A low temperature resistant elastic conductive paste and its preparation method and application

Through the composite system of thermoplastic elastomer and resin and curing agent, the elasticity and low-temperature resistance of flexible conductive paste are improved, and the stability of existing conductive paste in high and low temperature environments is solved, and the efficient application of conductive lines is achieved. .

CN115394473BActive Publication Date: 2024-11-22BEIJING DREAM INK TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211196332.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-29
Publication Date
2024-11-22
Estimated Expiration
2042-09-29

AI Technical Summary

Technical Problem

The existing flexible or stretchable conductive pastes have poor resilience and poor low-temperature resistance, making it difficult to maintain the stability and adhesion of conductive lines in high and low-temperature environments.

Method used

Using a composite system of thermoplastic elastomer and specific resins and curing agents, the combination method and ratio of resins can be adjusted to improve the elasticity and low temperature resistance of the conductive paste, and on this basis, conductive fillers and composite solvents are added to improve the conductivity. Sex and adhesion.

Benefits of technology

The conductive paste has achieved good rebound in high and low temperature environments, small resistance changes, and small resistance changes under 20% repeated stretching, which significantly improves the low temperature resistance of the conductive lines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003870807850000091
    Figure BDA0003870807850000091
Patent Text Reader

Abstract

The present invention relates to the field of new material technology, and in particular to a low-temperature resistant elastic conductive paste and a preparation method and application thereof. The conductive paste includes 1-10wt% of a curing agent and 4.5-13wt% of a composite resin; wherein the composite resin includes a first resin and a second resin in a mass ratio of (0.5-3): (4-10); the first resin is selected from one or more of polyester resin, polyurethane resin, epoxy resin, acrylic resin, phenolic resin, alkyd resin, silicone resin, chlorovinyl resin, and polyimide resin; the second resin is a thermoplastic elastomer. The present invention provides a low-temperature resistant elastic conductive paste, and the conductive circuit formed by the conductive paste has a small resistance change and excellent resilience under 20% repeated stretching, and the resistance change rate of the conductive circuit in the high and low temperature impact test is small.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new materials, and in particular to a low-temperature resistant elastic conductive slurry and a preparation method and application thereof. Background Art

[0002] In recent years, people in this field usually use conductive paste to form circuit patterns on substrates to obtain conductive circuits; while flexible printed circuits (FPCs) use flexible materials (such as polyethylene terephthalate PET, etc.) as substrates, and use flexible or stretchable conductive pastes to form circuit patterns on the above substrates. Flexible printed circuits have advantages that traditional rigid printed circuits do not have. They are a type of electronic device that can maintain normal functions during bending, folding, or even stretching deformation under external forces. Compared with traditional electronic products based on rigid printed circuit board technology, flexible printed circuits can be directly applied to three-dimensional free-form surface working environments, promote human-machine information fusion and interaction in the fields of biomedicine, leisure and entertainment, and meet the use requirements of portability, comfort, etc., which will greatly expand the application scope of current electronic products, and therefore have received widespread attention from academia and industry.

[0003] In the prior art, the existing flexible or stretchable conductive pastes generally have a certain degree of ductility. However, the conductive circuits formed by such conductive pastes have poor resilience and poor low-temperature resistance. How to solve the problems of poor resilience and poor low-temperature resistance of conductive pastes is a technical problem that technical personnel in this field urgently need to solve.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a conductive paste having the characteristics of good resilience and good low temperature resistance; another object of the present invention is to provide a preparation method and application of the conductive paste.

[0006] Specifically, the present invention provides the following technical solutions:

[0007] The present invention provides a conductive paste, which includes 1-10wt% of a curing agent and 4.5-13wt% of a composite resin;

[0008] Wherein, the composite resin comprises a first resin and a second resin in a mass ratio of (0.5-3):(4-10);

[0009] The first resin is selected from one or more of polyester resin, polyurethane resin, epoxy resin, acrylic resin, phenolic resin, alkyd resin, silicone resin, chloroacetic resin, and polyimide resin; the second resin is a thermoplastic elastomer.

[0010] The present invention aims to develop a low-temperature resistant elastic conductive paste, and has tried a large number of resin monomers and resin compounding methods. During the research and development process, it was found that, on the one hand, although a low-temperature resistant elastic conductive paste can be obtained by compounding with a variety of commonly used silicone resins in different combinations and different proportions, the conductivity of the silicone system conductive paste is not good, and its adhesion to the substrate after forming a conductive circuit is not good; on the other hand, although a low-temperature resistant elastic conductive paste can be obtained by compounding with a variety of commonly used rubber resins in different combinations and different proportions, the rubber system conductive paste is not resistant to high temperatures, and it is difficult to form a stable conductive circuit during actual application. Through a large number of experiments, it was found that by using a thermoplastic elastomer as the main body and supplemented with a first resin (selected from one or more of polyester resin, polyurethane resin, epoxy resin, acrylic resin, phenolic resin, alkyd resin, silicone resin, chloroacetic resin, and polyimide resin), the resulting composite resin improves the resilience of the conductive paste without affecting the conductivity and adhesion of the conductive paste, and the high temperature resistance of the conductive paste is maintained in an ideal state; in addition, further adding a certain amount of curing agent on the basis of the composite resin can significantly optimize the low temperature resistance of the conductive paste.

[0011] Further controlling the mass ratio of the first resin and the thermoplastic elastomer within the range of (0.5-3):(4-10), and controlling the proportions of the curing agent and the composite resin in the system within the range of 1-10wt% and 4.5-13wt%, respectively, can further improve the resilience and low temperature resistance of the conductive paste.

[0012] Those skilled in the art can arrange other functional components in the formula according to common knowledge, and they can all obtain the effects equivalent to the above description of the present invention. However, there are also better technical solutions for other components, and for this reason, the present invention further explores and obtains the following preferred solutions.

[0013] Preferably, the second resin is polyether TPU.

[0014] The present invention also finds that by using polyether TPU as the second resin, the resulting composite resin, after being compounded with a curing agent, has better resilience and low temperature resistance of the conductive paste.

[0015] Furthermore, in order to further optimize the compounding effect of the polyether TPU and the first resin, the present invention also provides a preparation method thereof, which is as follows:

[0016] Preferably, the preparation method of the polyether TPU comprises: using hard segment components and soft segment components as raw materials, and carrying out condensation reaction under the action of a chain extender;

[0017] Further, the hard segment component is a polyisocyanate, and the polyisocyanate is selected from one or more of MDI (diphenylmethane diisocyanate), HDI (hexamethylene diisocyanate), HMDI (4,4'-dicyclohexylmethane diisocyanate), IPDI (isophorone diisocyanate), and PAPI (polymethylene polyphenyl polyisocyanate); the soft segment component is selected from one or more of polyoxypropylene diol, polyoxypropylene triol, and polytetramethylene ether diol, and the molecular weight of the soft segment component is 400-4000; the chain extender is 1,4-butanediol;

[0018] In terms of molar ratio, hard segment component: soft segment component: chain extender = 0.5-1.5: 0.5-2: 0.1-1 (preferably 1.0-1.3: 0.9-1.2: 0.1-0.3).

[0019] In the present invention, when the above-mentioned polyether TPU is used, the effect is better.

[0020] Preferably, the curing agent is selected from one or more of isocyanate, phenolic resin and amine compounds; preferably, it is one or a combination of two of difunctional isocyanate and trifunctional isocyanate.

[0021] Preferably, the first resin is acrylic resin.

[0022] For the slurry system of the present invention, the curing agent and the first resin compatible therewith are as described above; when the above curing agent and the first resin are selected, it is more conducive to improving the resilience and low temperature resistance of the conductive slurry.

[0023] Preferably, the conductive paste further comprises 60-90wt% of a conductive filler;

[0024] The conductive filler is selected from one or more of gallium, indium, tin, zinc, bismuth, gold, silver, iron, nickel, aluminum, copper, graphene, and silver-coated copper powder.

[0025] Furthermore, the conductive filler is spherical silver powder.

[0026] Preferably, the conductive paste further comprises 6-35wt% of a composite solvent;

[0027] The composite solvent comprises a first solvent and a second solvent in a mass ratio of (1-10):(5-25);

[0028] The first solvent is selected from one or more of lipids, ethers, hydrocarbons, and alcohols; preferably, one or more of DEAC (diethylene glycol ethyl ether acetate), DBE (dibasic acid ester), and diethylene glycol ethyl ether;

[0029] The second solvent is selected from one or more of ketones, amides, and furans; preferably one or more of DMF (N,N-dimethylformamide), DMAC (N,N-dimethylacetamide), ISOP (isophorone), CYC (cyclohexanone), and NMP (N-methylpyrrolidone).

[0030] The present invention also finds that the use of the composite solvent is beneficial to improving the solubility of each component, thereby improving the uniformity of the conductive paste; the conductive paste has good stability during subsequent applications.

[0031] Preferably, the conductive paste further comprises 0.5-3wt% of an auxiliary agent;

[0032] The auxiliary agent is selected from one or more of a dispersant, a wetting agent, a coupling agent, a leveling agent, a thixotropic agent, and a accelerator;

[0033] Furthermore, the auxiliary agent includes BYK061, BYK368, KH550 and DBU (1,8-diazabicycloundec-7-ene) in a mass ratio of (0.1-0.75):(0.1-0.75):(0.1-0.75); the effect is better when the above auxiliary agent is selected.

[0034] Those skilled in the art can combine the above technical solutions according to common sense to obtain preferred embodiments of the conductive paste of the present invention.

[0035] As a preferred embodiment of the present invention, the conductive paste comprises the following components in percentage by mass:

[0036] Acrylic resin 0.5-3wt%, polyether TPU 4-10wt%, isocyanate 1-10wt%, spherical silver powder 60-90wt%, DEAC 1-10wt%, DMF 5-25wt%, additive 0.5-3wt%; wherein,

[0037] The auxiliary agent includes BYK061, BYK368, KH550 and DBU in a mass ratio of (0.1-0.75):(0.1-0.75):(0.1-0.75).

[0038] As a preferred embodiment, the conductive paste comprises the following components in parts by weight:

[0039] 0.5-3 parts of acrylic resin, 4-10 parts of polyether TPU, 1-10 parts of isocyanate, 60-90 parts of spherical silver powder, 1-10 parts of DEAC, 5-25 parts of DMF, and 0.5-3 parts of additives; wherein,

[0040] The auxiliary agent includes BYK061, BYK368, KH550 and DBU in a mass ratio of (0.1-0.75):(0.1-0.75):(0.1-0.75).

[0041] The present invention also provides a method for preparing the conductive paste mentioned above, comprising: mixing the components and then grinding.

[0042] Preferably, the preparation method comprises the following steps:

[0043] S1:

[0044] Evenly mixing the first resin, the first solvent and a portion of the second solvent to obtain a first premix;

[0045] uniformly mixing the second resin and the remaining portion of the second solvent to obtain a second premix;

[0046] S2:

[0047] The first premix, the second premix, the curing agent, the conductive filler and the auxiliary agent are mixed evenly and then ground.

[0048] The present invention also finds that the above-mentioned method for preparing the conductive paste can further ensure that the components are mixed evenly and that the product properties do not change differentially.

[0049] In a specific embodiment, grinding is performed using a triple roll mill.

[0050] The present invention also provides the use of the above-mentioned conductive paste in a circuit board, preferably in a flexible circuit board.

[0051] The present invention further provides an electronic device, comprising a substrate and a conductive circuit located on the substrate, wherein the conductive circuit is formed by printing the conductive paste described above and then heating and curing it.

[0052] Preferably, the printing method is pad printing, screen printing, electrostatic spinning or printing.

[0053] Preferably, the substrate is made of elastic material.

[0054] Based on the above scheme, the beneficial effects of the present invention are as follows:

[0055] The present invention provides a low-temperature resistant elastic conductive paste. A conductive circuit formed by the conductive paste has a small resistance change and excellent resilience under 20% repeated stretching. In addition, the resistance change rate of the conductive circuit in a high-temperature impact test is small. DETAILED DESCRIPTION

[0056] The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.

[0057] In order to facilitate the comparison, the preparation method of the polyether TPU mentioned in the following examples is as follows:

[0058] (1) pre-dehydrating polyoxypropylene glycol having a molecular weight of 2000;

[0059] (2) 86.2 parts by weight of dehydrated polyoxypropylene glycol was added to a dry three-necked flask, and then 13 parts by weight of MDI was added. After stirring evenly, the temperature was raised to 80-85° C., and samples were taken every 30 minutes to measure the mass fraction of NCO until the measured value remained substantially unchanged, and then the temperature was lowered to 60° C.; 0.8 parts by weight of melted 1,4-butanediol was added and mixed rapidly, and when the temperature rose to 80° C., stirring was stopped, vacuum degassing was carried out for 5 minutes, and aging was carried out at 110° C. for 10 hours to obtain the polyether TPU.

[0060] The additives mentioned in the following examples are composed of BYK061, BYK368, KH550 and DBU in equal weight ratios.

[0061] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.

[0062] Example 1

[0063] This embodiment provides a conductive paste, and its formula is as follows:

[0064] 3 parts by weight of acrylic resin, 4 parts by weight of polyether TPU, 1 part by weight of isocyanate, 65 parts by weight of spherical silver powder, 6 parts by weight of DEAC, 20 parts by weight of DMF, and 1 part by weight of an auxiliary agent.

[0065] This embodiment further provides a method for preparing the conductive paste, which is as follows:

[0066] (1) mixing acrylic resin, DEAC and part of DMF, and stirring for 72 hours under heating (90° C.) until the mixture is uniform, to obtain a first premix;

[0067] The polyether TPU and the remaining DMF were mixed, and stirred for 72 hours under heating (90° C.) until they were uniform, to obtain a second premix;

[0068] (2) The first premix, the second premix, isocyanate, spherical silver powder and additives are uniformly mixed and then ground to obtain the product.

[0069] Example 2

[0070] This embodiment provides a conductive paste, and its formula is as follows:

[0071] 2 parts by weight of acrylic resin, 8 parts by weight of polyether TPU, 1 part by weight of isocyanate, 60 parts by weight of spherical silver powder, 4 parts by weight of DEAC, 24 parts by weight of DMF, and 1 part by weight of an auxiliary agent.

[0072] The preparation method of the conductive paste provided in this embodiment is the same as that in embodiment 1.

[0073] Example 3

[0074] This embodiment provides a conductive paste, and its formula is as follows:

[0075] 1 part by weight of acrylic resin, 6 parts by weight of polyether TPU, 1 part by weight of isocyanate, 65 parts by weight of spherical silver powder, 6 parts by weight of DEAC, 20 parts by weight of DMF, and 1 part by weight of auxiliary agent.

[0076] The preparation method of the conductive paste provided in this embodiment is the same as that in embodiment 1.

[0077] Example 4

[0078] This embodiment provides a conductive paste, and its formula is as follows:

[0079] 0.5 parts by weight of acrylic resin, 9.5 parts by weight of polyether TPU, 1 part by weight of isocyanate, 60 parts by weight of spherical silver powder, 3 parts by weight of DEAC, 25 parts by weight of DMF, and 1 part by weight of an auxiliary agent.

[0080] The preparation method of the conductive paste provided in this embodiment is the same as that in embodiment 1.

[0081] Example 5

[0082] This embodiment provides a conductive paste, and its formula is as follows:

[0083] 2.5 parts by weight of acrylic resin, 6 parts by weight of polyether TPU, 1.5 parts by weight of isocyanate, 70 parts by weight of spherical silver powder, 8 parts by weight of DEAC, 20 parts by weight of DMF, and 1 part by weight of an auxiliary agent.

[0084] The preparation method of the conductive paste provided in this embodiment is the same as that in embodiment 1.

[0085] Comparative Example 1

[0086] This comparative example provides a conductive paste, which is different from Example 1 in that in the formula, the polyether TPU is replaced by polyester TPU.

[0087] Comparative Example 2

[0088] This comparative example provides a conductive paste, which is different from Example 1 in that, in the formula, the amount of acrylic resin used is 0.2 parts by weight, the amount of polyether TPU used is 3 parts by weight, and the amount of isocyanate used is 0.5 parts by weight.

[0089] Comparative Example 3

[0090] This comparative example provides a conductive paste, which differs from Example 1 in that the polyether TPU is replaced by German Huntsman 85AE in the formula.

[0091] Test Example 1

[0092] In this test example, the conductive pastes of the embodiment and the comparative example were respectively used to form conductive circuits on an elastic substrate, and then the performance of each conductive circuit of the same shape was tested, as follows:

[0093] 1. Stretch-resistance test method: Use a tensile gauge / universal testing machine to stretch each conductive circuit, and then use a multimeter / resistance meter to test the resistance of each conductive circuit in the stretched state, and finally calculate the square resistance;

[0094] 2. Temperature resistance test method: Each conductive circuit is tested by high and low temperature impact test; wherein, the conditions of the high and low temperature impact test are: ① high temperature condition: 125±3℃ for 15 minutes; ② low temperature condition: -40±3℃ for 15 minutes; ③ temperature conversion time: <5 minutes; ④ high and low temperature cycle times: 100 times; when the resistance change rate of each conductive circuit after the above test is ≤10%, it is considered good.

[0095] 3. The test results are shown in Table 1.

[0096] Table 1

[0097]

[0098] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A conductive paste, It is characterized in that It includes the following components in percentage by mass: Acrylic resin 0.5-3 wt%, polyether TPU 4-10 wt%, isocyanate 1-10 wt%, spherical silver powder 60-90 wt%, DEAC 1-10 wt%, DMF 5-25 wt%, additive 0.5-3 wt%; wherein, The additives include BYK061, BYK368, KH550 and DBU in a mass ratio of (0.1-0.75):(0.1-0.75):(0.1-0.75); The preparation method of the polyether TPU comprises: using a hard segment component and a soft segment component as raw materials, and carrying out a condensation reaction under the action of a chain extender; The hard segment component is a polyisocyanate, and the polyisocyanate is selected from one or more of MDI, HDI, HMDI, IPDI, and PAPI; the soft segment component is selected from one or more of polyoxypropylene glycol, polyoxypropylene triol, and polytetramethylene glycol, and the molecular weight of the soft segment component is 400-4000; the chain extender is 1,4-butanediol; In terms of molar ratio, hard segment component: soft segment component: chain extender = 0.5-1.5: 0.5-2: 0.1-1.

2. The method for preparing the conductive paste according to claim 1, It is characterized in that include: The components are mixed and then ground.

3. The preparation method according to claim 2, It is characterized in that The preparation method comprises the following steps: S1: Mixing acrylic resin, DEAC and part of DMF uniformly to obtain a first premix; The polyether TPU and the remaining DMF are mixed uniformly to obtain a second premix; S2: The first premix, the second premix, isocyanate, spherical silver powder and additives are mixed evenly and then ground.

4. Use of the conductive paste according to claim 1 in a circuit board.

5. Use of the conductive paste according to claim 1 in a flexible circuit board.

6. An electronic device comprising a substrate and a conductive circuit located on the substrate, It is characterized in that The conductive circuit is formed by printing the conductive paste according to claim 1 and heating and curing it.

7. The electronic device according to claim 6, It is characterized in that The printing method is pad printing, screen printing, electrostatic spinning or printing.

8. The electronic device according to claim 7, It is characterized in that The material of the substrate is elastic material.