C-5): Perchlorooligophosphazene salts of - Alternatively, the subscript o may have an average value of 1 to 6, and alternatively, the subscript o may have an average value of 2. The anion may be a complex anion and may, for example, have the formula MX (v+1) , wherein M is an element having a Pauling electronegativity scale of 1.0 to 2.0 and a valence v, and X is a halogen atom. The element M may be, for example, phosphorus or antimony, or phosphorus. The halogen atom of X may be Cl. Alternatively, the anion Z - Can be [MX (v-y+1) R 11 y ] - complex anion, where each R 11 is an independently selected alkyl group having 1 to 12 carbon atoms, and subscript y has a value between 0 and v, as described in U.S. Pat. No. 5,457,220. Alternatively, in formula C-5), subscript o may have an average value of 2, and anion Z - Can be PCl6 - .
[0096] The phosphazene condensation reaction catalyst may be present in an amount of 1 to 200 or 2 to 200 parts per million, such as 5 to 50 parts per million, based on the combined weight of starting materials A) and B).
[0097] The starting material D) is an optional polydialkylsiloxane which can be added in step I) of the process for preparing a product comprising poly(meth)acrylate grafted polyorganosiloxane. The polydialkylsiloxane can have the unit formula D-1): (R 12 2SiO 2 / 2 ) m (R 12 3SiO 1 / 2 )2, where each R 12 is an independently selected alkyl group, and the subscript m is 1 to 250 or 1 to 50. 12 The alkyl groups include methyl, ethyl and propyl; or methyl. Examples of starting material D) include Di) trimethylsiloxy-terminated polydimethylsiloxane, Dii) triethylsiloxy-terminated polydiethylsiloxane, and Diii) a combination of Di) and Dii). Polydialkylsiloxanes are known in the art and are commercially available. For example, methyl silicone fluids such as trimethylsiloxy-terminated polydimethylsiloxane are commercially available from Gelest, see, for example, "Gelest: Silicone Fluids," https: / / www.gelest.com / themencode-pdf-viewer / ? file=https: / / www.gelest.com:443 / wp-content / uploads / Inert_Silicones.pdf, 2012, pp. 8-9, and under the trade name DOWSIL TM 200 Fluids are commercially available from Dow Silicones Corporation, Midland, Michigan USA. Trimethylsiloxy-terminated polydimethylsiloxane and triethylsiloxy-terminated polydiethylsiloxane are available from Power Chemical Corporation, Jiangsu, China. The amount of starting material D) depends on a variety of factors, including the molecular weight of the polydialkylsiloxane selected, however, when used, the amount may be 1% to 10% based on the weight of the starting materials A) to D) used in the process.
[0098] Starting material E) is a solvent that can be used in the above process. The solvent can be an aromatic hydrocarbon, such as toluene or xylene; or ethyl acetate. The amount and type of solvent are selected so as to solubilize both the polyorganosiloxane and the (meth)acrylate polymer or copolymer. However, when present, the solvent can be used in an amount of 30% to 80% or 40% to 70% based on the combined weight of starting materials A), B), C), D) and E).
[0099] Starting material F) is a neutralizing agent, which can be optionally used in step III) of the method for preparing a product comprising the above-mentioned poly(meth)acrylate grafted polyorganosiloxane. Starting material F) can be used to neutralize the product after the poly(meth)acrylate grafted polyorganosiloxane is formed. If a neutralizing agent is used, any neutralizing agent suitable for the selected catalyst can be used, see, for example, the neutralizing agent disclosed in U.S. Patent 8,580,862. Without wishing to be bound by theory, it is believed that the selection of the neutralizing agent depends on pKa and solubility. Neutralizing agents suitable for phosphazene-based condensation catalysts include, but are not limited to, alkylamines, such as trioctylamine, trimethylamine, triethylamine, trihexylamine and triisononylamine. Neutralizing agents are known in the art and can be commercially available, for example, from Millipore Sigma (St. Louis, Missouri, USA) in St. Louis, Missouri. The amount of neutralizing agent depends on a variety of factors including the amount of starting material C) condensation catalyst, however, starting material F) may be present in an amount sufficient to provide a molar ratio of neutralizing agent to catalyst (F:C ratio) of from 1:1 to 100:1, alternatively from 1:1 to 30:1; and alternatively from 1:1 to 20:1.
[0100] Poly(meth)acrylate grafted polyorganosiloxane
[0101] The above method produces a poly(meth)acrylate grafted polyorganosiloxane. The poly(meth)acrylate grafted polyorganosiloxane comprises a unit formula:
[0102] [R 3 w (R 5 -SR”)(OR 4 ) (2-w) Si-O 1 / 2 ] p [R 3 v (R 5 -SR”)(OR 4 ) (1-v) Si-O 2 / 2 ] q [(R 5 -SR”)Si-O 3 / 2 ] k (R 6 R 7 2SiO 1 / 2 ) r (R 7 2SiO 2 / 2 ) s (R 6 R 7 SiO 2 / 2 )t (R 7 3SiO 1 / 2 ) u , where each subscript w is independently 0, 1, or 2, each subscript v is independently 0 or 1, and each R 3 is an independently selected monovalent hydrocarbon group; each R 4 is an independently selected alkyl group; each R 5 is an independently selected divalent hydrocarbon group, each R" is independently a (meth)acrylate polymer or copolymer, each R 6 independently selected from the group consisting of hydroxyl groups and aliphatic unsaturated monovalent hydrocarbon groups, each R 7 is an independently selected monovalent hydrocarbon group free of aliphatic unsaturation, subscript p ≥ 0, subscript q ≥ 0, subscript k ≥ 0, the amount (p+q+k) ≥ 1, subscript r ≥ 0, subscript s ≥ 0, subscript t ≥ 0, subscript u ≥ 0, the amount (r+t) ≥ 2, and the amount (p+q+k+r+s+t+u) is sufficient to provide a molecular weight of at least 50 kDa to the poly(meth)acrylate-grafted polyorganosiloxane.
[0103] Alternatively, subscript w is 1 or 2. Alternatively, subscript p is 0 to 2 or 1 or 2. Alternatively, subscript q is 0 to 100. Alternatively, subscript k<5; alternatively, k may be 0, 1 or 2; and alternatively, k=0. Alternatively, the amount (p+q+k) is 1 to 100. Alternatively, subscript r is 0 to 2. Alternatively, subscript s is 0 to 100. Alternatively, subscript t is 0 to 100. Alternatively, subscript u is 0 to 2. Alternatively, the amount (p+q+r+s+t+u) is sufficient to provide the poly(meth)acrylate-grafted polyorganosiloxane with a molecular weight of 50 kDa to 1,000 kDa, or 60 kDa to 1,000 kDa, or 50 kDa to 600 kDa, or 60 kDa to 300 kDa. Alternatively, the amount (p+r+u) = 2. Alternatively, the amount (p+q) is from 1 to 100. Alternatively, the amount (r+t) is from 1 to 100. Alternatively, the amount (p+q+r+s+t+u) is sufficient to provide the functionalized polyorganosiloxane with a molecular weight of 50 kDa to 1,000 kDa.
[0104] Alternatively, in the above unit formula of the poly(meth)acrylate-grafted polyorganosiloxane, each R 3 may have 1 to 18 carbon atoms. 3 It may be an alkyl group of 1 to 6 carbon atoms. 4 may have 1 to 6 carbon atoms. 4 It may be an alkyl group of 1 to 6 carbon atoms. 5 may have 1 to 18 carbon atoms.5 It can be an alkylene group of 2 to 8 carbon atoms. 6 It may be a hydroxyl group or an alkenyl group having 2 to 18 carbon atoms. 6 It may be a hydroxyl group or an alkenyl group selected from vinyl, allyl and hexenyl. 6 Two or more examples of may be hydroxyl groups. Alternatively, R 6 Two or more examples of are aliphatic unsaturated monovalent hydrocarbon groups. Alternatively, each R 6 Alternatively, each R 7 may have 1 to 18 carbon atoms. 7 It may be an alkyl group of 1 to 6 carbon atoms. Alternatively, each R" may have a DP of 1 to 1,000; alternatively 5 to 600.
[0105] Free radical reaction curable hybrid pressure sensitive adhesive composition
[0106] The poly(meth)acrylate grafted polyorganosiloxane is a starting material (IA) that can be used in a free radical reaction curable hybrid PSA composition (hybrid PSA composition). The hybrid PSA composition may contain:
[0107] (I) A pressure-sensitive adhesive matrix comprising a physical mixture of starting materials (IA) and (IB) in an amount sufficient to provide 15 wt % to 40 wt % of the starting material (IA) and 5 wt % to 60 wt % of the starting material (IB), a reaction product of the starting materials (IA) and (IB), or a combination of the physical mixture and the reaction product; wherein the starting material (IA) is the poly(meth)acrylate grafted polyorganosiloxane described above, and the starting material (IB) is a polyorganosilicate resin. Alternatively, the starting material (IA) may be present in an amount of 17 wt % to 25 wt %. Alternatively, the starting material (IB) may be present in an amount of 25 wt % to 40 wt %. Alternatively, the matrix may include a reaction product of the starting materials (IA) and (IB). Alternatively, the R of the starting material (IA) is 6 All or part of can be used as hydroxyl groups, and the matrix can include the reaction product of starting materials (IA) and (IB). The mixed PSA composition further includes (II) a peroxide catalyst. The mixed PSA composition can optionally further include (III) a solvent.
[0108] (IB) Polyorganosilicate resin
[0109] The polyorganosilicate resin used as the starting material (IB) in the mixed PSA composition is essentially composed of R 14 3SiO1 / 2 Unit and SiO 4 / 2 MQ resin composed of units, where each R 14 are independently selected from the group consisting of hydroxyl groups and monovalent hydrocarbon groups. 14 The monovalent hydrocarbon group of can be selected from the group consisting of: an alkyl group of 1 to 18 carbon atoms, an alkenyl group of 2 to 18 carbon atoms, and an aryl group or aralkyl group of 6 to 18 carbon atoms. Suitable alkyl groups, alkenyl groups, aryl groups and aralkyl groups are defined as follows. Alternatively, each R 14 It may be a hydroxyl group or an alkyl group such as a methyl group.
[0110] Alternatively, the polyorganosilicate resin may have the following unit formula: (R 15 2R 16 SiO 1 / 2 ) x (R 15 3SiO 1 / 2 ) y (SiO 4 / 2 ) z , where R 15 is an alkyl group, an aryl group or an aralkyl group, such as methyl and phenyl; and R 16 is an alkenyl group having 2 to 18 carbon atoms, such as vinyl, allyl or hexenyl; subscript x≥0, subscript y≥0, subscript z>0, the amount (x+y)>0, and subscripts x, y and z have values such that 0.9≤(x+y) / z≤1.3. Alternatively, the polyorganosilicate resin may have a unit formula (III): (R 15 3SiO 1 / 2 ) w (SiO 4 / 2 ) z , where each R 15 As above, subscript z is as above, and subscript w>4.
[0111] The polyorganosilicate resin may contain an average of 0 to 30 mol% alkenyl groups, alternatively 3 to 30 mol% alkenyl groups, alternatively 0.1 to 30 mol%, alternatively 0.1 to 5 mol%, alternatively 3 to 10 mol% alkenyl groups. The mole percentage of alkenyl groups in the resin is the ratio of the number of moles of siloxane units containing alkenyl groups in the resin to the total number of moles of siloxane units in the resin multiplied by 100.
[0112] The Mn of the polyorganosilicate resin is typically greater than 1,500 Da, alternatively >1,500 Da to 8,000 Da, and alternatively 2,000 Da to 7,500 Da. Mn can be measured by GPC using the following method.
[0113] Methods for preparing the resins are well known in the art. For example, the resins can be prepared by treating a resin copolymer produced by the silica hydrosol capping method described by Daudt et al. with at least one capping agent such as hexamethyldisilazane or an alkenyl-containing capping agent. The method described by Daudt et al. is disclosed in U.S. Pat. No. 2,676,182.
[0114] The method of Daudt et al. involves reacting a silica hydrosol with a hydrolyzable triorganosilane (such as trimethylchlorosilane), a siloxane (such as hexamethyldisiloxane), or a mixture thereof under acidic conditions, and recovering a copolymer having M units and Q units. The resulting copolymer typically contains 2 to 5 weight percent hydroxyl groups.
[0115] The resin (typically containing less than 2% silicon-bonded hydroxyl groups) can be prepared by reacting the product described by Daudt et al. with an end-capping agent such as an end-capping agent containing alkenyl groups and / or an end-capping agent free of aliphatic unsaturated groups in an amount sufficient to provide 0 to 30 mole % of unsaturated organic groups in the final product. Examples of end-capping agents include, but are not limited to, silazanes, siloxanes, and silanes. Suitable end-capping agents are known in the art and are exemplified in U.S. Patents 4,584,355, 4,591,622, and 4,585,836. A single end-capping agent or a mixture of such agents can be used to prepare the resin.
[0116] Various suitable polyorganosilicate resins are commercially available from sources such as Dow Silicones, Midland, Michigan, USA, Momentive Performance Materials, Albany, NY, USA, and Bluestar Silicones USA Corp., East Brunswick, NJ, USA. For example, DOWSIL TM MQ-1600 solid resin, DOWSIL TM MQ-1601 solid resin and DOWSIL TM 1250 surfactant, DOWSIL TM 7466 resin and DOWSIL TM 7366 resin is suitable for use herein. Such resins may be provided in organic solvents.
[0117] (II) Peroxide
[0118] The starting material (II) in the mixed PSA composition is a free radical curing catalyst comprising an organic peroxide compound. Suitable organic peroxide compounds include dibenzoyl peroxide; 4-monochlorobenzoyl peroxide; diisopropylbenzene peroxide; tert-butyl peroxybenzoate; tert-butyl peroxide isopropylbenzene; tert-butyl oxide 2,5-dimethyl-2,5-di-tert-butyl peroxyhexane; 2,4-dichlorobenzoyl peroxide; di-tert-butyl peroxy-diisopropylbenzene; 1,1-bis(tert-butyl peroxy)-3,3,5-trimethylcyclohexane; 2,5-di-tert-butyl peroxyhexane-3,2,5-dimethyl-2,5-bis(tert-butyl peroxy)hexane or isopropylbenzene-tert-butyl peroxide. The starting material (III) may be one organic peroxide compound or a combination of two or more organic peroxide compounds. Alternatively, the starting material (II) may be benzoyl peroxide.
[0119] The amount of starting material (II) added to the mixed PSA composition depends on various factors, including the type and amount of catalyst selected, the choice of starting materials A) and B), and whether starting material A) has hydroxyl groups or aliphatically unsaturated groups (for R 6 ). However, starting material (II) may be present in an amount of at least 2 wt % based on the combined weight of starting materials (I), (II) and (III). Alternatively, when each R in starting material (A) 6 When all R in the starting material (A) are hydroxyl groups, the peroxide catalyst is present in an amount of 2 to 4 wt%. 6 When all are aliphatically unsaturated monovalent hydrocarbon groups, the peroxide catalyst is present in an amount of at least 3 wt%, alternatively 3 wt% to 4 wt%.
[0120] (III) Solvent
[0121] Solvents may be optionally used in the mixed PSA compositions described herein. Solvents may facilitate the flow of the mixed PSA compositions and the introduction of certain starting materials (such as polyorganosilicate resins and / or peroxide compounds). The solvents used herein are solvents that help the starting materials of the mixed PSA compositions to fluidize but do not substantially react with these starting materials. The solvent may be selected based on the solubility and volatility of the starting materials in the mixed PSA compositions. Solubility refers to the solvent being sufficient to dissolve and / or disperse the starting materials of the mixed PSA compositions. Volatility refers to the vapor pressure of the solvent. If the solvent volatility is too high (having too high a vapor pressure), bubbles may be formed in the mixed PSA compositions during the curing reaction, and the bubbles may cause cracks or otherwise weaken or adversely affect the properties of the reaction products. However, if the solvent volatility is not enough (the vapor pressure is too low), the solvent may be retained in the reaction product of the mixed PSA compositions as a plasticizer.
[0122] The solvent may include an organic solvent. The organic solvent may be an alcohol such as methanol, ethanol, isopropanol, butanol or n-propanol; a ketone such as acetone, methyl ethyl ketone or methyl isobutyl ketone; an aromatic hydrocarbon such as benzene, toluene or xylene; an aliphatic hydrocarbon such as heptane, hexane or octane; a glycol ether such as propylene glycol methyl ether, dipropylene glycol methyl ether, propylene glycol n-butyl ether, propylene glycol n-propyl ether or ethylene glycol n-butyl ether; a halogenated hydrocarbon such as dichloromethane, 1,1,1-trichloroethane or methylene chloride; chloroform; dimethyl sulfoxide; dimethylformamide, acetonitrile; tetrahydrofuran; petroleum solvent; solvent oil; naphtha; N-methylpyrrolidone; or a combination thereof. Alternatively, the solvent may be selected from the group consisting of ethyl acetate, benzene, toluene, xylene, heptane, tetrahydrofuran and a combination of two or more thereof.
[0123] Suitable solvents include polyorganosiloxanes with suitable vapor pressures, such as hexamethyldisiloxane, octamethyltrisiloxane, hexamethylcyclotrisiloxane, and other low molecular weight polyorganosiloxanes, such as 0.5 cSt to 1.5 cSt DOWSIL 9000, commercially available from Dow Silicones Corporation, Midland, Michigan, USA. TM 200 Fluid and DOWSIL TM OS Fluid.
[0124] The amount of solvent will depend on a variety of factors, including the type of solvent selected, and the amount and type of other starting materials selected. However, based on the weight of all starting materials in the mixed PSA composition, the amount of solvent can be in the range of 0 wt % to 70 wt %, alternatively 2 wt % to 50 wt %, and alternatively 40 wt % to 60 wt %. The solvent can be added during the preparation of the mixed PSA composition, for example to aid in mixing and delivering one or more starting materials. After the mixed PSA composition is prepared, all or a portion of the solvent can be optionally removed.
[0125] Method for preparing hybrid PSA composition
[0126] The hybrid PSA composition can be prepared by a process comprising combining all of the starting materials by any convenient means, such as mixing at RT. The process can also include delivering one or more starting materials in a solvent (e.g., polyorganosilicate resin and / or peroxide catalyst) that can be dissolved in the solvent when combined with one or more other starting materials in the hybrid PSA composition, and thereafter removing all or substantially all of the solvent by conventional means such as stripping and / or distillation (optionally at reduced pressure).
[0127] When preparing a hybrid PSA composition, starting material (IA) - grafted polyorganosiloxane and starting material (IB) - polyorganosilicate resin can be combined to form a matrix while combining (II) peroxide and (III) solvent (if any), for example, by mixing all starting materials in any order. Alternatively, the matrix can be prepared by combining starting material (IA) and starting material (IB) before adding (II) peroxide.
[0128] In one embodiment, starting material (IA) - grafted polyorganosiloxane and starting material (IB) - polyorganosilicate resin can be combined by physical mixing at ambient temperature. Alternatively, one or both of starting materials (IA) and (IB) can be dissolved in (III) solvent prior to physical mixing.
[0129] In an alternative embodiment, starting materials (IA) and (IB) can be reacted to form the matrix before adding starting material (II) peroxide. For example, when starting material (IA) contains a 6 When the hydroxyl groups of the mixed pressure-sensitive adhesive matrix are present, the mixed pressure-sensitive adhesive matrix can be prepared by a method comprising the following steps:
[0130] 1) The starting materials are combined as follows:
[0131] (IA) a functionalized polyorganosiloxane having a poly(meth)acrylate group, wherein the functionalized polyorganosiloxane comprises the above unit formula and R 6 Two or more instances of are hydroxyl groups,
[0132] (IB) the above-mentioned polyorganosilicate resin,
[0133] Optionally (III) the above solvent,
[0134] Optionally (IC) silyl phosphate, and
[0135] (ID) condensation reaction catalyst; thereby preparing a reaction mixture; thereby forming a reaction product and by-products of the starting materials (IA) and (IB);
[0136] 2) removing all or part of the by-products during and / or after step 1);
[0137] The method may further include:
[0138] 3) combining (above) (II) peroxide catalyst, and optionally adding further additional (III) solvent to the reaction product in step 2); thereby forming a polyorganosiloxane hybrid pressure-sensitive adhesive composition.
[0139] Step 1) can be carried out by any convenient means (such as mixing). Step 1) can be carried out under inert conditions, such as nitrogen or other inert gases. Combining the starting materials can be carried out at ambient temperature. A solvent can be optionally added, for example, to facilitate combining the starting materials. The starting material (IC) is a silyl phosphate that can be used in step 1) for example to neutralize impurities. When present, the amount of the starting material (IC) can be up to 0.02 weight %. Silyl phosphates and methods for their preparation are described in, for example, U.S. Patents 4,177,200, 5,099,051 and 5,481,014 and references cited therein.
[0140] The starting material (ID) used in step 1) - condensation reaction catalyst can be a carboxylic acid. Some available carboxylic acids include but are not limited to propionic acid, 2-methylpropionic acid, butyric acid, valeric acid (valeric acid), caproic acid (caprylic acid), 2-ethylhexanoic acid, enanthic acid, caproic acid, caprylic acid (caprylic acid), oleic acid, linoleic acid, linolenic acid, cyclohexanecarboxylic acid, cyclohexyl acetic acid, cyclohexene carboxylic acid, benzoic acid, phenylacetic acid, malonic acid (malic acid), succinic acid (succinic acid), adipic acid (fatty acid), 2-butenedioic acid (maleic acid), lauric acid, stearic acid, myristic acid, palmitic acid, isononanoic acid (isoanoic acid) or a combination of two or more thereof. In one embodiment, the acidic compound can be a mixture comprising branched alkyl carboxylic acids. In one embodiment, the acidic compound is a mixture of mainly aliphatic C10 tertiary carboxylic acids. The amount depends on various factors, including the type of starting material (IA) and (IB) and the amount of hydroxyl groups. However, the amount of starting material (ID) may be 0.1 wt% to 5 wt%, alternatively 0.1 wt% to 1 wt%, based on the combined weight of all starting materials.
[0141] Step 2) can be carried out by heating the resulting mixture, for example, to reflux the selected solvent. When the starting materials react, by-products are produced. The by-products may include water. All or part of the by-products may be removed during and / or after step 1). Without wishing to be bound by theory, it is believed that removing the by-products can drive the reaction to completion. The by-products may be removed by any convenient means such as stripping.
[0142] Step 3) may be carried out by combining (II) a peroxide catalyst and optionally (III) additional solvent to the reaction product of starting materials (IA) and (IB) from step 2) by any convenient means such as mixing at ambient temperature.
[0143] Adhesive products
[0144] The hybrid PSA composition prepared as described above can be used to form an adhesive article on a substrate, for example, a hybrid PSA (prepared by curing the hybrid PSA composition described above). Thus, the method can further include applying the hybrid PSA composition to a substrate.
[0145] The mixed PSA composition can be applied to the substrate by any convenient means. For example, the mixed PSA composition can be applied to the substrate by a grooved roll coater, a notched wheel coater, a rubber roll coater, a rubber-groove roll coater, a roll coater, a reverse roll coater, an air knife coater, or a curtain coater.
[0146] The substrate can be any material that can withstand the curing conditions (described below) for curing the mixed PSA composition to form a mixed pressure-sensitive adhesive on the substrate. For example, any substrate that can withstand heat treatment at a temperature equal to or greater than 120°C, alternatively 150°C is suitable. Examples of materials suitable for such substrates include plastic films such as polymethyl methacrylate (PMMA), polyimide (PI), polyetheretherketone (PEEK), polyethylene naphthalate (PEN), liquid crystal polyarylate, polyamideimide (PAI), polyether sulfide (PES), polyethylene terephthalate (PET), polyethylene (PE) or polypropylene (PP). Alternatively, the substrate can be a plastic as described above coated on a paper backing. Alternatively, the substrate can be a metal foil, such as aluminum foil or copper foil. The thickness of the substrate is not important; however, the thickness can be 5 microns to 300 microns.
[0147] Alternatively, the substrate may be a fluorosilicone release liner, such as any of the substrates described above coated with a fluorosilicone release coating.
[0148] To improve the bonding of the hybrid PSA to the surface of the substrate, the method for forming the adhesive article may also optionally include treating the surface of the substrate prior to applying the hybrid PSA composition. Treating the surface of the substrate may be performed by any convenient means, such as applying a primer, or subjecting the substrate to corona discharge treatment, etching, or plasma treatment prior to applying the hybrid PSA composition to the surface of the substrate.
[0149] Adhesive articles (such as films or tapes) can be prepared by applying the above-mentioned mixed PSA composition to the surface of the above-mentioned substrate. When a solvent is present, the method may also optionally include removing all or part of the solvent before and / or during curing. Removal of the solvent may be carried out in any convenient manner, such as heating at a temperature that evaporates the solvent without fully curing the mixed PSA composition, for example, heating at a temperature of 70°C to 120°C, or 50°C to 100°C, and or 70°C to 80°C for a time sufficient to remove all or part of the solvent (e.g., 30 seconds to 1 hour or 1 minute to 5 minutes).
[0150] The mixed PSA composition is cured (and when a solvent is present, the solvent is removed) by heating at a temperature of 80°C to 210°C, alternatively 90°C to 205°C, alternatively 100°C to 205°C, and alternatively 110°C to 200°C for a time sufficient to cure the mixed PSA composition (e.g., 30 seconds to one hour, alternatively 1 minute to 5 minutes). This forms a mixed PSA on the surface of the substrate. Curing can be performed by placing the substrate in an oven. The amount of the mixed PSA composition to be applied to the surface of the substrate depends on the specific application, however, the amount may be sufficient to make the thickness of the mixed PSA after curing be 5 microns to 100 microns, and for a protective film, the thickness may be 6 microns to 50 microns, alternatively 8 microns to 40 microns, and alternatively 10 microns to 30 microns.
[0151] The methods described herein may also optionally include applying a removable release liner to the hybrid PSA opposite the substrate, for example to protect the hybrid PSA prior to use of the adhesive article. The release liner may be applied before, during or after curing the hybrid PSA composition; alternatively applied after curing.
[0152] Alternatively, when the hybrid PSA is formed on a release liner, then the method further comprises applying a substrate (as described above) to the hybrid PSA after curing.
[0153] Example
[0154] These examples are intended to illustrate the invention and should not be construed as limiting the scope described in the claims.The starting materials used in the examples are shown in Table 2 below.
[0155] Table 2. Starting materials
[0156]
[0157]
[0158]
[0159] In this Reference Example A, a description of the method for preparing macromonomer Example MM-1 (100 BMA, nomenclature refers to weight percentage and BMA=butyl methacrylate) having 1.9 wt % of a monomer based on (3-mercaptopropyl)methyldimethoxysilane is provided. Ethyl acetate (EtOAc) was dried over molecular sieves and the other ingredients were used as supplied. A monomer mixture containing EtOAc (75 g), BMA (370 g) and (3-mercaptopropyl)methyldimethoxysilane (7 g) was prepared. EtOAc (100 g) and were added to a 4-neck 1 liter glass reactor equipped with a condenser and an overhead mixer. The mixture was heated to 77° C. and bubbled with nitrogen for 30 minutes. A solution of Trigonox 125-C75 (tAPPiv, 1 g) in EtOAc (10 g) was added to the reactor and held for 5 minutes. The temperature was slowly raised to 85°C, and then the monomer mixture was fed at a rate of 0.1 mL / min for 180 min, and the initiator solution (20 g EtOAc; 2 g Trigonox 125-C75) was fed in 240 min (180 min plus 60 min overfeed after the end of the monomer feed). After the initiator feed was finished, the reaction was kept at 85°C for 180 min, and then the resulting mixture was cooled to room temperature. The resulting mixture was dried in a vacuum oven.
[0160] In this Reference Example B, a description of the method for preparing macromonomer Example MM-2 (37BMA / 63MMA, the nomenclature refers to weight percentage and BMA=butyl methacrylate and MMA=methyl methacrylate) having 8.2 wt% of a monomer based on (3-mercaptopropyl)methyldimethoxysilane is provided. This method is used to prepare another alkoxysilyl functionalized (meth)acrylate macromonomer (Example MM-3) by varying the appropriate starting materials and their amounts, as shown in Table 3 below. A monomer mixture of toluene (5 g), MMA (252 g), BMA (148 g) and (3-mercaptopropyl)methyldimethoxysilane (36 g) is prepared. Toluene (80 g) is added to a 4-neck 1 liter glass reactor equipped with a condenser and an overhead mixer. The solvent was heated to 85°C, then the monomer mixture (441 g) was fed over a 1 hour period, and the initiator solution (30 g of toluene and 16.5 g of Trigonox 25-C75tBPPiv) was fed over a 3 hour period. After 2 hours, BA (butyl acrylate, 10 g) was added over a 30 minute period. After the initiator feed was complete, the reaction was held at 85°C for 80 minutes, and then the mixture was cooled to room temperature and collected. For MM-2, the reaction mixture was diluted with 160 g of toluene before collection, and no additional dilution was required for MM-3.
[0161] Table 3. The alkoxysilyl functional (meth)acrylate macromonomers prepared in Reference Examples AB total
[0162]
[0163] *BOM=Based on monomer
[0164] Table 4. Characterization results of alkoxysilyl functionalized (meth)acrylate macromonomers
[0165]
[0166] a. Molecular weight distribution measured on GPC using THF as eluent.
[0167] b. Residual monomer concentration measured by HS-GC. In addition to the internal standard (about 20 mg), a sample of the reaction mixture (about 20 mg) was added to the vial and the vial was packed. Headspace gas chromatography was performed by heating the vial and sampling the headspace to determine the ppm level of residual monomer.
[0168] c. Through 29 Percent condensation of siloxane moieties measured by Si NMR.
[0169] d.ND = Not determined
[0170] In this Example C, grafted polysiloxane GP-1 was synthesized as follows: dihydroxy-terminated polydimethylsiloxane with polybutyl methacrylate pendant groups. Before the experiment began, a 1-liter 4-neck round-bottom flask with a stir bar and blade was pre-weighed and recorded. 181.3 grams of OH-terminated PDMS 1 was added to the flask, 18.17 grams of the macromonomer of Example MM-1 (which had Mn=8,000 g / mol and BMA=100%) and 239.61 grams of toluene were charged to the round-bottom flask, which was equipped with an overhead mechanical stirrer, a thermocouple, and a Dean Stark apparatus with a water-cooled condenser attached to a nitrogen bubbler. When the kettle temperature reached 80 to 100° C. under a nitrogen blanket, 0.47 mL of phosphazene catalyst 1 was added. As the reaction mixture continued to heat, water, methanol, and toluene distillates were collected in the Dean Stark apparatus. After enough toluene was distilled off to obtain a final concentration of 50% solid solution, heating was stopped. When a final concentration of 50% solid was reached, 0.20 mL of trioctylamine was added to the reaction flask with stirring to neutralize the reaction mixture, and the resulting mixture was allowed to cool to room temperature. After cooling to room temperature, the round bottom flask with a stir bar and paddle was weighed and recorded. The NVC was then calculated based on the mass balance (difference between the pre-weight and the final weight) assuming that all polymer content remained in the flask.
[0171] In this Reference Example D, the alkoxysilyl functionalized (meth)acrylate macromonomers of Examples MM-1 to MM-3 above are used to prepare poly(meth)acrylate grafted polyorganosiloxanes. Example D is provided as a description of the method for preparing grafted polysiloxane GP-2: Before the start of the experiment, a 1 liter 4-neck round bottom flask with a stirring bar and blade is pre-weighed and recorded. To the flask is added 181.0 grams of OH-terminated PDMS 1, 5.65 grams of Vi-terminated PDMS 1, 3.73 grams of Example MM-2 (which has Mn=2.3 kDa and BMA=37%) and 238 grams of toluene are charged into the round bottom flask, which is equipped with an overhead mechanical stirrer, a thermocouple and a Dean Stark apparatus with a water-cooled condenser attached to a nitrogen bubbler. A heating jacket is inserted into the temperature controller to prevent the reaction mixture from heating to a temperature greater than 120°C. When the pot temperature reaches 80°C, 0.47mL of phosphazene catalyst 1 is added. As the reaction mixture continues to be heated to 101°C, water, methanol and toluene distillates are collected in a Dean Stark apparatus. Heating is interrupted after distilling enough toluene to obtain a final concentration of about 60% solid solution, usually by removing 45g-100g of distillate. When the final concentration of 60% solids is reached, 0.20mL of trioctylamine is added to the reaction flask under stirring to neutralize the reaction mixture, and the resulting mixture is cooled to room temperature. After cooling to room temperature, a round-bottom flask with a stirring rod and a paddle is weighed and recorded. It is then assumed that all polymer content is retained in the flask, and the NVC is calculated based on mass balance (the difference between the pre-weight and the final weight). In addition, the vinyl content of the solution is calculated.
[0172] Examples GP-3 to GP-6 were repeated using the procedure in Reference Example D above, except that the alkoxysilyl functionalized (meth)acrylate macromonomer prepared in Example MM-2 was replaced with a different alkoxysilyl functionalized (meth)acrylate macromonomer and the weight % of the alkoxysilyl functionalized (meth)acrylate macromonomer was varied. These examples are listed in Table 5.
[0173] Table 5. Summary of synthetic PDMS prepared in Reference Examples CD and selected properties
[0174]
[0175] a MW and PDI determined by GPC analysis
[0176] *Ultra-high MW material may be present but filtered out during GPC injection
[0177] Preparation of reactive silicone pressure-sensitive adhesive composition
[0178] For the benchmark, a 500 ml 3-neck round bottom flask with a stirring rod and blade was used to prepare a silicone PSA. 56.60 g of OH-terminated PDMS 2, 90.66 g of resin 2, 34.02 g of resin 1, 67.97 g of toluene and 0.30 g of silyl phosphate solution were loaded into a flask equipped with an overhead mechanical stirrer, a thermocouple and a Dean Stark device with a water-cooled condenser attached to a nitrogen bubbler. The heating jacket was inserted into a temperature controller to prevent the reaction mixture from being heated to a temperature greater than 175 ° C. Stirring was started and continued until the material became a uniform mixture. 0.44 g of benzoic acid was added at room temperature and heating was started. Reflux was observed at 120 ° C. Water and aromatic solvent (toluene, xylene) distillates were collected in the Dean Stark device. Heating was stopped after two hours. The resulting PSA was cooled to about 50 ° C and poured out.
[0179] Preparation of reactive mixed pressure sensitive adhesive compositions
[0180] In this Example E, a 500 ml 3-neck round bottom flask with a stirring bar and blades was used to prepare a mixed PSA-1. 112.91 g of a dihydroxy-terminated polydimethylsiloxane (NVC=50.03%) with polybutyl methacrylate side groups synthesized as described above for GP-1, 11.68 g of solvent (toluene), 90.66 g of resin 2, 34.02 g of resin 1, and 0.31 g of silyl phosphate solution were charged into a flask equipped with an overhead mechanical stirrer, a thermocouple, and a Dean Stark apparatus with a water-cooled condenser attached to a nitrogen bubbler. A heating jacket was inserted into the temperature controller to prevent the reaction mixture from heating to a temperature greater than 175°C. Stirring was started and continued until the material became a uniform mixture. 0.45 g of benzoic acid was added at room temperature and heating was started. Reflux was observed at 95°C. Water and aromatic solvent (toluene, xylene) distillates were collected in the Dean Stark apparatus. Heating was stopped after two hours. The resulting PSA was cooled to about 50°C and poured.
[0181] Preparation of physical mixture polyorganosiloxane mixed pressure-sensitive adhesive composition
[0182] In this Reference Example F, the poly(meth)acrylate grafted polyorganosiloxanes of Examples GP-1 to GP-5 above are used to prepare a hybrid PSA. Example F is provided as a description of a method for preparing a hybrid PSA-2. In a glass vial, the following starting materials are combined and mixed: 11.28 g grafted polyorganosiloxane GP-1, 11.35 g resin 1, and 2.35 g xylene. Prepare a 10% dibenzoyl peroxide solution (dibenzoyl peroxide dissolved in 90% toluene). Charge 15.00 g PSA-2, the dibenzoyl peroxide solution according to the desired peroxide content, and optionally toluene according to the desired NVC into a SpeedMixer. TM cups, and in the FlackTek SpeedMixer TM Mix at 3,000 RPM for 30 seconds.
[0183] Examples PSA-3 to PSA-7 were repeated using the procedure in Reference Example F above, except that the grafted polyorganosiloxane prepared in Example GP-1 was replaced with a different grafted polyorganosiloxane. These examples are listed in Tables 6 and 7.
[0184] Table 6. Summary of the hybrid pressure-sensitive adhesives prepared in Reference Examples EF
[0185]
[0186] Table 7. Summary of hybrid pressure-sensitive adhesives prepared in Reference Examples EF and selected properties
[0187]
[0188] Comparative Example PSA-8—Cure with 1% Benzoyl Peroxide
[0189] In this comparative example PSA-8, GP-2, Resin 1, and xylene were added to a glass vial in the same ratios as in PSA-3 and PSA-4 using the procedure in Reference Example F. Comparative Example PSA-8 differs in that dibenzoyl peroxide is added to a desired level of 1%. Table 8 shows the same PSA composition, differing only in the dibenzoyl peroxide content. At least 2% dibenzoyl peroxide is required to achieve cure.
[0190] Table 8. Curing of hybrid pressure sensitive adhesives at different dibenzoyl peroxide levels and selected properties Summary
[0191]
[0192] Comparative Example PSA-9—Physical Mixture of Vinyl-Functionalized Grafted Polyorganosiloxanes for Mixing PSA
[0193] In this comparative example PSA-9, a hybrid PSA was prepared using the procedure in reference example F above, except that GP-6 was used to replace the grafted polyorganosiloxane prepared in example GP-1. Table 9 shows the use of the same macromonomer in different hybrid PSAs. Table 10 shows the selected properties. Comparative example PSA-9 is a physical mixture using vinyl-functionalized grafted polysiloxanes; this results in unqualified "wet" peel force and "dry" peel force. PSA-2 is a physical mixture using OH-functionalized grafted polysiloxanes; this results in qualified "dry" peel force, but unqualified "wet" peel force. PSA-1 uses an OH-functionalized grafted polysiloxane reaction; this results in qualified "wet" peel force and "dry" peel force.
[0194] Table 9. Summary of hybrid pressure sensitive adhesives sharing the same macromer .
[0195]
[0196] Table 10. Summary of hybrid pressure sensitive adhesives sharing the same macromer and selected properties
[0197]
[0198] Reference Example G—Membrane Sample Preparation
[0199] Film Formation: Place a piece of paper on a vacuum plate with vacuum turned on, then place a 2 mil thick polyester sheet or a 2 mil thick polyester sheet coated with a fluorosilicone release coating on the paper. Pour the desired composition prepared as described above for Reference Example F onto the polyester or polyester coated with a fluorosilicone release coating and use a 4 mil coating rod to prepare a film. Place the film on a Despatch TM In an oven; each sheet was dried at 80°C for 2 minutes and then cured at 180°C for 2 minutes.
[0200] Reference Example H—GPC Experiment Details
[0201] Molecular weight data were determined by analysis on a Waters 2695 GPC. Poly(meth)acrylate grafted polyorganosiloxane was dissolved in THF at a concentration of 5 mg solid / mL and filtered through a 0.45 μm PTFE syringe filter before injecting a 100 μL sample aliquot. The GPC was equipped with two Polymer Laboratories PLgel 5 μm Mixed-C columns (300 mm × 7.5 mm) preceded by a PLgel 5 μm guard column (50 mm × 7.5 mm) at 35 °C with a flow rate of 1.0 mL / min. Detection was performed using a Waters 2410 differential refractive index detector. Conventional calibration and fitting of 16 narrow polystyrene standards covering a range of 580 g / mol to 2,300,000 g / mol were performed into a third-order polynomial curve.
[0202] Reference Example I—NMR
[0203] 29 Si NMR spectra were obtained on an Agilent 500 MHz DD2 (mi-MR-06) system equipped with a 16 mm silicon-free AutoX probe. Samples were prepared with CDCl3 + 0.02M Cr(acac)3 in Si-free Teflon NMR tubes. Standard parameters applied except nt=1024. 1 H NMR spectra were obtained on a Bruker Avance III HD NMR spectrometer equipped with a 5 mm TCI HC / Si cryoprobe (mi-MR-07). Samples were prepared with CDCl3 in 5 mm NMR tubes. Standard parameters were applied.
[0204] Reference Example J—Synthesis of HSPrMe2SiOMe
[0205] A 3M solution of CH3MgBr in diethyl ether (50 mL, 0.15 mol) was added dropwise to a solution of 3-mercaptopropyltrimethoxysilane (8.5 g, 0.043 mol) in 50 mL THF while maintaining the temperature between 0 and 10°C. The reaction mixture was stirred at 0°C for 1 hour and then treated with dropwise addition of CH3OH (40 mL). The solid was filtered. The crude material was used directly in the next reaction. 5.4 g was collected to obtain a 75% yield of pure product. NMR is consistent with reference Agina, EV, ACS Applied Materials & Interfaces, 2015, 22, 11755-11764.
[0206] Reference Example K—Peel Adhesion (PMMA)
[0207] 1 inch x 81 / 2 strips were cut from 2 mil polyester films prepared as described in Reference Example G and transferred to a clean PMMA panel using an approximately 5 pound roller. Peel adhesion (180°) was tested according to PSTC-101 standards. A 1 inch wide hybrid PSA strip was pulled at 12 inches / minute using a TMI peel and adhesion tester. Results were reported in grams / inch. If the sample showed clean removal of the adhesive failure / strip from the PMMA panel, the sample was qualified.
[0208] Reference Example L—Viscosity
[0209] Tack was tested according to ASTM D-2979. Tack measurements were obtained using a PT-1000 probe tack tester from a blended PSA sample coated onto a 2 mil polyester film prepared as described in Reference Example G. The dwell time was set to 1.0 seconds. Results are reported in grams.
[0210] Reference Example M—“Wet” Peel Force
[0211] A sample of a mixed PSA composition prepared using a 2 mil thick polyester sheet coated with a fluorosilicone release coating as described in Reference Example G was clamped with a 2 mil thick polyester sheet to prepare a laminate (release liner / adhesive / 2 mil polyester film). The release force was measured using a TMI peel and adhesion tester by pulling the release liner side of the laminate from the polyester film side of a 1 inch wide laminate strip at 12 inches / minute.
[0212] Reference Example N—"Dry" Peel Force
[0213] A sample of the mixed PSA composition prepared using a 2 mil thick polyester sheet as described in Reference Example G was clamped with a 2 mil thick polyester sheet coated with a fluorosilicone release coating to prepare a laminate (release liner / adhesive / 2 mil polyester film). The release force was measured using a TMI peel and adhesion tester by pulling the release liner side of the laminate from the polyester film side of a 1 inch wide laminate strip at 12 inches / minute.
[0214] Definition and usage of terms
[0215] The Summary and Abstract are hereby incorporated by reference. Table 7 shows the abbreviations used herein.
[0216] Table 7 Abbreviations
[0217]
[0218]
[0219] Unless otherwise indicated, all amounts, ratios and percentages are by weight. Unless otherwise indicated in the context of this specification, the articles "a", "a kind of" and "the" each refer to one (a kind) or more (multiple). The disclosure of a range includes the range itself and any values and endpoints contained therein. For example, the disclosure of a range of 2.0 to 4.0 not only includes a range of 2.0 to 4.0, but also includes 2.1, 2.3, 3.4, 3.5 and 4.0 and any other number contained therein individually. In addition, for example, the disclosure of a range of 2.0 to 4.0 includes subsets such as 2.1 to 3.5, 2.3 to 3.4, 2.6 to 3.7 and 3.8 to 4.0 and any other subset contained therein. Similarly, the disclosure of a Markush group includes the entire group and also includes any individual member and subgroup contained therein. For example, disclosure of the Markush group a hydrogen atom, an alkyl group, an aryl group, or an aralkyl group includes the individual member alkyl; the subgroups alkyl and aryl; and any other individual members and subgroups contained therein.
[0220] "Alkyl" means an acyclic, branched or unbranched saturated monovalent hydrocarbon group. Examples of alkyl groups include, but are not limited to, methyl, ethyl, propyl (e.g., isopropyl and / or n-propyl), butyl (e.g., isobutyl, n-butyl, tert-butyl and / or sec-butyl), pentyl (e.g., isopentyl, neopentyl and / or tert-pentyl), hexyl, heptyl, octyl, nonyl and decyl, and branched saturated monovalent hydrocarbon groups having 6 or more carbon atoms.
[0221] "Alkenyl" means an acyclic, branched or unbranched monovalent hydrocarbon group having a double bond between two carbon atoms. Examples of alkenyl groups include, but are not limited to, vinyl, allyl, butenyl, pentenyl, and hexenyl, including branched and straight chain species.
[0222] "Aryl" means a cyclic, fully unsaturated hydrocarbon group. Examples of aryl groups include, but are not limited to, cyclopentadienyl, phenyl, anthracenyl, and naphthyl. Monocyclic aryl groups may have 5 to 9 carbon atoms, or 6 to 7 carbon atoms, and or 5 to 6 carbon atoms. Polycyclic aryl groups may have 10 to 17 carbon atoms, or 10 to 14 carbon atoms, and or 12 to 14 carbon atoms.
[0223] "Aralkyl" means an alkyl group having a pendant aryl group and / or a terminal aryl group or an aryl group having a pendant alkyl group. Exemplary aralkyl groups include tolyl, xylyl, benzyl, phenethyl, phenylpropyl and phenylbutyl.
[0224] "Carbocycle" and "carbocyclic" each mean a hydrocarbon ring. A carbocycle may be monocyclic, or alternatively may be a fused polynuclear ring, a bridged polynuclear ring, or a spiro polynuclear ring. A monocyclic carbocycle may have 3 to 9 carbon atoms, or 4 to 7 carbon atoms, and or 5 to 6 carbon atoms. A polycyclic carbocycle may have 7 to 17 carbon atoms, or 7 to 14 carbon atoms, and or 9 to 10 carbon atoms. A carbocycle may be saturated or partially unsaturated.
[0225] "Cycloalkyl" means a saturated carbocyclic ring. Examples of monocyclic cycloalkyl groups are cyclobutyl, cyclopentyl, and cyclohexyl.
[0226] "Halohydrocarbon" means a hydrocarbon in which one or more hydrogen atoms bonded to a carbon atom have been formally replaced by a halogen atom. Halogenated hydrocarbon groups include haloalkyl groups, halogenated carbocyclic groups, and haloalkenyl groups. Haloalkyl groups include fluorinated alkyl groups such as trifluoromethyl (CF3), fluoromethyl, trifluoroethyl, 2-fluoropropyl, 3,3,3-trifluoropropyl, 4,4,4-trifluorobutyl, 4,4,4,3,3-pentafluorobutyl, 5,5,5,4,4,3,3-heptafluoropentyl, 6,6,6,5,5,4,4,3,3-nonafluorohexyl, and 8,8,8,7,7-pentafluorooctyl; and chlorinated alkyl groups such as chloromethyl and 3-chloropropyl. Halogenated carbocyclic groups include fluorinated cycloalkyl groups such as 2,2-difluorocyclopropyl, 2,3-difluorocyclobutyl, 3,4-difluorocyclohexyl and 3,4-difluoro-5-methylcycloheptyl; and chlorinated cycloalkyl groups such as 2,2-dichlorocyclopropyl, 2,3-dichlorocyclopentyl. Halogenated alkenyl groups include chloroallyl.
[0227] As used herein and in the appended claims, the term "(meth)acrylic acid" is intended to be used as a general expression covering either or both acrylic acid and methacrylic acid.
[0228] As used herein and in the appended claims, the term "(meth)acrylate" is intended to be used as a general expression covering either or both acrylates and methacrylates.
[0229] "M-unit" means a unit having the formula R3SiO 1 / 2 A siloxane unit of the formula R2SiO 2 / 2 A siloxane unit of the formula RSiO 3 / 2 A siloxane unit of the formula SiO 4 / 2 of siloxane units.
Claims
1. A polyorganosiloxane mixed pressure-sensitive adhesive composition, comprising: (I) a pressure sensitive adhesive matrix comprising a physical mixture of starting materials (IA) and (IB), a reaction product of starting materials (IA) and (IB), or a combination of both the physical mixture and the reaction product in an amount sufficient to provide 15 wt % to 40 wt % of starting material (IA) and 5 wt % to 60 wt % of starting material (IB); wherein The starting material (IA) is a functionalized polyorganosiloxane having poly(meth)acrylate groups, wherein the functionalized polyorganosiloxane has the following unit formula: [R 3 w (R 5 -SR”)(OR 4 ) (2-w) Si-O 1 / 2 ] p [R 3 v (R 5 -SR”)(OR 4 ) (1-v) Si-O 2 / 2 ] q [(R 5 -SR”)Si-O 3 / 2 ] k (R 6 R 7 2SiO 1 / 2 ) r (R 7 2SiO 2 / 2 ) s (R 6 R 7 SiO 2 / 2 ) t (R 7 3SiO 1 / 2 ) u , where each subscript w is independently 0, 1, or 2, each subscript v is independently 0 or 1, and each R 3 is an independently selected monovalent hydrocarbon group; each R 4 is an independently selected alkyl group; each R 5 is an independently selected divalent hydrocarbon group, each R" is independently a (meth)acrylate polymer, each R 6 Selected from the group consisting of hydroxyl groups and aliphatic unsaturated monovalent hydrocarbon groups, each R 7is an independently selected monovalent hydrocarbon group free of aliphatic unsaturation, subscript p ≥ 0, subscript q ≥ 0, subscript k ≥ 0, (p+q+k) ≥ 1, subscript r ≥ 0, subscript s ≥ 0, subscript t ≥ 0, subscript u ≥ 0, (r+t) ≥ 1, and (p+q+k+r+s+t+u) is sufficient to provide the polyorganosiloxane with a molecular weight of at least 50 kDa; and The starting material (IB) is a polyorganosilicate resin having a unit formula (R 15 2R 16 SiO 1 / 2 ) x (R 15 3SiO 1 / 2 ) y (SiO 4 / 2 ) z , where R 15 is an alkyl group, an aryl group or an aralkyl group; and R 16 is an alkenyl group having 2 to 18 carbon atoms; subscripts x, y and z are mole fractions; subscript x≥0, subscript y≥0, subscript z>0, (x+y)>0, (x+y+z)≤1, and subscripts x, y and z have values such that 0.9≤(x+y) / z≤1.3; the polyorganosilicate resin further comprises a hydroxyl group content of up to 5% by weight based on the weight of the polyorganosilicate resin; and the polyorganosilicate resin has a number average molecular weight greater than 1,500 Da and less than or equal to 8,000 Da as measured by gel permeation chromatography; Starting material (II) a peroxide catalyst, wherein each R in starting material (IA) 6 When each R in the starting material (IA) is hydroxyl, the peroxide catalyst is present in an amount of 2 wt % to 4 wt %, and when each R in the starting material (IA) is 6 When is an aliphatic unsaturated monovalent hydrocarbon group, the peroxide catalyst is present in an amount of 3 wt % to 4 wt %; and 0 wt % to 70 wt % of a starting material (III) solvent; wherein all percentages are by weight based on the combined weight of all starting materials in the polyorganosiloxane hybrid pressure-sensitive adhesive composition.
2. The composition according to claim 1, wherein in the starting material (IA), R 3 has 1 to 18 carbon atoms, R 4 has 1 to 6 carbon atoms, R 5 has 1 to 18 carbon atoms, R 6 is a hydroxyl or alkenyl group of 2 to 18 carbon atoms, and R 7having 1 to 18 carbon atoms, R" having a DP of 1 to 1,000; (p+r+u)=2, subscript k=0, (p+q) is 1 to 100, (r+t) is 1 to 100, and (p+q+r+s+t+u) is sufficient to provide the functionalized polyorganosiloxane with a molecular weight of 50 kDa to 1,000 kDa.
3. The composition according to claim 2, wherein the subscript p is 1 or 2, each R 3 is an alkyl group having 1 to 6 carbon atoms, each R 4 is an alkyl group having 1 to 6 carbon atoms, each R 5 is an alkylene group of 2 to 8 carbon atoms, R" has a DP of 5 to 600, each R 6 is a hydroxyl group or an alkenyl group selected from vinyl and hexenyl, and each R 7 It is an alkyl group of 1 to 6 carbon atoms.
4. The composition according to claim 1, wherein in the starting material (IB), the subscript x=0, and the polyorganosilicate resin has the following unit formula: (R 15 3SiO 1 / 2 ) y’ (SiO 4 / 2 ) z , where subscript y'>4.
5. The composition according to claim 1, wherein each R" is independently a (meth)acrylate copolymer, R 15 is methyl or phenyl, R 16 It is vinyl, allyl or hexenyl.
6. The composition of claim 1, wherein the peroxide catalyst is selected from the group consisting of: dibenzoyl peroxide; 4-monochlorobenzoyl peroxide; diisopropyl benzene peroxide; tert-butyl peroxybenzoate; tert-butyl peroxide isopropyl benzene; tert-butyl oxide 2,5-dimethyl-2,5-di-tert-butylperoxyhexane; 2,4-dichlorobenzoyl peroxide; di-tert-butylperoxy-diisopropylbenzene; 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane; 2,5-di-tert-butylperoxyhexane-3,2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane; cumyl-tert-butyl peroxide; and combinations of two or more thereof.
7. The composition of claim 6, wherein the peroxide catalyst comprises dibenzoyl peroxide.
8. The composition of claim 1, wherein the solvent is present and comprises an aromatic hydrocarbon.
9. The composition of claim 1, wherein the solvent is selected from the group consisting of ethyl acetate, benzene, toluene, xylene, heptane, tetrahydrofuran, and combinations of two or more thereof.
10. The composition of claim 1, wherein starting material (IA) is present in an amount of 17 wt % to 25 wt %; starting material (IB) is present in an amount of 25 wt % to 40 wt %; starting material (III) is present in an amount of 40 wt % to 60 wt %; wherein all percentages are by weight based on the combined weight of all starting materials in the composition, the sum of the weight percentages of all starting materials in the composition being 100%.
11. The composition according to any one of claims 1 to 10, wherein in the starting material (IA), R 6 Two or more examples of are hydroxyl groups.
12. The composition according to any one of claims 1 to 10, wherein in the starting material (IA), R 6 Two or more examples of are aliphatically unsaturated monovalent hydrocarbon groups.
13. A method for preparing the polyorganosiloxane hybrid pressure-sensitive adhesive composition according to claim 11, wherein the method comprises: 1) The starting materials are combined as follows: (IA) The functionalized polyorganosiloxane having a poly(meth)acrylate group, wherein the functionalized polyorganosiloxane has the following unit formula: [R 3 w (R 5 -SR”)(OR 4 ) (2-w) Si-O 1 / 2 ] p [R 3 v (R 5 -SR”)(OR 4 ) (1-v) Si-O 2 / 2 ] q [(R 5 -SR”)Si-O 3 / 2 ] k (R 6 R 7 2SiO 1 / 2 ) r (R 7 2SiO 2 / 2 ) s (R 6 R 7 SiO 2 / 2 ) t (R 7 3SiO 1 / 2 ) u , where each subscript w is independently 0, 1, or 2, each subscript v is independently 0 or 1, and each R 3 is an independently selected monovalent hydrocarbon group; each R 4 is an independently selected alkyl group; each R 5 is an independently selected divalent hydrocarbon group, each R" is independently a (meth)acrylate polymer, each R 6 is selected from the group consisting of a hydroxyl group and an aliphatic unsaturated monovalent hydrocarbon group, provided that R 6 Two or more instances of are hydroxyl groups, each R 7 is an independently selected monovalent hydrocarbon group free of aliphatic unsaturation, subscript p ≥ 0, subscript q ≥ 0, subscript k ≥ 0, (p+q+k) ≥ 1, subscript r ≥ 0, subscript s ≥ 0, subscript t ≥ 0, subscript u ≥ 0, (r+t) ≥ 1, and (p+q+k+r+s+t+u) is sufficient to provide the polyorganosiloxane with a molecular weight of at least 50 kDa; (IB) the polyorganosilicate resin, Optionally (III) the solvent, Optionally (IC) silyl phosphate, and (ID) a condensation reaction catalyst; thereby preparing a reaction mixture comprising a reaction product of the starting materials (IA) and (IB) and by-products; 2) removing all or part of the byproducts during and / or after step 1); 3) adding (II) the peroxide catalyst and optionally adding further additional (III) solvent to the reaction product in step 2); thereby forming the polyorganosiloxane hybrid pressure-sensitive adhesive composition.
14. The method of claim 13, wherein each R" is independently a (meth)acrylate copolymer. 15 . A hybrid polyorganosiloxane pressure-sensitive adhesive composition prepared by the method according to claim 13 .
16. A method for preparing the polyorganosiloxane hybrid pressure-sensitive adhesive composition according to claim 12, wherein the method comprises: 1) The starting material combination includes the following (IA) The functionalized polyorganosiloxane having a poly(meth)acrylate group, wherein the functionalized polyorganosiloxane has the following unit formula: [R 3 w (R 5 -SR”)(OR 4 ) (2-w) Si-O 1 / 2 ] p [R 3 v (R 5 -SR”)(OR 4 ) (1-v) Si-O 2 / 2 ] q [(R 5 -SR”)Si-O 3 / 2 ] k (R 6 R 7 2SiO 1 / 2 ) r (R 7 2SiO 2 / 2 ) s (R 6 R 7 SiO 2 / 2 ) t (R 7 3SiO 1 / 2 ) u , where each subscript w is independently 0, 1, or 2, each subscript v is independently 0 or 1, and each R 3 is an independently selected monovalent hydrocarbon group; each R 4 is an independently selected alkyl group; each R 5 is an independently selected divalent hydrocarbon group, each R" is independently a (meth)acrylate polymer, each R 6 is selected from the group consisting of a hydroxyl group and an aliphatic unsaturated monovalent hydrocarbon group, provided that R 6 Two or more examples of are aliphatic unsaturated monovalent hydrocarbon groups, each R 7 is an independently selected monovalent hydrocarbon group free of aliphatic unsaturation, subscript p ≥ 0, subscript q ≥ 0, subscript k ≥ 0, (p+q+k) ≥ 1, subscript r ≥ 0, subscript s ≥ 0, subscript t ≥ 0, subscript u ≥ 0, (r+t) ≥ 1, and (p+q+k+r+s+t+u) is sufficient to provide the polyorganosiloxane with a molecular weight of at least 50 kDa; (IB) the polyorganosilicate resin, (II) the peroxide catalyst, and and optionally (III) the solvent, thereby forming the polyorganosiloxane hybrid pressure-sensitive adhesive composition.
17. The method of claim 16, wherein each R" is independently a (meth)acrylate copolymer.
Citation Information
Patent Citations
Process for preparing (mercaptoorganyl)alkoxysilanes
US20050124821A1
Copolymeric siloxanes and methods of preparing them
US2676182A
Silyl phosphates as neutralizing agents for alkali metal hydroxides
US4177200A
Silicone pressure-sensitive adhesive process and product with improved lap-shear stability-I
US4584355A
Silicone pressure-sensitive adhesive process and product with improved lap-shear stability-II
US4585836A