A highly selective carbon monoxide gas sensor and its preparation method and application
Through the design of copper oxide nanosheets/titanium dioxide nanorod composite structural layer and interdigital electrode, the cross-sensitivity problem of hydrogen and carbon monoxide of semiconductor carbon monoxide sensor is solved, and a high selectivity and sensitivity room temperature carbon monoxide detection is achieved, reducing cost and complexity .
Patent Information
- Application Number
- CN202211010514.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-08-23
AI Technical Summary
Existing semiconductor carbon monoxide sensors have the problem of cross-sensitivity of hydrogen and carbon monoxide, which has poor selectivity and is difficult to effectively detect carbon monoxide at room temperature. The common anti-hydrogen interference methods are costly or complex.
Copper oxide nanosheets/titanium dioxide nanorod composite structural layer and interfinger electrode were prepared by hydrothermal method and water bath method to construct a heterojunction of copper oxide nanosheets/titanium dioxide nanorods, and the relative thickness of the two layers was controlled to improve the response of carbon monoxide. and inhibit hydrogen response.
High selectivity and sensitivity detection of carbon monoxide at room temperature is achieved, hydrogen interference is reduced, sensor stability and detection accuracy are improved, and the preparation method is simple and cost-effective.
Smart Images

Figure CN115389571B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of gas sensors, and in particular to a highly selective carbon monoxide gas sensor and a preparation method and application thereof. Background Art
[0002] Gas monitoring plays an important role in climate environment, energy, human health and safety. Carbon monoxide is a toxic gas that is flammable and explosive. It can easily cause poisoning of human tissues and endanger human health. Even a small amount of carbon monoxide can cause harm to the human body. And because carbon monoxide is colorless and odorless, it is difficult to detect, resulting in poisoning and explosion incidents. Therefore, it is necessary to effectively monitor and control carbon monoxide.
[0003] Common carbon monoxide sensors include electrochemical sensors, semiconductor sensors, etc., among which semiconductor sensors are the most widely studied and applied. The principle is to detect gas concentration by using the redox reaction of carbon monoxide on the surface of the semiconductor to cause a change in resistance. Although the current semiconductor carbon monoxide sensors have low cost and long service life, they need to work at high temperatures and have poor selectivity. They are prone to cross-sensitivity to hydrogen and carbon monoxide, which limits their practical application to a certain extent.
[0004] Patent CN111624237A proposes a nickel oxide / titanium dioxide nanorod composite structure gas sensor, in which nickel oxide and titanium dioxide are used to construct a heterojunction. The resulting sensor has a good response to both hydrogen and carbon monoxide at room temperature. However, precisely because of the good response to both hydrogen and carbon monoxide, it is more likely to have cross-sensitivity problems between hydrogen and carbon monoxide during detection, and has poor selectivity for carbon monoxide. When faced with accurate detection of carbon monoxide, the presence of hydrogen in the environment is likely to affect the detection results.
[0005] At present, although the research on gas sensors based on oxide semiconductors and their heterojunction structures is relatively extensive, this type of sensor generally has the problem of responding to multiple gases and poor selectivity, especially when detecting carbon monoxide. Since both carbon monoxide and hydrogen are reducing gases, they will cause changes in the conductivity of semiconductors and are therefore easily interfered by hydrogen. There are two common types of carbon monoxide sensors that are resistant to hydrogen interference. One is to reduce the cross-interference of hydrogen by adding a special catalyst that is less sensitive to hydrogen; the other is to use multiple electrodes, including at least one electrode for detecting CO and one electrode for detecting hydrogen. The two electrodes measure the concentrations of CO and hydrogen respectively, and then subtract the gas reading of hydrogen from the gas reading of CO. The gas-sensitive materials used in these two sensors do not have the function of resisting hydrogen interference. Both use additional means to avoid hydrogen interference. The former sensor requires the use of special catalysts, and the latter sensor requires multiple electrodes, both of which are relatively expensive.
[0006] Patent CN108287183A discloses a method for reducing the cross sensitivity of semiconductor hydrogen sensors to carbon monoxide, wherein a sensor circuit is established, a two-dimensional calibration experiment is conducted, a neural network sample file is made from the collected data, and then a model is constructed through a series of statistical processing, and the output results of the sample are verified by model calculation, thereby correcting the detection results. This method requires complex experiments and a large amount of data in the early stage, which is relatively complicated, and the establishment of the sensor circuit requires multiple different semiconductor sensors, which is costly. In addition, the purpose of the patent is to reduce the interference of carbon monoxide on the hydrogen sensor, but there is no explanation on how to reduce the interference of hydrogen on the carbon monoxide sensor.
[0007] In addition, in this field, TiO2 and CuO are both common semiconductor sensor materials, and there have been reports on the preparation of TiO2 films and CuO films by hydrothermal or water bath methods. However, both sensors have low selectivity for carbon monoxide, and there are no reports in this field on using the two to form a heterojunction to improve CO selectivity, especially to resist hydrogen interference.
[0008] Therefore, there is currently no good solution to the problem of cross-sensitivity between hydrogen and carbon monoxide in semiconductor sensors in the art, and there are very few reports on semiconductor sensors with high selectivity for carbon monoxide. Summary of the invention
[0009] In view of this, the present invention provides a highly selective carbon monoxide gas sensor and its preparation method and application. The carbon monoxide gas sensor provided by the present invention has high sensitivity and good stability at room temperature, and high selectivity for carbon monoxide, which can well solve the problem of cross-sensitivity of semiconductor sensors to hydrogen and carbon monoxide in the prior art.
[0010] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0011] A highly selective carbon monoxide gas sensor comprises a substrate, a copper oxide nanosheet / titanium dioxide nanorod composite structure layer and interdigital electrodes which are stacked in sequence; the copper oxide nanosheet / titanium dioxide nanorod composite structure layer consists of copper oxide nanosheets and titanium dioxide nanorods.
[0012] Preferably, the copper oxide nanosheet / titanium dioxide nanorod composite structure layer comprises a titanium dioxide nanorod layer and a copper oxide nanosheet layer filled between the titanium dioxide nanorods;
[0013] Or, comprising a titanium dioxide nanorod / copper oxide nanosheet composite layer and a copper oxide nanosheet layer grown on the upper surface of the titanium dioxide nanorod / copper oxide nanosheet composite layer;
[0014] Or, it includes a titanium dioxide nanorod layer and a copper oxide nanosheet layer grown on the upper surface of the titanium dioxide nanorod layer.
[0015] Preferably, when the copper oxide nanosheet / titanium dioxide nanorod composite structure layer comprises titanium dioxide nanorods and a copper oxide nanosheet layer filled between the titanium dioxide nanorods, the thickness of the copper oxide nanosheet / titanium dioxide nanorod composite structure layer is 6 to 8 μm, and the thickness of the copper oxide nanosheet layer is 3 to 4 μm;
[0016] When the copper oxide nanosheet / titanium dioxide nanorod composite structure layer comprises a titanium dioxide nanorod / copper oxide nanosheet composite layer and a copper oxide nanosheet layer grown on the upper surface of the titanium dioxide nanorod / copper oxide nanosheet composite layer, the thickness of the titanium dioxide nanorod / copper oxide nanosheet composite structure layer is 8 to 10 μm, and the thickness of the copper oxide nanosheet layer is 4 to 6 μm;
[0017] When the copper oxide nanosheet / titanium dioxide nanorod composite structure layer includes a titanium dioxide nanorod layer and a copper oxide nanosheet layer grown on the upper surface of the titanium dioxide nanorod layer, the thickness of the titanium dioxide nanorod / copper oxide nanosheet composite structure layer is 9 to 11 μm, and the thickness of the copper oxide nanosheet layer is 5 to 7 μm.
[0018] Preferably, the substrate is an FTO substrate; and the interdigital electrodes are platinum interdigital electrodes.
[0019] The present invention also provides a method for preparing the gas sensor described in the above scheme, comprising the following steps:
[0020] (1) preparing a titanium dioxide nanorod film on a substrate surface by a hydrothermal method and performing a first annealing;
[0021] (2) growing copper oxide nanosheets on the titanium dioxide nanorod film after the first annealing, and performing a second annealing to obtain a copper oxide nanosheet / titanium dioxide nanorod composite structure layer;
[0022] (3) preparing interdigital electrodes on the surface of the copper oxide nanosheet / titanium dioxide nanorod composite structure to obtain a highly selective carbon monoxide gas sensor.
[0023] Preferably, the hydrothermal temperature of the hydrothermal method in step (1) is 120-180° C., and the hydrothermal time is 6-16 hours; and the solvent used in the hydrothermal method is a mixed solvent of water and ethanol.
[0024] Preferably, the temperature of the first annealing is 300-500° C., the time is 20-60 min, and the annealing atmosphere is air.
[0025] Preferably, the method for growing copper oxide nanosheets in step (2) is a water bath method or a hydrothermal method; the water bath temperature of the water bath method is 60-90°C, and the water bath time is 0.5-6h; the hydrothermal temperature of the hydrothermal method is 150-180°C, and the hydrothermal time is 8-16h.
[0026] Preferably, the temperature of the second annealing is 100-400° C., the time is 60-120 min, and the annealing atmosphere is air.
[0027] The present invention also provides the application of the highly selective carbon monoxide gas sensor described in the above scheme in carbon monoxide testing.
[0028] The present invention provides a highly selective carbon monoxide gas sensor, comprising a substrate, a copper oxide nanosheet / titanium dioxide nanorod composite structure layer and an interdigital electrode which are stacked in sequence; the copper oxide nanosheet / titanium dioxide nanorod composite structure layer is composed of copper oxide nanosheets and titanium dioxide nanorods. The gas sensor provided by the present invention comprises a copper oxide nanosheet / titanium dioxide nanorod composite structure layer, wherein the copper oxide nanosheet and the titanium dioxide nanorod are composited to form a heterojunction, which can improve the gas sensitivity of the carbon monoxide sensor. Copper oxide, as a P-type semiconductor material, exhibits different responses to different reducing gases. Compared with hydrogen, carbon monoxide has a greater adsorption performance on the surface of copper oxide, so it is easier to adsorb on the surface of copper oxide. When carbon monoxide and hydrogen are introduced, the copper oxide layer on the surface plays a major role, so the copper oxide layer adsorbs more carbon monoxide and a small amount of hydrogen. At the same time, the lower titanium dioxide and the upper copper oxide layer form a heterojunction to improve the response to carbon monoxide.
[0029] Furthermore, the present invention controls the physical adsorption of carbon monoxide and hydrogen in the copper oxide layer and the titanium dioxide layer respectively by controlling the relative thickness of the two layers, thereby further increasing the sensor's response to carbon monoxide, inhibiting the response to hydrogen, and improving selectivity. In addition, when copper oxide comes into contact with the reducing gas carbon monoxide, carbon monoxide reacts with the surface adsorbed oxygen to return the released electrons to the copper oxide, the hole concentration decreases, the hole accumulation layer becomes thinner, and the resistance of the heterojunction film increases. The titanium dioxide layer and the copper oxide layer form a pn heterojunction. The interface effect and barrier effect brought about by the presence of the heterojunction increase the surface gas adsorption amount and increase the resistance variation range. By controlling the relative thickness of the two layers, the internal space charge region of the material can be regulated. The change of the depletion layer plays a vital role in the rise and fall of the resistance value of carbon monoxide gas during the test process, which is manifested as the rise and fall of the sensitivity to carbon monoxide gas. Therefore, the present invention can also effectively improve the sensitivity of the sensor by regulating the relative thickness of the two layers.
[0030] In summary, the present invention introduces in-situ grown copper oxide nanosheets on the surface of titanium dioxide nanorods, and constructs a copper oxide nanosheet / titanium dioxide nanorod heterojunction, which effectively solves the problem of cross-sensitivity between hydrogen and carbon monoxide in the detection process, greatly improves the carbon monoxide selectivity of the sensor, and the sensor of the present invention can operate at room temperature, has high sensitivity to carbon monoxide at room temperature, and has good stability.
[0031] The present invention also provides a method for preparing the highly selective carbon monoxide gas sensor described in the above scheme. The preparation method provided by the present invention has simple steps, low cost, strong operability, low equipment requirements, and can be used for large-scale synthesis. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The resistance-time curve of the TiO2 nanorod gas sensor in Comparative Example 1 in response to carbon monoxide;
[0033] Figure 2 is the XRD pattern of the CuO film (after annealing) in Comparative Example 2;
[0034] Figure 3 This is the surface FESEM image of the CuO film (after annealing) in Comparative Example 2;
[0035] Figure 4 The resistance-time curve of the CuO thin film gas sensor in Comparative Example 2 in response to carbon monoxide;
[0036] Figure 5 This is the surface FESEM image of the CuO / TiO2 nanorod composite structure gas sensor in Example 1;
[0037] Figure 6This is a cross-sectional FESEM image of the CuO / TiO2 nanorod composite structure gas sensor in Example 1;
[0038] Figure 7 The resistance-time curve of the CuO / TiO2 nanorod composite structure gas sensor in Example 1 in response to carbon monoxide;
[0039] Figure 8 This is the surface FESEM image of the CuO / TiO2 nanorod composite structure gas sensor in Example 2;
[0040] Fig. 9 This is a cross-sectional FESEM image of the CuO / TiO2 nanorod composite structure gas sensor in Example 2;
[0041] Fig.10 The resistance-time curve of the CuO / TiO2 nanorod composite structure gas sensor in Example 2 in response to carbon monoxide;
[0042] Fig.11 The resistance-time variation curve of the CuO / TiO2 nanorod composite structure gas sensor in Example 2 in response to hydrogen;
[0043] Fig.12 This is the surface FESEM image of the CuO / TiO2 nanorod composite structure gas sensor in Example 3;
[0044] Fig.13 This is a cross-sectional FESEM image of the CuO / TiO2 nanorod composite structure gas sensor in Example 3;
[0045] Fig.14 This is the resistance-time variation curve of the CuO / TiO2 nanorod composite structure gas sensor in response to carbon monoxide in Example 3. DETAILED DESCRIPTION
[0046] The invention provides a highly selective carbon monoxide gas sensor, comprising a substrate, a copper oxide nanosheet / titanium dioxide nanorod composite structure layer and interdigital electrodes which are stacked in sequence; the copper oxide nanosheet / titanium dioxide nanorod composite structure layer consists of copper oxide nanosheets and titanium dioxide nanorods.
[0047] The gas sensor provided by the present invention includes a substrate. In the present invention, the substrate is preferably an FTO substrate, and the size of the FTO substrate is preferably 2.5 cm×2.5 cm; the present invention has no special requirements on the thickness of the FTO substrate, and an FTO substrate well known to those skilled in the art can be used.
[0048] The gas sensor provided by the present invention comprises a copper oxide nanosheet / titanium dioxide nanorod composite structure layer arranged on the upper surface of a substrate. In the present invention, the copper oxide nanosheet / titanium dioxide nanorod composite structure layer is obtained by in-situ growth of copper oxide nanosheets on the surface of the titanium dioxide nanorod layer. Due to different preparation conditions (detailed description will be given in the subsequent introduction to the preparation method), the thickness of the copper oxide nanosheet layer is different, so the specific structure of the copper oxide nanosheet / titanium dioxide nanorod composite structure layer can be divided into the following three cases:
[0049] 1. When there are fewer copper oxide nanosheets grown on the surface of titanium dioxide nanorods, the copper oxide nanosheets can be filled between the titanium dioxide nanorods during growth. At this time, the copper oxide nanosheet / titanium dioxide nanorod composite structure layer includes a titanium dioxide nanorod layer and a copper oxide nanosheet layer filled between the titanium dioxide nanorods; at this time, the thickness of the copper oxide nanosheet / titanium dioxide nanorod composite structure layer is preferably 6 to 8 μm, more preferably 6 to 7 μm, and further preferably 6.911 μm, and the thickness of the copper oxide nanosheet layer is preferably 3 to 4 μm.
[0050] 2. When the number of copper oxide nanosheets grown on the surface of titanium dioxide nanorods is moderate, the copper oxide nanosheets are first filled between the titanium dioxide nanorods to form a titanium dioxide nanorod / copper oxide nanosheet composite layer (i.e., the structure in case 1), and then continue to grow to form a copper oxide nanosheet layer. At this time, the copper oxide nanosheet / titanium dioxide nanorod composite structure layer includes the titanium dioxide nanorod / copper oxide nanosheet composite layer and the copper oxide nanosheet layer grown on the upper surface of the titanium dioxide nanorod / copper oxide nanosheet composite layer; in this case, the thickness of the titanium dioxide nanorod / copper oxide nanosheet composite structure layer is preferably 8 to 10 μm, more preferably 8 to 9 μm, and further preferably 8.409 μm, the size of the titanium dioxide nanorods is preferably 3 to 4 μm, and the thickness of the copper oxide nanosheet layer is preferably 4 to 6 μm, more preferably 4.5 to 5.5 μm, and further preferably 5.172 μm.
[0051] 3. When there are more copper oxide nanosheets grown on the surface of titanium dioxide nanorods, the copper oxide nanosheets grow directly on the upper surface of the titanium dioxide nanorod layer. At this time, the copper oxide nanosheet / titanium dioxide nanorod composite structure layer includes the titanium dioxide nanorod layer and the copper oxide nanosheet layer grown on the upper surface of the titanium dioxide nanorod layer; in this case, the thickness of the titanium dioxide nanorod / copper oxide nanosheet composite structure layer is preferably 9-11 μm, more preferably 9-10 μm, and further preferably 9.689 μm; the thickness of the titanium dioxide nanorod layer is preferably 3-4 μm, and the thickness of the copper oxide nanosheet layer is preferably 5-7 μm, more preferably 5-6 μm, and further preferably 5.952 μm.
[0052] In a specific embodiment of the present invention, the structure of the copper oxide nanosheet / titanium dioxide nanorod composite structure layer is preferably the second case, in which case the obtained sensor has the highest sensitivity to carbon monoxide and good selectivity.
[0053] The present invention does not specifically limit the morphology of the copper oxide nanosheets in the copper oxide nanosheet / titanium dioxide nanorod composite structure layer, and copper oxide nanosheets with common morphologies in the art may be used.
[0054] The gas sensor provided by the present invention comprises an interdigital electrode arranged on the upper surface of the copper oxide nanosheet / titanium dioxide nanorod composite structure layer. In the present invention, the interdigital electrode is preferably a platinum interdigital electrode, and the thickness of the interdigital electrode is preferably 800-900nm.
[0055] The present invention provides a method for preparing the above-mentioned gas sensor, comprising the following steps:
[0056] (1) preparing a titanium dioxide nanorod film on a substrate surface by a hydrothermal method, and then performing a first annealing;
[0057] (2) growing copper oxide nanosheets on the titanium dioxide nanorod film after the first annealing, and then performing a second annealing to obtain a copper oxide nanosheet / titanium dioxide nanorod composite structure layer;
[0058] (3) preparing interdigital electrodes on the surface of the copper oxide nanosheet / titanium dioxide nanorod composite structure to obtain a highly selective carbon monoxide gas sensor.
[0059] The present invention adopts a hydrothermal method to prepare a titanium dioxide nanorod film on the substrate surface, and then performs drying and first annealing. In the present invention, the substrate is preferably cleaned and dried before use; the cleaning is preferably performed in acetone, ethanol and deionized water in sequence.
[0060] In the present invention, the hydrothermal temperature of the hydrothermal method for preparing titanium dioxide nanorod film is preferably 120-180°C, more preferably 150°C, and the hydrothermal time is preferably 6-16h, more preferably 8h; the solvent used in the hydrothermal method is preferably water or a mixed solvent of water and ethanol, and the ethanol is preferably anhydrous ethanol. In a specific embodiment of the present invention, the volume of the solvent used in the hydrothermal method is preferably fixed to 30mL, specifically using a mixed solvent of 28mL water and 2mL ethanol; in the present invention, adding ethanol to the solvent can enhance the condensation kinetics, thereby promoting nucleation and growth, and providing more seeds.
[0061] In a specific embodiment of the present invention, the hydrothermal method for preparing titanium dioxide nanorod film specifically comprises the following steps:
[0062] (a) mixing water, ethanol, concentrated hydrochloric acid and a titanium source to obtain a titanium dioxide precursor solution;
[0063] (b) Place two FTO substrates with the conductive surface facing downward in a V shape against the inner wall of the reactor, and transfer the titanium dioxide precursor solution into the reactor for hydrothermal reaction.
[0064] In the present invention, the concentrated hydrochloric acid is used to provide an acidic environment to inhibit hydrolysis of the titanium source, and the pH value of the acidic environment is specifically 2; the titanium source is preferably tetrabutyl titanate, titanium tetrachloride or titanium isopropoxide; the volume fraction of the titanium source in the titanium dioxide precursor solution is preferably 1.5% to 5%; the volume ratio of water, ethanol, concentrated hydrochloric acid and titanium source is preferably 28:2:30:1.
[0065] After the hydrothermal reaction is completed, the present invention preferably washes and dries the substrate on which the titanium dioxide nanorods are grown in sequence to obtain a titanium dioxide nanorod film on the substrate. In the present invention, the washing detergent is preferably deionized water, and the washing method is specifically as follows: soaking the substrate of the titanium dioxide nanorod film in deionized water for 6 hours, changing the water every 3 hours; the drying temperature is preferably 60 to 90°C.
[0066] After obtaining the titanium dioxide nanorod film, the present invention performs a first annealing on the nanorod film. In the present invention, the temperature of the first annealing is preferably 300-500°C, more preferably 350-400°C, the time of the first annealing is preferably 20-60 minutes, more preferably 30-40 minutes, and the atmosphere of the first annealing is preferably air. The present invention improves the crystallinity of the TiO2 nanorods and the adhesion to FTO through the first annealing.
[0067] After the first annealing is completed, the present invention grows copper oxide nanosheets on the titanium dioxide nanorod film after the first annealing, and then performs a second annealing to obtain a copper oxide nanosheet / titanium dioxide nanorod composite structure layer. In the present invention, the method for growing copper oxide nanosheets is preferably a water bath method or a hydrothermal method; when the water bath method is used, the water bath temperature of the water bath method is preferably 60 to 90°C, more preferably 70 to 80°C, and the water bath time is preferably 0.5 to 6 hours, more preferably 2 to 4 hours, wherein the longer the water bath time, the greater the growth thickness of the copper oxide nanosheet; when the hydrothermal method is used, the hydrothermal temperature of the hydrothermal method is preferably 150 to 180°C, more preferably 150°C, and the hydrothermal time is preferably 8 to 16 hours, more preferably 10 to 12 hours.
[0068] In the present invention, the water bath method for growing copper oxide nanosheets preferably comprises the following steps:
[0069] (i) mixing a copper source, water and aqueous ammonia to obtain a copper oxide precursor solution;
[0070] (ii) Two substrates with titanium dioxide nanorod films grown thereon are placed with the titanium dioxide nanorod films facing downwards in a V-shape against the inner wall of a beaker, and the copper oxide precursor solution is transferred into the beaker for a water bath reaction.
[0071] In the present invention, the copper source is preferably copper nitrate pentahydrate or copper chloride dihydrate; the copper source, water and ammonia water usage ratio is preferably 0.5-3g:80-100mL:2-6mL, more preferably 0.7-0.8g:80mL:4mL, 0.9-1g:80mL:4mL or 2.9-3.0g:80mL:4mL; the water is preferably deionized water. The present invention adjusts the pH value of the copper oxide nanosheet precursor solution to 8-10 by adding ammonia water. The present invention has no requirements for the concentration of the ammonia water, and the pH value of the precursor solution can be adjusted to the above range. In a specific embodiment of the present invention, the more the amount of copper source is used, the more copper oxide nanosheets are generated. As the amount of copper source increases successively, the resulting copper oxide nanosheet / titanium dioxide nanorod composite structure layers correspond to the above-mentioned case one, case two and case three, respectively.
[0072] After the water bath reaction is completed, the present invention preferably takes out the sample with grown copper oxide nanosheets, and then washes and dries them in sequence to obtain copper oxide nanosheets grown on the titanium dioxide nanorod film; the washing detergent is preferably deionized water; and the drying temperature is preferably 60-90°C.
[0073] In the present invention, the hydrothermal method for growing copper oxide nanosheets preferably comprises the following steps:
[0074] (I) mixing a copper source, water and ethylene glycol to obtain a copper oxide nanosheet precursor solution;
[0075] (II) Two FTO substrates with titanium dioxide nanorod films grown thereon are placed with the titanium dioxide nanorod films facing downwards in a V-shape against the inner wall of a reactor, and a copper oxide nanosheet precursor solution is transferred into the reactor for a hydrothermal reaction.
[0076] In the present invention, the copper source is preferably cupric chloride dihydrate; the amount ratio of the copper source, water and ethylene glycol is preferably 1-3 g:30 mL:0-20 mL. When the amount of ethylene glycol is 0, that is, the solvent used is water, and the addition of ethylene glycol is omitted during the preparation; the water is preferably deionized water.
[0077] After the hydrothermal reaction is completed, the present invention takes out the sample with the copper oxide nanosheets grown, and then washes and dries it in sequence to obtain the copper oxide nanosheets grown on the titanium dioxide nanorod film; the washing detergent is preferably deionized water; and the drying temperature is preferably 60-90°C.
[0078] In the present invention, the temperature of the second annealing is preferably 100-400°C, more preferably 200-300°C, the time of the second annealing is preferably 30-90 minutes, more preferably 60-80 minutes; the atmosphere of the second annealing is preferably air. The present invention improves the crystallinity of the copper oxide nanosheets and the contact with titanium dioxide through the second annealing.
[0079] After obtaining the copper oxide nanosheet / titanium dioxide nanorod composite structure layer, the present invention prepares interdigital electrodes on the surface of the copper oxide nanosheet / titanium dioxide nanorod composite structure to obtain a copper oxide nanosheet / titanium dioxide nanorod composite structure gas sensor. The present invention has no special requirements for the method of preparing the interdigital electrodes, and a method familiar to those skilled in the art can be used. In a specific embodiment of the present invention, it is preferably prepared by a DC magnetron sputtering method; the parameters of the DC magnetron sputtering method preferably include: a back vacuum degree of 6×10 -4 Pa, Ar flow rate is 10-20 sccm, working gas pressure is 0.5-1 Pa, DC sputtering power is 40-60 W, sputtering time is 5-10 min, and the sputtering target is preferably a Pt target with a purity of 99.99%.
[0080] The technical solutions of the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention, but they should not be understood as limiting the protection scope of the present invention.
[0081] Comparative Example 1
[0082] The FTO substrate was cleaned in acetone, ethanol and deionized water in turn and then dried. The dried FTO substrate was placed in a V shape against the inner wall of the polytetrafluoroethylene of the hydrothermal reactor, and a titanium dioxide precursor solution prepared by 28 mL of deionized water, 2 mL of anhydrous ethanol, 30 mL of concentrated hydrochloric acid and 1 mL of tetrabutyl titanate was poured into it. The TiO2 nanorod film was obtained by hydrothermal reaction at 150°C for 8 hours. After the reactor was cooled to room temperature, the film was washed with deionized water, immersed in deionized water for 3 hours, dried at a constant temperature of 70°C, annealed at 400°C in an air atmosphere of a tubular furnace for 20 minutes, and then used for later use.
[0083] The Pt target with a purity of 99.99% was installed at the cathode target position of the magnetron sputtering system. The distance between the target and the substrate was fixed at 60 mm. A cross-finger mask was placed on the surface of the TiO2 film. The mechanical pump and the solenoid valve molecular pump were turned on respectively. When the background vacuum reached 6×10 -4 When the argon gas flow rate was set to 14.4 sccm, the chamber working pressure was maintained at 0.5 Pa, the DC sputtering power was set to 40 W, and the target material was sputtered for 5 min to prepare a metal Pt interdigital electrode to obtain a TiO2 nanorod gas sensor.
[0084] The obtained TiO2 nanorod gas sensor was used to detect carbon monoxide at room temperature, and the carbon monoxide concentration range was 1 to 200 ppm. The results are as follows Figure 1 As shown. Figure 1 It can be seen that the obtained gas sensor has a very low response to carbon monoxide, and what occurs is a reaction in which the resistance value decreases after the introduction of CO. After calculation, when 200ppm CO is introduced, the sensitivity is only 1.04 (the calculation formula of the sensitivity is S = R air / R gas In the following comparative examples and embodiments, the calculation formula of sensitivity is the same and will not be repeated hereafter).
[0085] Comparative Example 2
[0086] The FTO substrate was cleaned in acetone, ethanol and deionized water in sequence and then dried for use.
[0087] Mix 2.33 g of copper nitrate pentahydrate, 80 mL of deionized water, and 4 mL of ammonia water to obtain a copper oxide precursor solution. The precursor solution is placed in a beaker, and two FTO sheets are placed in a V shape on the inner wall of the beaker for a water bath reaction. The temperature of the water bath reaction is 75°C and the time is 3 hours to obtain CuO nanosheets grown on the FTO substrate. After the reaction is completed, the beaker is taken out and cooled to room temperature. The film is washed with deionized water and immersed in deionized water. After soaking for 3 hours, it is dried at a constant temperature of 70°C, annealed at 200°C in an air atmosphere of a tube furnace for 60 minutes, and then set aside.
[0088] The Pt target with a purity of 99.99% was installed at the cathode target position of the magnetron sputtering system. The distance between the target and the substrate was fixed at 60 mm. A cross-finger mask was placed on the surface of the CuO film. The mechanical pump and the solenoid valve molecular pump were turned on respectively. When the background vacuum reached 6×10 -4 When the pressure was 0.5 Pa, the argon gas flow rate was set to 14.4 sccm, the chamber working pressure was maintained at 0.5 Pa, the DC sputtering power was set to 40 W, and the target was sputtered for 5 min to prepare a metal Pt interdigital electrode to obtain a CuO thin film gas sensor.
[0089] Figure 2 The XRD pattern of CuO film (after annealing) shows that the obtained sample has exposed (11-1)(111)(200) CuO crystal planes;
[0090] Figure 3 FESEM surface image of CuO film (after annealing).
[0091] The obtained CuO thin film gas sensor was used to detect carbon monoxide at room temperature, and the carbon monoxide concentration was 1 to 200 ppm. The results are as follows Figure 4 As shown. Figure 4 It can be seen that the obtained gas sensor has an extremely low response to carbon monoxide, and what occurs is a reaction in which the resistance value increases after the introduction of CO. According to calculations, when 200ppmCO is introduced, the sensitivity is only 1.38.
[0092] Example 1
[0093] The FTO substrate was cleaned in acetone, ethanol and deionized water in turn and then dried. The dried FTO substrate was placed in a V shape against the inner wall of the polytetrafluoroethylene of the hydrothermal reactor, and a titanium dioxide precursor solution prepared by 28 mL of deionized water, 2 mL of anhydrous ethanol, 30 mL of concentrated hydrochloric acid and 1 mL of tetrabutyl titanate was poured into it. The TiO2 nanorod film was obtained by hydrothermal reaction at 150°C for 8 hours. After the reactor was cooled to room temperature, the film was washed with deionized water, immersed in deionized water for 3 hours, dried at a constant temperature of 70°C, annealed at 400°C in an air atmosphere of a tubular furnace for 20 minutes, and then used for later use.
[0094] A copper oxide precursor solution was prepared with 0.773 g of copper nitrate pentahydrate, 80 mL of deionized water and 4 mL of ammonia water. The copper oxide precursor solution was placed in a beaker. Two FTO sheets with TiO2 nanorods grown on them were placed in a V-shape on the inner wall of a polytetrafluoroethylene reactor for a water bath reaction. The temperature of the water bath reaction was 75°C for 3 hours, and CuO was grown on the TiO2 nanorods as the substrate. After the reaction was completed, the beaker was taken out and cooled to room temperature. The film was washed with deionized water and immersed in deionized water. After soaking for 3 hours, it was dried at a constant temperature of 70°C and annealed at 200°C in an air atmosphere of a tubular furnace for 60 minutes to obtain a CuO / TiO2 nanorod composite film.
[0095] The Pt target with a purity of 99.99% was installed at the cathode target position of the magnetron sputtering system. The distance between the target and the substrate was fixed at 60 mm. A cross-finger mask was placed on the surface of the CuO / TiO2 nanorod composite film. The mechanical pump and the solenoid valve molecular pump were turned on respectively. When the background vacuum reached 6×10 -4 When the argon gas flow rate was set to 14.4 sccm, the chamber working pressure was maintained at 0.5 Pa, the DC sputtering power was set to 40 W, and the target was sputtered for 5 min to prepare the metal Pt interdigital electrode. The obtained sensor was recorded as the CuO / TiO2 nanorod composite structure gas sensor.
[0096] Figure 5 This is the surface FESEM image of the CuO / TiO2 nanorod composite structure gas sensor obtained in Example 1;
[0097] Figure 6 This is a cross-sectional FESEM image of the CuO / TiO2 nanorod composite structure gas sensor obtained in Example 1.
[0098] Combination Figures 5-6 as well as Figure 4 It can be seen that the CuO / TiO2 nanorod composite structure is successfully synthesized in this embodiment, and the composite structure is composed of titanium dioxide nanorods and copper oxide nanosheets filled between the titanium dioxide nanorods (ie, the above-mentioned case 1), and the thickness of the composite structure is 6.911 μm.
[0099] The obtained CuO / TiO2 nanorod composite structure gas sensor was tested in a carbon monoxide atmosphere at room temperature, with a carbon monoxide concentration range of 1 to 200 ppm. The results are as follows Figure 7 The results show that the sensor exhibits a lower sensitivity to carbon monoxide (sensitivity is 3.28 when 200 ppm CO is introduced), but compared with the sensors of pure TiO2 nanorods or pure CuO nanosheets in Comparative Examples 1-2, the carbon monoxide detection performance of the sensor obtained in Example 1 is improved.
[0100] Example 2
[0101] The FTO substrate was cleaned in acetone, ethanol and deionized water in turn and then dried. The dried FTO substrate was placed in a V shape against the inner wall of the polytetrafluoroethylene of the hydrothermal reactor, and a titanium dioxide precursor solution prepared by 28 mL of deionized water, 2 mL of anhydrous ethanol, 30 mL of concentrated hydrochloric acid and 1 mL of tetrabutyl titanate was poured into it. The TiO2 nanorod film was obtained by hydrothermal reaction at 150°C for 8 hours. After the reactor was cooled to room temperature, the film was washed with deionized water, immersed in deionized water for 3 hours, dried at a constant temperature of 70°C, annealed at 400°C in an air atmosphere of a tubular furnace for 20 minutes, and then used for later use.
[0102] A copper oxide precursor solution was prepared with 0.966 g of copper nitrate pentahydrate, 80 mL of deionized water and 4 mL of ammonia water. The copper oxide precursor solution was placed in a beaker, and two FTO sheets with TiO2 nanorods grown on them were placed in a V-shape on the inner wall of the beaker for a water bath reaction at a temperature of 75°C for 3 hours to grow CuO on the TiO2 nanorods as a substrate. After the reaction was completed, the beaker was taken out and cooled to room temperature. The film was washed with deionized water and then immersed in deionized water for 3 hours, and then dried at a constant temperature of 70°C. It was annealed at 200°C in an air atmosphere in a tubular furnace for 60 minutes to obtain a CuO / TiO2 nanorod composite film.
[0103] The Pt target with a purity of 99.99% was installed at the cathode target position of the magnetron sputtering system. The distance between the target and the substrate was fixed at 60 mm. A cross-finger mask was placed on the surface of the CuO / TiO2 nanorod composite film. The mechanical pump and the solenoid valve molecular pump were turned on respectively. When the background vacuum reached 6×10 -4When the pressure was 0.5 Pa, the argon gas flow rate was set to 14.4 sccm, the chamber working pressure was maintained at 0.5 Pa, the DC sputtering power was set to 40 W, and the target material was sputtered for 5 min to prepare a metal Pt interdigital electrode to obtain a CuO / TiO2 nanorod composite structure gas sensor.
[0104] Figure 8 This is the surface FESEM image of the CuO / TiO2 nanorod composite structure gas sensor obtained in Example 2;
[0105] Fig. 9 This is a cross-sectional FESEM image of the CuO / TiO2 nanorod composite structure gas sensor obtained in Example 2.
[0106] Combination Figures 8-9 It can be seen that the CuO / TiO2 nanorod composite structure synthesized in this embodiment is composed of a titanium dioxide nanorod / copper oxide nanosheet composite layer (including titanium dioxide nanorods and copper oxide nanosheets filled between the titanium dioxide nanorods) and a copper oxide nanosheet layer grown on the upper surface of the titanium dioxide nanorod / copper oxide nanosheet composite layer (ie, the above-mentioned case 2), wherein the thickness of the titanium dioxide nanorod / copper oxide nanosheet composite structure layer is 8.409 μm, and the thickness of the copper oxide nanosheet layer is 5.172 μm.
[0107] The obtained CuO / TiO2 nanorod composite structure gas sensor was tested in a carbon monoxide atmosphere at room temperature, with a carbon monoxide concentration range of 1 to 200 ppm. The results are as follows Fig.10 shown.
[0108] The obtained CuO / TiO2 nanorod composite structure gas sensor was tested in a hydrogen atmosphere at room temperature with a hydrogen concentration range of 1 to 200 ppm. The results are as follows Fig.11 As shown. Figure 10-11 It can be seen that the sensor prepared in Example 2 has high sensitivity to carbon monoxide (specifically, when 200 ppm CO is introduced, the sensitivity is 23.03), and extremely low sensitivity to hydrogen (specifically, when 200 ppm H2 is introduced, the sensitivity is 2.34). It also has good repeatability, and can well solve the cross-sensitivity problem between carbon monoxide and hydrogen.
[0109] Example 3
[0110] The FTO substrate was cleaned in acetone, ethanol and deionized water in turn and then dried. The dried FTO substrate was placed in a V shape against the inner wall of the polytetrafluoroethylene of the hydrothermal reactor, and a titanium dioxide precursor solution prepared by 28 mL of deionized water, 2 mL of anhydrous ethanol, 30 mL of concentrated hydrochloric acid and 1 mL of tetrabutyl titanate was poured into it. The TiO2 nanorod film was obtained by hydrothermal reaction at 150°C for 8 hours. After the reactor was cooled to room temperature, the film was washed with deionized water, immersed in deionized water for 3 hours, dried at a constant temperature of 70°C, annealed at 400°C in an air atmosphere of a tubular furnace for 20 minutes, and then used for later use.
[0111] A copper oxide precursor solution was prepared with 2.91 g of copper nitrate pentahydrate, 80 mL of deionized water and 4 mL of ammonia water. The copper oxide precursor solution was placed in a beaker, and two FTO sheets with TiO2 nanorods grown on them were placed in a V-shape on the inner wall of a polytetrafluoroethylene reactor for a water bath reaction at a temperature of 75°C for 3 hours to grow CuO on the TiO2 nanorods as a substrate. After the reaction was completed, the beaker was taken out and cooled to room temperature. The film was washed with deionized water and then immersed in deionized water for 3 hours, and then dried at a constant temperature of 70°C. It was annealed at 200°C in an air atmosphere in a tubular furnace for 60 minutes to obtain a CuO / TiO2 nanorod composite film.
[0112] The Pt target with a purity of 99.99% was installed at the cathode target position of the magnetron sputtering system. The distance between the target and the substrate was fixed at 60 mm. A cross-finger mask was placed on the upper surface of the CuO / TiO2 nanorod composite film. The mechanical pump and the solenoid valve molecular pump were turned on respectively. When the background vacuum reached 6×10 -4 When ρ = 40.5 Pa, the argon gas flow rate was set to 14.4 sccm, the chamber working pressure was maintained at 0.5 Pa, the DC sputtering power was set to 40 W, and the target was sputtered for 5 min to prepare a metal Pt interdigital electrode.
[0113] Fig.12 This is the surface FESEM image of the CuO / TiO2 nanorod composite structure gas sensor;
[0114] Fig.13 This is the cross-sectional FESEM image of the CuO / TiO2 nanorod composite structure gas sensor.
[0115] according to Figures 12-13 It can be seen that the copper oxide nanosheet / titanium dioxide nanorod composite structure layer prepared in this embodiment is composed of a titanium dioxide nanorod layer and a copper oxide nanosheet layer grown on the upper surface of the titanium dioxide nanorods (i.e., case three), wherein the thickness of the titanium dioxide nanorod layer is 3.737 μm, and the thickness of the copper oxide nanosheet layer is 5.952 μm.
[0116] The obtained CuO / TiO2 nanorod composite structure gas sensor was tested in a carbon monoxide atmosphere at room temperature. The results are as follows Fig.14 As shown. Fig.14 It can be seen that the sensitivity of the sensor prepared in Example 3 is 5.3 when 200 ppm CO is introduced. Compared with Example 2, the sensor prepared in Example 3 has a lower response to carbon monoxide. Considering that as the surface copper oxide nanosheets increase, nanosheets will accumulate, hindering the adsorption of gas on the exposed surface, resulting in reduced sensor performance. However, compared with the sensors with pure TiO2 nanorods or pure CuO nanosheet structures prepared in Comparative Examples 1 to 2, the performance of the sensor in Example 3 to carbon monoxide is improved.
[0117] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A highly selective carbon monoxide gas sensor, It is characterized in that It comprises a substrate, a copper oxide nanosheet / titanium dioxide nanorod composite structure layer and an interdigitated electrode which are stacked in sequence; the copper oxide nanosheet / titanium dioxide nanorod composite structure layer is composed of copper oxide nanosheets and titanium dioxide nanorods; The copper oxide nanosheet / titanium dioxide nanorod composite structure layer comprises a titanium dioxide nanorod / copper oxide nanosheet composite layer and a copper oxide nanosheet layer grown on the upper surface of the titanium dioxide nanorod / copper oxide nanosheet composite layer; the titanium dioxide nanorod / copper oxide nanosheet composite structure layer has a thickness of 8 to 10 μm, and the copper oxide nanosheet layer has a thickness of 4 to 6 μm; The method for preparing the gas sensor comprises the following steps: (1) preparing a titanium dioxide nanorod film on a substrate surface by a hydrothermal method and performing a first annealing; (2) growing copper oxide nanosheets on the titanium dioxide nanorod film after the first annealing, and performing a second annealing to obtain a copper oxide nanosheet / titanium dioxide nanorod composite structure layer; (3) preparing interdigital electrodes on the surface of the copper oxide nanosheet / titanium dioxide nanorod composite structure layer to obtain a highly selective carbon monoxide gas sensor.
2. The gas sensor according to claim 1, It is characterized in that The substrate is an FTO substrate; and the interdigital electrodes are platinum interdigital electrodes.
3. A method for preparing a gas sensor according to any one of claims 1 to 2, It is characterized in that The following steps are involved: (1) preparing a titanium dioxide nanorod film on a substrate surface by a hydrothermal method and performing a first annealing; (2) growing copper oxide nanosheets on the titanium dioxide nanorod film after the first annealing, and performing a second annealing to obtain a copper oxide nanosheet / titanium dioxide nanorod composite structure layer; (3) preparing interdigital electrodes on the surface of the copper oxide nanosheet / titanium dioxide nanorod composite structure layer to obtain a highly selective carbon monoxide gas sensor.
4. The preparation method according to claim 3, It is characterized in that The hydrothermal temperature of the hydrothermal method in step (1) is 120-180° C., and the hydrothermal time is 6-16 hours; the solvent used in the hydrothermal method is a mixed solvent of water and ethanol.
5. The preparation method according to claim 3 or 4, It is characterized in that The temperature of the first annealing is 300-500° C., the time is 20-60 minutes, and the annealing atmosphere is air.
6. The preparation method according to claim 3, It is characterized in that The method for growing copper oxide nanosheets in step (2) is a water bath method or a hydrothermal method; the water bath temperature of the water bath method is 60-90°C, and the water bath time is 0.5-6h; the hydrothermal temperature of the hydrothermal method is 150-180°C, and the hydrothermal time is 8-16h.
7. The preparation method according to claim 3 or 6, It is characterized in that The temperature of the second annealing is 100-400° C., the time is 60-120 min, and the annealing atmosphere is air.
8. Use of the highly selective carbon monoxide gas sensor according to any one of claims 1 to 2 in carbon monoxide testing; the operating temperature of the highly selective carbon monoxide gas sensor is room temperature.