Alkali metal quaternary nanomaterials

By developing alkali metal quaternary crystalline nanomaterials, the problem of insufficient open circuit voltage of zinc yellow tin ore thin film solar cells is solved, the efficiency of solar cells is improved, and a more economical and efficient synthesis method is provided, suitable for the application of solar photovoltaic cells .

CN115348948BActive Publication Date: 2024-11-08UNIVERSITY OF THE WITWATERSRAND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180025410.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-11
Filing Date
2021-03-11
Publication Date
2024-11-08
Estimated Expiration
2041-03-11

AI Technical Summary

Technical Problem

The existing thin-film solar cells based on zinc yellow tin ore have insufficient open circuit voltage, resulting in limited conversion efficiency, and production and synthesis methods that are harsh, difficult to replicate, and difficult to compact, lack cost-effective and time-saving synthetic methods.

Method used

An alkali metal quaternary crystalline nanomaterial was developed, with the general formula I2-II-IV-VI4, including Li2ZnSnSe4, Na2ZnSnSe4, Li2ZnSnS4 and Na2ZnSnS4. The chalcogens were dissolved under inert conditions, combined with CuCl, LiCl and NaCl, and heat treatment was carried out. and flocculation steps are prepared to form nanoparticles with original mixed Cu-Au-shaped structures, and solar cells are constructed based on this.

Benefits of technology

It improves the open circuit voltage and conversion efficiency of solar cells, provides a more cost-effective and time-saving synthetic method, enhances physical and chemical characteristics, and is suitable for providing reliable solar photovoltaic cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The present disclosure relates to the manufacture of alkali metal quaternary crystalline nanomaterials. The alkali metal quaternary crystalline nanomaterial has the general formula A (I2-II-IV-VI4); and wherein I is sodium (Na) or lithium (Li), II and IV are Zn or Sn, and VI is a chalcogen selected from the group including: sulfur (S), selenium (Se) and tellurium (Te). The crystalline phase of the alkali metal quaternary crystalline nanomaterial may be a primitive mixed Cu-Au-like structure (PMCA) and may have a space group: P42m. The nanomaterial may be suitable for providing a solar cell. A manufacturing method is also provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the production of alkali metal quaternary crystalline nanomaterials. Background Art

[0002] In the African and developing world context, providing a continuous and reliable supply of electricity in rural areas and informal settlements not connected to the formal grid remains an ongoing challenge. In particular, providing lighting is often a major challenge.

[0003] In many cases, due to lack of proper infrastructure, candles and kerosene lamps have to be used. This presents safety and health risks. Innovative and cost-effective solutions are needed to improve this problem.

[0004] Solar-based power solutions have been extensively researched to provide greater access to electricity and a continuous supply of electricity. It is particularly important to be able to provide a solar panel of relatively small size that is efficient and affordable to manufacture so that in use it can be easily transported to remote areas and provide a reliable supply of electricity. In recent years, thin-film photovoltaics have been studied to provide high efficiency solar solutions.

[0005] In particular, quaternary materials have shown promise, including kesterite-based structures having the general formula I2-II-IV-VI4. The efficiency of kesterite-based thin-film solar cells has been as high as 12.6%, but has been stagnant.

[0006] The main technical problem of existing kesterite-based thin-film solar cells is the open circuit voltage (V oc ) is insufficient. oc The disadvantage is that there are many defects and / or disorder in the crystal structure. These have an impact on the electronic band structure of the absorber, thus resulting in limited solar energy conversion efficiency. Although other quaternary materials have been synthesized, it has been shown that retaining a structure based on kesterite is advantageous and superior to other structures, such as those based on kesterite.

[0007] Typically, attention has been paid to transition metals in kesterites, typically copper-containing kesterites such as Cu2ZnSnSe4 (CZTSe). Transition metal chemistry is very specific, and in order to avoid the kesterite-based structure changing into another crystal form, prior art variants of kesterites have included only minimal doping with other metals in order to improve the described limiting inefficiency. However, excessive doping risks space group changes, which would have a negative impact on efficiency. Kesterites are Space groups have a particular packing arrangement that is advantageous for its physicochemical properties when used. The prior art teaches away from changing the kesterite crystal phase because specific crystal phases have been shown to provide efficiency in use.

[0008] Furthermore, known synthesis methods for producing quaternary materials use harsh synthesis conditions, are difficult to replicate, and once synthesized cannot be compacted to comply with quaternary solar cell fabrication methods that require solution-based synthesis techniques.

[0009] New innovative nanomaterials for use in a solar or sustainable energy economy are needed. Less harsh, more cost-effective and less time-consuming synthesis methods are also needed. Summary of the invention

[0010] According to the first aspect of the present disclosure, there is provided an alkali metal quaternary crystalline nanomaterial having a general formula A.

[0011] wherein formula A is I2-II-IV-VI4;

[0012] And wherein I can be sodium (Na) or lithium (Li)

[0013] and wherein II and IV may be transition metals;

[0014] and wherein VI may be a chalcogen element, which includes sulfur (S), selenium (Se) or tellurium (Te);

[0015] And the crystal phase of the crystalline nanomaterial may not be kesterite and / or stannite.

[0016] Alkali metal quaternary crystalline nanomaterials, wherein the crystalline phase of the nanomaterials can be a primitive mixed Cu-Au-like structure (PMCA) (having a space group: ).

[0017] An alkali metal quaternary crystalline nanomaterial, wherein in formula A, I may be Li, II may be Zn, IV may be Sn, and VI may be Se, such that the nanomaterial may be Li2ZnSnSe4 (LZTSe), and wherein the crystalline phase of the nanomaterial may be a pristine mixed Cu-Au like structure (PMCA), and wherein the nanomaterial may have a space group:

[0018] An alkali metal quaternary crystalline nanomaterial, wherein in formula A, I may be Na, II may be Zn, IV may be Sn, and VI may be Se, such that the nanomaterial may be Na2ZnSnSe4 (NZTSe), and wherein the crystalline phase of the nanomaterial may be a pristine mixed Cu-Au like structure (PMCA), and wherein the nanomaterial may have a space group:

[0019] An alkali metal quaternary crystalline nanomaterial, wherein in formula A, I may be Li, II may be Zn, IV may be Sn, and VI may be Se, such that the nanomaterial may be Li2ZnSnS4 (LZTS), and wherein the crystalline phase of the nanomaterial may be a pristine mixed Cu-Au like structure (PMCA), and wherein the nanomaterial may have a space group:

[0020] Alkali metal quaternary crystalline nanomaterial, wherein in formula A, I may be Na, II may be Zn, IV may be Sn, and VI may be S, so that the nanomaterial may be Na2ZnSnS4 (NZTS), and wherein the crystalline phase of the nanomaterial may be a pristine mixed Cu-Au like structure (PMCA), and wherein the nanomaterial may have a space group:

[0021] The alkali metal quaternary crystalline nanomaterial may be Li2ZnSnSe4 (LZTSe), wherein the crystalline phase may not be kesterite and / or stannite, and may be a pristine mixed Cu-Au like structure (PMCA) (having a space group: ).

[0022] The alkali metal quaternary crystalline nanomaterial may be Na2ZnSnSe4 (NZTSe), wherein the crystalline phase may not be kesterite and / or stannite, and may be a pristine mixed Cu-Au like structure (PMCA) (having a space group: ).

[0023] The alkali metal quaternary crystalline nanomaterial may be Li2ZnSnS4 (LZTS), wherein the crystalline phase may not be kesterite and / or stannite, and may be a pristine mixed Cu-Au like structure (PMCA) (having a space group: ).

[0024] The alkali metal quaternary crystalline nanomaterial may be Na2ZnSnS4 (NZTS), wherein the crystalline phase may not be kesterite and / or stannite, and may be a pristine mixed Cu-Au-like structure (PMCA) (having a space group: ).

[0025] The alkali metal quaternary crystalline nanomaterial according to the present disclosure may be provided as nanoparticles.

[0026] Alkali metal quaternary crystalline nanomaterials can be suitable for providing solar photovoltaic cells.

[0027] Applicants surprisingly provide alkali metal quaternary crystalline nanomaterials of formula A, wherein the crystalline phase is not kesterite or stannite. The unique solid-state properties of the alkali metal quaternary crystalline nanomaterials disclosed herein provide enhanced physicochemical properties. Without being limited by theory, the enhanced physicochemical properties may be due to quantum confinement effects promoted by the unique crystal structure and / or size and / or morphology of the alkali metal quaternary crystalline nanomaterials described herein.

[0028] According to a second aspect of the present disclosure, there is provided a method for chemically synthesizing the alkali metal quaternary crystalline nanomaterial having the general formula A as described in the first aspect of the present disclosure, the method comprising the following steps:

[0029] dissolving a VI selected from the group consisting of sulfur (S), selenium (Se) or tellurium (Te) in an amphiphilic capping agent under inert conditions to form a first solution;

[0030] heating the solvent under reflux to between about 75°C and about 120°C, preferably about 100°C, to form a second solution;

[0031] blending the first and second solutions and heating to between about 120° C. and about 220° C., preferably about 200° C., to form a third solution;

[0032] dissolving at least one of the group of CuCl, LiCl, Li(acac), Li2S, and NaCl in an amphiphilic capping agent to form a fourth solution;

[0033] adding the fourth solution to the third solution to form a fifth solution;

[0034] adding at least one of zinc chloride or tin chloride to the fifth solution to form a sixth solution;

[0035] The sixth solution is maintained heated at between about 120°C and about 220°C, preferably about 200°C, for 30 minutes to 2 hours, preferably 1 hour.

[0036] The method may further comprise the step of adding a flocculant, preferably an alcohol.

[0037] The method may further comprise the step of washing away excess capping agent.

[0038] The method may further comprise a centrifugation step to provide collection of the alkali metal quaternary crystalline nanomaterial.

[0039] The capping agent may be one of the following group: hexadecylamine, oleic acid, trioctylphosphine oxide, and oleylamine.

[0040] The solvent may be one of the following group: hexadecylamine, oleic acid, trioctylphosphine oxide and oleylamine. It should be understood that the capping agent, when used, may include at least four roles: it may cap the nanoparticles; it may control the growth of the crystalline nanomaterial; it may provide a high boiling point solvent; and it may provide a reducing agent.

[0041] According to a third aspect of the present disclosure, there is provided a solar cell comprising a substrate having the alkali metal quaternary crystalline nanomaterial of the first aspect applied thereon.

[0042] The substrate may be glass coated with molybdenum.

[0043] The alkali metal quaternary crystalline nanomaterial may be applied to the substrate by means of coating, preferably spin coating.

[0044] The solar cell may also include a CdS coating.

[0045] The solar cell may also include a ZnO coating.

[0046] The solar cell may also include Al.

[0047] Typically, solar cells are provided in a layered arrangement, preferably as a sandwich.

[0048] According to a fourth aspect of the present disclosure, there is provided a method for manufacturing the solar cell of the third aspect, the method comprising:

[0049] (i) providing a solution of the alkali metal quaternary crystalline nanomaterial of the first aspect in a solvent, preferably toluene;

[0050] (ii) coating, preferably spin coating, the alkali metal quaternary crystalline nanomaterial solution onto a glass substrate coated with molybdenum to form a substrate coated with the alkali metal quaternary crystalline nanomaterial;

[0051] (iii) drying the substrate coated with the alkali metal quaternary crystalline nanomaterial at a temperature between about 60° C. and 80° C.;

[0052] (iv) providing a solution of CdS in a solvent, preferably toluene;

[0053] (v) coating, preferably spin coating, the dried alkali metal quaternary crystalline nanomaterial-coated substrate with a CdS solution to provide a CdS-coated substrate; and

[0054] (vi) ZnO is coated, preferably spin coated, onto the CdS coated substrate.

[0055] In a preferred embodiment, the manufacturing method is carried out in the order provided above to provide a sandwich arrangement.

[0056] The method may further comprise the step of sputtering aluminum onto the CdS coated substrate, preferably under thermal evaporation in high vacuum. There is also provided any of the first to fourth disclosures, substantially as described, illustrated and / or illustrated herein with reference to any of the examples and / or drawings herein. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] FIG1 shows the crystal structures of prior art CZTSe, (a) kesterite and (b) stannite;

[0058] Figure 2 shows XRD patterns of CZTSe and LZTSe and NZTSe according to the present disclosure;

[0059] FIG3 shows Raman spectra of (a) CZTSe, (b) LZTSe, and (c) NZTSe;

[0060] FIG4 shows TEM images of (a) CZTSe, (b) LZTSe, and (c) NZTSe;

[0061] FIG5 shows a solar cell design of a solar cell according to the present disclosure in (a) diagrammatic form and (b) as a photograph of an exemplary embodiment of the preparation;

[0062] FIG6 shows the JV curves of (a) CZTSe, (b) LZTSe, and (c) NZTSe derivative devices;

[0063] Figure 7 The synthesis process of LZTS is shown;

[0064] FIG8 shows the (a) kesterite, (b) stannite, and (c) PMCA structures of LZTS;

[0065] FIG9 shows X-ray diffraction patterns of LZTS nanoparticles synthesized using different lithium sources (LiCl, Li(acac), Li2S) at different precursor ratios (1:1:1:1 and 2:1:0.25:2), wherein (a) shows LiCl at 1:1:1:1 (b) shows LiCl at 2:1:0.25:2 (c) shows Li(acac) at 1:1:1:1, (d) shows Li(acac) at 2:1:0.25:2, (e) shows Li2S at 1:1:1:1 and (f) shows Li2S at 2:1:0.25:2;

[0066] FIG10 shows TEM micrographs of LZTS nanoparticles synthesized using different lithium sources (LiCl, Li(acac), Li2S) at different precursor ratios (1:1:1:1 and 2:1:0.25:2), wherein (a) shows LiCl at 1:1:1:1 (b) shows LiCl at 2:1:0.25:2 (c) shows Li(acac) at 1:1:1:1, (d) shows Li(acac) at 2:1:0.25:2, (e) shows Li2S at 1:1:1:1 and (f) shows Li2S at 2:1:0.25:2;

[0067] Fig.11 The results show that LiCl, Li(acac) and Li2S 7 Li MAS NMR spectrum and corresponding LZTS spectrum;

[0068] FIG12 shows Tauc plots derived from UV-vis absorption spectra of LZTS nanoparticles synthesized using different lithium sources (LiCl, Li(acac), Li2S) at different precursor ratios (1:1:1:1 and 2:1:0.25:2), wherein (a) shows LiCl, (b) shows Li(acac) and (c) shows Li2S;

[0069] Fig.13 Raman spectra of LZTS nanoparticles synthesized using Li2S and 2:1:0.25:2 ratio are shown;

[0070] Figure 14 shows (a) Pt and LZTS at 50mV.s -1 Cyclic voltammetry at scan rate, (b) Nyquist plot of EIS of a symmetric cell with LZTS on GC and (c) electrochemical equivalent circuit;

[0071] FIG. 15 shows Nyquist plots of EIS of symmetric cells with Pt and LZTS on ITO and FTO substrates in (a) and (b), Tafel plots of Pt and LZTS electrodes on ITO and FTO substrates in (c) and (d); and (e) electrochemical equivalent circuit

[0072] FIG. 16 shows the DSSC setup, energy band diagrams, and JV curves of the DSSCs of LZTS on ITO and FTO substrates in (a) to (d). DETAILED DESCRIPTION

[0073] The general provisions of the summary of the invention are repeated here by reference, and need not be repeated in full to avoid repetition. The detailed description and examples below will include specific embodiments of the present disclosure and should not be considered to be limiting in any way. Those skilled in the art may envision several alternatives that do not depart from the scope of the present disclosure.

[0074] According to a first aspect of the present disclosure, there is provided an alkali metal quaternary crystalline nanomaterial having a general formula A (I2-II-IV-VI4);

[0075] And wherein I is sodium (Na) or lithium (Li), II and IV are Zn or Sn, and VI is a chalcogen selected from the group consisting of: sulfur (S), selenium (Se) or tellurium (Te).

[0076] The crystalline phase of the alkali metal quaternary crystalline nanomaterial according to the present disclosure is not kesterite and / or stannite. The crystalline phase of the alkali metal quaternary crystalline nanomaterial may be a primitive mixed Cu-Au-like structure (PMCA) (having a space group: ).

[0077] Preferably, the alkali metal quaternary crystalline nanomaterial is Li2ZnSnSe4 (LZTSe), wherein the crystalline phase is a primitive mixed Cu-Au-like structure (PMCA) (having a space group: ), or the alkali metal quaternary crystalline nanomaterial is Na2ZnSnSe4 (NZTSe), in which the crystalline phase is a primitive mixed Cu-Au-like structure (PMCA) (with space group: ).

[0078] In another embodiment, the alkali metal quaternary crystalline nanomaterial is Li2ZnSnS4 (LZTS), wherein the crystalline phase is a primitive mixed Cu-Au like structure (PMCA) (having space group: ), or the alkali metal quaternary crystalline nanomaterial is Na2ZnSnS4 (NZTS), in which the crystalline phase is a primitive mixed Cu-Au-like structure (PMCA) (with space group: ).

[0079] It should be understood that the alkali metal quaternary crystalline nanomaterials may be suitable for providing solar photovoltaic cells, and the following provides a method of manufacturing as an example.

[0080] According to a second aspect of the present disclosure, there is provided a method for chemically synthesizing the alkali metal quaternary crystalline nanomaterial having the general formula A as described in the first aspect of the present disclosure, the method comprising the following steps:

[0081] (i) dissolving VI4 selected from the group consisting of sulfur (S), selenium (Se) or tellurium (Te) in an amphiphilic capping agent under inert conditions to form a first solution;

[0082] (ii) heating the solvent under reflux to between about 75° C. and about 120° C., preferably about 100° C., to form a second solution;

[0083] (iii) combining the first and second solutions and heating to between about 120° C. and about 220° C., preferably about 200° C., to form a third solution;

[0084] (iv) dissolving at least one of the group consisting of CuCl, LiCl, Li(acac), Li2S and NaCl in an amphiphilic capping agent to form a fourth solution;

[0085] (v) adding the fourth solution to the third solution to form a fifth solution;

[0086] (vi) adding at least one of zinc chloride or tin chloride to the fifth solution to form a sixth solution;

[0087] (vii) maintaining the sixth solution heated at between about 120°C and about 220°C, preferably about 200°C, for 30 minutes to 2 hours, preferably 1 hour.

[0088] The method typically further comprises the step of adding a flocculant, preferably an alcohol. The method typically further comprises the step of washing away excess capping agent.

[0089] The method further comprises a centrifugation step to provide collection of the alkali metal quaternary crystalline nanomaterial.

[0090] A preferred method of manufacture is provided in the examples below.

[0091] According to a third aspect of the present disclosure, there is provided a solar cell comprising a substrate having the alkali metal quaternary crystalline nanomaterial of the first aspect applied thereon.

[0092] The substrate may be glass coated with molybdenum. To the glass coated with molybdenum, alkali metal quaternary crystalline nanomaterials, CdS, ZnO, and finally sputtered Al are added in a layered format. The layered format is preferably in the form of a sandwich.

[0093] According to a fourth aspect of the present disclosure, there is provided a method for manufacturing the solar cell of the third aspect, the method comprising:

[0094] (i) providing a solution of the alkali metal quaternary crystalline nanomaterial of the first aspect in a solvent, preferably toluene;

[0095] (ii) coating, preferably spin coating, the alkali metal quaternary crystalline nanomaterial solution onto a glass substrate coated with molybdenum to form a substrate coated with the alkali metal quaternary crystalline nanomaterial;

[0096] (iii) drying the substrate coated with the alkali metal quaternary crystalline nanomaterial at a temperature between about 60° C. and 80° C.;

[0097] (iv) providing a solution of CdS in a solvent, preferably toluene;

[0098] (v) coating, preferably spin coating, the dried alkali metal quaternary crystalline nanomaterial-coated substrate with a CdS solution to provide a CdS-coated substrate; and

[0099] (vi) ZnO is coated, preferably spin coated, onto the CdS coated substrate.

[0100] In a preferred embodiment, the manufacturing method is carried out in the order provided above to provide a sandwich arrangement. The method may further comprise the step of sputtering aluminum onto the CdS coated substrate, preferably under thermal evaporation in a high vacuum. A preferred method is described below in an example.

[0101] The following non-limiting examples are provided to illustrate and illustrate preferred embodiments of the present disclosure.

[0102] Example

[0103] Example 1 - Li2ZnSnSe4 (LZTSe) and Na2ZnSnSe4 (NZTSe)

[0104] Chemicals

[0105] Copper chloride (CuCl), lithium chloride (LiCl), sodium chloride (NaCl), zinc chloride (ZnCl2), tin chloride (SnCl4.5H2O), elemental selenium, oleylamine (OLA), ethanol, and toluene were purchased from Sigma-Aldrich and used without further purification.

[0106] Synthesis of nanocrystals

[0107] In a three-necked round-bottom flask, 15 mL of end-capping agent (OLA) was added, and nitrogen was then purged to provide inert conditions. Under reflux and strong magnetic stirring, the solvent was heated to 100 ° C, and then 4 mmol of selenium dissolved in the end-capping agent was added, the temperature was further raised to 200 ° C, and then 2 mmol of CuCl / LiCl / NaCl, which was also dissolved in the end-capping agent, was added, and then 1 mmol of zinc chloride and tin chloride were added. The reaction was carried out at 200 ° C and run for 1 hour. Ethanol was added to flocculate the particles and wash off the excess end-capping agent. The nanocrystals were then collected by centrifugation and dried at room temperature before characterization.

[0108] Characterization techniques

[0109] The secondary graphite monochromated CuKα radiation was used at 30 kV and 10 mA. The powder XRD patterns of the synthesized materials were measured on a Bruker D2 phase detector (D2-205530) diffractometer. The measurements were performed at an angle of 2° using a grazing incidence detector, a step size of 0.036°, a step time of 0.5 s, and a temperature of 25°C for 2θ values ​​in the range of 5-90°.

[0110] Raman analysis was performed using a T64000 Series II Triple Spectrometer System from Jobin Yvon Technology of HORIBA Scientific. Raman spectra were acquired using a 514.5 nm argon laser through an Olympus microscope with a 50X objective and a laser power of 1.5 mW.

[0111] Transmission electron microscopy (TEM) was performed on a FEI Technai T12 TEM microscope, which was operated in TEM mode at an accelerating voltage of 120 kV with a beam spot size of 3. The sample was initially suspended in toluene, and a drop of the suspended nanomaterial was then placed on an irregular carbon copper grid. The grid was dried at room temperature before analysis. Varian CaryEclipse (Cary 50) UV-Vis spectrophotometer was used to measure the absorption of nanocrystals. The absorption spectrum was obtained in toluene and placed in a quartz cuvette (1 cm optical path length).

[0112] Solar cell manufacturing

[0113] The device assembly was made by spin coating 50 μL of a toluene solution of different nanoparticles (CZTSe, LZTSe or NZTSe) at 300 rpm on a glass substrate coated with molybdenum. The formed film was dried and baked at 70°C. A toluene solution containing CdS was also spin coated at 5000 rpm to form a very thin window layer. The ZnO layer was then spin coated at 3000 rpm. Aluminum top contacts were sputtered through a shadow mask to produce a patterned electrode array. Al was deposited by thermal evaporation in high vacuum. 0.08 cm 2 The final device area of ​​​​is defined by the overlap between the Mo and Al electrodes. Photovoltaic characteristics such as current (I) and voltage (V) were measured in the dark and under illumination of a Newport ABA solar simulator using a digital source meter (Keithley Instruments Inc., Model 2400) at AM 1.5, 100 mWcm -2 Operate under standard conditions.

[0114] Results and Discussion

[0115] Prior Art Bulk crystal structures of CZTSe and LZTSe have been previously reported in the literature. CZTSe crystallizes in two main crystal structures, called kesterite and stannite, which are tetragonal systems. The two crystal structures are very similar; both have cations located in tetrahedral positions, but the stacking arrangement of Cu and Zn atoms along the c-axis is different. The crystal structure and atomic arrangement of the kesterite and stannite structures are illustrated in Figure 1. In the kesterite structure, the cation layers along the c-axis are arranged in the manner of Cu-Sn, Cu-Zn, Cu-Sn and Cu-Zn. One Cu atom is located at the 2a position; the Zn atom and another Cu atom are located at the 2d and 2c positions, respectively, with corresponding Madelung potentials of -15.04V, -21.88V and -15.21V. In the kesterite structure, the periodic arrangement of Zn-Sn cation layers sandwiched between Cu-Cu layers is repeated, with two Cu atoms located at the 4d position and the Zn atom at the 2a position, with Madelung potentials of -15.30 V and -21.62 V, respectively. The Sn atomic site is located at the 2b position in both structures. Theoretical studies predict that kesterite is slightly lower in energy compared to the kesterite phase and should therefore be thermodynamically more stable than its kesterite counterpart, so most particles crystallize in the kesterite form.

[0116] LZTSe single crystals have been shown to crystallize in a wurtzite structure that can be viewed as a superstructure of hexagonal carbon, i.e., rare hexagonal diamond. Applicants were very surprised that LZTSe according to the present disclosure exhibits The PMCA structure of the tetragonal system of the space group is surprising and unexpected. Without being limited by theory, the unique chemical synthesis method can provide an unexpected crystal system. It is usually a combination of physical properties, such as crystal structure and / or size and / or morphology, that provide unique properties when used.

[0117] Figure 2 Shown are XRD patterns of synthesized CZTSe, LZTSe and NZTSe nanocrystals. The XRD pattern of CZTSe shows that all diffraction peaks are consistent with the kesterite phase (PDF 00-052-0868). Except for the single crystal derived x-ray diffraction pattern of LZTSe consistent with wurtz-kesterite, there are no other reports about LZTSe and NZTSe, but in this article, the pattern is different from the common kesterite and stannite patterns associated with quaternary materials. In addition, the observed pattern does not match common impurities such as ZnSe, SnSe2, Li2Se or Na2Se. For the wurtz-kesterite phase, it is expected that there are three peaks in the region between 20 °-30 °, but these peaks do not exist in the observed LZTSe and NZTSe diffraction patterns. The observed pattern indicates a PMCA-like phase. This is surprising and unexpected.

[0118] To further probe the structure, Raman spectroscopy was performed and the results are shown in Figure 3. The Raman spectrum of CZTSe shows 177 cm -1 、187cm -1 、213cm -1 and 231cm -1 The Raman spectrum of LZTSe shows four expected peaks at lower wavenumbers (127 cm -1 ) is different from that of CZTSe, and this is also found in the NZTSe spectrum (121 cm -1 ) can also be seen on LZTSe. -1 231cm with CZTSe -1 The peaks are similar but slightly shifted. 247cm -1 The peaks at 400 nm and 400 nm may indicate some structural differences between LZTSe and NZTSe. Raman results confirm that the LZTSe and NZTSe nanoparticle crystal structures may be XRD data of PMCA. PMCA is similar to kesterite and stannite, but it can be considered as a combination of two kesterite and stannite unit cells. This structure has not been experimentally observed in the prior art.

[0119] The TEM images in Fig. 4 show that all particles are spherical. The average particle sizes of CZTSe, LZTSe and NZTSe are 9.0 ± 1.07 nm, 6.06 ± 0.9 nm and 8.3 ± 2.7 nm respectively. The standard deviation of NZTSe particles is slightly larger than that of CZTSe and LZTSe particles, indicating more dispersed samples. However, all particles are below 10 nm and are likely to be affected by the quantum confinement effect.

[0120] Nanocrystals for solar cell applications can produce unique properties different from bulk materials, such as multi-exciton generation and hot carrier injection, which are desirable properties. The synthesized nanocrystals were then used to make solar cells, the construction of which is shown in Figure 5. The different layers were solution processed and the Al electrode was sputter coated. The device area corresponding to the connection between the Mo electrode and the Al strip was 0.08 cm 2 Patterning the electrodes creates arrays of small devices, thereby maximizing the output of the solar cell by minimizing defects.

[0121] The current density-voltage (JV) curve produced by a solar cell is shown in Figure 6. The JV curve can be used to evaluate the performance of the solar cell and important parameters can be extracted and used to calculate the efficiency using the following formula:

[0122] P max =V oc J sc FF (1)

[0123]

[0124] Where V oc is the open circuit voltage, J sc is the short circuit current, and FF is the fill factor. Using AM 1.5 and 100mWcm- 2 Standard lighting conditions for evaluating solar cells.

[0125] The extracted parameters are shown in Table 1. The band gap of the synthesized materials was determined using UV-Vis absorption spectroscopy. Similar devices cited in this article do not provide the exact band gap of the material, however, the band gap of CZTSe is reported to be generally between 1.03-1.5eV. Here, the band gaps of CZTSe, LZTSe, and NZTSe are 1.03eV, 1.91eV, and 1.59eV, respectively. They are firmly in the visible region of the solar spectrum. Reducing the size of LZTSe and NZTSe will shift the band gap toward the desired Shockley-Queisser efficiency limit, which occurs at 1.34eV. The Shockley-Queisser efficiency limit refers to the maximum theoretical efficiency of a solar cell that uses a single pn junction to collect energy from a cell.

[0126] Table 1: Solar cell parameters

[0127]

[0128] Compared with the reported CZTSe devices, the fabricated CZTSe solar cells show lower J sc 、V oc and FF values, and thus lower efficiency. However, using the same fabrication conditions, NZTSe and LZTSe in particular show improved results compared to CZTSe. Jsc and Voc (46.9 mA cm for LZTSe) as intrinsic properties of the absorber layer -2 and 486mV, NZTSe is 19.5mAcm- 2 and 405 mV) are even much higher than those reported for CZTSe devices. This indicates that the alkali metal quaternary crystalline nanomaterials disclosed in the present invention improve the open circuit voltage (V oc This is an unexpected and surprising improvement.

[0129] Table 2: Effect of improving FF on efficiency

[0130]

[0131]

[0132] The FF in this case can be increased by improving the quality and thickness of the active layer. Defects in the film coating can be seen from the device in Figure 5. This is common when using a solvent with a lower viscosity (such as toluene) as a spin coating medium. As subsequent layers are added, they re-dissolve the lower layer because good adhesion to the substrate cannot be achieved. This leads to pinholes in the device, resulting in short circuits, which reduces the shunt resistance. Table 2 shows the effect of increasing the FF to 60%, which is an achievable value for zinc stannite solar cells, which can also be seen in the literature. In particular, by increasing the FF of LZTSe solar cells, the efficiency will increase dramatically from 5.65% to 18.95%, an increase of more than three times. This is far higher than any reported solar cell device based on laboratory-scale zinc stannite nanocrystal solutions.

[0133] Example 2 - Li2ZnSnS4 (LZTS)

[0134] Experimental Section

[0135] Material

[0136] Lithium chloride (LiCl, 99.98%), lithium acetylacetonate (Li(acac), 99.95%), lithium sulfide (LiS, 99.98%), zinc chloride (ZnCl2, 98%), tin chloride (SnCl4·5H2O, 97.5%), elemental sulfur (S, ≥99%), oleylamine (OLA, 70%), methanol (96%), ethanol (96%), toluene (anhydrous, 95%), hexane (anhydrous, 95%), isopropanol (anhydrous, 99%), lithium perchlorate (≥95%), lithium iodide (99.9%), sodium iodide (anhydrous, ≥99.9%), 4-tert-butylpyridine (98%), N-methyl-2-pyrrolidone (anhydrous NMP, 99.5%), white titanium dioxide slurry reflector (TiO2, 20.0wt%), Whatman TM Glass microfiber filter paper, glass slides coated with indium-doped tin oxide (surface resistivity of about 8-12Ω / sq), glass slides coated with fluorine-doped tin oxide (surface resistivity of about 7Ω / sq), and N-719 dye (95%) were used for the synthesis and analysis of quaternary chalcogenide nanoparticles. All chemicals were purchased from Sigma-Aldrich, except tin chloride, which was purchased from Saarchem. All chemicals were used without any further purification.

[0137] Colloidal Synthesis of LZTS Nanoparticles

[0138] Hot injection colloid method was used to synthesize nanoparticles. Oleylamine (OLA–10 mL) was heated to 100 °C while stirring under nitrogen. This served as a solvent / surfactant purge process. At 100 °C, Figure 7The component precursors were added in the order listed in the set. After the last precursor was added, the temperature was raised to 200°C and held for 45 minutes. The molar ratios of the precursors were varied to produce 1:1:1:1 and 2:1:0.25:2 Li:Zn:Sn:S samples in all three reactions. The resulting particles were then flocculated using ethanol, recovered by centrifugation at 3000 rpm and dried at room temperature.

[0139] Fabrication of dye-sensitized solar cells (DSSC)

[0140] Typically, a DSSC includes a dye-modified nanocrystalline titanium dioxide (TiO2) electrode made on a transparent conductive oxide (TCO), a platinum (Pt) counter electrode (CE), and an electrolyte solution with an iodide ion / triiodide ion redox couple dissolved between the electrodes. The best DSCCs have achieved efficiencies slightly below 12%. The modest efficiency can be balanced by further reducing the price of DSSCs; this can be achieved by replacing some components. Platinum is an excellent electrocatalyst, however, it is well known that it is an expensive material. Several studies have reported the use of CZTS and its derivatives as CE in DSSCs. The synthesis of PVP-CZTS and CA-CZTS nanofibers is known to be used as CE in DSSCs, and they show power conversion efficiencies (PCEs) of 3.10% and 3.90%, respectively. The PCE of the nanomaterial was found to be in the range of 7.4% to 7.8%.

[0141] Counter electrode fabrication

[0142] The ink for the counter electrode was prepared by dispersing 40 mg of LZTS nanoparticles (Li2S source, ratio of 2:1:0.25:2) in a mixture of 1 mL toluene and 0.1 mL NMP. After vigorous stirring for 24 h, the homogeneous solution was sonicated for 10 min. The solution was then drop-cast onto a pre-cleaned and pre-heated (at 80 °C) ITO / FTO substrate (area of ​​approximately 3.13 cm 2 Once the ink was dry, each counter electrode was annealed at 80° C. for another 10 minutes. Platinum was sputter coated on pre-cleaned ITO / FTO as a reference for comparative studies.

[0143] Photoanode fabrication

[0144] Titanium dioxide (TiO2) slurry was printed onto a pre-cleaned ITO / FTO substrate using a doctor blade method. The screen-printed substrate was then annealed at 350°C for 30 min to remove any residual organic compounds and to allow for better contact between TiO2 and N-719 dye. N-719 dye was then dissolved in methanol (3.0 × 10 -4M) and used to sensitize TiO2. A drop of the dye mixture was placed on the annealed TiO2 and dried overnight in dark ambient conditions.

[0145] Device Assembly

[0146] The photoanode is placed with the active layer facing up and the counter electrode facing down. The two electrodes are mutually biased, and the Whatman filter paper is placed in the middle to define the active area and act as a sponge supporting the redox electrolyte solution. The supporting redox electrolyte solution providing a negative electrochemical potential for the reduction process is composed of 0.05M iodine, 0.1M lithium iodide, 0.1M potassium iodide, 0.1M sodium iodide and 0.5M 4-tert-butylpyridine. The assembled device is fixed together longitudinally by the foldback clips on both sides to form a uniform distribution.

[0147] Characterization

[0148] The nanoparticles were characterized using the following techniques: UV-vis absorption measurements were performed using a Varian Cary Eclipse (Cary 50) UV-vis spectrophotometer. Powdered samples were dispersed in toluene and placed in a 1 cm path length quartz cuvette for spectral analysis. X-ray diffraction (XRD) measurements were performed using a Bruker D2 phaser powder X-ray diffractometer using Cu-Kα1 radiation. The images were obtained at 30 kV / 30 mA, using a grazing incidence detector at an angle of 2°, with a step size of 0.026°, a step time of 37 s, and at a temperature of 25°C for 2θ values ​​between 10-90°. A few milligrams of sample were placed on a zero background holder and flattened with a glass slide. The morphology was obtained using a transmission electron microscope (TEM) FEI Tecnai T12 operated at 200 kV. The samples were dispersed in methanol and sonicated for 10 minutes. A drop of the suspended nanomaterial was then placed on a copper grid with irregular carbon and allowed to dry at room temperature before analyzing the sample. Raman spectra were obtained using a Bruker Raman Senterra spectrophotometer after placing the sample in a quartz holder, which used a 532 nm excitation laser and a very low laser power of 0.5 mV. X-ray photoelectron spectroscopy (XPS) analysis was performed using a Physical Electronics PHI 5700 spectrometer using non-monochromatic Mg Kα X-rays (300 W, 15 kV, and 1253.6 eV) as the excitation source. 7 Li MAS NMR experiments were performed on a 7.05T Bruker Avance III 300MHz spectrometer ( 7The m0 of Li = 116.6 MHz) was performed using a Bruker 2.5 mm HFX MAS probe at a rotation speed of 30 kHz. Cyclic voltammetry (CV), electrochemical impedance spectroscopy (EIS) and Tafel polarization measurements were performed using a Biologic: VMP300. A three-electrode system was used to use a triiodide (I2) consisting of 0.1 M LiClO4, 0.01 M LiI and 0.001 M I2 dissolved in anhydrous acetonitrile. - / I3 - ) redox electrolyte, at 50 mV s -1 The scanning rate was 0.07 cm and the active area was about 0.07 cm. 2 ), platinum (Pt, active area = 0.05 cm 2 ), ITO and FTO (active area is about 1.56cm 2 ) after which CV measurements were performed using Pt as the counter electrode, Ag / AgCl as the reference electrode, and the synthesized CZTS / CZTSe as the working electrode. EIS measurements were obtained using a symmetrical cell with two identical electrodes in a redox electrolyte for DSSC in the dark. The electrodes were analyzed at different open circuit potentials for each sample between 100 kHz and 100 MHz. Tafel polarization analysis was performed at a potential window of -1.0 to 1.0 V with a frequency of 100 mVs -1 The photocurrent-voltage (JV) characteristics of the DSCC were obtained using an HP 4141B source measure unit (SMU) at 100 mW cm -2 (AM 1.5G) measured under controlled lighting.

[0149] Results and Discussion

[0150] Synthesis and Characterization of Li2ZnS4(LZTS)

[0151] Generally, LZTS can crystallize in structures similar to CZTS and CZTSe, kesterite (space group I4), stannite (space group I42m), or pristine mixed Cu-Au (PMCA; space group P42m) crystal structures, and these structures are shown in FIG. 8 .

[0152] The kesterite and stannite structures are body-centered tetragonal lattices with c≈2a and can be considered as two sulfur face-centered cubic (FCC) lattices stacked on top of each other, with Li, Zn, and Sn occupying half of the tetrahedral voids within the FCC lattice. The PMCA structure is a primitive tetragonal lattice with c≈a, as shown in Figure 8. Differences in the arrangement and packing of metal cations within the tetrahedral voids result in these three different structures. The kesterite structure consists of two alternating cation layers, each containing Li and Zn or Li and Sn, while in the kesterite and PMCA structures, one layer of Li alternates with one layer of Zn and Sn. In the kesterite structure, Zn and Sn atoms on the same layer exchange positions every other layer. This exchange of positions between Zn and Sn every other layer is absent in PMCA, making it a primitive tetragonal lattice and distinguishing it from the kesterite structure. The X-ray diffraction of these structures is very similar, with only minor distinguishing features. Due to the larger deformation of stannite and PMCA, the kesterite phase is typically displaced by 0.2°. Kesterite and PMCA are largely indistinguishable; however, kesterite is the more stable phase. Nevertheless, using the XRD experimental data, the lattice constants a, b, and c can be calculated using equation (3) and matched to the reference constants to distinguish the two. The lattice constants are listed in Table 3.

[0153]

[0154] Table 3: Lattice parameters of known tetragonal ZTS structures

[0155]

[0156]

[0157] Figures 9(a) to (f) show the XRD patterns of LZTS synthesized with different lithium precursors and different precursor ratios according to the present disclosure and the standard reference pattern of kesterite. The LiCl and Li(acac) sources configured in two molar ratios do not fully match the reference pattern, indicating the presence of impurities. However, when the source is changed to Li2S, the 2:1:0.25:2 ratio fully matches the reference pattern, but not all planes diffract, indicating a preferred orientation. Because there is no reference pattern for PMCA, equation (3) is used to calculate the lattice constant.

[0158] The values ​​obtained are closer to PMCA. The possible reason why LZTS forms a PMCA structure is due to the different atomic radii of Cu (128pm) and Li (152pm). In addition, transition metals (Cu) are harder than alkali metals because they have a larger number of unpaired electrons in their valence shells, which can promote the deformation of the tetragonal lattice in LZTS. TEM images of LZTS synthesized using different lithium sources and different molar ratios. LiCl-based nanoparticles are quasi-spherical, polydisperse and agglomerated. An increase in size was observed with increasing concentration. Li(acac)-based nanoparticles are very small and form an agglomerated cloud-like morphology. No significant changes were observed with the change in ratio. Li2S-derived particles are small quasi-spherical nanoparticles that are very dispersed. A slight increase in size was observed with the change in ratio.

[0159] X-ray photoelectron spectroscopy (XPS) is a useful technique to evaluate the surface chemistry and bonding of the resulting particles. XPS survey spectra of particles synthesized with different lithium sources and molar ratios were obtained. The spectra show all components of LZTS except lithium. XPS has very low sensitivity to lithium because of its small atomic number. The C1s, N1s, and O1s observed in all spectra are attributed to the capping agent OLA and its oxidation.

[0160] The Li 1s high-resolution spectra of LZTS nanoparticles synthesized using different lithium sources (LiCl, Li(acac), Li2S) at different precursor ratios (1:1:1:1 and 2:1:0.25:2) were investigated. For all samples, lithium was detected. The high-resolution spectra were more sensitive to low concentrations compared to the survey spectra. Metallic lithium (Li 0 ) and Li-S. The intensity of the Li2S derived particles (2:1:0.25:2) ratio is much higher than the other particles and this may indicate the formation of LZTS. This is consistent with the observed XRD results. High resolution spectra of Zn 2p, Sn 3d, S 2p of LZTS nanoparticles synthesized using different Li2S precursor ratios of 2:1:0.25:2 were obtained. The Zn 2p spectrum of the LiCl source shows a double peak, which is deconvoluted into two peaks at 1045.4eV and 1022.3eV with a peak spacing of 23.06eV, which is attributed to Zn 2+ species. In addition, the Sn 3d core-level spectrum illustrates two peaks, which are deconvoluted into 3d3 / 2 (495.2 eV) and 3d5 / 2 (486.7 eV). The peak spacing of 8.41 eV is attributed to Sn 4+ The high-resolution spectrum of S 2p shows two peaks, each of which is deconvoluted into two other peaks. Both the 2p3 / 2 and 2p1 / 2 doublets are related to S 2-In general, similar results were observed for Li(acac) and Li2S derived LZTS nanoparticles, except that the Zn 2p spectrum of Li(acac) showed a double peak still attributed to Zn 2+ ions, and the S2p spectrum of Li2S shows the presence of SO x To further confirm the formation of LZTS, different lithium precursors and the corresponding LZTS nanoparticles were used. 7 Li MAS NMR spectroscopy Fig.11 The characteristic lithium peak at 2-3 ppm is observed for the commercial precursors LiCl, Li(acac) and Li2S. The peak is also observed in the corresponding LZTS nanoparticles, although slightly shifted. This shift confirms the coordination of Li.

[0161] The optical properties of LZTS nanoparticles synthesized using different precursors and ratios are shown in Figures 12(a) to (c). The band gaps of 1:1:1:1 LiCl, Li(acac) and Li2S derived particles are 2.42 eV, 2.39 eV and 3.09 eV, respectively, and when changing the ratio, the band gaps are 3.13 eV, 3.23 eV and 3.14 eV, respectively. The band gap of LZTS nanoparticles derived from Li2S does not change with the change of ratio.

[0162] Based on the XRD, TEM, XPS and NMR results, the best sample was clearly the LZTS nanoparticles synthesized from Li2S using a 2:1:0.25:2 Li:Zn:Sn:S ratio. Therefore, from this point on, all characterizations and applications were based on this sample. The Raman spectrum of LZTS was Fig.13 The A1 mode at 318 cm-1 attributed to the tetragonal PMCA structure was observed. -1 At about 248cm -1 and about 330cm -1 –363cm -1 The additional peaks at 4 and 7 are attributed to the B2 and A1 modes, respectively. This further confirms the formation of LZTS. In addition, Raman analysis shows no evidence of a second phase.

[0163] Application of LZTS as counter electrode in dye-sensitized solar cells

[0164] LZTS nanoparticles synthesized from Li2S (2:1:0.25:2) were drop-cast onto a glassy carbon electrode to study the electrocatalytic activity for the reduction of triiodide ions. Cyclic voltammetry measurements were performed using a three-electrode system to obtain cyclic voltammograms (CVs). The CV shown with two pairs of redox peaks corresponds to the following equation:

[0165]

[0166]

[0167] The catalytic activity depends on two parameters, namely the peak current |J_Red-1| and the peak-to-peak spacing (Epp). The peak current values ​​of Pt and LZTS are 3.53 and 3.16 mA.cm -2 , Epp values ​​are 0.33 and 0.61 V, respectively (Table 4). Higher peak current and lower Epp values ​​indicate better catalytic performance and greater reduction rate. The RedI shift observed near lower potentials indicates poor reversibility of the reaction.

[0168] Table 4: CV and EIS parameters of LZTS counter electrode drop-cast on glassy carbon electrode

[0169]

[0170] EIS was used to evaluate the charge transfer from the CE to the electrolyte. This was performed on a symmetric simulated cell with two identical electrodes that were charged with I3 - / I - The electrolyte is sandwiched in between. Figures 14(a) to (c) show the Nyquist plots of Pt and LZTS and the electrochemical equivalent circuit, whose components represent the four impedance characteristics. Abbreviation, R s represents the series resistance, and R ct represents the charge transfer resistance at the CE / electrolyte interface. dl corresponds to the double layer capacitance, which is used when a perfect semicircle is obtained from the Nyquist plot and explains the charge storage capacity of the CE. Finally, Zw represents the Nernst diffusion element, which is usually taken when a line is 45° to the semicircle at the low frequency region, and explains whether the interaction between the CE and the electrolyte is diffusion controlled. Two key parameters R s and R ct These are summarized in Table 4. High R ct The value indicates poor charge transfer.

[0171] To evaluate the effect of substrate on the electrocatalytic properties of LZTS, the nanoparticles were drop-cast onto ITO and FTO substrates and used for EIS and Tafel plot measurements, see Figure 15. For the symmetric cell EIS measurements, the same equivalent circuit model as that of GC was observed, as shown in Figure 15(e). s and R ct The values ​​are reported in Table 5. When using ITO as the substrate, Pt has the lowest R s Similarly, when the substrate is ITO, LZTS has a lower R sCompared with LZTS, the lower R s The value indicates that Pt is more conductive. The charge transfer process represented by the diameter of the semicircle on the high frequency region is reflected in R ct The lower the R ct Values ​​are ranked later because they result in higher J sc and FF values. Changing the substrate to FTO results in higher R s and R ct Therefore, this suggests that the performance of solar cells using FTO may be poor.

[0172] Table 5: Electrochemical performance parameters obtained from EIS and Tafel polarization plots based on LZTS nanoparticles on ITO and FTO substrates

[0173]

[0174] The Tafel polarization curves are depicted in Figure 15, where the interfacial charge transfer characteristics of the symmetric simulated counter electrode cell are studied. Two important parameters are observed from the polarization curves, namely the exchange current density (J0) and the limiting diffusion current density (Jlim). Both parameters are affected by the anodic or cathodic contribution of each counter electrode and can be described using the following equations;

[0175] J0=RT / nFR c (6)

[0176] J lim =2nFDC / l (7)

[0177] Where R is the gas constant, T is the temperature (298K), F is the Faraday constant, n (n = 2) is the number of electrons, and R ct is the charge transfer resistance, D is the diffusion coefficient, C is I 3- The concentration and l is the thickness of the spacer layer. According to equation (6), J0 and R ct is inversely proportional to. Therefore, J0 can be related to the electrocatalytic activity of CE, which means that a larger J0 value implies a better catalytic activity. Similarly, a larger Jlim value indicates a larger diffusion coefficient D, which leads to a higher catalytic activity based on equation (7). The J0 value of LZTS-ITO is comparable to that of Pt at the current state of the art, indicating that it has good electrocatalytic activity. However, the Jlim value of LZTS using an ITO substrate is less than that of Pt, indicating a lower catalytic activity. On the contrary, the J0 and Jlim of LZTS using an ITO substrate are higher than those of the corresponding FTO, further indicating that ITO should be the preferred substrate.

[0178] The LZTS nanoparticles were then used as CE in DSSCs. Figure 16(a) shows the solar cell architecture, band structure and the resulting current density-voltage (JV) curves derived from both substrates. The performance of LZTS is compared to state-of-the-art Pt electrodes, however it must be noted that these devices require optimization. The results are also summarized in Table 6. It was observed that the type of substrate used has an impact on the overall performance of the solar cell. The ITO substrate performed slightly better than the FTO substrate, and although consistent with the electrochemical data, the degree of change was less than expected. This strongly indicates that the fabrication process needs to be optimized. It is also worth noting that the data in Figure 16 and Table 6 are the low FF values ​​in all samples. The low FF values ​​are due to the high R s value and low shunt resistance (R sh ) values, which are caused by increased recombination at the DSSC interface.

[0179] Table 6: JV parameters of DSSCs of Pt, CZTS and CZTSe on VC, ITO and FTO substrates

[0180]

[0181] LZTS nanoparticles were successfully synthesized for the first time using hot injection method. Changing the lithium source from LiCl to Li(acac) and Li2S and changing the Li:Zn:Sn:S ratio from 1:1:1:1 to 2:1:0.25:2 resulted in the formation of LZTS nanoparticles with different properties. It was observed from the XRD patterns that LiCl and Li(acac) derived particles resulted in the formation of impurities regardless of the ratio used. XPS, 7 Li MAS NMR and Raman spectroscopy confirmed the presence of lithium and the formation of LZTS. A Li2S source and a ratio of 2:1:0.25:2 produced the purest particles and were therefore used as a CE in a DSSC for the first time. Two types of substrates were utilized, ITO and FTO. LZTS was successfully used as an electrocatalyst in DSSCs. Using different substrates resulted in different PCEs. LZTS nanoparticles on ITO performed the best, with a PCE of 2.26%. It must be noted that this was a preliminary study and the device has not yet been optimized. Nonetheless, we have demonstrated that LZTS can be used as a CE in DSSCs.

[0182] The applicant is surprised to find that, compared with the prior art, the alkali metal quaternary crystalline nano material described herein shows enhanced properties. Not limited by theory, it is believed that the unique physicochemical properties given due to the unique solid-state properties are very important in this regard. In addition, the manufacturing method is very important for obtaining unique solid-state properties. The applicant envisions further experiments to finally show the advantages compared with the solar device of the prior art. Although the present disclosure has been described in detail for specific embodiments and / or its examples, it should be understood that those skilled in the art, after obtaining an understanding of the foregoing, can easily think of changes, variations and equivalents to these embodiments. Therefore, the scope of the present disclosure should be estimated as the scope of the claims and any equivalents thereof, and these claims should be attached herein.

Claims

1. An alkali metal quaternary crystalline nanomaterial having a general formula A, wherein the formula A is I2-II-IV-VI4; and wherein I is Na or Li; and wherein II and IV are Zn or Sn; and wherein VI is a chalcogen selected from the group consisting of: S, Se and Te; And wherein the crystal phase of the crystalline nanomaterial is not kesterite and / or stannite, the crystal phase of the nanomaterial is a pristine mixed Cu-Au-like structure, and the nanomaterial has a space group:

2. The alkali metal quaternary crystalline nanomaterial according to claim 1, wherein in formula A, I is Li, II is Zn, IV is Sn, and VI is Se, so that the nanomaterial is Li2ZnSnSe4, and wherein the crystalline phase of the nanomaterial is a pristine mixed Cu-Au-like structure, and wherein the nanomaterial has a space group:

3. The alkali metal quaternary crystalline nanomaterial according to claim 1, wherein in formula A, I is Na, II is Zn, IV is Sn, and VI is Se, such that the nanomaterial is Na2ZnSnSe4, and wherein the crystalline phase of the nanomaterial is a pristine mixed Cu-Au-like structure, and wherein the nanomaterial has a space group:

4. The alkali metal quaternary crystalline nanomaterial according to claim 1, wherein in formula A, I is Li, II is Zn, IV is Sn, and VI is S, such that the nanomaterial is Li2ZnSnS4, and wherein the crystalline phase of the nanomaterial is a pristine mixed Cu-Au-like structure, and wherein the nanomaterial has a space group:

5. The alkali metal quaternary crystalline nanomaterial according to claim 1, wherein in formula A, I is Na, II is Zn, IV is Sn, and VI is S, such that the nanomaterial is Na2ZnSnS4, and wherein the crystalline phase of the nanomaterial is a pristine mixed Cu-Au-like structure, and wherein the nanomaterial has a space group:

6. The alkali metal quaternary crystalline nanomaterial according to any one of claims 1 to 5, suitable for providing solar photovoltaic cells.

7. A method for chemically synthesizing an alkali metal quaternary crystalline nanomaterial having a general formula A according to any one of claims 1 to 6, wherein the formula A is I2-II-IV-VI4, the method comprising the following steps: Selecting a VI of said group selected from S, Se or Te and dissolving in an amphiphilic capping agent under inert conditions to form a first solution; heating the solvent to between 75° C. and 120° C. under reflux to form a second solution; blending the first and second solutions and heating to between 120° C. and 220° C. to form a third solution; dissolving at least one of the group consisting of CuCl, LiCl, lithium acetylacetonate, Li2S, and NaCl in an amphiphilic capping agent to form a fourth solution; adding the fourth solution to the third solution to form a fifth solution; adding at least one of zinc chloride or tin chloride to the fifth solution to form a sixth solution; The sixth solution is heated between 120°C and 220°C for 30 minutes to 2 hours. 8 . The method for chemically synthesizing alkali metal quaternary crystalline nanomaterials according to claim 7 , comprising heating the solvent to 100° C. under reflux to form the second solution.

9. The method for chemically synthesizing alkali metal quaternary crystalline nanomaterials according to claim 7, comprising blending the first and second solutions and heating them to 200°C to form the third solution.

10. The method for chemically synthesizing alkali metal quaternary crystalline nanomaterials according to claim 7, comprising keeping the sixth solution heated at 200°C for 1 hour.

11. The method for chemically synthesizing alkali metal quaternary crystalline nanomaterials according to claim 7, further comprising the step of adding a flocculant.

12. The method for chemically synthesizing alkali metal quaternary crystalline nanomaterials according to claim 11, wherein the flocculant is alcohol.

13. The method for chemically synthesizing alkali metal quaternary crystalline nanomaterials according to any one of claims 7 to 12, wherein the capping agent is selected from one of the following groups: hexadecylamine, oleic acid, trioctylphosphine oxide and oleylamine.

14. The method for chemically synthesizing alkali metal quaternary crystalline nanomaterial according to any one of claims 7 to 12, further comprising the step of washing away excess capping agent.

15. The method for chemically synthesizing alkali metal quaternary crystalline nanomaterials according to any one of claims 7 to 12, wherein the solvent is selected from one of the following groups: hexadecylamine, oleic acid, trioctylphosphine oxide and oleylamine.

16. A solar cell comprising a substrate having the alkali metal quaternary crystalline nanomaterial according to any one of claims 1 to 6 applied thereto.

17. The solar cell of claim 16, wherein the substrate is glass coated with molybdenum.

18. The solar cell according to claim 16, further comprising a CdS, ZnO or Al coating.

19. A method for manufacturing the solar cell according to claim 18, the method comprising: (i) providing a solution of the alkali metal quaternary crystalline nanomaterial according to any one of claims 1 to 6 in a first solvent; (ii) coating the alkali metal quaternary crystalline nanomaterial solution onto a glass substrate coated with molybdenum to form a substrate coated with the alkali metal quaternary crystalline nanomaterial; (iii) drying the substrate coated with the alkali metal quaternary crystalline nanomaterial at a temperature between 60° C. and 80° C.; (iv) providing a solution of CdS in a second solvent; (v) coating the dried alkali metal quaternary crystalline nanomaterial-coated substrate with a CdS solution to provide a CdS-coated substrate; and (vi) coating ZnO onto the CdS-coated substrate.

20. The method of claim 19, wherein the first solvent is toluene.

21. The method of claim 19, wherein the second solvent is toluene.

22. The method of claim 19, wherein in steps (ii), (v) and (vi), the coating is spin coating.