Lewis base catalysts and methods thereof

By using a catalyst compound formed by coordinating a Lewis base tridentate ligand with a transition metal center, combined with an activator, the problem of controlling the molecular weight and melting point of polymers at high temperatures is solved, and efficient polymer production is achieved.

CN115427464BActive Publication Date: 2024-10-29EXXONMOBIL CHEMICAL PATENTS INC
View PDF 34 Cites 0 Cited by

Patent Information

Application Number
CN202180029278.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-02-11
Publication Date
2024-10-29
Estimated Expiration
2041-02-11

AI Technical Summary

Technical Problem

Existing technologies are difficult to produce polyolefins with high melting points and high molecular weights at high reactor temperatures, and catalyst activity is difficult to maintain at high temperatures, resulting in difficulty in controlling the mechanical properties and molecular weight of the polymer.

Method used

Catalyst compounds consisting of eight-membered and five-membered metal cyclic rings formed by coordination of Lewis base tridentate ligands and transition metal centers are used, combined with activators to form a stable catalyst system for polymerizing olefins at high temperatures.

Benefits of technology

It achieves the production of polymers with high melting point and high stereoregularity at high temperatures, and can control the molecular weight distribution of the polymer, thereby improving the activity of the catalyst and the polymerization rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003895265740000031
    Figure BDA0003895265740000031
  • Figure BDA0003895265740000141
    Figure BDA0003895265740000141
  • Figure BDA0003895265740000161
    Figure BDA0003895265740000161
Patent Text Reader

Abstract

The present disclosure relates to Lewis base catalysts. The catalysts, catalyst systems and methods of the present disclosure can provide high temperature ethylene polymerization, propylene polymerization or copolymerization. In at least one embodiment, the catalyst compound belongs to a family of compounds comprising amino-phenolate-heterocyclic ligands coordinated to a Group 4 transition metal. The tridentate ligand can include a central neutral heterocyclic donor group, an anionic phenolate donor and an anionic amino donor. In some embodiments, the present disclosure provides a catalyst system comprising an activator and a catalyst of the present disclosure. In some embodiments, the present disclosure provides a polymerization method comprising a) contacting one or more olefin monomers with a catalyst system, the catalyst system comprising: i) an activator and ii) a catalyst of the present disclosure.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Inventor: Georgy P. Goryunov, Mikhail I. Sharikov, Vladislav A. Popov, Dmitry V. Uborsky, Alexander Z. Voskoboynikov, John R. Hagadorn, Jo Ann M. Canich

[0002] CROSS-REFERENCE TO RELATED APPLICATIONS

[0003] This application claims the benefit of priority to U.S. Provisional Application No. 62 / 980,814, filed on February 24, 2020, the disclosure of which is incorporated herein by reference.

[0004] field

[0005] The present disclosure relates to Lewis base transition metal complexes, catalyst systems comprising Lewis base transition metal complexes, and polymerization processes for producing polyolefin polymers, such as polyethylene-based polymers and polypropylene-based polymers.

[0006] background

[0007] Olefin polymerization catalysts have many uses in industry and polyolefins are widely used commercially due to their robust physical properties. Therefore, there is interest in finding new catalyst systems that improve the market value of catalysts and allow the production of currently provided polymers and new polymers at high reactor temperatures with greater efficiency and higher catalyst productivity. Physical properties (such as transition temperature, viscosity, etc.) and mechanical properties (such as strength, stiffness and toughness) depend on the molecular weight of the polymer and vary according to application.

[0008] Polyolefins with high molecular weight, such as high molecular weight polyethylene (HMWPE) or ultra-high molecular weight polyethylene (UHMWPE), generally have valuable mechanical properties. However, it remains a challenge to develop highly active catalysts capable of operating at high reactor temperatures for the production of controlled molecular weight polyolefins.

[0009] In addition, the melting temperature (Tm) of a polymer indicates the crystallinity of the polymer. For example, a polymer with a high Tm value generally provides a harder and more thermally stable material compared to a polymer with a lower Tm value. Therefore, the mechanical properties of the polymer can be regulated by the Tm of the polymer. In semi-crystalline thermoplastic polymers, for example, a crystalline structure can contribute to the strength properties of the material formed by the polymer (for example, a crystalline material can be tough and hard, and may require high stress to be destroyed). In addition, the crystallinity improvement can lead to the improvement of, for example, density, stiffness, strength, toughness, specific gravity and elastic modulus. Crystallinity can also affect the optical properties of the material formed by the polymer, which can be important for optical fiber production. However, the examples of catalysts for realizing the production of polymers with high melting points and glass transition temperatures are limited. In addition, it is generally difficult to produce high melting point polymers, for example polypropylene, particularly to use non-metallocene catalysts.

[0010] In addition, the procatalyst (neutral unactivated complex) should be thermally stable at or above ambient temperature because they are often stored for weeks before use. The performance of a given catalyst is closely affected by reaction conditions such as monomer concentration and temperature. For example, solution methods that benefit from operation at temperatures above 100°C or 120°C are particularly challenging for catalyst development. At such high reactor temperatures, it is often difficult to maintain high catalyst activity, which decreases quite consistently with the increase in reactor temperature. For a wide range of desired polyolefin products, from high-density polyethylene (HDPE) to elastomers (e.g., thermoplastic elastomers (TPE), ethylene-propylene-diene (EPDM)), many different catalyst systems may be required because it is unlikely that a single catalyst will be able to address all the needs for producing these various polyolefin products. The stringent requirements required for the development and production of new polyolefin products make it a highly challenging endeavor to determine the appropriate catalyst for a given product and production method.

[0011] New and improved catalysts, catalyst systems and methods for the polymerization of olefins are needed to achieve polymer properties such as high melting points, high melting temperatures, while controlling the molecular weight of the polymer (e.g., high molecular weight). In addition, catalysts, catalyst systems and methods for the polymerization of olefins are needed to provide polymers with desired melting points based on easy adjustment of the chemical structure of the catalyst (e.g., non-metallocene catalysts).

[0012] References of interest include: American Chemical Society (ACS), "The Scientific & Technical Information Network" (STN TM) Registration Nos. 1821304-39-5 and 1241906-25-1, Japanese Patent JP2015 / 199919; U.S. Patent US 8,592,615; and Tole, T. et al. (2018) "Synthesis and Application of the Transition Metal Complexes of α-Pyridinyl Alcohols, α-Bipyridinyl Alcohols, α, α'-Pyridinyl Diols and α, α'-Bipyridinyl Diols in Homogeneous Catalysis," Molecules, Vol. 23, p. 60.

[0013] Overview

[0014] The present disclosure relates to catalyst compounds represented by formula (I):

[0015]

[0016] in:

[0017] M is a Group 3, 4, 5 or 6 metal;

[0018] A 1 and A 2 wherein each is independently selected from the group consisting of aryl, substituted aryl, heteroaryl, and substituted heteroaryl groups;

[0019] J comprises a heterocyclic Lewis base;

[0020] E 1 Selected from the group consisting of hydrocarbon, substituted hydrocarbon, silyl and substituted silyl, wherein J and E 1 optionally joined to form one or more hydrocarbyl rings, substituted hydrocarbyl rings, heterocyclic rings, or substituted heterocyclic rings;

[0021] Each L is independently a Lewis base;

[0022] Each X is independently an anionic ligand;

[0023] n is 1, 2, or 3;

[0024] m is 0, 1, or 2;

[0025] n+m is not greater than 4;

[0026] R 1 Select from the following: C1-C 40 Hydrocarbyl, substituted C1-C 40Hydrocarbyl groups, heteroatom-containing groups and substituted heteroatom-containing groups;

[0027] Any two L groups can be joined together to form a bidentate Lewis base;

[0028] The X group can be joined to the L group to form a monoanionic bidentate group; and

[0029] Any two X groups can be joined together to form a dianionic ligand group.

[0030] In at least one embodiment, the catalyst compound belongs to the family of compounds comprising an amino-phenolate-heterocyclic ligand coordinated to a transition metal of Group 4. The tridentate ligand comprises a central neutral heterocyclic donor group, an anionic phenolate donor, and an anionic amino donor.

[0031] In some embodiments, the present disclosure provides a catalyst system comprising an activator and a catalyst of the present disclosure.

[0032] In some embodiments, the present disclosure provides a polymerization process comprising a) contacting one or more olefin monomers with a catalyst system comprising: i) an activator and ii) a catalyst of the present disclosure.

[0033] In some embodiments, the present disclosure provides polyolefins formed by the catalyst systems and / or methods of the present disclosure.

[0034] In some embodiments, the present disclosure provides a method for producing an ethylene alpha-olefin copolymer, comprising reacting ethylene and (optionally) at least one C3-C 20 α-olefins are contacted with a catalyst system to polymerize ethylene and (optionally) at least one C3-C 20 α-Olefins.

[0035] In some embodiments, the present disclosure provides a process for producing a propylene alpha-olefin copolymer comprising reacting propylene and at least one ethylene and / or at least one C4-C4 copolymer in preferably at least one continuous stirred tank reactor or loop reactor. 20 The α-olefin is contacted with a catalyst system to polymerize propylene and (optionally) at least one ethylene and / or (optionally) C4-C 20 α-Olefins.

[0036] In at least one embodiment, the catalyst compound represented by formula (I) features one eight-membered and one five-membered metallocyclic ring. The eight-membered metallocyclic ring contains atoms from: a metal M, an oxygen atom (usually part of a group, such as a phenolate), an aryl or heteroaryl group A 1 Two atoms, aryl or heteroaryl A2 The five-membered metallocyclic ring contains atoms from: the metal M, nitrogen, and two atoms from the bridging Lewis base group E. 1 an atom from the bridging Lewis base group J.

[0037] In at least one embodiment, the catalyst compound represented by formula (I) features one eight-membered and one five-membered metallocyclic ring. The eight-membered metallocyclic ring contains atoms from: metal M, phenolate oxygen, aryl or heteroaryl group A 1 Two atoms, aryl or heteroaryl A 2 The five-membered metallocyclic ring contains atoms from: the metal M, nitrogen, and two atoms from the bridging Lewis base group E. 1 an atom from the bridging Lewis base group J.

[0038] Details

[0039] The present disclosure relates to novel catalyst compounds and methods for polymerizing olefins, including contacting the novel catalyst compounds with an activator and one or more monomers. The novel catalyst compounds include Lewis base tridentate ligands coordinated to transition metal centers to form eight-membered rings and five-membered rings, catalyst systems including such catalyst compounds and uses thereof. The catalyst compounds of the present disclosure may be compounds containing Group 4 transition metals with amino-phenolate-heterocyclic ligands and Lewis bases. In another class of embodiments, the present disclosure relates to a polymerization method for producing polyolefin polymers by a catalyst system, the catalyst system including one or more olefin polymerization catalysts, at least one activator and an optional carrier. The polyolefin polymer may be a polyethylene polymer or a polypropylene polymer.

[0040] Lewis base tridentate ligands are a class of tridentate ligands that can use heterocycles such as pyridine groups or benzimidazoles. These ligands coordinate to transition metals in a "tridentate" manner, meaning that the ligand forms three different bonds to the metal center. Amino-phenolate-heterocycle complexes are characterized, for example, in that the ligands bind in a tridentate manner to form eight-membered and five-membered metallocycle rings. This new aspect creates asymmetry on opposite sides of the metal center of the catalyst.

[0041] With ligands coordinated to the metal in this manner, the complex is believed to lack symmetry. Without being bound by theory, it has been found that when these complexes are used as catalyst compounds for the production of polyethylene and other polymers of C2 and higher alpha olefins, the lack of symmetry is beneficial to the production of poly(alpha olefins) because it enhances the ability of the catalyst to produce polymers of high stereoregularity. In addition, the specific structural features of having 5- and 8-membered rings can produce high catalyst activity at high reactor temperatures while maintaining the ability to adjust polymer properties such as increased molecular weight and narrow molecular weight distribution.

[0042] The inventors have discovered that pyridyl-amino groups, when used together with phenoxide groups, provide a new family of catalysts having improved performance in polymer synthesis.

[0043] The catalysts, catalyst systems and methods of the present disclosure can provide high temperature ethylene polymerization, propylene polymerization, ethylene alpha-olefin (e.g., ethylene-1-octene) copolymerization or propylene alpha-olefin copolymerization because the Lewis base catalyst, such as the amino-phenolate-heterocyclic Lewis base catalyst, is stable at high polymerization temperatures and has good activity at high polymerization temperatures. Stable catalysts with good activity can provide the formation of polymers with high melting points, high stereoregularity and the ability to prepare increased amounts of polymers in a given reactor compared to conventional catalysts because polymerization typically occurs at higher rates at higher temperatures. In addition, stable catalysts with good activity can also provide the formation of polymers with low to very low molecular weights compared to conventional catalysts because polymerization typically occurs at higher rates at higher temperatures.

[0044] For purposes of this disclosure, the numbering scheme for the periodic table groups as described in Chemical and Engineering News, Vol. 63(5), p. 27 (1985) is used. Thus, a "Group 4 metal" is an element from Group 4 of the periodic table such as Hf, Ti, or Zr. As used herein, unless otherwise specified, all abbreviations are used as described in the periodic table. For example, Pd refers to palladium, Cl refers to chlorine, Hf refers to hafnium, and Zr refers to zirconium.

[0045] The following abbreviations may be used herein: Me is methyl, Et is ethyl, iPr is isopropyl, Ph is phenyl, nBu is n-butyl, tBu is tert-butyl, MAO is methylaluminoxane, MOMCl is chloromethyl methyl ether, THF is tetrahydrofuran, PDI is the polydispersity index defined as the weight average molecular weight divided by the number average molecular weight, NMR is nuclear magnetic resonance, t is time, s is seconds, h is hours, psi is pounds per square inch, psig is pounds per square inch gauge, equiv is equivalent weight, and RPM is revolutions per minute.

[0046] The specification describes transition metal complexes. The term complex is used to describe molecules in which an auxiliary ligand is coordinated to a central transition metal atom. The ligand is bulky and stably attached to the transition metal, thereby maintaining its influence during the use of the catalyst, such as during polymerization. The ligand can be coordinated to the transition metal by covalent bonds and / or electron donation or intermediate bonds. Transition metal complexes are usually activated using an activator to exert their polymerization or oligomerization functions, without being bound by theory, and the activator is believed to produce cations as a result of removing anionic groups (commonly referred to as leaving groups) from the transition metal.

[0047] As used herein, "olefin polymerization catalyst(s)" refers to any catalyst, such as an organometallic complex or compound capable of coordination addition polymerization, in which successive monomers are added to a monomer chain at an organometallic active center.

[0048] The terms "substituent," "radical," "group," and "moiety" are used interchangeably.

[0049] "Conversion" is the amount of monomer converted to polymer product and is reported as mol% and is calculated based on polymer yield and the amount of monomer fed to the reactor.

[0050] "Catalyst activity" is a measure of the activity level of a catalyst and is reported as the mass of product polymer (P) produced per mole (or mmol) of transition metal catalyst (Cat) used (kgP / molCat or gP / mmolCat or kgP / mmolCat), and catalyst activity can also be expressed per unit time, such as per hour (hr), for example (kg P / mmolCat / h).

[0051] The term "heteroatom" refers to any Group 13-17 element, excluding carbon. Heteroatoms may include B, Si, Ge, Sn, N, P, As, O, S, Se, Te, F, Cl, Br, and I. The term "heteroatom-containing group" may include the aforementioned elements with attached hydrogen, such as BH, BH2, SiH2, OH, NH, NH2, etc. The term "substituted heteroatom-containing group" describes a heteroatom-containing group having one or more hydrogen atoms replaced by a hydrocarbyl or substituted hydrocarbyl group(s).

[0052] "Olefins" or "alkenes" are compounds of linear, branched or cyclic carbon and hydrogen having at least one double bond. For the purposes of this specification and the appended claims, when a polymer or copolymer is referred to as comprising an olefin, the olefin present in such a polymer or copolymer is the polymerized form of the olefin. For example, when a copolymer is said to have an "ethylene" content of 35% to 55% by weight, it is understood that the monomer (mer) units in the copolymer are derived from ethylene in the polymerization reaction, and the derived units are present at 35% to 55% by weight based on the weight of the copolymer. "Polymers" have two or more identical or different monomer units. "Homopolymers" are polymers having identical monomer units. "Copolymers" are polymers having two or more monomer units that are different from each other. "Terpolymers" are polymers having three monomer units that are different from each other. "Different" used to refer to monomer units means that the monomer units differ from each other by at least one atom or are isomerically different. Therefore, as used herein, the definition of copolymers includes terpolymers. An "ethylene polymer" or "ethylene copolymer" is a polymer or copolymer comprising at least 50 mol% ethylene-derived units, a "propylene polymer" or "propylene copolymer" is a polymer or copolymer comprising at least 50 mol% propylene-derived units, and so forth.

[0053] The term "α-olefin" refers to an olefin having a terminal carbon-carbon double bond in its structure ((R 1 R 2 )-C=CH2, where R 1 and R 2 can be independently hydrogen or any hydrocarbon group; for example, R 1 is hydrogen and R 2 is an alkyl group). A "linear alpha-olefin" is an alpha-olefin as defined in this paragraph wherein R 1 is hydrogen, and R 2 is hydrogen or a linear alkyl group.

[0054] For purposes of this disclosure, ethylene shall be considered an alpha-olefin.

[0055] As used herein, and unless otherwise specified, the term “C n " means a hydrocarbon (one or more) having n carbon atoms per molecule, where n is a positive integer. The term "hydrocarbon" means a class of compounds containing hydrogen bonded to carbon, and encompasses (i) saturated hydrocarbon compounds, (ii) unsaturated hydrocarbon compounds, and (iii) mixtures of hydrocarbon compounds (saturated and / or unsaturated), including mixtures of hydrocarbon compounds having different values ​​of n. Similarly, a "Cm-Cy" group or compound refers to a group or compound containing a total number of carbon atoms within the range my. Thus, C1-C 50An alkyl group refers to an alkyl group containing a total number of carbon atoms in the range of 1-50.

[0056] Unless otherwise indicated (e.g., the definition of "substituted hydrocarbyl," "substituted aryl," etc.), the term "substituted" means that at least one hydrogen atom has been replaced by at least one non-hydrogen group, such as a hydrocarbyl group, a heteroatom or a heteroatom-containing group, such as a halogen (e.g., Br, Cl, F, or I), or at least one functional group such as -NR*2, -OR*, -SeR*, -TeR*, -PR*2, -AsR*2, -SbR*2, -SR*, -BR*2, -SiR*3, -GeR*3, -SnR*3, -PbR*3, wherein each R* is independently a hydrocarbyl or a halogenated hydrocarbyl, and two or more R* may be joined together to form a substituted or unsubstituted fully saturated, partially unsaturated or aromatic cyclic or polycyclic ring structure, or wherein at least one heteroatom has been inserted into the hydrocarbyl ring.

[0057] The term "substituted hydrocarbyl" means a hydrocarbyl group in which at least one hydrogen atom of the hydrocarbyl group has been replaced by at least one heteroatom (e.g., a halogen, such as Br, Cl, F or I) or a heteroatom-containing group (e.g., a functional group, such as -NR*2, -OR*, -SeR*, -TeR*, -PR*2, -AsR*2, -SbR*2, -SR*, -BR*2, -SiR*3, -GeR*3, -SnR*3, -PbR*3, wherein each R* is independently a hydrocarbyl or a halogenated hydrocarbyl group, and two or more R* may be joined together to form a substituted or unsubstituted fully saturated, partially unsaturated or aromatic cyclic or polycyclic ring structure), or wherein at least one heteroatom is inserted into the hydrocarbyl ring.

[0058] The term "hydrocarbyl-substituted phenyl" means a phenyl group having 1, 2, 3, 4 or 5 hydrogen groups replaced by hydrocarbyl or substituted hydrocarbyl groups. In at least one embodiment, the "hydrocarbyl-substituted phenyl" group can be represented by the formula: Where R a , R b , R c , R d and R e Each of which can be independently selected from hydrogen, C1-C 40 Hydrocarbon or C1-C 40 Substituted hydrocarbon group, heteroatom or heteroatom-containing group (provided that R a , R b , R c , R d and R e At least one of them is not H), or R a , R b , R c, R d and R e Two or more of these can join together to form C4-C 62 Cyclic or polycyclic hydrocarbon ring structures, or combinations thereof.

[0059] For the purpose of this article, the notation The use of indicates attachment to another group.

[0060] The term "substituted aryl" means an aryl group having one or more hydrogen radicals replaced by a hydrocarbyl, substituted hydrocarbyl, heteroatom, or heteroatom-containing group.

[0061] The term "substituted phenyl" means a phenyl group having one or more hydrogen radicals replaced by a hydrocarbyl group, a substituted hydrocarbyl group, a heteroatom, or a heteroatom-containing group.

[0062] The term "substituted carbazole" means a carbazole group having one or more hydrogen groups replaced by a hydrocarbyl group, a substituted hydrocarbyl group, a heteroatom, or a heteroatom-containing group.

[0063] The term "substituted naphthyl" means a naphthyl group having one or more hydrogen groups replaced by a hydrocarbyl group, a substituted hydrocarbyl group, a heteroatom, or a heteroatom-containing group.

[0064] The term "substituted benzyl" means a benzyl group having one or more hydrogen groups replaced by a hydrocarbyl group, a substituted hydrocarbyl group, a heteroatom or a group containing a heteroatom. For example, the substituted benzyl group is represented by the formula: Where R a’ , R b’ , R c’ , R d’ and R e’ and Z are each independently selected from hydrogen, C1-C 40 Hydrocarbon or C1-C 40 Substituted hydrocarbon group, heteroatom or heteroatom-containing group (provided that R a’ , R b’ , R c’ , R d’ and R e’ and Z is not H), or R a’ , R b’ , R c’ , R d’ and R e’ Two or more of Z and C4 may be joined together to form C4-C 62 Cyclic or polycyclic ring structures, or combinations thereof.

[0065] The terms "alkoxy" and "alkoxide" refer to an alkyl or aryl group bonded to an oxygen atom, such as an alkyl ether or aryl ether group / residue attached to an oxygen atom and may include groups wherein the alkyl / aryl group is C1-C 10 The alkyl groups may be straight chain, branched or cyclic. The alkyl groups may be saturated or unsaturated. Examples of suitable alkoxy groups may include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, sec-butoxy, tert-butoxy, phenoxy. A substituted alkoxy group is a group in which at least one hydrogen atom of the alkoxy group has been replaced by at least one non-hydrogen group, such as a hydrocarbon group, a heteroatom or a group containing a heteroatom, such as a halogen (e.g., Br, Cl, F or I) or at least one functional group such as -NR*2, -OR*, -SeR*, -TeR*, -PR*2, -AsR*2, -SbR*2, -SR*, -BR*2, -SiR*3, -GeR*3, -SnR*3, -PbR*3, and each R* is independently a hydrocarbon group or a halogenated hydrocarbon group, and two or more R* may be joined together to form a substituted or unsubstituted fully saturated, partially unsaturated or aromatic cyclic or polycyclic ring structure, or wherein at least one heteroatom has been inserted into the hydrocarbon ring.

[0066] The term "alkenyl" means a straight, branched or cyclic hydrocarbon group having one or more double bonds. These alkenyl groups may be optionally substituted. Examples of suitable alkenyl groups may include vinyl, propenyl, allyl, 1,4-butadienyl, cyclopropenyl, cyclobutenyl, cyclopentenyl, cyclohexenyl, cyclooctenyl, including their substituted analogs.

[0067] The terms "alkyl group" and "alkyl" are used interchangeably in this disclosure. For the purposes of this disclosure, an "alkyl group" is defined as a C1-C 100Alkyl, which may be linear, branched or cyclic. Examples of such groups may include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, isopentyl, hexyl, octyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cyclooctyl, including substituted analogs thereof. A substituted alkyl group is a group in which at least one hydrogen atom of the alkyl group has been replaced by at least one non-hydrogen group, such as a hydrocarbon group, a heteroatom or a heteroatom-containing group, such as a halogen (e.g., Br, Cl, F or I) or at least one functional group such as -NR*2, -OR*, -SeR*, -TeR*, -PR*2, -AsR*2, -SbR*2, -SR*, -BR*2, -SiR*3, -GeR*3, -SnR*3 or -PbR*3, and each R* is independently a hydrocarbon group or a halogenated hydrocarbon group, and two or more R* may be joined together to form a substituted or unsubstituted fully saturated, partially unsaturated or aromatic cyclic or polycyclic ring structure, or in which at least one heteroatom has been inserted into the hydrocarbon ring.

[0068] The term "aryl" or "aryl group" means an aromatic ring such as phenyl. Similarly, heteroaryl means an aryl group in which a ring carbon atom (or two or three ring carbon atoms) has been replaced by a heteroatom or a substituted heteroatom such as NP, B, NH or NMe. "Substituted aryl groups" are aryl groups containing non-hydrogen non-carbon atoms such as 2-methyl-phenyl, xylyl and 4-bromo-xylyl. As used herein, the term "aromatic" also refers to pseudo-aromatic heterocycles, which are heterocyclic substituents having properties and structures similar to aromatic heterocyclic ligands (almost planar), but are not aromatic by definition. The term "silyl group" means a group containing silicon and optionally hydrogen and / or carbon. The silyl group may be saturated or unsaturated, linear or branched, cyclic or acyclic, aromatic or non-aromatic, and the silicon atom is in the cyclic / aromatic ring and / or in a side group. "Substituted silyl groups" are silyl groups containing non-hydrogen non-carbon atoms.

[0069] When isomers of a given alkyl, alkenyl, alkoxy or aryl group exist (e.g., n-butyl, isobutyl, sec-butyl and tert-butyl), reference to one member of the group (e.g., n-butyl) shall explicitly disclose the remaining isomers in the group (e.g., isobutyl, sec-butyl and tert-butyl). Likewise, reference to an alkyl, alkenyl, alkoxy or aryl group without specifying a particular isomer (e.g., butyl) explicitly discloses all isomers (e.g., n-butyl, isobutyl, sec-butyl and tert-butyl).

[0070] The term "ring atom" means an atom that is part of a cyclic ring structure. According to this definition, a benzyl group has six ring atoms and tetrahydrofuran has five ring atoms.

[0071] A heterocyclic ring is a ring having heteroatoms in the ring structure, in contrast to a heteroatom-substituted ring in which the hydrogen atoms on the ring are replaced by heteroatoms. For example, tetrahydrofuran is a heterocyclic ring and 4-N,N-dimethylamino-phenyl is a heteroatom-substituted ring. Other examples of heterocycles can include pyridine, imidazoles and thiazole. A substituted heterocyclic ring is a heterocyclic ring in which the hydrogen on the ring atoms is replaced by heteroatoms.

[0072] The terms "hydrocarbyl radical," "hydrocarbyl group," or "hydrocarbyl" are used interchangeably and are defined to mean a group consisting only of hydrogen and carbon atoms. For example, a hydrocarbyl radical may be C1-C 100 The term "group" refers to a group which may be linear, branched or cyclic and may be aromatic or non-aromatic when cyclic. Examples of such groups include, but are not limited to, alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, isopentyl, hexyl, octyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cyclooctyl and aryl groups such as phenyl, benzyl, naphthyl.

[0073] Unless otherwise indicated, as used herein, "low comonomer content" is defined as a polyolefin having less than 8 weight percent comonomer, based on the total weight of the polyolefin. As used herein, "high comonomer content" is defined as a polyolefin having greater than or equal to 8 weight percent comonomer, based on the total weight of the polyolefin.

[0074] As used herein, Mn is the number average molecular weight, Mw is the weight average molecular weight, and Mz is the z average molecular weight, wt% is the weight percent and mol% is the mole percent. Molecular weight distribution (MWD), also known as polydispersity index (PDI), is defined as Mw divided by Mn. Unless otherwise indicated, all molecular weight units (e.g., Mw, Mn, Mz) are g / mol.

[0075] Unless otherwise indicated, as used herein, "high molecular weight" is defined as a weight average molecular weight (Mw) value of 50,000 g / mol or greater. "Low molecular weight" is defined as a Mw value of less than 50,000 g / mol.

[0076] Unless otherwise indicated, all melting points (Tm) are differential scanning calorimetry (DSC) second melts.

[0077] "Catalyst system" is a combination of at least one catalyst compound, at least one or activators, optional co-activators, and optional support materials. The terms "catalyst compound", "catalyst complex", "transition metal complex", "transition metal compound", "procatalyst compound" and "procatalyst complex" can be used interchangeably. When "catalyst system" is used to describe such a pair before activation, it means the unactivated catalyst complex (procatalyst) together with the activator and optional co-activator. When it is used to describe such a pair after activation, it means the activated complex and the activator or other charge-balanced structural parts. The transition metal compound can be neutral (as in the procatalyst), or a charged species with a counter ion (as in the activated catalyst system). For the purposes of the present disclosure and the claims thereto, when the catalyst system is described as comprising a neutral stable form of a component, it will be fully understood by those of ordinary skill in the art that the ionic form of the component is a form that reacts with a monomer to produce a polymer. A polymerization catalyst system is a catalyst system that can polymerize monomers into polymers. In addition, the catalyst compounds and activators represented by the chemical formulas herein are intended to include both neutral and ionic forms of the catalyst compounds and activators.

[0078] In the description herein, the catalyst may be described as a catalyst, a catalyst precursor, a procatalyst compound, a catalyst compound, or a transition metal compound, and these terms may be used interchangeably.

[0079] "Anionic ligands" are negatively charged ligands that donate one or more pairs of electrons to a metal ion. "Lewis bases" are electrically neutral ligands that donate one or more pairs of electrons to a metal ion. Examples of Lewis bases can include ethyl ether, trimethylamine, pyridine, tetrahydrofuran, dimethyl sulfide, and triphenylphosphine. The term "heterocyclic Lewis base" refers to a Lewis base that is also a heterocyclic ring. Examples of heterocyclic Lewis bases can include pyridine, imidazole, thiazole, and furan. Amino-phenolate-heterocyclic Lewis base ligands are tridentate ligands that bind to a metal via two anionic donors (e.g., phenolate and amino) and a central neutral heterocyclic donor (e.g., a pyridine group).

[0080] Scavengers are compounds that can be added to promote polymerization by removing impurities. Some scavengers can also act as activators and can be referred to as co-activators. Co-activators (which are not scavengers) can also be used in conjunction with activators to form an active catalyst. In at least one embodiment, the co-activator can be premixed with the transition metal compound to form an alkylated transition metal compound.

[0081] Non-coordinating anions (NCA) are defined as meaning anions that are not coordinated with the catalyst metal cation or coordinated with the metal cation, but only weakly coordinated. The term NCA is also defined as including multi-component activators such as tetrakis (pentafluorophenyl) borate N, N-dimethylanilinium, which contain acidic cationic groups and non-coordinating anions. The term NCA is also defined as including neutral Lewis acids such as tris (pentafluorophenyl) boron, which can react with the catalyst to form an activated substance by taking away anionic groups. Lewis acids are defined as compounds or elements that can react with electron donors to form bonds. NCA coordination is weak enough so that Lewis bases such as olefin monomers can displace it from the catalyst center. Any metal or metalloid that can form a compatible weakly coordinated complex can be used or contained in the non-coordinating anion. Suitable metals include, but are not limited to, aluminum, gold and platinum. Suitable metalloids include, but are not limited to, boron, aluminum, phosphorus and silicon.

[0082] The term "continuous" means a system that operates without interruption or stopping. For example, a continuous process to produce a polymer would be one in which reactants are continuously introduced into one or more reactors and polymer product is continuously withdrawn.

[0083] Solution polymerization refers to a polymerization process in which the polymer is dissolved in a liquid polymerization medium (e.g., an inert solvent or monomer(s) or a blend thereof). Solution polymerization may be homogeneous. Homogeneous polymerization is a polymerization in which the polymer product is dissolved in the polymerization medium. Suitable systems may not be turbid, as described in Oliveira, JV et al. (2000) Ind. Eng. Chem. Res., Vol. 29, p. 4627.

[0084] Bulk polymerization refers to a polymerization process in which the monomers and / or comonomers being polymerized are used as solvents or diluents, with little or no use of inert solvents as solvents or diluents. A small portion of the inert solvent may be used as a carrier for the catalyst and scavenger. The bulk polymerization system contains less than 25% by weight of an inert solvent or diluent, such as less than 10% by weight, such as less than 1% by weight, such as 0% by weight.

[0085] Transition Metal Complexes

[0086] In at least one embodiment, the present disclosure is directed to novel catalyst compounds having a Lewis base tridentate ligand coordinated to a Group 3, 4, 5, or 6 transition metal center to form a five-membered metallacycle ring and an eight-membered metallacycle ring.

[0087] For example, the phenolate group is part of an eight-membered group that is joined to the metal center. For example, the phenolate group is phenylphenolate. Alternatively, the phenolate group is tert-butylphenolate. A neutral heterocyclic donor and an anion donor can each coordinate to the transition metal center. The neutral heterocyclic donor can be a pyridyl group, and the anion donor can be an amino and / or phenolate group. In some embodiments, the five-membered metal ring includes a pyridyl-amino moiety. For example, the pyridyl group is joined to the amino group by a methylene bridge. Alternatively, the pyridyl group is joined to the amino group by a methylene bridge substituted with 2-isopropylphenyl.

[0088] In some aspects of the present disclosure, the five-membered metal cyclic ring is characterized by a benzimidazole-amino group. For example, the neutral heterocyclic donor can be a benzimidazole, and the anion donor is an amino group and / or a phenolate group. For example, the phenolate group can be a phenylphenolate. For example, the phenolate group can be a tert-butylphenolate. This aspect further produces asymmetry from opposite sides of the catalyst, characterized by a five-membered metal cyclic ring comprising a benzimidazole-amino portion. Without being bound by theory, it is believed that the use of, for example, a benzimidazole group adjacent to the amino group enhances catalyst stability. Therefore, high temperature productivity during polymerization can be achieved. For example, the benzimidazole group is directly bonded to the amino nitrogen and there is no linking group such as a methylene bridge. In some polymerization processes, especially at high reactor temperatures, a linking group such as a methylene bridge can be a highly reactive region and is prone to degradation in some cases. Therefore, the inventors have found that the catalyst produced by the benzimidazole group is highly productive and less prone to degradation at high temperatures.

[0089] The catalyst compound of the present disclosure may be represented by formula (I):

[0090]

[0091] in:

[0092] M is a Group 3, 4, 5 or 6 metal;

[0093] A 1 and A 2 wherein each is independently selected from the group consisting of aryl, substituted aryl, heteroaryl, and substituted heteroaryl groups;

[0094] J comprises a heterocyclic Lewis base;

[0095] E 1 Selected from the group consisting of hydrocarbon, substituted hydrocarbon, silyl and substituted silyl, wherein J and E 1 optionally joined to form one or more hydrocarbyl rings, substituted hydrocarbyl rings, heterocyclic rings, or substituted heterocyclic rings;

[0096] Each L is independently a Lewis base;

[0097] Each X is independently an anionic ligand;

[0098] n is 1, 2, or 3;

[0099] m is 0, 1, or 2;

[0100] n+m is not greater than 4;

[0101] R 1 Select from the following: C1-C 40 Hydrocarbyl, substituted C1-C 40 Hydrocarbyl groups, heteroatom-containing groups and substituted heteroatom-containing groups;

[0102] Any two L groups can be joined together to form a bidentate Lewis base;

[0103] The X group can be joined to the L group to form a monoanionic bidentate group; and

[0104] Any two X groups can be joined together to form a dianionic ligand group.

[0105] In at least one embodiment, each L of the catalyst represented by formula (I) may be independently selected from the following: ether, amine, phosphine, thioether, ester, Et2O, MeOtBu, Et3N, PhNMe2, MePh2N, tetrahydrofuran and dimethyl sulfide. In at least one embodiment, m of the catalyst represented by formula (I) is 0. In at least one embodiment, each X of the catalyst represented by formula (I) may be independently selected from the following: methyl, benzyl, trimethylsilyl, neopentyl, ethyl, propyl, butyl, phenyl, hydrogen, chloro, fluoro, bromo, iodo, trifluoromethanesulfonate, dimethylamino, diethylamino, dipropylamino and diisopropylamino, such as chloro, such as methyl. In at least one embodiment, n of the catalyst represented by formula (I) is 2.

[0106] In some embodiments, E 1 Can be selected from C(R 8 )(R 9 ) and Si(R 8 )(R 9 ). 8 and R 9 Each of which can be independently selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 A hydrocarbon group, a heteroatom, a group containing a heteroatom, and a substituted group containing a heteroatom, or R 8 and R 9 Can be joined to form one or more C3-C 20An alkyl group, a hydrocarbyl ring, a substituted hydrocarbyl ring, a heterocyclic ring, or a substituted heterocyclic ring, each having 5, 6, 7, or 8 ring atoms, and wherein the substituents on the rings may join to form additional rings. 1 Can be C1-C 40 Hydrocarbon or substituted C1-C 40 In at least one embodiment, R 1 is selected from the group consisting of a tert-butylphenyl group, a di-tert-butylphenyl group, and a tri-tert-butylphenyl group. 1 Selected from the group consisting of methyl, ethyl, and all isomers of propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl and decyl.

[0107] In at least one embodiment, J of formula (I) can be represented by the following formula:

[0108]

[0109] Where R 2 , R 3 and R 4 Each of which is independently selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 Hydrocarbon groups, heteroatoms and groups containing heteroatoms, or R 2 and R 3 or R 3 and R 4 One or more pairs of R may join to form one or more hydrocarbyl rings, substituted hydrocarbyl rings, heterocyclic rings, or substituted heterocyclic rings, each having 5, 6, 7, or 8 ring atoms, and wherein the substituents on the rings may join to form additional rings. In at least one embodiment, R 2 , R 3 and R 4 Each of which is independently selected from hydrogen and C1-C 10 In at least one embodiment, R 2 , R 3 and R 4 wherein each is independently selected from the group consisting of hydrogen, methyl, ethyl, and all isomers of propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl and decyl.

[0110] In at least one embodiment, J and E of Formula (I) 1 are joined to form a ring represented by the formula:

[0111]

[0112] Where E 2 Selected from the following: O, S and N (R 10 ), where R5 , R 6 , R 7 and R 10 Each of which is independently selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 A hydrocarbon group, a heteroatom, a group containing a heteroatom, and a substituted group containing a heteroatom, or R 5 and R 6 or R 6 and R 7 One or more pairs of R may join to form one or more hydrocarbyl rings, substituted hydrocarbyl rings, heterocyclic rings, or substituted heterocyclic rings, each having 5, 6, 7, or 8 ring atoms, and wherein the substituents on the rings may join to form additional rings. In at least one embodiment, R 5 , R 6 , R 7 and R 10 Each of which is independently selected from hydrogen and C1-C 10 In at least one embodiment, R 5 , R 6 , R 7 and R 10 wherein each is independently selected from the group consisting of hydrogen, methyl, ethyl, and all isomers of propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl and decyl.

[0113] In at least one embodiment, E 2 Selected from the following: NH, C1-C 20 Alkyl-N and C4-C 20 Aryl-N. In at least one embodiment, E 2 It is C1-C 20 Alkyl-N, where C1-C 20 The alkyl group is selected from the group consisting of methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl. 2 It is C4-C 20 Aryl-N, where C4-C 20 The aryl group is selected from phenyl and substituted phenyl.

[0114] In at least one embodiment, J and E 1 are joined to form a ring represented by the formula:

[0115]

[0116] Where R 5 , R 6 , R 7 , R 10 and R 15Each of which is independently selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 A hydrocarbon group, a heteroatom and a heteroatom-containing group, and a substituted heteroatom-containing group, or R 5 and R 6 or R 6 and R 7 or R 7 and R 10 or R 10 and R 15 One or more pairs of R may join to form one or more hydrocarbyl rings, substituted hydrocarbyl rings, heterocyclic rings, or substituted heterocyclic rings, each having 5, 6, 7, or 8 ring atoms, and wherein the substituents on the rings may join to form additional rings. In at least one embodiment, R 5 , R 6 , R 7 , R 10 and R 15 Each of which is independently selected from the following: hydrogen, C1-C 40 Hydrocarbyl and substituted C1-C 40 In at least one embodiment, R 5 , R 6 , R 7 , R 10 and R 15 wherein each is independently selected from the group consisting of hydrogen, methyl, ethyl, and all isomers of propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl and decyl.

[0117] In at least one embodiment, A of formula (I) 1 is aryl or substituted aryl. For example, in some embodiments, A of formula (I) 1 It is phenyl or substituted phenyl.

[0118] In at least one embodiment, A of formula (I) 2 It is expressed by the following formula:

[0119]

[0120] Where R 11 , R 12 , R 13 and R 14 Each of which is independently selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 In at least one embodiment, R 11 , R 12 , R 13 and R 14Each of which is independently selected from hydrogen and C1-C 10 In at least one embodiment, R 11 , R 12 , R 13 and R 14 wherein each is independently selected from the group consisting of hydrogen, methyl, ethyl, and all isomers of propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl. 11 It is C1-C 20 In some embodiments, R 11 Can be C1-C 10 Alkyl such as tert-butyl or R 11 Can be substituted C1-C 10 Alternatively, R 11 It can be an aryl or substituted aryl such as a di-tert-butylphenyl group. In some embodiments, R 11 yes:

[0121]

[0122] In at least one embodiment, E of formula (I) 1 Can be C(R 8 )(R 9 ), where R 8 and R 9 is independently selected from hydrogen, alkyl, and substituted alkyl. 8 and R 9 is independently selected from the group consisting of hydrogen, methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl. 8 is hydrogen and R 9 is a tert-butylphenyl group. Alternatively, E 1 It can be CH2.

[0123] In at least one embodiment, M of formula (I) is a Group 4 transition metal such as titanium, hafnium, or zirconium. In some embodiments, M of formula (I) may be zirconium or hafnium.

[0124] In at least one embodiment, the catalyst compound of formula (I) is selected from the following:

[0125]

[0126]

[0127]

[0128] Method for preparing catalyst compound

[0129] The following is a general scheme for preparing the catalysts described herein and further illustrated in the Examples. As a representative example, Scheme 1 illustrates the amino-phenolate-heterocyclic Lewis base complex, the free ligand, and the key fragments of the free ligand. This type of catalyst compound can be synthesized as shown below, where the free ligand can be obtained by a plurality of reaction methods using coupling reactions to join the three fragments (i.e., the heterocyclic group, the aryl group, and the phenolate group) together.

[0130]

[0131]

[0132] As a representative example, Scheme 2 illustrates the general synthetic route of preparing the example amine phenol ligand for preparing the transition metal catalyst of the present disclosure. By way of example, compound A is prepared by the condensation of 2-bromo-6-pyridine carboxaldehyde with amine, followed by reduction with NaBH3(CN). In some embodiments, compound C can be prepared by the reaction of BuLi or Mg metal with 2-bromo-6-alkyl protected phenol. As used herein, the term "protected group" such as "protected phenol" refers to a functional group modified to obtain chemical selectivity in a subsequent chemical reaction such as in a multi-step reaction. As used herein, the term "protecting group" is a molecule that changes the functional group in the "protected group". For example, in Scheme 2, "P" is a protecting group such as methoxymethyl ether (MOM), tetrahydropyranyl (THP) and benzyl (Bn). In some embodiments, compound C can react with compound D such as 1-bromo-2-chlorobenzene to form compound E. In at least one embodiment, compound C can be reacted with compound D, such as 2-bromo-phenylboronic acid, in a Pd-catalyzed coupling (e.g., in a Suzuki reaction or a Negishi reaction) to form compound E. In some embodiments, compound E can be metallated by reaction with BuLi or Mg metal to form compound B. In some embodiments, compound A and compound B can be converted to aminophenol ligands via Pd-catalyzed coupling. The aminophenol ligand can be reacted with a transition metal reagent containing a basic anionic ligand to form a transition metal aminophenolate complex. For example, the Group 4 reagent can be selected from the following: MBn4, M(CH2SiMe3)4, MBn2Cl2(OEt2) n, M(NMe2)2Cl2(dme), M(NMe2)4, M(NEt2)4, and M is either Zr or Hf. In some embodiments, the Group 4 reagent is an in situ formed Group 4 alkyl prepared by reacting a Group 4 halide with a Grignard reagent, an organoaluminum reagent, or an organozinc reagent. In some embodiments, the aminophenol ligand can be deprotonated by reaction with a main group metal base (e.g., alkyl lithium, Grignard reagent) to form a dianionic aminophenolate ligand, which can then react with a transition metal halide such as ZrCl4 or HfCl4 to produce an aminophenolate transition metal complex.

[0133]

[0134] Activator

[0135] The terms "co-catalyst" and "activator" are used interchangeably herein and are compounds that can activate any of the catalyst compounds of the present disclosure by converting a neutral catalyst compound into a catalytically active catalyst compound cation.

[0136] In some embodiments, the catalyst system described herein may include a catalyst complex and an activator such as aluminoxane or a non-coordinating anion, and may be formed by combining the catalyst components described herein with an activator (including combining them with a carrier such as silica) in any manner known from the literature. The catalyst system may also be added to solution polymerization or bulk polymerization (in monomer) or produced in solution polymerization or bulk polymerization (in monomer). The catalyst system of the present disclosure may have one or more activators and one, two or more catalyst components. Non-limiting activators may include, for example, aluminoxanes, alkylaluminums, ionizing activators (which may be neutral or ionic) and conventional type cocatalysts. Suitable activators may include aluminoxane compounds, modified aluminoxane compounds, and ionizing anion precursor compounds, which capture reactive σ-bonded metal ligands, thereby making the metal compound a cation and providing non-coordinating or weakly coordinating anions such as non-coordinating anions that balance charge.

[0137] In at least one embodiment, the catalyst system includes an activator and a catalyst compound of formula (I).

[0138] Aluminoxane Activator

[0139] Aluminoxane activators are used as activators in the catalyst systems described herein. Aluminoxanes are generally a ”')-O-subunit oligomer compound, wherein R a"' is an alkyl group. Examples of aluminoxanes include methylaluminoxane (MAO), modified methylaluminoxane (MMAO), ethylaluminoxane and isobutylaluminoxane. Alkylaluminoxanes and modified alkylaluminoxanes are suitable for use as catalyst activators, especially when the abstractable ligand is an alkyl, halide, alkoxy or amino group. Mixtures of different aluminoxanes and modified aluminoxanes can also be used. It may be appropriate to use visually clear methylaluminoxane. The turbid or gelled aluminoxane can be filtered to produce a clear solution or the clear aluminoxane can be decanted from the turbid solution. A useful aluminoxane is modified methylaluminoxane (MMAO) cocatalyst type 3A (commercially available from Akzo Chemicals, Inc. under the trade name Modified Methylalumoxane Type 3A, covered in Patent No. US 5,041,584, which is incorporated herein by reference). Another useful aluminoxane is as described in US 9,340,630, US 8,404,880 and US Solid polymethylaluminoxanes are described in 8,975,209, which is incorporated herein by reference.

[0140] When the activator is an aluminoxane (modified or unmodified), at least one embodiment selects a maximum activator amount of up to 5,000 times molar excess Al / M relative to the catalyst compound (per metal catalytic site). The minimum activator to catalyst compound ratio may be a 1:1 molar ratio. Alternative ranges may include 1:1-500:1, alternatively 1:1-200:1, alternatively 1:1-100:1, or alternatively 1:1-50:1.

[0141] In alternative embodiments, little or no alumoxane is used in the polymerization methods described herein. For example, alumoxane may be present at zero mole %, alternatively alumoxane may be present at a molar ratio of aluminum to catalyst compound transition metal of less than 500:1, such as less than 300:1, such as less than 100:1, such as less than 1:1.

[0142] Ionizing / Non-coordinating Anion Activators

[0143] The term "non-coordinating anion" (NCA) means an anion that does not coordinate to a cation or only weakly coordinates to a cation, thereby remaining sufficiently unstable to be displaced by a Lewis base. "Compatible" non-coordinating anions are those that are not degraded to neutrality when the initially formed complex decomposes. In addition, the anion will not transfer anionic substituents or fragments to the cation so that it forms a neutral transition metal compound and neutral byproducts from the anion. Non-coordinating anions useful in accordance with the present disclosure are those that are compatible, stabilize the transition metal cation in the sense of balancing its ionic charge with +1, and also remain sufficiently unstable to allow displacement during the polymerization process. The ionizing activators useful herein typically comprise NCAs, particularly compatible NCAs.

[0144] It is within the scope of the present disclosure to use neutral or ionic ionizing activators. It is also within the scope of the present disclosure to use neutral or ionic activators alone or in combination with aluminoxane or modified aluminoxane activators. For descriptions of suitable activators, see US 8,658,556 and US 6,211,105.

[0145] The catalyst system of the present disclosure may include at least one non-coordinating anion (NCA) activator. In at least one embodiment, a boron-containing NCA activator represented by the following formula may be used:

[0146] Z d + (A d- )

[0147] wherein Z is (LH) or a reducible Lewis acid; L is a Lewis base; H is hydrogen; (L–H) is a Bronsted acid; A d- is a non-coordinating anion containing boron having a charge d-; d is 1, 2 or 3.

[0148] Cationic component Z d+ A Bronsted acid such as a proton or protonated Lewis base or a reducible Lewis acid can be included which is capable of protonating or abstracting a moiety such as an alkyl or aryl group from a bulky ligand transition metal catalyst precursor to produce a cationic transition metal species.

[0149] Activated cation Z d+ It can also be the following structural parts, such as silver, (tropillium), carbon Ferrocene and mixtures such as carbon and ferrocene Z d+ Can be triphenyl carbon The reducible Lewis acid may be a triarylcarbonyl (Wherein the aryl group may be substituted or unsubstituted, for example, by the formula: (Ar3C + ) wherein Ar is an aromatic group or is substituted by a heteroatom, C1-C 40 Hydrocarbon or substituted C1-C 40 Hydrocarbyl-substituted aryl groups, such as reducible Lewis acids "Z" may include those represented by the formula: (Ph3C) wherein Ph is a substituted or unsubstituted phenyl group, such as substituted by: C1-C 40 Hydrocarbon or substituted C1-C 40 Hydrocarbon, such as C1-C 20 Alkyl or aromatic compounds or substituted C1-C 20 Alkyl or aromatic compounds, for example, Z is triphenylcarbon

[0150] When Z d + Is the activated cation (L–H) d + When it is a Brønsted acid, it can donate protons to transition metal catalyst precursors to generate transition metal cations, including ammonium, oxygen Silane and mixtures thereof, for example methylamine, aniline, dimethylamine, diethylamine, N-methylaniline, diphenylamine, trimethylamine, triethylamine, N,N-dimethylaniline, methyldiphenylamine, pyridine, p-bromo-N,N-dimethylaniline, p-nitro-N,N-dimethylaniline, ammonium dioctadecylmethylamine, ammonium from triethylphosphine, triphenylphosphine and diphenylphosphine Oxygen from ethers such as dimethyl ether, diethyl ether, tetrahydrofuran and dioxane Sulfonium from sulfides such as diethyl sulfide, tetrahydrothiophene, and mixtures thereof.

[0151] Anionic component A d- Including having the formula [M k+ Q n ] d- Those wherein k is 1, 2 or 3; n is 1, 2, 3, 4, 5 or 6 (e.g., 1, 2, 3 or 4); nk = d; M is an element selected from Group 13 of the Periodic Table of Elements, such as boron or aluminum, and Q is independently a hydrogen group, a bridged or unbridged dialkylamino, a halo group, an alkoxy group, an aryloxy group, a hydrocarbyl group, a substituted hydrocarbyl group, a halohydrocarbyl group, a substituted halohydrocarbyl group, and a halogen-substituted hydrocarbyl group, wherein Q has up to 40 carbon atoms, provided that Q is a halo group in no more than 1 occurrence. Each Q may be a fluorinated hydrocarbyl group having 1 to 30 carbon atoms, for example, each Q is a fluorinated aryl group, and for example, each Q is a pentafluoroaryl group. Suitable A d-Examples also include diboron compounds as disclosed in US 5,447,895, which is fully incorporated herein by reference.

[0152] Illustrative but non-limiting examples of boron compounds that can be used as activating co-catalysts are the compounds described as (and particularly those specifically listed as) activators in US Pat. No. 8,658,556, which is incorporated herein by reference.

[0153] Ionic stoichiometric activator Z d+ (A d- ) may be one or more of the following: N,N-dimethylanilinium tetrakis(perfluorophenyl)borate, N,N-dimethylanilinium tetrakis(perfluoronaphthyl)borate, dioctadecylmethylammonium tetrakis(perfluorophenyl)borate, N,N-dimethylanilinium tetrakis(perfluorobiphenyl)borate, N,N-dimethylanilinium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate, triphenylcarbon tetrakis(perfluoronaphthyl)borate Tetrakis(perfluorobiphenyl) borate triphenylcarbon triphenylcarbon tetrakis(3,5-bis(trifluoromethyl)phenyl)borate or triphenylcarbon tetrakis(perfluorophenyl)borate

[0154] Bulk activators may also be used as NCAs herein. As used herein, "bulky activator" refers to an anionic activator represented by the formula:

[0155]

[0156] in:

[0157] Each R A are independently halo, such as fluoro;

[0158] Ar is a substituted or unsubstituted aryl group (eg, a substituted or unsubstituted phenyl group), for example, substituted with C1-C 40 Hydrocarbon groups such as C1-C 20 Alkyl or aromatic compounds.

[0159] Each R B are independently halogen, C6-C 20 A substituted aromatic hydrocarbon group or a substituted aromatic hydrocarbon group having the formula -O-Si-R D A silyloxy group, wherein R D It is C1-C 20 A hydrocarbyl or hydrocarbylsilyl group (eg, R B is a fluorine group or a perfluorinated phenyl group);

[0160] Each R C It is a halogen, C6-C 20A substituted aromatic hydrocarbon group or a substituted aromatic hydrocarbon group having the formula -O-Si-R D A silyloxy group, wherein R D It is C1-C 20 A hydrocarbyl or hydrocarbylsilyl group (eg, R D is a fluoro group or a C6 perfluoroaromatic hydrocarbon group); wherein R B and R C One or more saturated or unsaturated, substituted or unsubstituted rings (eg, R B and R C Forming a perfluorophenyl ring);

[0161] L is a Lewis base; (L–H) + is a Bronsted acid; d is 1, 2 or 3;

[0162] wherein the anion has a molecular weight greater than 1,020 g / mol; and

[0163] At least three of the substituents on the B atom each have a value greater than Optionally greater than or alternatively greater than The molecular volume of .

[0164] For example, (Ar3C) d + Can be (Ph3C) d + , wherein Ph is a substituted or unsubstituted phenyl group, for example substituted with C1-C 40 Hydrocarbon or substituted C1-C 40 Hydrocarbon, such as C1-C 20 Alkyl or aromatic compounds or substituted C1-C 20 Alkyl or aromatic compounds.

[0165] "Molecular volume" is used herein as an approximation of the spatial volume of an activator molecule in solution. Comparing substituents having different molecular volumes allows a substituent having a smaller molecular volume to be considered "less bulky" than a substituent having a larger molecular volume. Conversely, a substituent having a larger molecular volume can be considered "more bulky" than a substituent having a smaller molecular volume.

[0166] Molecular volume can be calculated as reported in "A Simple "Back of the Envelope" Method for Estimating the Densities and Molecular Volumes of Liquids and Solids", Journal of Chemical Education, Vol. 71(11), November 1994, pp. 962-964, which is incorporated herein by reference. The following formula is used to calculate the density of Molecular volume (MV): MV = 8.3V s , where V s is the scaled volume. s is the sum of the relative volumes of the constituent atoms and is calculated from the molecular formula of the substituent using the relative volumes in the table below. For fused rings, each fused ring V s Reduced by 7.5%.

[0167] element Relative volume H 1 The first short period, Li to F 2 Second short cycle, Na to Cl 4 The first long cycle, K to Br 5 The second longest period, Rb to I 7.5 The third longest period, Cs to Bi 9

[0168] A list of suitable bulky activators is found in US 8,658,556, which is incorporated herein by reference.

[0169] In another embodiment, one or more of the NCA activators are selected from the activators described in US 6,211,105.

[0170] In at least one embodiment, the activator is selected from one or more of the following: triarylcarbonyl (e.g. triphenylcarbon tetraphenylborate Triphenylcarbon tetrakis(pentafluorophenyl)borate Triphenylcarbon tetrakis(2,3,4,6-tetrafluorophenyl)borate Triphenylcarbon tetrakis(perfluoronaphthyl)borate Tetrakis(perfluorobiphenyl) borate triphenylcarbon triphenylcarbon tetrakis(3,5-bis(trifluoromethyl)phenyl)borate ).

[0171] In another embodiment, the activator is selected from one or more of the following: trialkylammonium tetrakis(pentafluorophenyl)borate, N,N-dialkylanilinium tetrakis(pentafluorophenyl)borate, dioctadecylmethylammonium tetrakis(pentafluorophenyl)borate, dioctadecylmethylammonium tetrakis(perfluoronaphthyl)borate, N,N-dimethyl-(2,4,6-trimethylanilinium tetrakis(pentafluorophenyl)borate, trialkylammonium tetrakis(2,3,4,6-tetrafluorophenyl)borate, N,N-dialkylanilinium tetrakis(2,3,4,6-tetrafluorophenyl)borate, trialkylammonium tetrakis(perfluoronaphthyl)borate ammonium tetrakis(perfluoronaphthyl)borate, trialkylammonium tetrakis(perfluorobiphenyl)borate, N,N-dialkylanilinium tetrakis(perfluorobiphenyl)borate, trialkylammonium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate, N,N-dialkylanilinium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate, N,N-dialkyl-(2,4,6-trimethylanilinium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate, di(isopropyl)ammonium tetrakis(pentafluorophenyl)borate, (wherein alkyl is methyl, ethyl, propyl, n-butyl, sec-butyl or tert-butyl).

[0172] Activators such as ammonium or The metallate or metalloid activator compound may comprise (1) ammonium or A group and a long chain aliphatic hydrocarbon group and (2) a metal acid group or a metalloid anion such as a borate or aluminate. When used in olefin polymerization with one or more catalyst compounds described herein, a polymer can be formed to have high comonomer incorporation, low molecular weight and / or a melting temperature of about 120° C. or greater. In some embodiments, the activator is soluble in an aliphatic solvent.

[0173] In some embodiments, the activator compound is represented by Formula (AI):

[0174] [R 1 R 2 R 3 EH] d + [M k+ Q n ] d- (AI)

[0175] in:

[0176] E is nitrogen or phosphorus, preferably nitrogen;

[0177] d is 1, 2 or 3 (preferably 3); k is 1, 2 or 3 (preferably 3); n is 1, 2, 3, 4, 5 or 6 (preferably 4, 5 or 6); nk = d (preferably d is 1, 2 or 3, k is 3, n is 4, 5 or 6, preferably when M is B, n is 4);

[0178] R1 , R 2 and R 3 wherein each is independently H, optionally substituted C1-C 40 Alkyl (e.g. branched or linear alkyl) or optionally substituted C5-C 50 -aryl (optionally R 1 , R 2 and R 3 Each of which is independently unsubstituted or substituted by at least one of the following: halogen, C5-C 50 Aryl, C6-C 35 Arylalkyl, C6-C 35 Alkaryl, and in C5-C 50 In the case of aromatic groups, C1-C 50 alkyl); wherein R 1 , R 2 and R 3 Contains 15 or more carbon atoms in total.

[0179] M is an element selected from Group 13 of the Periodic Table, preferably B or Al, preferably B; and

[0180] Each Q is independently selected from the group consisting of hydrogen, bridged or unbridged dialkylamino, halo, alkoxy, substituted alkoxy, aryloxy, substituted aryloxy, hydrocarbyl, substituted hydrocarbyl, halohydrocarbyl, substituted halohydrocarbyl, and halo-substituted hydrocarbyl groups, such as fluorinated aryl groups, such as fluoro-phenyl or fluoro-naphthyl, such as perfluorophenyl or perfluoronaphthyl.

[0181] In some embodiments of the activator compound represented by Formula (AI), R 1 , R 2 and R 3 At least one of them is a linear or branched C3-C 40 Alkyl (optionally linear or branched C7-C 40 alkyl).

[0182] In some embodiments, the activator compound can be represented by Formula (AII):

[0183] [R 1 R 2 R 3 EH] + [BR 4 R 5 R 6 R 7 ] - (AII)

[0184] in:

[0185] E is nitrogen or phosphorus, for example nitrogen;

[0186] R 1 , R 2 and R 3 Each of which is independently C1-C 40 Linear or branched alkyl or C5-C 50 -Aryl (e.g. C5-C 22 ), where R 1 , R 2 and R 3 Each of which is independently unsubstituted or substituted with halogen, C5-C 50 Aryl, C6-C 35 Arylalkyl, C6-C 35 At least one of the alkylaryl groups, and 50 In the case of aryl groups, there are C1-C 50 Alkyl; wherein R 1 , R 2 and R 3 Contains 15 or more carbon atoms in total (e.g. 18 or more carbon atoms, such as 20 or more carbon atoms, such as 22 or more carbon atoms, such as 25 or more carbon atoms, such as 30 or more carbon atoms, such as 35 or more carbon atoms, such as 40 or more carbon atoms); and

[0187] R 4 , R 5 , R 6 and R 7 Each of them is phenyl or naphthyl, wherein R 4 , R 5 , R 6 and R 7 At least one of them is substituted by 1 to 7 fluorine atoms.

[0188] In some embodiments, R 1 , R 2 and R 3 At least one of them is a linear or branched C3-C 40 Alkyl (e.g. linear or branched C7-C 40 alkyl).

[0189] The cationic component of the activators described herein (e.g., those of Formula (AI) and (AII) above) may be a protonated Lewis base that may be capable of protonating a moiety from a transition metal compound, such as an alkyl or aryl group. Thus, upon release of a neutral leaving group (e.g., an alkane produced by the combination of a proton provided by the cationic component of the activator and an alkyl substituent of the transition metal compound), a transition metal cation is produced that is a catalytically active species. In at least one embodiment of Formula (AI) or (AII), wherein the cation is [R1 R 2 R 3 EH] + , E is nitrogen or phosphorus, preferably nitrogen; R 1 , R 2 and R 3 Each of which is independently hydrogen, C1-C 40 Branched or linear alkyl or C5-C 50 -aryl, where R 1 , R 2 and R 3 Each of which is independently unsubstituted or substituted by at least one of the following: halo, C5-C 50 Aryl, C6-C 35 Arylalkyl, C6-C 35 Alkaryl, and in C5-C 50 In the case of aromatic groups, it is C1-C 50 Alkyl; wherein R 1 , R 2 and R 3 A total of 15 or more carbon atoms, for example 18 or more carbon atoms, for example 20 or more carbon atoms, for example 22 or more carbon atoms, for example 25 or more carbon atoms, for example 30 or more carbon atoms, for example 35 or more carbon atoms, for example 37 or more carbon atoms, for example 40 or more carbon atoms, for example 45 or more carbon atoms are contained.

[0190] The anionic component of the activator described above may include an anionic component of the formula [M k+ Q n ] wherein k is 1, 2 or 3; n is 1, 2, 3, 4, 5 or 6 (e.g., 1, 2, 3 or 4); M is an element selected from Group 13 of the Periodic Table, such as boron or aluminum, and Q is independently hydrogen, bridged or unbridged dialkylamino, halo, alkoxy, aryloxy, hydrocarbyl, substituted hydrocarbyl, halohydrocarbyl, substituted halohydrocarbyl, and halogen-substituted hydrocarbyl groups, said Q having up to 20 carbon atoms, provided that Q is halo in no more than 1 occurrence. In any embodiment of formula (I) or (AI), R 1 , R 2 and R 3 Each of which can be independently selected from:

[0191] 1) optionally substituted linear alkyl (e.g., methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, n-dodecyl, n-tridecyl, n-tetradecyl, n-pentadecyl, n-hexadecyl, n-heptadecyl, n-octadecyl, n-nonadecyl, n-icosyl, n-heneicosyl, n-docosyl, n-tricosyl, n-tetracosyl, n-pentacosyl, n-hexacosyl, n-heptacosyl, n-octacosyl, n-nonacosyl or n-triacontyl);

[0192] 2) optionally substituted branched alkyl groups (e.g., alkyl-butyl, alkyl-pentyl, alkyl-hexyl, alkyl-heptyl, alkyl-octyl, alkyl-nonyl, alkyl-decyl, alkyl-undecyl, alkyl-dodecyl, alkyl-tridecyl, alkyl-tetradecyl, alkyl-pentadecyl, alkyl-hexadecyl, alkyl-heptadecyl, alkyl-octadecyl, alkyl-nonadecyl, alkyl-eicosyl (including polyalkyl analogs, i.e., dialkyl-butyl, dialkyl-pentyl, dialkyl-hexyl, dialkyl-heptyl, dialkyl-octyl, dialkyl-nonyl, dialkyl-decyl, dialkyl-undecyl, dialkyl-dodecyl, dialkyl-tridecyl, di ... trialkyl-octyl, trialkyl-nonadecyl, trialkyl-eicosyl, trialkyl-butyl, trialkyl-pentyl, trialkyl-hexyl, trialkyl-heptyl, trialkyl-octyl, trialkyl-nonyl, trialkyl-decyl, trialkyl-undecyl, trialkyl-dodecyl, trialkyl-tridecyl, trialkyl-tetradecyl, trialkyl-pentadecyl, trialkyl-hexadecyl, trialkyl-heptadecyl, trialkyl-octadecyl, trialkyl-nonadecyl, and trialkyl-eicosyl, and the like), and isomers thereof, wherein each alkyl group is independently C1-C 40 (or C2-C 30 , or C3-C 20 ) linear, branched or cyclic alkyl groups), preferably the alkyl group is methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, heneicosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, nonacosyl or triacontyl);

[0193] 3) optionally substituted aralkyl groups, for example (methylphenyl, ethylphenyl, propylphenyl, butylphenyl, pentylphenyl, hexylphenyl, heptylphenyl, octylphenyl, nonylphenyl, decylphenyl, undecylphenyl, dodecylphenyl, tridecylphenyl, tetradecylphenyl, pentadecylphenyl, hexadecylphenyl, heptadecylphenyl, octadecylphenyl, nonadecylphenyl, eicosylphenyl, heneicosylphenyl, docosylphenyl, tricosylphenyl, tetracosylphenyl, pentacosylphenyl, hexacosylphenyl, heptacosylphenyl, octacosylphenyl, nonacosylphenyl, triacontylphenyl, 3,5,5-trimethylhexylphenyl, dioctylphenyl, 3,3,5-trimethylhexylphenyl, 2,2,3,3,4-pentamethylpentylphenyl, etc.);

[0194] 4) optionally substituted silyl, such as trialkylsilyl, wherein each alkyl group is independently an optionally substituted C1-C 20 Alkyl (e.g., trimethylsilyl, triethylsilyl, tripropylsilyl, tributylsilyl, trihexylsilyl, triheptylsilyl, trioctylsilyl, trinonylsilyl, tridecylsilyl, tri-undecylsilyl, tri-dodecylsilyl, tri-tridecylsilyl, tri-tetradecylsilyl, tri-pentadecylsilyl, tri-hexadecylsilyl, tri-heptadecylsilyl, tri-octadecylsilyl, tri-nonadecylsilyl, tri-eicosylsilyl);

[0195] 5) optionally substituted alkoxy (e.g., -OR*, wherein R* is an optionally substituted C1-C 20 Alkyl or aryl (e.g., methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, phenyl, alkylphenyl (e.g., methylphenyl, propylphenyl, etc.), naphthyl or anthracenyl);

[0196] 6) halogen (such as Br or Cl); and

[0197] 7) Halogen-containing groups (eg bromomethyl, bromophenyl, etc.).

[0198] In any embodiment of Formula (I) or (AI), R 1 It's methyl.

[0199] In any embodiment of Formula (I) or (AI), R 2 is unsubstituted phenyl or substituted phenyl. In at least one embodiment, R 2is phenyl, methylphenyl, n-butylphenyl, n-octadecylphenyl or isomers thereof, preferably R 2 It is meta- or para-substituted phenyl, for example meta- or para-substituted alkyl-substituted phenyl.

[0200] In any embodiment of Formula (I) or (AI), R 3 is a linear or branched alkyl group such as methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, n-dodecyl, n-tridecyl, n-tetradecyl, n-pentadecyl, n-hexadecyl, n-heptadecyl, n-octadecyl, n-nonadecyl, n-eicosyl, n-heneicosyl, n-docosyl, n-tricosyl, n-tetracosyl, n-pentacosyl, n-hexacosyl, n-heptacosyl, n-octacosyl, n-nonacosyl, n-triacontyl, isopropyl, isobutyl, isopentyl, isohexyl , isoheptyl, isooctyl, isononyl, isodecyl, isoundecyl, isododecyl, isotridecyl, isotetradecyl, isopentadecyl, isohexadecyl, isohexadecyl, isoheptadecyl, isooctadecyl, isononadecyl, isoeicosyl, isoheneicosyl, isodocosyl, isotricosyl, isotetracosyl, isopentacosyl, isohexacosyl, isoheptacosyl, isooctacosyl, isononacosyl or isotriacontyl, alkyl-butyl, alkyl-pentyl, alkyl-hexyl, alkyl-heptyl, alkyl-octyl, alkyl-nonyl, alkyl-decyl, alkyl-undecyl alkyl-dodecyl, alkyl-tridecyl, alkyl-tetradecyl, alkyl-pentadecyl, alkyl-hexadecyl, alkyl-heptadecyl, alkyl-octadecyl, alkyl-nonadecyl, alkyl-eicosyl (including polyalkyl analogs, i.e., dialkyl-butyl, dialkyl-pentyl, dialkyl-hexyl, dialkyl-heptyl, dialkyl-octyl, dialkyl-nonyl, dialkyl-decyl, dialkyl-undecyl, dialkyl-dodecyl, dialkyl-tridecyl, dialkyl-tetradecyl, dialkyl-pentadecyl, dialkyl-hexadecyl, dialkyl-heptadecyl, trialkyl-octadecyl, trialkyl-nonadecyl, trialkyl-eicosyl, trialkyl-butyl, trialkyl-pentyl, trialkyl-hexyl, trialkyl-heptyl, trialkyl-octyl, trialkyl-nonyl, trialkyl-decyl, trialkyl-undecyl, trialkyl-dodecyl, trialkyl-tridecyl, trialkyl-tetradecyl, trialkyl-pentadecyl, trialkyl-hexadecyl, trialkyl-heptadecyl, trialkyl-octadecyl, trialkyl-nonadecyl and trialkyl-eicosyl, etc.), and isomers thereof, wherein each alkyl group is independently C1-C 40 (or C2-C 30 , or C3-C 20) linear, branched or cyclic alkyl groups), preferably the alkyl group is methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, heneicosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, nonacosyl or triacontyl). Cationic components useful in formula (AI) or (I) include those represented by the following formula:

[0201]

[0202]

[0203] Cationic components useful in formula (AI) or (I) include those represented by the following formula:

[0204]

[0205] Activator compounds may include one or more of the following:

[0206] [Tetra(perfluorophenyl)borate] N,N-di(hydrogenated tallow)methylammonium,

[0207] [Tetrakis(perfluorophenyl)boric acid] N-methyl-4-nonadecylated-N-octadecylanilinium,

[0208] [Tetrakis(perfluorophenyl)boric acid] N-methyl-4-hexadecyl-N-octadecylanilinium,

[0209] [Tetrakis(perfluorophenyl)boric acid] N-methyl-4-tetradecyl-N-octadecylanilinium,

[0210] [Tetrakis(perfluorophenyl)boric acid] N-methyl-4-dodecyl-N-octadecylanilinium,

[0211] [Tetrakis(perfluorophenyl)boric acid] N-methyl-4-decyl-N-octadecylanilinium,

[0212] [Tetrakis(perfluorophenyl)boric acid] N-methyl-4-octyl-N-octadecylanilinium,

[0213] [Tetrakis(perfluorophenyl)boric acid] N-methyl-4-hexyl-N-octadecylanilinium,

[0214] [Tetrakis(perfluorophenyl)boric acid] N-methyl-4-butyl-N-octadecylanilinium,

[0215] [Tetrakis(perfluorophenyl)boric acid] N-methyl-4-octadecyl-N-decylanilinium,

[0216] [Tetrakis(perfluorophenyl)boric acid] N-methyl-4-nonadecylammonium-N-dodecylanilinium,

[0217] [Tetrakis(perfluorophenyl)boric acid] N-methyl-4-nonadecylammonium-N-tetradecylanilinium,

[0218] [Tetrakis(perfluorophenyl)boric acid] N-methyl-4-nonadecylated-N-hexadecylanilinium,

[0219] [Tetrakis(perfluorophenyl)boric acid] N-ethyl-4-nonadecylated-N-octadecylanilinium,

[0220] [Tetrakis(perfluorophenyl)borate]N-methyl-N,N-dioctadecylammonium,

[0221] [Tetrakis(perfluorophenyl)borate] N-methyl-N,N-dihexadecyl ammonium,

[0222] [Tetrakis(perfluorophenyl)borate] N-methyl-N,N-di(tetradecyl)ammonium,

[0223] [Tetrakis(perfluorophenyl)borate] N-methyl-N,N-didodecylammonium,

[0224] [Tetrakis(perfluorophenyl)borate] N-methyl-N,N-didecylammonium,

[0225] [Tetrakis(perfluorophenyl)borate] N-methyl-N,N-dioctylammonium,

[0226] [Tetrakis(perfluorophenyl)borate] N-ethyl-N,N-dioctadecylammonium,

[0227] [Tetrakis(perfluorophenyl)borate] N,N-dioctadecyltolylammonium,

[0228] [Tetrakis(perfluorophenyl)borate] N,N-di(hexadecyl)tolylammonium,

[0229] [Tetrakis(perfluorophenyl)borate] N,N-di(tetradecyl)tolylammonium,

[0230] [Tetrakis(perfluorophenyl)borate] N,N-di(dodecyl)tolylammonium,

[0231] [Tetrakis(perfluorophenyl)borate] N-octadecyl-N-hexadecyl-tolyl ammonium,

[0232] [Tetrakis(perfluorophenyl)borate] N-octadecyl-N-hexadecyl-tolyl ammonium,

[0233] [Tetrakis(perfluorophenyl)borate] N-octadecyl-N-tetradecyl-tolylammonium,

[0234] [Tetrakis(perfluorophenyl)borate] N-octadecyl-N-dodecyl-tolyl ammonium,

[0235] [Tetrakis(perfluorophenyl)borate] N-octadecyl-N-decyl-tolyl ammonium,

[0236] [Tetrakis(perfluorophenyl)borate] N-hexadecyl-N-tetradecyl-tolylammonium,

[0237] [Tetrakis(perfluorophenyl)borate] N-hexadecyl-N-dodecyl-tolyl ammonium,

[0238] [Tetrakis(perfluorophenyl)borate] N-hexadecyl-N-decyl-tolyl ammonium,

[0239] [Tetrakis(perfluorophenyl)borate] N-tetradecyl-N-dodecyl-tolyl ammonium,

[0240] [Tetrakis(perfluorophenyl)borate] N-tetradecyl-N-decyl-tolyl ammonium,

[0241] [Tetrakis(perfluorophenyl)borate] N-dodecyl-N-decyl-tolyl ammonium,

[0242] [Tetrakis(perfluorophenyl)borate] N-methyl-N-octadecylanilinium,

[0243] [Tetrakis(perfluorophenyl)borate] N-methyl-N-hexadecylanilinium,

[0244] [Tetrakis(perfluorophenyl)borate] N-methyl-N-tetradecylanilinium,

[0245] [Tetrakis(perfluorophenyl)borate] N-methyl-N-dodecylanilinium,

[0246] [Tetrakis(perfluorophenyl)borate] N-methyl-N-decylanilinium

[0247] [Tetrakis(perfluorophenyl)borate] N-methyl-N-octylanilammonium.

[0248] Suitable activator to catalyst ratios, such as all NCA activators to catalyst ratios, can be about 1:1 molar ratios. Alternative ranges include 0.1:1-100:1, alternatively 0.5:1-200:1, alternatively 1:1-500:1, alternatively 1:1-1000:1. Particularly useful ranges are 0.5:1-10:1, such as 1:1 to 5:1.

[0249] It is also within the scope of the present disclosure that the catalyst compound may be combined with a combination of alumoxane and NCA (see, for example, US 5,153,157, US 5,453,410, EP 0 573 120 Bl, WO 1994 / 07928 and WO 1995 / 014044 which discuss the use of alumoxanes in combination with ionizing activators).

[0250] Useful chain transfer agents may be hydrogen, alkylaluminoxanes, compounds represented by the formula AlR3, ZnR2 (wherein each R is independently a C1-C8 aliphatic group, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl or isomers thereof), or combinations thereof, such as diethylzinc, methylaluminoxane, trimethylaluminum, triisobutylaluminum, trioctylaluminum, or combinations thereof.

[0251] Additionally, the catalyst system of the present disclosure may include a metal hydrocarbenyl chain transfer agent represented by the formula:

[0252] Al(R') 3-v (R”) v

[0253] Each R' can be independently C1-C 30 The hydrocarbon group and / or each R" may independently be a C4-C 20 a hydrocarbenyl group; and v may be 0.1-3.

[0254] Optional scavenger or co-activator

[0255] In addition to these activator compounds, scavengers or co-activators may be used. Alkyl aluminum or aluminoxane compounds that may be used as scavengers or co-activators may include, for example, trimethyl aluminum, triethyl aluminum, triisobutyl aluminum, tri-n-hexylaluminum, tri-n-octylaluminum, diisobutyl aluminum hydride, and diethyl zinc.

[0256] Chain transfer agents can be used in the methods and / or compositions described herein. Useful chain transfer agents are typically alkylaluminoxanes, compounds represented by the formula AlR3, ZnR2 (wherein each R is independently a C1-C8 aliphatic group, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl or isomers thereof) or combinations thereof, such as diethylzinc, methylaluminoxane, trimethylaluminum, triisobutylaluminum, trioctylaluminum or combinations thereof.

[0257] Optional carrier material

[0258] In embodiments herein, the catalyst system may include an inert support material. The support material may be a porous support material such as talc and an inorganic oxide. Other support materials include zeolites, clays, organoclays or other organic or inorganic support materials, or mixtures thereof.

[0259] The support material may be an inorganic oxide in a subdivided form. Suitable inorganic oxide materials for use in the catalyst system herein may include metal oxides of Groups 2, 4, 13 and 14 such as silica, alumina and mixtures thereof. Other inorganic oxides that may be used alone or in combination with silica or alumina may be magnesium oxide, titanium dioxide, zirconium oxide. However, other suitable support materials may be used, such as subdivided functionalized polyolefins such as subdivided polyethylene. Examples of suitable supports may include magnesium oxide, titanium dioxide, zirconium oxide, montmorillonite, phyllosilicates, zeolites, talc, clay. In addition, combinations of these support materials may be used, such as silica-chromium, silica-alumina, silica-titania. In at least one embodiment, the support material is selected from Al2O3, ZrO2, SiO2, SiO2 / Al2O3, SiO2 / TiO2, silica clay, silica / clay or mixtures thereof.

[0260] Support materials such as inorganic oxides may have a surface area of ​​about 10 m 2 / g-about 700m 2 / g, the pore volume is about 0.1cm 3 / g-about 4.0cm 3 / g, and the average particle size is in the range of about 5 μm to about 500 μm. The surface area of ​​the support material can be about 50 m 2 / g-about 500m 2 / g, the pore volume is about 0.5cm 3 / g-about 3.5cm 3 / g, and an average particle size of about 10 μm to about 200 μm. For example, the surface area of ​​the support material is about 100 m 2 / g-about 400m 2 / g, the pore volume is about 0.8cm 3 / g-about 3.0cm 3 / g, and an average particle size of about 5 μm to about 100 μm. The average pore size of the support material useful in the present disclosure is For example to about and for example to about In at least one embodiment, the support material is a high surface area amorphous silica (surface area = 300 m 2 / gm, pore volume is 1.65cm 3 / gm). For example, suitable silica can be obtained from Davison Chemical Division of WR Graze and Company under the trade name DAVISON TM 952 or DAVISON TM 955. In other embodiments, DAVISON TM 948. Alternatively, the silica may be, for example, ES-70 calcined (e.g., at 875°C). TM Silica (PQ Corporation, Malvern, PA).

[0261] The support material should be dry, i.e., free of absorbed water. Drying of the support material can be achieved by heating or calcining at about 100°C to about 1,000°C, for example, at least about 600°C. When the support material is silica, it is heated to at least 200°C, for example, about 200°C to about 850°C, and for example at about 600°C; and for a period of about 1 minute to about 100 hours, about 12 hours to about 72 hours, or about 24 hours to about 60 hours. The calcined support material must have at least some reactive hydroxyl (OH) groups to produce the supported catalyst system of the present disclosure. The calcined support material is then contacted with at least one polymerization catalyst comprising at least one catalyst compound and an activator.

[0262] The support material with reactive surface groups (e.g., hydroxyl groups) is slurried in a nonpolar solvent and the resulting slurry is contacted with a solution of a catalyst compound and an activator. In at least one embodiment, the slurry of the support material is first contacted with the activator for a period of about 0.5 hours to about 24 hours, about 2 hours to about 16 hours, or about 4 hours to about 8 hours. The solution of the catalyst compound is then contacted with the separated support / activator. In at least one embodiment, the catalyst system of the original position generation load. In an alternative embodiment, the slurry of the support material is first contacted with the catalyst compound for a period of about 0.5 hours to about 24 hours, about 2 hours to about 16 hours, or about 4 hours to about 8 hours. The slurry of the catalyst compound of the load is then contacted with an activator solution.

[0263] The mixture of catalyst, activator and support is heated from about 0° C. to about 70° C., for example from about 23° C. to about 60° C., for example at room temperature. The contact time can be from about 0.5 hours to about 24 hours, for example from about 2 hours to about 16 hours or from about 4 hours to about 8 hours.

[0264] Suitable non-polar solvents are materials in which all of the reactants used herein (e.g., activators and catalyst compounds) are at least partially soluble and are liquid at the reaction temperature. The non-polar solvent can be an alkane such as isopentane, hexane, n-heptane, octane, nonane, and decane, but various other materials can also be used, including cycloalkanes such as cyclohexane, aromatic compounds such as benzene, toluene, and ethylbenzene.

[0265] Aggregation methods

[0266] The present disclosure relates to a polymerization process in which monomers (e.g., ethylene, propylene) and optional comonomers are contacted with a catalyst system comprising an activator and at least one catalyst compound as described above. The catalyst compound and the activator may be combined in any order. The catalyst compound and the activator may be combined prior to contact with the monomers. Alternatively, the catalyst compound and the activator may be introduced into a polymerization reactor, respectively, where they subsequently react to form an active catalyst.

[0267] The monomers include substituted or unsubstituted C2-C 40 α-olefins, such as C2-C 20 α-olefins, such as C2-C 12 α-olefins, such as ethylene, propylene, butene, pentene, hexene, heptene, octene, nonene, decene, undecene, dodecene and isomers thereof. In at least one embodiment, the monomers include ethylene and optional comonomers comprising one or more C3-C 40 Olefins, such as C4-C 20 Olefins, such as C6-C 12 Olefins. C3-C 40 The olefin monomers may be linear, branched or cyclic. 40 The cyclic olefins may be strained or unstrained, monocyclic or polycyclic, and may optionally include heteroatoms and / or one or more functional groups. In another embodiment, the monomers include propylene and optional comonomers comprising one or more ethylene or C4-C 40 Olefins, such as C4-C 20 Olefins, such as C6-C 12 Olefins. C4-C 40 The olefin monomers may be linear, branched or cyclic. 40 The cyclic olefins may be strained or unstrained, monocyclic or polycyclic, and may optionally include heteroatoms and / or one or more functional groups.

[0268] Exemplary C2-C 40The olefin monomers and optional comonomers may include ethylene, propylene, butene, pentene, hexene, heptene, octene, nonene, decene, undecene, dodecene, norbornene, norbornadiene, dicyclopentadiene, cyclopentene, cycloheptene, cyclooctene, cyclooctadiene, cyclododecene, 7-oxanorbornene, 7-oxanorbornene, substituted derivatives thereof and isomers thereof, such as hexene, heptene, octene, nonene, decene, dodecene, cyclooctene, 1,5-cyclooctadiene, 1-hydroxy-4-cyclooctene, 1-acetoxy-4-cyclooctene, 5-methylcyclopentene, cyclopentene, dicyclopentadiene, ethylidene norbornene, vinyl norbornene, norbornene, norbornadiene and their respective homologs and derivatives, such as norbornene, norbornadiene and dicyclopentadiene.

[0269] In at least one embodiment, one or more dienes are present in the polymer produced herein at up to 10 wt %, such as at 0.00001 to 1.0 wt %, such as 0.002 to 0.5 wt %, such as 0.003 to 0.2 wt %, based on the total weight of the composition. In at least one embodiment, 500 ppm or less, such as 400 ppm or less, such as 300 ppm or less of diene is added to the polymerization. In other embodiments, at least 50 ppm or 100 ppm or more or 150 ppm or more of diene is added to the polymerization.

[0270] Suitable diene monomers useful in the present disclosure include any hydrocarbon structure having at least two unsaturated bonds, such as C4-C 30, wherein at least two of the unsaturated bonds are readily incorporated into the polymer by stereoregular or non-stereoregular catalysts (one or more). The diene monomer may be selected from α,ω-diene monomers (i.e., divinyl monomers). The diene monomer may be a linear divinyl monomer, such as those containing 4-30 carbon atoms. Examples of suitable dienes include butadiene, pentadiene, hexadiene, heptadiene, octadiene, nonadiene, decadiene, undecadiene, dodecadiene, tridecadiene, tetradecadiene, pentadecadiene, hexadecadiene, heptadecadiene, octadecadiene, nonadecadiene, eicosadiene, heneicosadiene, docosadiene, tricosadiene, tetracosadiene, pentacosadiene, hexacosadiene, heptacosadiene, octacosadiene, nonacosadiene, triacontadiene, for example dienes include 1,6-heptadiene, 1,7-octadiene, 1,8-nonadiene, 1,9-decadiene, 1,10-undecadiene, 1,11-dodecadiene, 1,12-tridecadiene, 1,13-tetradecadiene, and low molecular weight polybutadiene (Mw less than 1000 g / mol). Suitable cyclic dienes include cyclopentadiene, vinyl norbornene, norbornadiene, ethylidene norbornene, divinylbenzene, dicyclopentadiene or higher ring containing dienes with or without substituents at various ring positions.

[0271] The polymerization process of the present disclosure can be carried out in any suitable manner. Any suitable suspension, homogeneous, bulk, solution, slurry or gas phase polymerization process can be used. Such a process can be operated in batch, semi-batch or continuous mode. Homogeneous polymerization processes and slurry processes can be used. (A homogeneous polymerization process is defined as a process in which at least 90% by weight of the product is soluble in the reaction medium.) The homogeneous polymerization process can be a bulk homogeneous process. (A bulk process is defined as a process in which the monomer concentration in the feed of all reactors is 70% by volume or greater.) Alternatively, there is no or no added solvent or diluent in the reaction medium (except for a small amount of carrier used as a catalyst system or other additive, or the amount found with the monomer, such as propane in propylene). In another embodiment, the process is a slurry process. As used herein, the term "slurry polymerization process" means a polymerization process carried out in a hydrocarbon solvent, wherein a supported catalyst is used and the monomers are polymerized at a temperature below the melting point of the produced polymer on the supported catalyst particles. At least 95% by weight of the polymer product derived from the supported catalyst is in pelletized form as solid particles (not dissolved in the diluent).

[0272] Suitable diluents / solvents for polymerization may include non-coordinating inert liquids. Examples of diluents / solvents for polymerization may include straight and branched chain hydrocarbons such as isobutane, butane, pentane, isopentane, hexane, isohexane, heptane, octane, dodecane, and mixtures thereof; cyclic and alicyclic hydrocarbons such as cyclohexane, cycloheptane, methylcyclohexane, methylcycloheptane, and mixtures thereof, such as commercially available (Isopar TM ); perhalogenated hydrocarbons, such as perfluorinated C4-C 10 Alkanes, chlorobenzenes, and aromatic compounds and alkyl-substituted aromatic compounds, such as benzene, toluene, mesitylene and xylene. Suitable solvents can also include liquid olefins, which can act as monomers or comonomers, including ethylene, propylene, 1-butene, 1-hexene, 1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-octene, 1-decene and their mixtures. In at least one embodiment, aliphatic hydrocarbon solvents are used as solvents, such as isobutane, butane, pentane, isopentane, hexane, isohexane, heptane, octane, dodecane and their mixtures; cyclic and alicyclic hydrocarbons such as cyclohexane, cycloheptane, methylcyclohexane, methylcycloheptane and their mixtures. In another embodiment, the solvent is not aromatic, such as aromatic compounds are present in the solvent with less than 1% by weight, such as less than 0.5% by weight, such as less than 0% by weight, based on the weight of the solvent.

[0273] In at least one embodiment, the feed concentration of monomers and comonomers used in the polymerization is 60 volume % solvent or less, such as 40 volume % or less, such as 20 volume % or less, based on the total volume of the feed stream. In at least one embodiment, the polymerization is carried out in a bulk process.

[0274] Polymerization can be carried out at any temperature and / or pressure suitable for obtaining the desired polymer. Typical temperatures and / or pressures include temperatures in the range of about 0°C to about 300°C, such as about 20°C to about 200°C, such as about 35°C to about 160°C, such as about 80°C to about 160°C, such as about 90°C to about 140°C, and pressures in the range of about 0.1 MPa to about 25 MPa, such as about 0.45 MPa to about 6 MPa or about 0.5 MPa to about 4 MPa.

[0275] In suitable polymerizations, the run time of the reaction may be up to 300 minutes, such as about 5 minutes to 250 minutes, such as about 10 minutes to 120 minutes, such as about 20 minutes to 90 minutes, such as about 30 minutes to 60 minutes. In a continuous process, the run time may be the average residence time of the reactor.

[0276] In at least one embodiment, hydrogen is present in the polymerization reactor at a partial pressure of 0.001 psig to 50 psig (0.007 kPa to 345 kPa), e.g., 0.01 psig-25 psig (0.07 kPa to 172 kPa), e.g., 0.1 psig-10 psig (0.7 kPa to 70 kPa).

[0277] In at least one embodiment, little or no alumoxane is used in the process for producing the polymer. For example, the alumoxane may be present at 0 mol%, alternatively the alumoxane may be present at a molar ratio of aluminum to transition metal of less than 500:1, such as less than 300:1, such as less than 100:1, such as less than 1:1.

[0278] In at least one embodiment, the polymerization is: 1) carried out at a temperature of 0°C to 300°C (e.g., 25°C to 250°C, e.g., 80°C to 160°C, e.g., 100°C to 140°C); 2) carried out at a pressure of atmospheric pressure to 10 MPa (e.g., 0.35 MPa-10 MPa, e.g., 0.45 MPa-6 MPa, e.g., 0.5 MPa-4 MPa); 3) carried out in an aliphatic hydrocarbon solvent (e.g., isobutane, butane, pentane, isopentane, hexane, isohexane, heptane, octane, decane, and mixtures thereof; cyclic and alicyclic hydrocarbons such as cyclohexane, cycloheptane, methylcyclohexane, methylcycloheptane, and mixtures thereof; e.g., wherein the aromatic compound is present in the solvent at less than 1 wt %, e.g., less than 0.5 wt %, e.g., at 0 wt %, based on the weight of the solvent); 4) wherein the catalyst system used in the polymerization comprises less than 0.5 mol %, such as 0 mol % aluminoxane, alternatively aluminoxane is present at a molar ratio of aluminum to transition metal of less than 500:1, such as less than 300:1, such as less than 100:1, such as less than 1:1; 5) polymerization occurs in one reaction zone; 6) scavenger (such as trialkylaluminum compound) is optionally absent (e.g., present at zero mol %, or the scavenger is present at a molar ratio of scavenger metal to transition metal of less than 100:1, such as less than 50:1, such as less than 15:1, such as less than 10:1); and 7) hydrogen is optionally present at a partial pressure of 0.001 psig to 50 psig (0.007 kPa to 345 kPa) (e.g., 0.01 psig-25 psig (0.07 kPa to 172 kPa), such as 0.1 psig to 10 psig (0.7 kPa to 70 kPa)). In at least one embodiment, the catalyst system used in the polymerization includes no more than one catalyst compound. A "reaction zone" (also referred to as a "polymerization zone") is a vessel, such as a stirred tank reactor or a loop reactor, in which polymerization occurs. When multiple reactors are used in a continuous polymerization process, each reactor is considered a separate polymerization zone. For multistage polymerization in a batch polymerization process, each polymerization stage is considered a separate polymerization zone. In at least one embodiment, polymerization occurs in one reaction zone. Room temperature is 23°C unless otherwise stated.

[0279] In at least one embodiment, the present disclosure provides a method for producing an ethylene-based polymer, comprising: polymerizing ethylene to form an ethylene-based polymer by contacting ethylene with the catalyst system of the present disclosure described above in one or more continuous stirred tank reactors or loop reactors in series or parallel at a reactor pressure of 0.05 MPa to 1,500 MPa and a reactor temperature of 30° C. to 230° C. In at least one embodiment, hydrogen is present in the polymerization reactor at a partial pressure of about 5 psig to about 300 psig, such as about 10 psig to about 250 psig, such as about 20 psig to about 200 psig, such as about 30 psig to about 150 psig, such as about 50 psig to about 100 psig (e.g., 75 psig). In at least one embodiment, the activity of the catalyst is at least 1,000 gP.mmolcat -1 .h -1 , for example, about 1,000 gP.mmolcat -1 .h -1 -About 10,000,000 gP.mmolcat -1 .h -1 , for example, about 1,500 gP.mmolcat -1 .h -1 -About 8,000,000 gP.mmolcat -1 .h -1 , for example, about 1,800 gP.mmolcat -1 .h -1 -About 1,000,000 gP.mmolcat -1 .h -1 , or about 10,000 gP.mmolcat -1 .h -1 -About 8,000,000 gP.mmolcat -1 .h -1 .

[0280] In another embodiment, the present disclosure provides a method for producing a propylene-based polymer, comprising: polymerizing propylene to form a propylene-based polymer by contacting propylene with the catalyst system of the present disclosure described above in one or more continuous stirred tank reactors or loop reactors in series or parallel at a reactor pressure of 0.5 MPa to 1,500 MPa and a reactor temperature of 30° C. to 230° C. In at least one embodiment, hydrogen is present in the polymerization reactor at a partial pressure of about 10 psig to about 300 psig, such as about 20 psig to about 250 psig, such as about 30 psig to about 200 psig, such as about 40 psig to about 150 psig, such as about 50 psig to about 100 psig (e.g., 75 psig). In at least one embodiment, the activity of the catalyst is at least 1,000 gP.mmolcat -1 .h -1 , for example 1,000 g P.mmolcat -1 .h -1 -About 1,000,000 gP.mmolcat -1 .h -1 , for example 2,000 gP.mmolcat -1 .h -1 - About 3,000 gP.mmolcat -1 .h -1 , alternatively 10,000 g P.mmolcat -1 .h -1 -About 750,000 gP.mmolcat -1 .h -1 , for example 50,000 gP.mmolcat -1 .h -1 -About 500,000 gP.mmolcat -1 .h -1 , for example 100,000 g P.mmolcat -1 .h -1 -About 250,000 gP.mmolcat -1 .h -1 , optionally about 1,000,000 g P.mmolcat -1 .h -1 -About 6,000,000 gP.mmolcat -1 .h -1 , for example about 2,000,000 gP.mmolcat -1 .h -1 - About 4,000,000 gP.mmolcat -1 .h-1 .

[0281] In another embodiment, the present disclosure provides a method for producing an ethylene alpha-olefin copolymer, comprising: reacting ethylene and at least one C3-C4 copolymer in one or more continuous stirred tank reactors or loop reactors connected in series or in parallel at a reactor pressure of 0.05 MPa to 1,500 MPa and a reactor temperature of 30° C. to 230° C. 20 The α-olefin is contacted with the catalyst system described above to polymerize ethylene and at least one C3-C 20 α-olefins to form ethylene α-olefin copolymers. In at least one embodiment, hydrogen is present in the polymerization reactor at a partial pressure of about 10 psig to about 300 psig, such as about 20 psig to about 250 psig, such as about 30 psig to about 200 psig, such as about 40 psig to about 150 psig, such as about 50 psig to about 100 psig (e.g., 75 psig) or about 150 psig to about 300 psig (e.g., 200 psig). In at least one embodiment, the activity of the catalyst is at least 1,000 gP.mmolcat -1 .h -1 , for example, about 1,000 gP.mmolcat -1 .h -1 -About 10,000,000 gP.mmolcat -1 .h -1 , for example, about 1,500 gP.mmolcat -1 .h -1 -About 8,000,000 gP.mmolcat -1 .h -1 , for example, about 1,800 gP.mmolcat -1 .h -1 -About 1,000,000 gP.mmolcat -1 .h -1 , or about 10,000 gP.mmolcat -1 .h -1 -About 8,000,000 gP.mmolcat -1 .h -1 .

[0282] In another embodiment, the present disclosure provides a method for producing a propylene alpha-olefin copolymer, comprising: reacting propylene and at least one ethylene and / or at least one C3-C4 copolymer in one or more continuous stirred tank reactors or loop reactors connected in series or in parallel at a reactor pressure of 0.05 MPa to 1,500 MPa and a reactor temperature of 30° C. to 230° C. 20The α-olefins are contacted with the catalyst system described above to polymerize propylene and at least one ethylene and / or at least one C4-C 20 α-olefins to form ethylene α-olefin copolymers. In at least one embodiment, hydrogen is present in the polymerization reactor at a partial pressure of about 10 psig to about 300 psig, such as about 20 psig to about 250 psig, such as about 30 psig to about 200 psig, such as about 40 psig to about 150 psig, such as about 50 psig to about 100 psig (e.g., 75 psig) or about 150 psig to about 300 psig (e.g., 200 psig). In at least one embodiment, the activity of the catalyst is at least 1,000 gP.mmolcat -1 .h -1 , for example, about 1,000 gP.mmolcat -1 .h -1 -About 10,000,000 gP.mmolcat -1 .h -1 , for example, about 1,500 gP.mmolcat -1 .h -1 -About 8,000,000 gP.mmolcat -1 .h -1 , for example, about 1,800 gP.mmolcat -1 .h -1 -About 1,000,000 gP.mmolcat -1 .h -1 , or about 10,000 gP.mmolcat -1 .h -1 -About 8,000,000 gP.mmolcat -1 .h -1 .

[0283] In at least one embodiment, the conversion of olefin monomer is at least 10%, based on polymer yield and weight of monomer entering the reaction zone, such as 20% or more, such as 30% or more, such as 50% or more, such as 80% or more.

[0284] In at least one embodiment, little or no alumoxane is used in the process for producing the polymer. For example, the alumoxane is present at 0 mol%, or the alumoxane is present at a molar ratio of aluminum to transition metal of less than 500:1, such as less than 300:1, such as less than 100:1, such as less than 1:1.

[0285] In at least one embodiment, little or no scavenger is used in the process for producing ethylene polymers. For example, the scavenger (e.g., trialkylaluminum) is present at 0 mol%, alternatively the scavenger is present at a molar ratio of scavenger metal to transition metal of less than 100:1, such as less than 50:1, such as less than 15:1, such as less than 10:1.

[0286] If desired, other additives may also be used in the polymerization, such as one or more scavengers, hydrogen, aluminum alkyls, or chain transfer agents.

[0287] Gas Phase Polymerization

[0288] Typically, in a gas fluidized bed process for producing polymers, a gaseous stream containing one or more monomers is continuously circulated through a fluidized bed in the presence of a catalyst under reaction conditions. The gaseous stream is withdrawn from the fluidized bed and recycled back to the reactor. Simultaneously, the polymer product is withdrawn from the reactor and fresh monomer is added to replace the polymerized monomer. (See, e.g., U.S. Pat. Nos. 4,543,399, 4,588,790, 5,028,670, 5,317,036, 5,352,749, 5,405,922, 5,436,304, 5,453,471, 5,462,999, 5,616,661, and 5,668,228, all of which are incorporated herein by reference in their entirety.

[0289] Slurry Phase Polymerization

[0290] Slurry polymerization processes are typically operated at a pressure range of 1 to about 50 atmospheres (15 psi to 735 psi, 103 kPa to 5068 kPa) or even greater and at a temperature in the range of 0°C to about 120°C. In slurry polymerization, a suspension of solid particulate polymer is formed in a liquid polymerization diluent medium to which monomers and comonomers are added along with a catalyst. The suspension including the diluent is intermittently or continuously removed from the reactor, wherein the volatile components are separated from the polymer (optionally after distillation) and recycled to the reactor. The liquid diluent used in the polymerization medium is typically an alkane such as a branched alkane having 3-7 carbon atoms. The medium employed should be liquid and relatively inert under polymerization conditions. When a propane medium is used, the method must be operated above the critical temperature and pressure of the reaction diluent. For example, a hexane or isobutane medium is employed.

[0291] In at least one embodiment, the polymerization process is a particle form polymerization, or a slurry process, in which the temperature is kept below the temperature at which the polymer enters the solution. Such techniques are well known in the art and are described in, for example, U.S. Pat. No. 3,248,179, which is fully incorporated herein by reference. The temperature in the particle form process may be from about 85°C to about 110°C. Two example polymerization processes for slurry processes are a process using a loop reactor and a process using a plurality of stirred reactors in series, in parallel, or a combination thereof. Non-limiting examples of slurry processes include continuous loop or stirred tank processes. In addition, other examples of slurry processes are described in U.S. Pat. No. 4,613,484, which is fully incorporated herein by reference.

[0292] In another embodiment, the slurry process is carried out continuously in a loop reactor. The catalyst (either as a slurry in isohexane or as a dry free-flowing powder) is regularly injected into a reactor loop which is itself filled with a circulating slurry of polymer particles grown in an isohexane diluent containing monomer and optional comonomer. Optionally, hydrogen may be added as a molecular weight control. (In one embodiment, 50 ppm to 500 ppm, e.g., 100 ppm to 400 ppm, e.g., 150 ppm to 300 ppm of hydrogen is added.)

[0293] The reactor can be maintained at a pressure of 2,000 kPa to 5,000 kPa, such as 3620 kPa-4309 kPa, and a temperature of about 60°C to about 120°C, depending on the desired polymer melt characteristics. Since most of the reactor is in the form of a double-jacketed tube, the heat of reaction is removed through the loop wall. The slurry is allowed to leave the reactor at regular intervals or continuously, in sequence to a heated low-pressure flash vessel, a rotary dryer, and a nitrogen purge column for removal of isohexane diluent and all unreacted monomers and comonomers. The resulting hydrocarbon-free powder is then compounded for use in various applications.

[0294] If desired, other additives may also be used in the polymerization, such as one or more scavengers, promoters, modifiers, chain transfer agents (eg, diethyl zinc), reducing agents, oxidizing agents, hydrogen, aluminum alkyls, or silanes.

[0295] Useful chain transfer agents are typically alkylaluminoxanes, compounds represented by the formula AlR3, ZnR2 (wherein each R is independently a C1-C8 hydrocarbon group, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl or isomers thereof). Examples may include diethylzinc, methylaluminoxane, trimethylaluminum, triisobutylaluminum, trioctylaluminum or combinations thereof.

[0296] Solution polymerization

[0297] In at least one embodiment, the polymerization process using the catalyst compounds of the present disclosure is a solution polymerization process.

[0298] Solution polymerization is a polymerization method in which a polymer is dissolved in a liquid polymerization medium (e.g., an inert solvent or monomer (one or more) or a blend thereof). Solution polymerization is generally homogeneous. Homogeneous polymerization is a polymerization in which the polymer product is dissolved in a polymerization medium. As described in Oliveira, JV et al. (2000) Ind. Eng, Chem. Res., Vol. 29, 2000, p. 4627, such a system is not turbid. Solution polymerization may include polymerization in a continuous reactor, wherein the formed polymer, the supplied starting monomer and the catalyst material are stirred to reduce or avoid a concentration gradient, and wherein the monomer acts as a diluent or solvent or wherein hydrocarbons are used as diluents or solvents. Suitable methods may be operated at a temperature of about 0° C. to about 250° C., such as about 50° C. to about 170° C., such as about 80° C. to about 150° C., such as about 100° C. to about 140° C. and / or at a pressure of about 0.1 MPa or greater, such as 2 MPa or greater. The upper pressure limit is not strictly limited but can be about 200MPa or less, such as 120MPa or less, such as 30MPa or less. Temperature control in the reactor can be obtained by balancing the heat of polymerization with reactor cooling, which is carried out by the reactor jacket or cooling coil to cool the contents of the reactor, automatic refrigeration, pre-cooling feed, evaporation of liquid medium (diluent, monomer or solvent) or a combination of all three. Adiabatic reactors with pre-cooled feed can also be used. The purity, type and amount of the solvent can be optimized to obtain the maximum catalyst productivity of a particular type of polymerization. The solvent can also be introduced as a catalyst carrier. Depending on the pressure and temperature, the solvent can be introduced as a gas phase or a liquid phase. Advantageously, the solvent can be maintained in the liquid phase and introduced as a liquid. The solvent can be introduced into the polymerization reactor in the feed.

[0299] The method described herein may be a solution polymerization process, which may be carried out in an intermittent manner (e.g., intermittent, semi-intermittent) or in a continuous process. Suitable reactors may include kettles, loops, and tube designs. In at least one embodiment, the method is carried out in a continuous manner and uses a double loop reactor in a series configuration. In at least one embodiment, the method is carried out in a continuous manner and uses a double continuous stirred tank reactor (CSTR) in a series configuration. In addition, the method may be carried out in a continuous manner and may use a tube reactor. In another embodiment, the method is carried out in a continuous manner and uses a loop reactor and a CSTR in a series configuration. The method may also be carried out in an intermittent manner and may use a single stirred tank reactor.

[0300] Polyolefin products

[0301] The present disclosure relates to compositions of matter produced by the methods described herein.

[0302] In at least one embodiment, the methods described herein produce C2-C 20 Olefin homopolymers (e.g. polyethylene, polypropylene), or C2-C 20 Olefin copolymers (e.g. ethylene-octene, ethylene-propylene) and / or propylene-α-olefin copolymers, e.g. C3-C 20 In at least one embodiment, the process described herein produces C3-C 20 Isotactic olefin homopolymers, such as isotactic polypropylene, such as highly isotactic polypropylene.

[0303] The term "isotactic" is defined as 13 Analysis by C NMR has at least 20% or more isotactic pentads.

[0304] In at least one embodiment, the ethylene-based polymer (homopolymer) has one or more of the following: a Mw value of 5,000 g / mol or greater, such as from about 5,000 g / mol to about 4,000,000 g / mol, such as from about 150,000 g / mol to about 300,000 g / mol, alternatively from about 500,000 g / mol to about 700,000 g / mol, such as from about 550,000 g / mol to about 650,000 g / mol, alternatively from about 800,000 g / mol to about 1,200,000 g / mol, such as from about 900,000 g / mol to 1,200,000 g / mol, alternatively from about 3,000,000 g / mol to about 3,800,000 g / mol. 0 g / mol; an Mn value of 70,000 g / mol or more, for example, about 70,000 g / mol to about 2,400,000 g / mol, for example, about 90,000 g / mol to about 120,000 g / mol, alternatively about 200,000 g / mol to about 500,000 g / mol, for example, about 250,000 g / mol to about 450,000 g / mol; and / or an Mz value of 300,000 g / mol or more, for example, about 300,000 g / mol to about 6,000,000 g / mol, for example, about 1,000,000 to about 2,500,000 g / mol, alternatively about 3,500,000 g / mol to about 4,000,000 g / mol.

[0305] In at least one embodiment, the ethylene-based polymer has a Mw / Mn (PDI) value of 1 to 10, such as 1 to 5, such as 1.2 to about 4, such as 1.5 to about 3.

[0306] In at least one embodiment, ethylene-based polymers (homopolymers) can be produced using exemplary catalysts of the present disclosure having high catalyst activity at high reactor temperatures. For example, the catalyst activity can be about 25,000 gP.mmolcat -1 .h -1 -About 200,000 gP.mmolcat -1 .h -1 , for example, about 50,000 gP.mmolcat -1 .h -1 - About 85,000 gP.mmolcat -1 .h -1 , optionally about 90,000 gP.mmolcat -1 .h -1 -About 140,000 gP.mmolcat -1 .h -1 .

[0307] In at least one embodiment, the propylene-based polymer (homopolymer) has one or more of the following: an Mw value of 20,000 g / mol or greater, such as from about 20,000 g / mol to about 1,000,000 g / mol, such as from about 20,000 g / mol to about 30,000 g / mol, alternatively from about 90,000 g / mol to about 170,000 g / mol, such as from about 100,000 g / mol to about 160,000 g / mol, alternatively from about 400,000 g / mol to about 650,000 g / mol, such as from about 430,000 g / mol to 550,000 g / mol, alternatively from about 600,000 g / mol to about 750,000 g / mol; an Mn value of 10, 000 g / mol or more, for example about 10,000 g / mol to about 450,000 g / mol, for example about 8,000 g / mol to about 10,000 g / mol, alternatively about 80,000 g / mol to about 100,000 g / mol, alternatively about 200,000 g / mol to about 400,000 g / mol, for example about 200,000 g / mol to about 300,000 g / mol; and / or an Mz value of 50,000 g / mol or more, for example about 50,000 g / mol to about 2,000,000 g / mol, for example about 50,000 g / mol to about 60,000 g / mol, alternatively about 300,000 g / mol to about 400,000 g / mol.

[0308] In at least one embodiment, the propylene-based polymer has a Mw / Mn (PDI) value of 1-10, such as 1-5, such as 1.2 to about 4, such as 1.5 to about 3.

[0309] In at least one embodiment, propylene-based polymers (homopolymers) can be produced using exemplary catalysts of the present disclosure having high catalyst activity at high reactor temperatures. For example, the catalyst activity can be about 950 gP.mmolcat -1 .h -1 -About 1,000,000 gP.mmolcat -1 .h -1 , for example about 400,000 gP.mmolcat -1 .h -1 -About 700,000 gP.mmolcat -1 .h -1 , optionally about 80,000 gP.mmolcat -1 .h -1 -About 100,000 gP.mmolcat -1 .h-1 , optionally about 8,000 gP.mmolcat -1 .h -1 - About 10,000 g P.mmolcat -1 .h -1 For example, the reactor temperature may be between about 70°C and 100°C.

[0310] In at least one embodiment, the ethylene- or propylene-based polymer has a melting point (Tm) of at least 80°C, such as about 80°C to about 180°C, such as about 100°C to about 165°C, such as about 120°C to about 160°C, such as about 130°C to about 160°C. It is often challenging to obtain polyethylene and polypropylene with high melting points (e.g., 100°C or greater), where the polymer is formed using a non-metallocene catalyst. However, non-metallocene catalysts such as the amino-phenolate-heterocyclic Lewis base catalysts of the present disclosure can provide ethylene- or propylene-based polymers with high Tm. Higher Tm indicates higher crystallinity of the polymer material and provides a harder and more thermally stable material. Therefore, the mechanical properties of the polymer can be adjusted by the Tm of the polymer. For example, in a semi-crystalline thermoplastic polymer, the crystalline structure can contribute to the strength properties of the plastic (e.g., a crystalline material can be tough and hard, and may require high stress to be broken). Increased crystallinity can lead to increases in, for example, density, stiffness, strength, toughness, specific gravity, and elastic modulus. In addition, crystallinity can affect the optical properties of the polymer material. The polymers of the present disclosure having one or more of the foregoing properties, such as high Tm, can be used in a variety of applications, such as optical fiber production. Without being bound by theory, it has been found that when a non-metallocene catalyst of the present disclosure, such as an amino-phenolate-heterocyclic Lewis base catalyst, is used, for example, by using E 1 and E 2 Substituents are larger to adjust the melting point. Thus, the difficulty in preparing high melting point polyolefins, such as high melting point polypropylene, using non-metallocene catalysts can be overcome by the ability to change the melting point of the polymer based on the ability to easily adjust the chemical structure of the catalyst of the present disclosure.

[0311] In at least one embodiment, the ethylene or propylene based polymer is an ethylene alpha-olefin copolymer or a propylene alpha-olefin copolymer having one or more of the following: a Mw value of 100,000 g / mol or greater, such as from about 100,000 g / mol to about 1,500,000 g / mol, such as from about 100,000 g / mol to about 500,000 g / mol, such as from about 300,000 g / mol to about 500,000 g / mol, alternatively from about 1,500,000 g / mol to about 3,500,000, such as from about 2,000,000 g / mol to about 3,000,000 g / mol; a Mn value of 50,000 g / mol or greater, such as from about 50,000 g / mol to about 2 , 300,000g / mol, for example, about 100,000g / mol-about 300,000g / mol, for example, about 100,000g / mol-about 200,000g / mol, alternatively about 1,000,000g / mol-about 2,300,000g / mol, for example, about 1,500,000g / mol-about 2,000,000g / mol; Mz value is 200,000g / mol or greater, for example, about 250,000g / mol-about 350,000g / mol, alternatively about 1,000,000g / mol-about 3,000,000g / mol, alternatively about 5,000,000g / mol-about 6,000,000g / mol.

[0312] In at least one embodiment, the ethylene α-olefin copolymer or propylene α-olefin copolymer has a comonomer content of 0.1 wt% to 99 wt%, such as 1 wt% to 40 wt%, such as 3 wt% to 33 wt%, such as 15 wt% to 30 wt%, alternatively about 40 wt% to about 95 wt%.

[0313] In at least one embodiment, the ethylene alpha-olefin copolymer or the propylene alpha-olefin copolymer has a Mw / Mn (PDI) value of 1 to 5, such as 2 to 4, such as 1.5 to 3.1.

[0314] In at least one embodiment, the ethylene alpha-olefin copolymer or propylene alpha-olefin copolymer has a melting point (Tm) of at least 80°C, such as from about 90°C to about 150°C, alternatively from about 110°C to about 130°C.

[0315] In at least one embodiment, ethylene α-olefin copolymers or propylene α-olefin copolymers can be produced using a catalyst of the present disclosure having high catalyst activity at high reactor temperatures. For example, the catalyst activity can be about 15,000 gP.mmolcat -1 .h -1-About 2,000,000 gP.mmolcat -1 .h -1 , for example about 80,000 gP.mmolcat -1 .h -1 -About 100,000 gP.mmolcat -1 .h -1 , optionally about 200,000 gP.mmolcat -1 .h -1 - About 400,000 gP.mmolcat - 1 .h -1 .

[0316] GPC 4-D

[0317] For the purposes of the claims, and unless otherwise indicated, the molecular weight moments and distributions (Mw, Mn, Mz, Mw / Mn, etc.), comonomer content, and branching index (g') are determined by using high temperature gel permeation chromatography (PolymerChar GPC-IR) equipped with a multi-channel bandpass filter based infrared detector IR5 having a coverage area of ​​about 2,700 cm, an 18-angle light scattering detector, and a viscometer. -1 - Approx. 3,000cm -1Bandpass region (representing saturated CH stretching vibration). Three Agilent PLgel 10-μm mixed-B LS columns are used to provide polymer separation. Reagent grade 1,2,4-trichlorobenzene (TCB) (from Sigma-Aldrich) containing ~300ppm antioxidant BHT is used as mobile phase with a nominal flow rate of ~1.0mL / min and a nominal injection volume of ~200μL. The entire system including transfer lines, columns and detectors can be accommodated in an oven maintained at ~145°C. A given amount of sample can be weighed and sealed in a standard vial, in which ~10μL flow markers (heptane) are added. After loading the vial in the autosampler, the oligomer or polymer can be automatically dissolved in an instrument with ~8ml added TCB solvent at ~160°C under continuous shaking. The sample solution concentration can be from ~0.2mg / ml to ~2.0mg / ml, with lower concentrations used for higher molecular weight samples. The concentration (c) at each point in the chromatogram can be calculated from the baseline-subtracted IR5 broadband signal (I) using the following equation: c = αI, where α is a mass constant determined using polyethylene or polypropylene standards. The mass recovery can be calculated from the ratio of the integrated area of ​​the concentration chromatogram within the elution volume to the injected mass (which is equal to the predetermined concentration multiplied by the injection loop volume). The conventional molecular weight (IR MW) is determined by combining a universal calibration relationship with a column calibration (which is performed using a series of monodisperse polystyrene (PS) standards ranging from 700 to 10M g / mol). The MW at each elution volume is calculated using the following equation:

[0318]

[0319] The variables with the subscript "PS" represent polystyrene, while those without the subscript represent the test sample. In this method, α PS =0.67 and K PS=0.000175, as published and calculated in the literature (Sun, T. et al. (2001) Macromolecules, Vol. 34, p. 6812) for other materials, except that for the purposes of the present disclosure and claims thereto, for ethylene, propylene, diene monomer copolymers, α=0.700 and K=0.0003931, for linear propylene polymers, α=0.705 and K=0.0002288, for linear butene polymers, α=0.695 and K=0.000181, for ethylene-butene copolymers, α is 0.695 and K is 0.000579*(1- 0.0087*w2b+0.000018*(w2b)^2) (where w2b is the bulk weight percent of butene comonomer), for ethylene-hexene copolymers α is 0.695 and K is 0.000579*(1-0.0075*w2b) (where w2b is the bulk weight percent of hexene comonomer), for ethylene-octene copolymers α is 0.695 and K is 0.000579*(1-0.0077*w2b) (where w2b is the bulk weight percent of octene comonomer), and for all other linear ethylene polymers α is 0.695 and K is 0.000579. Unless otherwise indicated, concentrations are in g / cm 3 The molecular weight is expressed in units of g / mole, and the intrinsic viscosity (and hence K in the Mark-Houwink equation) is expressed in units of dL / g.

[0320] The comonomer composition is determined by the ratio of the IR5 detector intensities corresponding to the CH2 and CH3 channels (calibrated with a series of PE and PP homo / copolymer standards with predetermined nominal values ​​by NMR or FTIR). In particular, this provides methyl groups per 1,000 total carbons (CH3 / 1000TC) as a function of molecular weight. The short chain branch (SCB) content per 1000TC as a function of molecular weight (SCB / 1000TC) is then calculated by applying a chain end correction to the CH3 / 1000TC function, assuming that each chain is linear and terminated by a methyl group at each end. The weight % comonomer is then obtained by the following expression, where f is 0.3, 0.4, 0.6, 0.8, etc. for comonomers such as C3, C4, C6, C8, etc., respectively:

[0321] w2=f*SCB / 1000TC

[0322] The bulk composition of the polymer from GPC-IR and GPC-4D analysis was obtained by considering the entire signal of the CH3 and CH2 channels between the integration limits of the concentration chromatogram. First, the following ratio was obtained:

[0323]

[0324] The same calibration of the CH3 and CH2 signal ratios (as mentioned previously in obtaining CH3 / 1000TC as a function of molecular weight) was then applied to obtain the bulk CH3 / 1000TC. The bulk methyl chain ends / 1000TC (bulk CH3 ends / 1000TC) was obtained by weighting the average chain end correction over the molecular weight range.

[0325] but

[0326] w2b=f*body CH3 / 1000TC

[0327] Bulk SCB / 1000TC=bulk CH3 / 1000TC-bulk CH3end / 1000TC and bulk SCB / 1000TC is converted to bulk w2 in the same manner as described above.

[0328] The LS detector was an 18-angle Wyatt Technology high temperature DAWN HELEOS II. The LS molecular weight (M) at each point in the chromatogram was determined by analyzing the output of the LS using the Zimm model for static light scattering (Light Scattering from Polymer Solutions, Huglin, MB ed., Academic Press, 1972):

[0329]

[0330] Here, ΔR(θ) is the excess Rayleigh scattering intensity measured at the scattering angle θ, c is the polymer concentration determined from the IR5 analysis, A2 is the second virial coefficient, P(θ) is the shape factor of the monodisperse random coil, and K o is the optical constant of the system:

[0331]

[0332] Where N A is the Avogadro constant, and (dn / dc) is the refractive index increment of the system. The refractive index of TCB at 145°C and λ=665nm is n=1.500. For the analysis of polyethylene homopolymers, ethylene-hexene copolymers and ethylene-octene copolymers, dn / dc=0.1048 ml / mg and A2=0.0015; for the analysis of ethylene-butene copolymers, dn / dc=0.1048*(1-0.00126*w2)ml / mg and A2=0.0015, where w2 is the weight percentage of butene comonomer.

[0333] The specific viscosity is determined using a high temperature Agilent (or Viscotek Corporation) viscometer (which has four capillaries arranged in a Wheatstone bridge configuration, and two pressure sensors). One sensor measures the total pressure drop across the detector, and the other sensor placed between the two sides of the bridge measures the pressure difference. The specific viscosity η of the solution flowing through the viscometer is calculated from their outputs. s . From the equation [η] = η s The intrinsic viscosity [η] at each point in the chromatogram is calculated as / c, where c is the concentration and is determined from the IR5 broadband channel output. The viscosity MW at each point is calculated as where α ps is 0.67 and K ps It is 0.000175.

[0334] The branching index (g') was calculated using the output of the GPC-IR5-LS-VIS method as follows: vis ). The average intrinsic viscosity of the sample [η] avg By the following calculation:

[0335]

[0336] where the sum is taken from all chromatographic slices i between the integration limits. Branching index g' vis Defined as Among them, M V is the viscosity average molecular weight based on the molecular weight determined by LS analysis and K and α are for reference linear polymers, which for purposes of this disclosure and claims thereto are α=0.700 and K=0.0003931 for ethylene, propylene, diene monomer copolymers, α=0.705 and K=0.0002288 for linear propylene polymers, α=0.695 and K=0.000181 for linear butene polymers, and α is 0.695 and K is 0.000579*(1-0.0087*w2b+0.00001 for ethylene-butene copolymers. 8*(w2b)^2) (where w2b is the bulk weight percent of the butene comonomer), for ethylene-hexene copolymers α is 0.695 and K is 0.000579*(1-0.0075*w2b) (where w2b is the bulk weight percent of the hexene comonomer), for ethylene-octene copolymers α is 0.695 and K is 0.000579*(1-0.0077*w2b) (where w2b is the bulk weight percent of the octene comonomer), and for all other linear ethylene polymers, α is 0.695 and K is 0.000579. Unless otherwise indicated, concentrations are in g / cm 3The w2b value is expressed in units of dL / g, the molecular weight is expressed in units of g / mole, and the intrinsic viscosity (and therefore K in the Mark-Houwink equation) is expressed in units of dL / g. The calculation of the w2b value is as discussed above.

[0337] Blends

[0338] In another embodiment, the polymers (e.g., polyethylene or polypropylene) produced herein are combined with one or more additional polymers prior to being formed into films, molded parts, or other articles. Other useful polymers include polyethylene, isotactic polypropylene, highly isotactic polypropylene, syndiotactic polypropylene, random copolymers of propylene and ethylene and / or butene and / or hexene, polybutene, ethylene vinyl acetate, LDPE, LLDPE, HDPE, ethylene vinyl acetate, ethylene methyl acrylate, copolymers of acrylic acid, polymethyl methacrylate, or any other polymer that can be polymerized by a high pressure free radical process, polyvinyl chloride, polybutene-1, isotactic polybutene, ABS resin, ethylene-propylene rubber (EPR), sulfurized EPR, EPDM, block copolymers, styrenic block copolymers, polyamides, polycarbonates, PET resins, crosslinked polyethylene, copolymers of ethylene and vinyl alcohol (EVOH), polymers of aromatic monomers such as polystyrene, poly-1 esters, polyacetals, polyvinylidene fluoride, polyethylene glycol, and / or polyisobutylene.

[0339] In at least one embodiment, the polymer (e.g., polyethylene or polypropylene) is present in the above blend at 10 wt%-99 wt%, such as 20 wt% to 95 wt%, such as at least 30 wt% to 90 wt%, such as at least 40 wt% to 90 wt%, such as at least 50 wt% to 90 wt%, such as at least 60 wt% to 90 wt%, such as at least 70 to 90 wt%, based on the weight of the polymer in the blend.

[0340] The blends described above can be produced by mixing a polymer of the present disclosure with one or more polymers (as described above), by connecting reactors together in series to make reactor blends, or by using more than one catalyst in the same reactor to produce multiple polymer species. The polymers can be mixed together before being placed in the extruder or can be mixed in the extruder.

[0341] The blend may be formed using conventional equipment and methods, such as by dry blending the individual components and then melt mixing in a mixer, or by mixing the components together directly in a mixer, such as a Banbury mixer, Haake mixer, Brabender internal mixer, or a single or twin screw extruder, which may include a compounding extruder and a side arm extruder used directly downstream of the polymerization process, which may include powders or pellets of the blended resins at the hopper of a film extruder. In addition, additives may be included in the blend, in one or more components of the blend, and / or in a product formed from the blend, such as a film, as desired. Such additives are well known in the art and may include, for example, fillers; antioxidants (e.g., hindered phenols such as IRGANOX available from Ciba-Geigy); TM 1010 or IRGANOX TM 1076); phosphites (e.g., IRGAFOS available from Ciba-Geigy TM 168); anti-cling additives; tackifiers such as polybutene, terpene resins, aliphatic and aromatic hydrocarbon resins, alkali metal and glyceryl stearates and hydrogenated rosin; UV stabilizers; heat stabilizers; antiblocking agents; mold release agents; antistatic agents; pigments; colorants; dyes; waxes; silica; fillers; talc.

[0342] membrane

[0343] Any of the aforementioned polymers, such as the aforementioned polypropylene or their blends, can be used in various end-use applications. Such applications include, for example, single-layer or multilayer blow molding, extrusion and / or shrink film. These films can be formed by any number of known extrusion or coextrusion techniques, such as blown bubble film processing technology, wherein the composition can be extruded through an annular die in a molten state and then expanded to form a uniaxial or biaxially oriented melt, then cooled to form a tubular blown film, which can then be axially cut and unfolded to form a flat film. The film can then be unoriented, uniaxially oriented or biaxially oriented to the same or different extents. One or more layers of the oriented film can be oriented in the horizontal and / or longitudinal directions to the same or different extents. Uniaxial orientation can be accomplished using common cold drawing (cold drawing) methods or hot drawing (hot drawing) methods. Biaxial orientation can be accomplished using a tentering machine device or a double bubble method, and biaxial orientation can occur before or after each layer is brought together. For example, a polyethylene layer can be extrusion coated or laminated to an oriented polypropylene layer or polyethylene and polypropylene can be coextruded together as a film and then oriented. Likewise, an oriented polypropylene can be laminated to an oriented polyethylene, or an oriented polyethylene can be coated onto polypropylene and then optionally the combination can be even further oriented. For example, the film is oriented in the machine direction (MD) at a ratio of up to 15, such as from about 5 to about 7, and in the transverse direction (TD) at a ratio of up to 15, such as from about 7 to about 9. However, in another embodiment, the film is oriented to the same extent in both the MD and TD directions.

[0344] Depending on the intended application, the film thickness may vary; however, films having a thickness of 1 μm to 50 μm may be suitable. Films intended for packaging may be 10 μm to 50 μm thick. The thickness of the sealing layer may be 0.2 μm to 50 μm. The sealing layer may be present on both the inner and outer surfaces of the film or may be present only on the inner or outer surface.

[0345] In another embodiment, one or more layers may be modified by corona treatment, electron beam irradiation, gamma irradiation, flame treatment, or microwaves.In at least one embodiment, one or both surface layers are modified by corona treatment.

[0346] Aspect List

[0347] The present disclosure provides, among other things, the following aspects, each of which may be considered to optionally include any alternative aspects.

[0348] Item 1. A catalyst compound represented by formula (I):

[0349]

[0350] in:

[0351] M is a Group 3, 4, 5 or 6 metal;

[0352] A 1 and A 2 wherein each is independently selected from the group consisting of aryl, substituted aryl, heteroaryl, and substituted heteroaryl groups;

[0353] J comprises a heterocyclic Lewis base;

[0354] E 1 Selected from the group consisting of hydrocarbon, substituted hydrocarbon, silyl and substituted silyl, wherein J and E 1 optionally joined to form one or more hydrocarbyl rings, substituted hydrocarbyl rings, heterocyclic rings, or substituted heterocyclic rings;

[0355] Each L is independently a Lewis base;

[0356] Each X is independently an anionic ligand;

[0357] n is 1, 2, or 3;

[0358] m is 0, 1, or 2;

[0359] n+m is not greater than 4;

[0360] R 1 Select from the following: C1-C 40 Hydrocarbyl, substituted C1-C 40 Hydrocarbyl groups, heteroatom-containing groups and substituted heteroatom-containing groups;

[0361] Any two L groups can be joined together to form a bidentate Lewis base;

[0362] The X group can be joined to the L group to form a monoanionic bidentate group; and

[0363] Any two X groups can be joined together to form a dianionic ligand group.

[0364] Item 2. The catalyst compound of Item 1, wherein the catalyst compound comprises an eight-membered metallacycle ring and a five-membered metallacycle ring.

[0365] Item 3. The catalyst compound of Item 1 or 2, wherein E 1 Selected from C(R 8 )(R 9 ) and Si(R 8 )(R 9 ), where R 8 and R 9 Each of which is independently selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C40 A hydrocarbon group, a heteroatom, a group containing a heteroatom, and a substituted group containing a heteroatom, or R 8 and R 9 Can be joined to form one or more C3-C 20 Alkyl groups, hydrocarbyl rings, substituted hydrocarbyl rings, heterocyclic rings, or substituted heterocyclic rings, each having 5, 6, 7, or 8 ring atoms, and wherein substituents on the rings may join to form additional rings.

[0366] Item 4. The catalyst compound of any one of Items 1 to 3, wherein J is represented by the formula:

[0367]

[0368] Where R 2 , R 3 and R 4 Each of which is independently selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 Hydrocarbon groups, heteroatoms and groups containing heteroatoms, or R 2 and R 3 or R 3 and R 4 One or more of the pairs may join to form one or more hydrocarbyl, substituted hydrocarbyl, heterocyclic, or substituted heterocyclic rings, each having 5, 6, 7, or 8 ring atoms, and wherein substituents on the rings may join to form additional rings.

[0369] Item 5. The catalyst compound of any one of Items 1 to 4, wherein J and E 1 are joined to form a ring represented by the formula:

[0370]

[0371] Where E 2 Selected from O, S and N (R 10 ), where R 5 , R 6 , R 7 and R 10 Each of which is independently selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 a hydrocarbon group, a heteroatom, a group containing a heteroatom, or a substituted group containing a heteroatom, or R 5 and R 6 or R 6 and R 7 One or more of the pairs may join to form one or more hydrocarbyl, substituted hydrocarbyl, heterocyclic, or substituted heterocyclic rings, each having 5, 6, 7, or 8 ring atoms, and wherein substituents on the rings may join to form additional rings.

[0372] Item 6. The catalyst compound of any one of Items 1 to 5, wherein J and E 1 are joined to form a ring represented by the formula:

[0373]

[0374] Where R 5 , R 6 , R 7 , R 10 and R 15 Each of which is independently selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 A hydrocarbon group, a heteroatom and a heteroatom-containing group, and a substituted heteroatom-containing group, or R 5 and R 6 or R 6 and R 7 or R 7 and R 10 or R 10 and R 15 One or more of the pairs may join to form one or more hydrocarbyl, substituted hydrocarbyl, heterocyclic, or substituted heterocyclic rings, each having 5, 6, 7, or 8 ring atoms, and wherein substituents on the rings may join to form additional rings.

[0375] Item 7. The catalyst compound of any one of Items 1 to 6, wherein M is a Group 4 transition metal.

[0376] Item 8. The catalyst compound of Items 1 to 7, wherein A 1 is an aryl group or a substituted aryl group.

[0377] Item 9. The catalyst compound of any one of Items 1 to 8, wherein A 2 It is expressed by the following formula: Where R 11 , R 12 , R 13 and R 14 Each of which is independently selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 Hydrocarbyl groups, heteroatoms, heteroatom-containing groups, and substituted heteroatom-containing groups.

[0378] Item 10. The catalyst compound of Item 9, wherein R 11 It is C1-C 20 A hydrocarbon group or a substituted hydrocarbon group.

[0379] Item 11. The catalyst compound of any one of Items 9 to 10, wherein R 11It is tert-butyl.

[0380] Item 12. The catalyst compound of any one of Items 9 to 10, wherein R 11 is a di-tert-butylphenyl group.

[0381] Item 13. The catalyst compound of Item 9, wherein R 11 It is expressed by the following formula:

[0382]

[0383] Item 14. The catalyst compound of Item 5, wherein E 2 Selected from the following: NH, C1-C 20 Alkyl-N and C4-C 20 Aryl-N.

[0384] Item 15. The catalyst compound of Item 4, wherein R 2 , R 3 and R 4 independently selected from hydrogen and C1-C 10 alkyl.

[0385] Item 16. The catalyst compound of any one of Items 1 to 15, wherein R 1 is a di-tert-butylphenyl group.

[0386] Item 17. The catalyst compound of any one of Items 1 to 16, wherein E 1 is C(R 8 )(R 9 ), where R 8 is hydrogen and R 9 is a tert-butylphenyl group.

[0387] Item 18. The catalyst compound of any one of Items 1 to 17, wherein E 1 It is CH2.

[0388] Item 19. The catalyst compound of any one of Items 1 to 18, wherein M is zirconium or hafnium.

[0389] Clause 20. The catalyst compound of any one of clauses 1 to 19, wherein the catalyst compound is selected from the following:

[0390]

[0391]

[0392]

[0393] Clause 21. The catalyst compound of any one of clauses 1 to 20, wherein the catalyst compound is:

[0394]

[0395] Item 22. A catalyst system comprising an activator and the catalyst compound of any one of items 1 to 21.

[0396] Clause 23. The catalyst system of any one of Clauses 1 to 22, further comprising a support material.

[0397] Item 24. The catalyst system of Item 23, wherein the support material is selected from Al2O3, ZrO2, SiO2, SiO2 / Al2O3, SiO2 / TiO2, silica clay, silica / clay or mixtures thereof.

[0398] Clause 25. The catalyst system of any one of Clauses 22 to 24, wherein the activator comprises a non-coordinating anion activator.

[0399] Clause 26. The catalyst system of any one of Clauses 22 to 25, wherein the activator is represented by the formula:

[0400] (Z d+ )(A d- )

[0401] Wherein Z is (LH) or a reducible Lewis acid, L is a Lewis base, H is hydrogen, (LH) + is a Bronsted acid; A d- is a non-coordinating anion having a charge of d-; and d is an integer from 1 to 3.

[0402] Clause 27. The catalyst system of any one of Clauses 22 to 25, wherein the activator is represented by the formula:

[0403] (Z d+ )(A d- )

[0404] Among them A d- is a non-coordinating anion having a charge d-; d is an integer from 1 to 3 and Z is a reducible Lewis acid represented by the formula: (Ar3C + ), wherein Ar is an aromatic group or is substituted by a heteroatom, C1-C 40 Hydrocarbon or substituted C1-C 40 Hydrocarbyl-substituted aryl.

[0405] Clause 28. The catalyst system of any one of clauses 22 to 27, wherein the activator is one or more of:

[0406] Dioctadecylmethylammonium tetrakis(pentafluorophenyl)borate,

[0407] Dioctadecylmethylammonium tetrakis(perfluoronaphthyl)borate,

[0408] N,N-Dimethylanilinium tetrakis(pentafluorophenyl)borate,

[0409] Triphenylcarbon tetrakis(pentafluorophenyl)borate

[0410] Trimethylammonium tetrakis(perfluoronaphthyl)borate,

[0411] Triethylammonium tetrakis(perfluoronaphthyl)borate,

[0412] Tripropylammonium tetrakis(perfluoronaphthyl)borate,

[0413] Tri(n-butyl)ammonium tetra(perfluoronaphthyl)borate,

[0414] Tri(tert-butyl)ammonium tetrakis(perfluoronaphthyl)borate,

[0415] N,N-dimethylanilinium tetrakis(perfluoronaphthyl)borate,

[0416] N,N-diethylanilinium tetrakis(perfluoronaphthyl)borate,

[0417] N,N-dimethyl-(2,4,6-trimethylanilinium tetrakis(perfluoronaphthyl)borate,

[0418] Tetrakis(perfluoronaphthyl)boric acid

[0419] Triphenylcarbon tetrakis(perfluoronaphthyl)borate

[0420] Triphenyl tetrakis(perfluoronaphthyl)borate

[0421] Triethylsilyltetrakis(perfluoronaphthyl)borate

[0422] Tetrakis(perfluoronaphthyl)benzene borate (diazo ),

[0423] Trimethylammonium tetrakis(perfluorobiphenyl)borate,

[0424] Triethylammonium tetrakis(perfluorobiphenyl)borate,

[0425] Tripropylammonium tetrakis(perfluorobiphenyl)borate,

[0426] Tri(n-butyl)ammonium tetrakis(perfluorobiphenyl)borate,

[0427] Tri(tert-butyl)ammonium tetrakis(perfluorobiphenyl)borate,

[0428] N,N-dimethylanilinium tetrakis(perfluorobiphenyl)borate,

[0429] N,N-Diethylanilinium tetrakis(perfluorobiphenyl)borate,

[0430] N,N-dimethyl-(2,4,6-trimethylanilinium tetrakis(perfluorobiphenyl)borate,

[0431] Tetrakis(perfluorobiphenyl)boric acid

[0432] Tetrakis(perfluorobiphenyl) borate triphenylcarbon

[0433] Tetrakis(perfluorobiphenyl)triphenyl borate

[0434] Triethylsilyltetrakis(perfluorobiphenyl)borate

[0435] Tetrakis(perfluorobiphenyl)benzene borate (diazo ),

[0436] [4-tert-butyl-PhNMe2H][(C6F3(C6F5)2)4B],

[0437] Trimethylammonium tetraphenylborate,

[0438] Triethylammonium tetraphenylborate,

[0439] Tripropylammonium tetraphenylborate,

[0440] Tri(n-butyl)ammonium tetraphenylborate,

[0441] Tri(tert-butyl)ammonium tetraphenylborate,

[0442] N,N-Dimethylanilinium tetraphenylborate,

[0443] N,N-Diethylanilinium tetraphenylborate,

[0444] N,N-dimethyl-(2,4,6-trimethylanilinium tetraphenylborate,

[0445] Tetraphenylboric acid

[0446] triphenylcarbon tetraphenylborate

[0447] triphenyl tetraphenyl borate

[0448] Triethylsilyl tetraphenylborate

[0449] Tetraphenylbenzene borate (diazo ),

[0450] Trimethylammonium tetrakis(pentafluorophenyl)borate,

[0451] Triethylammonium tetrakis(pentafluorophenyl)borate,

[0452] Tripropylammonium tetrakis(pentafluorophenyl)borate,

[0453] Tri(n-butyl)ammonium tetrakis(pentafluorophenyl)borate,

[0454] Tri(sec-butyl)ammonium tetrakis(pentafluorophenyl)borate,

[0455] N,N-Dimethylanilinium tetrakis(pentafluorophenyl)borate,

[0456] N,N-Diethylanilinium tetrakis(pentafluorophenyl)borate,

[0457] N,N-dimethyl-(2,4,6-trimethylanilinium tetrakis(pentafluorophenyl)borate,

[0458] Tetrakis(pentafluorophenyl)boric acid

[0459] Triphenylcarbon tetrakis(pentafluorophenyl)borate

[0460] Triphenyl tetrakis(pentafluorophenyl)borate

[0461] Triethylsilyltetrakis(pentafluorophenyl)borate

[0462] benzene tetrakis(pentafluorophenyl)borate (diazo ),

[0463] Trimethylammonium tetrakis(2,3,4,6-tetrafluorophenyl)borate,

[0464] Triethylammonium tetrakis(2,3,4,6-tetrafluorophenyl)borate,

[0465] Tripropylammonium tetrakis(2,3,4,6-tetrafluorophenyl)borate,

[0466] Tri(n-butyl)ammonium tetrakis(2,3,4,6-tetrafluorophenyl)borate,

[0467] Dimethyl(tert-butyl)ammonium tetrakis(2,3,4,6-tetrafluorophenyl)borate,

[0468] N,N-Dimethylanilinium tetrakis(2,3,4,6-tetrafluorophenyl)borate,

[0469] N,N-Diethylanilinium tetrakis(2,3,4,6-tetrafluorophenyl)borate,

[0470] N,N-dimethyl-(2,4,6-trimethylanilinium tetrakis(2,3,4,6-tetrafluorophenyl)borate,

[0471] Tetrakis(2,3,4,6-tetrafluorophenyl)boric acid

[0472] Triphenylcarbon tetrakis(2,3,4,6-tetrafluorophenyl)borate

[0473] Triphenyl tetrakis(2,3,4,6-tetrafluorophenyl)borate

[0474] Triethylsilyltetrakis(2,3,4,6-tetrafluorophenyl)borate

[0475] Tetrakis(2,3,4,6-tetrafluorophenyl)benzene borate (diazo ),

[0476] Trimethylanilinium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate,

[0477] Triethylanilinium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate,

[0478] Tripropylanilinium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate,

[0479] Tri(n-butyl)ammonium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate,

[0480] Tri(tert-butyl)ammonium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate,

[0481] N,N-Dimethylanilinium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate,

[0482] N,N-Diethylanilinium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate,

[0483] N,N-dimethyl-(2,4,6-trimethylanilinium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate,

[0484] Tetrakis(3,5-bis(trifluoromethyl)phenyl)boric acid

[0485] triphenylcarbon tetrakis(3,5-bis(trifluoromethyl)phenyl)borate

[0486] triphenyl tetrakis(3,5-bis(trifluoromethyl)phenyl)borate

[0487] Triethylsilyltetrakis(3,5-bis(trifluoromethyl)phenyl)borate

[0488] benzene tetrakis(3,5-bis(trifluoromethyl)phenyl)boronic acid ),

[0489] Di(isopropyl)ammonium tetrakis(pentafluorophenyl)borate,

[0490] Dicyclohexylammonium tetrakis(pentafluorophenyl)borate,

[0491] Tri(o-tolyl)tetrakis(pentafluorophenyl)borate

[0492] Tris(2,6-dimethylphenyl)tetrakis(pentafluorophenyl)borate

[0493] Triphenylcarbon tetrakis(pentafluorophenyl)borate

[0494] 1-(4-(Tris(pentafluorophenyl)boronic acid)-2,3,5,6-tetrafluorophenyl)pyrrolidine

[0495] 4-(tris(pentafluorophenyl)boronic acid)-2,3,5,6-tetrafluoropyridine, and

[0496] triphenylcarbon tetrakis(3,5-bis(trifluoromethyl)phenyl)borate

[0497] Clause 29. The catalyst system of any one of Clauses 22 to 25, wherein the activator is represented by formula (AI):

[0498] [R 1 R 2 R 3 EH] d + [Mk + Q n ] d- (AI)

[0499] in:

[0500] E is nitrogen or phosphorus;

[0501] d is 1, 2 or 3; k is 1, 2 or 3; n is 1, 2, 3, 4, 5 or 6; nk = d;

[0502] R 1 , R 2 and R 3 Each of which is independently hydrogen, C1-C 40 Alkyl or C5-C 50 -aryl, where R 1 , R 2 and R 3 Each of which is independently unsubstituted or substituted; wherein R1 , R 2 and R 3 Contains 15 or more carbon atoms in total;

[0503] M is an element selected from Group 13 of the Periodic Table; and

[0504] Each Q is independently selected from the group consisting of hydrogen, bridged or unbridged dialkylamino, halo, alkoxy, substituted alkoxy, aryloxy, substituted aryloxy, hydrocarbyl, substituted hydrocarbyl, halohydrocarbyl, substituted halohydrocarbyl, and halo-substituted hydrocarbyl groups.

[0505] Clause 30. The catalyst system of any one of Clauses 22 to 29, further comprising a metal hydrocarbenyl chain transfer agent represented by the formula:

[0506] Al(R') 3-v (R”) v

[0507] Wherein each R' is independently C1-C 30 Hydrocarbyl group; each R" is independently C4-C 20 a hydrocarbenyl group; and v is 0.1-3.

[0508] Clause 31. The catalyst system of any of Clauses 22 to 30, wherein the activator comprises an aluminoxane.

[0509] Item 32. The catalyst system of Item 31, wherein the aluminoxane is present in a molar ratio of aluminum to transition metal of the catalyst compound of 100:1 or greater.

[0510] Clause 33. A method for producing a polymer, comprising: polymerizing an olefin by contacting the olefin with the catalyst system of any one of clauses 22 to 31 in one or more continuous stirred tank reactors or loop reactors connected in series or in parallel at a reactor pressure of 0.05 MPa to 1,500 MPa and a reactor temperature of 30°C to 230°C.

[0511] Clause 34. The process of clause 33, wherein the polymer is a homopolymer polyethylene and the olefin is ethylene, wherein the homopolymer polyethylene has an M w The value is 155,000g / mol-1,200,000g / mol, M n Value is 90,000-550,000, M z The value is 350,000-4,000,000, and the PDI is 1.5-3.

[0512] Clause 35. The method of any one of clauses 31 to 34, wherein:

[0513] The melting temperature of the polymer is between about 135°C and 138°C, and

[0514] The catalyst compound is represented by:

[0515]

[0516] Where R 11 Selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 Hydrocarbyl groups, heteroatoms and groups containing heteroatoms.

[0517] Clause 36. The method of clause 35, wherein R 11 It is tert-butyl.

[0518] Clause 37. The method of clause 35, wherein R 11 is a di-tert-butylphenyl group.

[0519] Clause 38. The method of clause 35, wherein R 11 It is expressed by the following formula:

[0520]

[0521] Clause 39. The method of any one of clauses 33 to 34, wherein:

[0522] The melting temperature of the polymer is between about 135°C and 138°C, and

[0523] The catalyst compound is:

[0524]

[0525] Clause 40. The method of clause 33, wherein:

[0526] The polymer is an ethylene-octene copolymer,

[0527] The copolymer has an M w Value is 100,000-3,600,000, M n Value is 50,000-2,250,000, M z The value is 225,000-6,200,000, and the PDI is 1.5-3.

[0528] Clause 41. The method of clause 40, wherein:

[0529] The melting temperature of the polymer is 104°C-126°C, and

[0530] The catalyst compound is represented by:

[0531]

[0532] Where R 11 Selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 Hydrocarbyl groups, heteroatoms and groups containing heteroatoms.

[0533] Clause 42. The method of clause 41, wherein:

[0534] R 11 is tert-butyl, and

[0535] The melting temperature of the polymer is 121°C-126°C.

[0536] Clause 43. The method of clause 41, wherein R 11 It is di-tert-butylphenyl.

[0537] Clause 44. The method of clause 41, wherein:

[0538] The olefin is propylene,

[0539] The polymer is homopolypropylene, and

[0540] Homopolymer polypropylene has:

[0541] M w The value is 85,000g / mol-750,000g / mol,

[0542] M n The value is 55,000g / mol-400,000g / mol,

[0543] M z Values ​​range from 165,000 g / mol to 1,600,000 g / mol, and

[0544] PDI is 1.6-2.1.

[0545] Clause 45. The method of clause 44, wherein:

[0546] The reactor temperature is between about 60°C and 80°C,

[0547] The melting temperature of the polymer is 146°C-147°C, and

[0548] The catalyst compound is:

[0549] Example

[0550] General considerations for synthesis:

[0551] Unless otherwise noted, all reagents were purchased from commercial suppliers (Sigma Aldrich) and used as received. Solvents were purged with argon and passed through All chemical manipulations were performed under nitrogen atmosphere unless otherwise stated. Sigma Aldrich silica gel was used. (70 mesh–230 mesh) Flash column chromatography was performed using the specified solvent system. NMR spectra were recorded on a Bruker 400 and / or 500 NMR with chemical shifts referenced to the residual solvent peak. All anhydrous solvents were purchased from Fisher Chemical and degassed and dried over molecular sieves before use. Deuterated solvents were purchased from Cambridge Isotope Laboratories and degassed and dried over molecular sieves before use. 1H NMR spectral data were acquired at 400 MHz and at 100 MHz using solutions prepared by dissolving approximately 10 mg of sample in C6D6, CDCl3, DMSO-d6 or other deuterated solvents. 13 C NMR spectral data. The chemical shifts (δ) present relative to the residual protium in the deuterated solvent were located at 7.15 ppm, 7.25 ppm and 2.09 ppm for C6D6, CDCl3 and DMSO-d6, respectively. 13 The C-NMR chemical shifts were 128.0 ppm and 77.0 ppm for C6D6 and CDCl3, respectively.

[0552] Synthesis of ligands and catalysts (or complexes)

[0553] Catalyst 1 Synthesis

[0554] N-[-(6-Bromopyridin-2-yl)methylene]-2,6-diisopropylaniline

[0555]

[0556] A mixture of 85.0 g (457 mmol) of 6-bromopyridine-2-carbaldehyde and 80.9 g (457 mmol) of 2,6-diisopropylaniline in 1,000 mL of ethanol was heated to reflux for 8 hours under an argon atmosphere. The obtained solution was evaporated to dryness, and the resulting solid was recrystallized from 200 mL of methanol. Yield 113.5 g (72%) of a yellow crystalline solid. 1H NMR (CDCl3): δ8.24-8.26(m,2H),7.68-7.72(m,1H),7.59-7.61(m,1H),7.10-7.18(m,3H),2.91(sept,J=6.8Hz,2H),1.16(d,J=6.8Hz,12H).

[0557] N-[(6-Bromopyridin-2-yl)methyl]-2,6-diisopropylaniline

[0558]

[0559] Under an argon atmosphere, a mixture of 113.5 g (329 mmol) of N-[(6-bromopyridin-2-yl)methylene]-2,6-diisopropylaniline, 33.2 g (526 mmol) of NaBH3CN, 9 mL of glacial acetic acid and 1,000 mL of methanol was heated to reflux for 12 hours. The obtained mixture was cooled to room temperature, poured into 1,000 mL of water, and then extracted with 3×200 mL of ethyl acetate. The combined extracts were dried over Na2SO4 and evaporated to dryness. The residue was purified by flash chromatography on silica gel 60 (40-63 microns; eluent: hexane-ethyl acetate = 10:1 volume). Yield 104 g (91%) of yellow oil. 1 H NMR(CDCl3): δ7.51-7.55(m,1H),7.41-7.43(m,1H),7.31-7.33(m,1H),7.08-7.15(m ,3H),4.21(s,2H),3.96(br.s,1H),3.36(sept,J=6.8Hz,2H),1.26(d,J=6.8Hz,12H).

[0560] 2-(3'-(tert-butyl)-2'-(methoxymethoxy)-5'-methyl-[1,1'-biphenyl]-2-yl)-4,4,5,5-tetramethyl-1,3,2-dioxaborolane

[0561]

[0562] To 4.23 g (174 mmol) of vacuum dried magnesium powder, 150 mL of dry tetrahydrofuran and 10.0 g (34.8 mmol) of 1-bromo-3-(tert-butyl)-2-(methoxymethoxy)-5-methylbenzene were subsequently added. The reaction mixture was stirred at 55 ° C overnight, and then a solution of 6.99 g (36.5 mmol) of 1-bromo-2-chlorobenzene in 100 mL of tetrahydrofuran was added dropwise over 3 hours. The resulting suspension was stirred at 55 ° C overnight, and then 9.70 g (52.2 mmol) of 2-isopropoxy-4,4,5,5-tetramethyl-1,3,2-dioxaborolane was added after it was cooled to 0 ° C. The resulting mixture was stirred at room temperature overnight, and then 500 mL of water was poured. The mixture was extracted with 3×100 mL of dichloromethane. The combined organic extracts were dried over Na2SO4 and evaporated to near dryness. The residue was purified by flash chromatography on silica gel 60 (40-63 μm; eluent: hexane-ethyl acetate = 15:1 by volume). Yield 7.20 g (50%) of a yellow oil. 1 H NMR (CDCl3, 400MHz): δ7.75(dd,J=0.9,7.4Hz,1H),7.20-7.49(m,4H),7.11(d,J=1.9Hz,1H),6.85(d,J =1.7Hz,1H),4.44(d,J=15.0Hz,2H),3.21(s,3H),2.30(s,3H),1.47(s,9H),1.15(s,6H),1.20(s,6H).

[0563] 3-tert-Butyl-2'-(6-((2,6-diisopropylphenylamino)methyl)pyridin-2-yl)-5-methylbiphenyl-2-ol

[0564]

[0565] To a solution of 2.63 g (6.41 mmol) of 2-(3'-(tert-butyl)-2'-(methoxymethoxy)-5'-methyl-[1,1'-biphenyl]-2-yl)-4,4,5,5-tetramethyl-1,3,2-dioxaborolane and 2.23 g (6.41 mmol) of N-[(6-bromopyridin-2-yl)methyl]-2,6-diisopropylaniline in 30 mL of dioxane was added 5.23 g (16.04 mmol) of cesium carbonate and 20 mL of water. The resulting mixture was purged with argon for 30 minutes and then 370 mg (0.321 mmol) of Pd(PPh3)4 was added. The mixture was stirred at 95°C for 12 hours. The mixture was cooled to room temperature and then 50 mL of water was added. 50 mL of diethyl ether was added to the resulting two-phase mixture. The organic layer was separated and washed with brine. The solution produced was dried over Na2SO4 and then evaporated to dryness. The oil produced was subsequently added with 40mL of tetrahydrofuran, 40mL of methanol and 2.0mL of 12N hydrochloric acid. The reaction mixture was stirred overnight at 60°C and then poured into 200mL of water. Sodium bicarbonate was added until pH~7. The mixture obtained was extracted with dichloromethane (3×50mL), and the organic extracts combined were dried over Na2SO4 and then evaporated to dryness. The residue was purified by flash chromatography on silica gel 60 (40-63 microns, eluent: hexane-ethyl acetate-triethylamine=100:10:1 volume). Yield 1.50g (46%). 1 H NMR(CDCl3,400MHz): δ7.91(s,1H),7.54-7.59(m,2H),7.47-7.50(m,2H),7.3 0-7.32(m,1H),7.24(d,J=8.2Hz,1H),7.04-7.11(m,4H),7.02(d,J=1.9Hz,1H ),6.75(d,J=1.6Hz,1H),4.17-4.26(m,2H),3.81(br.s.,1H),3.25(sept,J=6 .8Hz,2H),2.23(s,3H),1.34(s,9H),1.20(d,J=6.8,6H),1.18(d,J=6.8,6H).

[0566] Hafnium dimethyl[3-tert-butyl-2'-(6-((2,6-diisopropylphenylamino)methyl)pyridin-2-yl)-5-methylbiphenyl-2-phenolate](CAT 1)

[0567]

[0568] To a suspension of 320 mg (1.00 mmol) of hafnium tetrachloride in 30 mL of dry toluene was added 1.67 mL (4.50 mmol, 2.7 M) of MeMgBr in diethyl ether at room temperature. The resulting suspension was stirred for 20 minutes. A solution of 500 mg (1.00 mmol) of 3-tert-butyl-2'-(6-((2,6-diisopropylphenylamino)methyl)pyridin-2-yl)-5-methylbiphenyl-2-phenol in 10 mL of dry toluene was then added dropwise over 5 minutes. The mixture was stirred at room temperature overnight and then evaporated to near dryness. The obtained solid was extracted with 2×20 mL of hot methylcyclohexane, and the combined organic extracts were filtered through a thin pad of Celite 503. Next, the filtrate was evaporated to dryness. The resulting solid was washed with 5 mL of n-pentane and then dried in vacuo. Yield 520 mg (73%) of white solid. C 37 H 46 Anal. Calcd. for HfN2O: C, 62.30, H, 6.50, N, 3.93. Found: C 62.46, H 6.68, N 3.74. 1 H NMR (C6D6, 400MHz): δ7.23-7.33(m,4H),7.17-7.21(m,1H),7.08-7.14(m,2H),6.99-7.08(m,1H),6.91(dd,J=0.6 7,2.33Hz,1H),6.66-6.73(m,1H),6.59(t,J=7.71Hz,1H),6.50(dd,J=1.00,7.54Hz,1H),6.24-6.30(m,1H),5.13( d,J=19.96Hz,1H),4.76(d,J=19.96Hz,1H),4.37(spt,J=6.84Hz,1H),3.78(spt,J=6.71Hz,1H),2.18(s,3H),1.53 -1.58(m,12H),1.50(d,J=6.76Hz,3H),1.40(d,J=6.88Hz,3H),1.22(d,J=6.88Hz,3H),0.30(s,3H),-0.03(s,3H). 13C NMR(CDCl3,100MHz): δ161.85,159.75,157.72,148.81,145.80,140.11,138.59, 137.83,137.41,132.38,130.94,130.82,129.20,129.02,128.83,128.22,127.6 1,126.90,126.88,125.28,125.02,124.07,123.86,123.49,119.48,66.10,53.44,49.10,34.54,29.88,27.67,27.35,27.16,26.70,24.92,24.09,21.47,20.82.

[0569] Catalyst 2 Synthesis

[0570] 3',5'-di-tert-butyl-2-(methoxymethoxy)-5-methyl-1,1'-biphenyl

[0571]

[0572] Vacuum dried magnesium chips (6.30 g, 259 mmol) were combined with 100 mL of dry tetrahydrofuran. The mixture was heated to 60 ° C. Then a solution of 69.8 g (259 mmol) of 3,5-di-tert-butyl-bromobenzene in 400 mL of dry tetrahydrofuran was added dropwise over 30 minutes. The resulting solution was heated to reflux for 1 hour and then cooled to room temperature. In addition, 50.0 g (216 mmol) of 2-bromo-1-(methoxymethoxy)-4-methylbenzene and 0.7 g (1.3 mmol) of Pd (P t The resulting mixture was stirred overnight at 60° C. and then poured into 500 mL of water. The crude product was extracted with 3×400 mL of dichloromethane. The combined organic extracts were dried over Na 2 SO 4 and evaporated to near dryness. The residue was distilled using a Kugelrohr apparatus (90° C., 0.3 mbar) to produce 73.0 g (99%) of the desired product as a colorless oil. 1 H NMR (CDCl3, 400MHz): δ7.40-7.47(m,3H),7.22(d,J=1.65Hz,1H),7.11-7.19(m,2H),5.11(s,2H),3.43(s,3H),2.40(s,3H),1.42(s,18H).

[0573] 2-(3',5'-di-tert-butyl-2-(methoxymethoxy)-5-methyl-[1,1'-biphenyl]-3-yl)-4,4,5,5-tetramethyl-1,3,2-dioxaborolane

[0574]

[0575] A solution was prepared from 30.0 g (88.1 mmol) of 3',5'-di-tert-butyl-2-(methoxymethoxy)-5-methyl-1,1'-biphenyl and 1,000 mL of diethyl ether. The mixture was cooled to 0°C. To the cooled mixture was added dropwise 70.5 mL (176 mmol, 2.5 M) of n BuLi. The resulting suspension was stirred at room temperature for 3 hours, then 53.9 mL (264 mmol) of 2-isopropoxy-4,4,5,5-tetramethyl-1,3,2-dioxaborolane was added at -50°C in one portion. The resulting mixture was stirred at room temperature overnight, then poured into 1,000 mL of water. The crude product was extracted with 3×500 mL of dichloromethane. The combined organic extracts were dried over Na2SO4 and evaporated to near dryness. The residue was triturated with 30 mL of methanol, and the precipitate obtained was filtered off and then washed with 30 mL of methanol. The precipitate was dried in vacuo to produce 26.1 g (64%) of the target product as a white solid. 1 H NMR (CDCl3, 400MHz): δ7.61(s,1H),7.34-7.44(m,3H),7.26-7.31(m,1H),4.82(s,2H),2.81(s,3H),2.38(s,3H),1.39(m,30H).

[0576] 2-Bromo-3",5"-di-tert-butyl-2'-(methoxymethoxy)-5'-methyl-1,1':3',1"-terphenyl

[0577]

[0578] To a solution of 13.0 g (27.9 mmol) of 2-(3',5'-di-tert-butyl-2-(methoxymethoxy)-5-methyl-[1,1'-biphenyl]-3-yl)-4,4,5,5-tetramethyl-1,3,2-dioxaborolane in 100 mL of 1,4-dioxane was added 8.69 g (30.7 mmol) of 1-bromo-2-iodobenzene, 9.63 g (69.7 mmol) of potassium carbonate and 50 mL of water. The obtained mixture was purged with argon for 10 minutes and then 1.61 g (1.39 mmol) of Pd(PPh3)4 was added. The mixture was stirred at 90°C for 12 hours, then cooled to room temperature and diluted with 50 mL of water. The obtained mixture was extracted with dichloromethane (3×100 mL). The combined organic extracts were dried over Na2SO4 and then evaporated to dryness. The residue was purified by flash chromatography on silica gel 60 (40-63 μm; eluent: hexane). Yield 12.0 g (87%) of a colorless glassy oil. 1 H NMR (CDCl3, 400MHz): δ7.72 (d, J = 7.98Hz, 1H), 7.47-7.54 (m, 3H), 7.33-7.47 (m, 2H), 7.19-7. 31(m,2H),7.09(d,J=1.65Hz,1H),4.29-4.42(m,2H),2.63(s,3H),2.44(s,3H),1.41(s,18H).

[0579] 2-(3',5'-di-tert-butyl-2-(methoxymethoxy)-5-methylbiphenyl-3-yl)-4,4,5,5-tetramethyl-1,3,2-dioxaborolane

[0580]

[0581] A solution of 3.00 g (6.06 mmol) of 2-bromo-3",5"-di-tert-butyl-2'-(methoxymethoxy)-5'-methyl-1,1':3',1"-terphenyl in 50 mL of tetrahydrofuran was cooled to -78°C. To this cold mixture was added dropwise 2.5 mL (6.24 mmol, 2.5 M) of n BuLi. The resulting solution was stirred at -78°C for 1 hour, then 1.9 mL (9.09 mmol) of 2-isopropoxy-4,4,5,5-tetramethyl-1,3,2-dioxaborolane was added at -78°C in one portion. The resulting mixture was stirred at room temperature overnight, then poured into 50 mL of water. The crude product was extracted with 3×30 mL of dichloromethane. The combined organic extracts were dried over Na2SO4 and evaporated to dryness. Yield 3.22 g (98%) of a colorless glassy oil. 1H NMR (CDCl3, 400MHz): δ7.75 (d, J = 7.3Hz, 1H), 7.42-7.47 (m, 3H), 7.29-7.38 (m, 3H), 7.15 (s,1H),7.08(s,1H),4.24(s,2H),2.55(s,3H),2.38(s,3H),1.35(s,18H),1.25(s,12H).

[0582] 3-(3,5-di-tert-butylphenyl)-2'-(6-((2,6-diisopropylphenylamino)methyl)pyridin-2-yl)-5-methylbiphenyl-2-ol

[0583]

[0584] To 2.06g (3.80mmol) of 2-(3', 5'-di-tert-butyl-2-(methoxymethoxy)-5-methylbiphenyl-3-yl)-4,4,5,5-tetramethyl-1,3,2-dioxaborolane and 1.20g (3.46mmol) of N-[(6-bromopyridin-2-yl)methyl]-2,6-diisopropylaniline in 30mL of 1,4-dioxane was added 4.23g (12.97mmol) of cesium carbonate and 20mL of water. After purging the obtained mixture with argon for 30 minutes, 370mg (0.321mmol) of Pd(PPh3)4 was added. This mixture was stirred at 95°C for 12 hours, then cooled to room temperature and diluted with 50mL of water. 50mL of diethyl ether was added to the obtained two-phase mixture. The organic layer was separated and washed with brine. The solution produced was dried over Na2SO4 and then evaporated to dryness. 40mL of tetrahydrofuran, 40mL of methanol and 1.8mL of 12N hydrochloric acid were added to the produced oil. The reaction mixture was stirred overnight at 60°C and then poured into 200mL of water. Sodium bicarbonate was added until pH~7. The mixture obtained was extracted with dichloromethane (3×50mL), and the combined organic extracts were dried over Na2SO4 and then evaporated to dryness. Residue was purified by flash chromatography on silica gel 60 (40-63 microns, eluent: hexane-ethyl acetate-triethylamine=100:10:1 volume). Yield 1.81g (82%) colorless glassy oil. 1H NMR (CDCl3, 400MHz): δ7.76-7.78(m,1H),7.46-7.53(m,4H),7.36-7.37(m,1H),7.19-7.20(m,2H),7.12(d,J=8.1Hz,1H),7.04-7.09(m,5H),6 .97(br.s.,1H),6.69(br.s.,1H),4.16(s,2H),3.95(br.s.,1H),3.24(sept,J=6.9Hz,2H),2.31(s,3H),1.31(s,18H),1.15(d,J=6.9Hz,12H).

[0585] Hafnium dimethyl[3-(3,5-di-tert-butylphenyl)-2'-(6-((2,6-diisopropylphenylamino)methyl)pyridin-2-yl)-5-methylbiphenyl-2-phenolate](CAT 2)

[0586]

[0587] To a suspension of 250 mg (0.782 mmol) of hafnium tetrachloride in 30 mL of dry toluene was added 1.30 mL (3.52 mmol, 2.7 M) of MeMgBr in diethyl ether at room temperature. The resulting suspension was stirred for 20 minutes. A solution of 500 mg (1.00 mmol) of 3-(3,5-di-tert-butylphenyl)-2'-(6-((2,6-diisopropylphenylamino)methyl)pyridin-2-yl)-5-methylbiphenyl-2-phenol in 10 mL of dry toluene was then added dropwise over 5 minutes. The reaction mixture was stirred overnight at room temperature and then evaporated to near dryness. The obtained solid was extracted with 2×20 mL of hot methylcyclohexane, and the combined organic extracts were filtered through a thin pad of Celite 503. Next, the filtrate was evaporated to dryness. The resulting solid was washed with 5 mL of n-pentane and then dried in vacuo. Yield 560 mg (85%) of white solid. C 47 H 58 Anal. Calcd. for HfN2O: C, 66.77, H, 6.91, N, 3.31. Found: C 67.00, H 7.02, N 3.18. 1H NMR(C6D6,400MHz): δ7.76(t,J=7.76Hz,1H),7.53-7.60(m,1H),7.37-7.49(m,3H),7.32(t,J=1.66Hz,1H),7.2 2-7.28(m,1H),7.14-7.22(m,3H),7.08-7.14(m,1H),7.01-7.08(m,1H),6.98(d,J=2.22Hz,1H),6.93(dd,J=1.5 5,7.54Hz,1H),6.82(d,J=2.22Hz,1H),4.70-4.88(m,2H),3.84-4.01(m,1H),2.59(spt,J=6.76Hz,1H),2.24(s ,3H),1.21-1.51(m,21H),1.18(d,J=6.88Hz,3H),0.94(d,J=6.88Hz,3H),0.33(d,J=6.76Hz,3H),-0.53(s,6H). 13 C NMR (CDCl3, 100MHz): δ162.40,160.09,155.88,148.47,145.41,145.04,139.80,13 8.89,138.40,138.02,132.91,132.07,131.93,131.11,130.72,129.20,129.03,12 8.95,128.22,127.94,127.04,125.29,124.83,123.58,123.54,122.08,119.83,67.04,54.60,47.54,34.89,31.67,27.67,27.39,26.25,26.14,24.95,23.30,20.40.

[0588] Catalyst 3 Synthesis

[0589] 4-(9H-carbazol-9-yl)-2-methyl-6H-dibenzo[c,e][1,2]oxaborinin-6-ol

[0590]

[0591] To 900 mg (37.1 mmol) of vacuum dried magnesium powder was added 50 mL of dry tetrahydrofuran and 2.94 g (7.42 mmol) of 1-bromo-3-(9H-carbazole-9-yl)-2-(methoxymethoxy)-5-methylbenzene. The reaction mixture was stirred at 55 ° C overnight, and then a solution of 1.49 g (7.79 mmol) of 1-bromo-2-chlorobenzene in 20 mL of tetrahydrofuran was added dropwise over 3 hours. The obtained suspension was stirred at 55 ° C overnight, and then 2.07 g (11.1 mmol) of 2-isopropoxy-4,4,5,5-tetramethyl-1,3,2-dioxaborolane was added after it was cooled to 0 ° C. The resulting mixture was stirred at room temperature overnight, and then 100 mL of water was poured. The crude product was extracted with 3×100 mL of dichloromethane. The combined organic extracts were dried over Na2SO4 and then evaporated to near dryness. The residue was purified by flash chromatography on silica gel 60 (40-63 μm; eluent: hexane-ethyl acetate = 10:1 by volume). Yield 1.05 g (36%) of dark red oil. 1 H NMR (CDCl3, 400MHz): δ8.26 (d, J = 8.32Hz, 1H), 8.12-8.17 (m, 2H), 8.11 (d, J = 2.11Hz, 1H), 8.06 (dd, J = 0.94, 7.49Hz, 1H), 7.73-7.80 ( m,1H),7.49(dt,J=0.89,7.37Hz,1H),7.35-7.40(m,3H),7.24-7.30(m,2H),7.17(td,J=0.79,8.18Hz,2H),4.29(s,1H),2.53(s,3H).

[0592] 3-(9H-carbazol-9-yl)-2'-(6-{[(2,6-diisopropylphenyl)amino]methyl}pyridin-2-yl)-5-methylbiphenyl-2-ol

[0593]

[0594] To a solution of 0.77 g (2.05 mmol) of 4-(9H-carbazole-9-yl)-2-methyl-6H-dibenzo[c,e][1,2]oxaborolane-6-ol in 8 mL of 1,4-dioxane was added 0.71 g (2.05 mmol) of N-[(6-bromopyridin-2-yl)methyl]-2,6-diisopropylaniline, 1.66 g (69.7 mmol) of cesium carbonate and 4 mL of water. After purging the obtained mixture with argon for 10 minutes, 0.119 g (0.10 mmol) of Pd(PPh3)4 was added. This mixture was stirred at 90°C for 12 hours, then cooled to room temperature and diluted with 20 mL of water. The obtained mixture was extracted with dichloromethane (3×30 mL). The combined organic extracts were dried over Na2SO4 and then evaporated to dryness. The residue was purified by flash chromatography on silica gel 60 (40-63 μm; eluent: hexane-ethyl acetate = 15:1). Yield 0.95 g (75%) of a white solid. 1 H NMR (CDCl3, 400MHz): δ8.13 (d, J = 7.98Hz, 2H), 7.64-7.76 (m, 2H), 7.51-7.63 (m, 3H), 7.23-7.51 (m, 7H), 7.19-7.23 (m, 1H), 7.14 -7.17(m,1H),7.04-7.09(m,3H),3.97(s,2H),3.78(br.s.,1H),3.12(spt,J=6.82Hz,2H),2.35(s,3H),1.10(d,J=6.88Hz,12H).

[0595] Hafnium dimethyl[3-(9H-carbazol-9-yl)-2'-(6-((2,6-diisopropylphenylamino)methyl)pyridin-2-yl)-5-methylbiphenyl-2-phenolate](CAT 3)

[0596]

[0597] To a suspension of 156 mg (0.487 mmol) of hafnium tetrachloride in 30 mL of dry toluene was added 0.755 mL (2.20 mmol, 2.7 M) of MeMgBr in diethyl ether at room temperature. The resulting suspension was stirred for 20 minutes. A solution of 300 mg (1.00 mmol) of 3-(9H-carbazole-9-yl)-2'-(6-((2,6-diisopropylphenylamino)methyl)pyridin-2-yl)-5-methylbiphenyl-2-phenol in 10 mL of dry toluene was then added dropwise over 5 minutes. The reaction mixture was stirred overnight at room temperature and then evaporated to near dryness. The obtained solid was extracted with 2×20 mL of boiling methylcyclohexane, and the combined organic extracts were filtered through a thin pad of Celite 503. Next, the filtrate was evaporated to dryness. The resulting solid was washed with 5 mL of n-pentane and then dried in vacuo. Yield 257 mg (64%) of white solid. C 45 H 45 Anal. Calcd. for HfN3O: C, 65.72, H, 5.52, N, 5.11. Found: C 65.95, H 5.67, N 4.98. 1 H NMR (C6D6, 400MHz): δ8.15(d,J=7.65Hz,1H),8.07-8.12(m,1H),7.49(d,J=8.10Hz,1H),7.43(dd,J=1.22,7.65Hz,1H),7. 17-7.37(m,5H),7.07-7.14(m,5H),6.79(dd,J=1.33,7.65Hz,1H),6.62-6.73(m,2H),6.49-6.59(m,2H),6.23-6.34(m,1H ),4.79(d,J=19.96Hz,1H),4.54(d,J=19.96Hz,1H),4.09(spt,J=6.88Hz,1H),2.33(spt,J=6.84Hz,1H),1.93-2.04(m,3H ),1.41(d,J=6.88Hz,3H),1.11(d,J=6.88Hz,3H),1.00(d,J=6.76Hz,3H),0.82-0.89(m,3H),-0.07(s,3H),-0.57(s,3H). 13C NMR(C6D6,100MHz): δ162.90,160.23,156.34,147.75,147.21,146.12,142.72,142.56,139.1 7,138.98,138.48,133.97,131.21,130.79,130.49,130.04,129.68,128.89,127.85,127.01, 126.32,125.71,125.19,124.87,124.30,124.22,123.98,121.39,120.73,120.58,120.23,119.88,112.16,109.59,66.27,55.05,50.74,28.44,28.26,28.18,27.26,25.35,23.80,20.73.

[0598] Catalyst 4 Synthesis

[0599] 1-(6-(3",5"-di-tert-butyl-2'-(methoxymethoxy)-5'-methyl-[1,1':3',1"-terphenyl]-2-yl)pyridin-2-yl)-N-(2,6-diisopropylphenyl)methylaniline

[0600]

[0601] To 1.50g (2.76mmol) of 2-(3',5'-di-tert-butyl-2-(methoxymethoxy)-5-methylbiphenyl-3-yl)-4,4,5,5-tetramethyl-1,3,2-dioxaborolane solution in 20mL of toluene was added 0.96g (2.76mmol) of N-[-(6-bromopyridin-2-yl)methylene]-2,6-diisopropylaniline, 0.73g (6.90mmol) of sodium carbonate, 15mL of water and 5mL of methanol. After purging the obtained mixture with argon for 10 minutes, 0.16g (0.14mmol) of Pd(PPh3)4 was added. The mixture was stirred at 90°C for 12 hours, then cooled to room temperature and diluted with 50mL of water. The obtained mixture was extracted with dichloromethane (3×60mL). The combined organic extracts were dried by Na2SO4 and then evaporated to dryness. The residue was purified by flash chromatography on silica gel 60 (40-63 μm; eluent: hexane-ethyl acetate = 15:1). Yield 1.47 g (78%) of a yellow solid. 1H NMR (CDCl3, 400MHz): δ8.15-8.32(m,2H),7.81-7.93(m,2H),7.61-7.81(m,2H),7.45-7.61(m,5H),7.31-7.43(m,2H),7.23-7.31(m,3H) ,6.95-7.23(m,12H),4.16(d,J=7.10Hz,2H),2.81-3.01(m,2H),2.48(s,3H),2.36-2.39(m,5H),1.28-1.32(m,18H),1.06-1.16(m,12H).

[0602] 3”,5”-di-tert-butyl-2-(6-(((2,6-diisopropylphenyl)amino)(2-isopropylphenyl)methyl)pyridin-2-yl)-5'-methyl-[1,1':3',1"-terphenyl]-2'-phenol

[0603]

[0604] To a solution of 1.44 g (2.11 mmol) of 1-(6-(3",5"-di-tert-butyl-2'-(methoxymethoxy)-5'-methyl-[1,1':3',1"-terphenyl]-2-yl)pyridin-2-yl)-N-(2,6-diisopropylphenyl)methylaniline in 100 mL of diethyl ether was added 0.80 g (6.34 mmol) of (2-isopropylphenyl)lithium. The resulting solution was stirred at room temperature overnight, and then poured into 200 mL of water. To the obtained two-phase mixture was added 100 mL of diethyl ether. The organic layer was separated and washed with brine. The reaction mixture was evaporated to room temperature by heating for 24 hours. 4Dry the resulting solution and then evaporate to dryness. Add 70mL of tetrahydrofuran, 70mL of methanol and 1.9mL of 12N hydrochloric acid to the resulting oil. The reaction mixture was stirred overnight at 60°C and then poured into 200mL of water. Sodium bicarbonate was added until pH~7. The obtained mixture was extracted with dichloromethane (3×50mL), and the combined organic extracts were dried over Na2SO4 and then evaporated to dryness. The residue was purified by flash chromatography on silica gel 60 (40-63 microns; eluent: hexane-ethyl acetate=10:1 volume). Yield 1.45g (91%) of white foam. 1H NMR (CDCl3, 400MHz): δ7.29-7.57(m,6H),7.08-7.23(m,5H),6.85-7.08(m,7H),6.63-6.85(m,1H),5.29-5.59(m,1H),3.16-3.45(m, 1H),3.02-3.16(m,1H),2.89-3.02(m,1H),2.87(br.s.,1H),2.77(br.s.,1H),2.14-2.43(m,3H),1.32(s,18H),0.73-1.03(m,18H).

[0605] Hafnium dimethyl[3”,5”-di-tert-butyl-2-(6-(((2,6-diisopropylphenyl)amino)(2-isopropylphenyl)methyl)pyridin-2-yl)-5'-methyl-[1,1':3',1”-terphenyl]-2'-phenolate](CAT 4)

[0606]

[0607] To a suspension of 211 mg (0.660 mmol) of hafnium tetrachloride in 30 mL of dry toluene was added 1.02 mL (2.97 mmol, 2.9 M) of MeMgBr in diethyl ether in one portion at room temperature. The resulting suspension was stirred for 20 minutes. A solution of 500 mg (0.66 mmol) of 3",5"-di-tert-butyl-2-(6-(((2,6-diisopropylphenyl)amino)(2-isopropylphenyl)methyl)pyridin-2-yl)-5'-methyl-[1,1':3',1"-terphenyl]-2'-phenol in 10 mL of dry toluene was then added dropwise over 5 minutes. The reaction mixture was stirred at room temperature overnight and then evaporated to near dryness. The obtained solid was extracted with 2×20 mL of hot methylcyclohexane, and the combined organic extracts were filtered through a thin pad of Celite 503. Next, the filtrate was evaporated to dryness. The resulting solid was washed with 5 mL of n-pentane and then dried in vacuo. Yield 198 mg (31%, approximately 80% pure mixture of isomers) of a dark yellow powder. 1H NMR (C6D6, 400MHz): δ7.47 (t, J = 1.77Hz, 1H), 7.18-7.42 (m, 3H), 6.87-7.14 (m, 8H), 6.72-6.82 (m, 1H) ,6.47-6.72(m,2H),6.26-6.47(m,2H),4.04-4.13(m,1H),3.15(td,J=6.58,13.56Hz,1H),2.74-3.02( m,1H),2.15-2.26(m,2H),2.02-2.15(m,1H),1.96(br.s.,1H),1.40-1.58(m,11H),1.18-1.39(m,15H ),1.06-1.16(m,3H),1.05(d,J=7.54Hz,1H),0.68-0.97(m,4H),0.48-0.68(m,5H),0.03-0.39(m,6H).

[0608] Catalyst 5 Synthesis

[0609] N-(2,6-Dibromo-4-methylphenyl)-N'-methylurea

[0610]

[0611] A solution was prepared from 92.0 g (347 mmol) of 2,6-dibromo-4-methylaniline and 2,000 mL of dry o-xylene. 123 g (296 mmol) of triphosgene was added to the mixture at room temperature in several portions. The reaction mixture was gently heated to 110 ° C and stirred at this temperature for 40 minutes (note: phosgene generation). The mixture was heated to reflux for 8 hours and then evaporated to dryness. The residue was diluted with 400 mL of dichloromethane and then 300 mL of 40% methylamine in water was added. The resulting suspension was stirred for 30 minutes, and the obtained product was then collected on a glass frit (G3). The precipitate was washed with methanol (300 mL) and then dried under reduced pressure. Yield 88.2 g (79%) of colorless solid. 1 H NMR (DMSO-d6): δ7.87 (br.s, 1H), 7.49 (s, 2H), 6.08 (br.s, 1H), 2.59 (d, J = 4.1Hz, 3H), 2.27 (s, 3H).

[0612] N-(2,6-Dibromo-4-methylphenyl)-N-(4-methoxybenzyl)-N'-methylurea

[0613]

[0614] A suspension of 88.0 g (273 mmol) of N-(2,6-dibromo-4-methylphenyl)-N'-methylurea in 1,000 mL of dry toluene was cooled to -25 ° C. To the suspension was added dropwise 111 mL (279 mmol, 2.5 M) of n-butyl lithium in hexane. The reaction mixture was stirred at room temperature for 3 hours and then evaporated to dryness. After the residue was diluted with 1,000 mL of dry tetrahydrofuran, 55.4 g (347 mmol) of 4-methoxybenzyl chloride and 50 mL of HMPA were added. The obtained mixture was stirred at 60 ° C for 18 hours, then cooled to room temperature and poured into 2,000 mL of water. The crude product was extracted with toluene (3 × 300 mL). The combined organic extracts were dried over Na2SO4, then passed through a pad of silica gel 60 (40-63 microns, 100 mL), and the eluent obtained was evaporated to dryness. The residue was washed with 120 mL of diethyl ether and the crystalline material thus obtained was dried under reduced pressure. Yield 78.0 g (64%) of a colorless crystalline solid. 1 H NMR (CDCl3): δ7.36(s,2H),7.14-7.17(m,2H),6.69-6.73(m,2H),4.75(s,2H),3.93(br.s,1H),3.74(s,3H),2.75(d,J=4.68Hz,3H),2.29(s,3H).

[0615] 4-Bromo-3-(4-methoxybenzyl)-1,6-dimethyl-1,3-dihydro-2H-benzimidazol-2-one

[0616]

[0617] A solution was prepared from 78.0 g (176 mmol) of N-(2,6-dibromo-4-methylphenyl)-N-(4-methoxybenzyl)-N'-methylurea and 1,200 mL of freshly distilled DMSO. To this mixture was added 19.8 g (352 mmol) of KOH. The mixture was stirred at 40° C. for 48 hours and then poured into 2,000 mL of water. The crude product was extracted with diethyl ether (3×400 mL). The combined organic extracts were dried over Na2SO4 and then passed through a pad of silica gel 60 (40-63 microns, 100 mL). The eluent obtained was evaporated to dryness. The residue was washed with 120 mL of diethyl ether and the crystalline material thus obtained was dried under reduced pressure. Yield 43.4 g (69%) of colorless crystals. 1H NMR (CDCl3): δ7.19-7.23(m,2H),6.99(m,1H),6.79-6.82(m,2H),6.72(m,1H),5.39(s,2H),3.75(s,3H),3.40(s,3H),2.34(s,3H).

[0618] 4-[(2,6-Diisopropylphenyl)amino]-1,6-dimethyl-1,3-dihydro-2H-benzimidazol-2-one

[0619]

[0620] A solution was prepared by 22.0 mL (124 mmol) of 2,6-diisopropylaniline and 900 mL of dry toluene. 45.5 mL (147 mmol, 2.5 M) of n-butyllithium was added dropwise to the mixture. The obtained suspension was heated to 100 ° C and then cooled to room temperature. 1.78 g (3.10 mmol) of Pd (dba) 2, 2.96 g (6.20 mmol) of XPhos and 37.3 g (103 mmol) of 4-bromo-3- (4-methoxybenzyl) -1,6-dimethyl -1,3-dihydro -2H- benzimidazole -2-one were added to the reaction mixture. The dark brown suspension thus obtained was heated to 100 ° C for 48 hours and then poured into 500 ml of water. The organic layer was separated, dried by Na2SO4 and then evaporated to dryness. The oil obtained is dissolved in a mixture of 340 mL of dichloromethane, 250 mL of trifluoroacetic acid and 75 mL of trifluoromethanesulfonic acid. The mixture is stirred at room temperature for 48 hours and then gently poured into a solution of 700 g of K2CO3 in 2000 mL of water. The organic layer is separated and the aqueous phase is additionally extracted with 3 × 400 ml of dichloromethane. The combined organic extracts are dried over Na2SO4 and then evaporated to dryness. The resulting solid is ground with 100 mL of diethyl ether and the suspension thus obtained is filtered off on a glass frit (G3). The precipitate is dried under reduced pressure. The yield is 24.6 g (71%) of white solid. 1 HNMR(CDCl3): δ7.28-7.32(m,1H), δ7.21-7.23(m,2H),6.66(br.s,1H),6.05(s,1 H),5.73(s,1H),3.43(br.s,2H),2.54(br.s,3H),2.20(s,3H),1.13(br.s,12H).

[0621] 2-Chloro-N-(2,6-diisopropylphenyl)-1,6-dimethyl-1H-benzimidazol-4-amine

[0622]

[0623] The flask was charged with 400 mL of phosphorus oxychloride. To this was added 24.6 g (73.0 mmol) of 4-[(2,6-diisopropylphenyl)amino]-1,6-dimethyl-1,3-dihydro-2H-benzimidazol-2-one at a time. The resulting suspension was heated at 105° C. for 40 hours and then evaporated to dryness. The resulting oil was ground with 200 mL of diethyl ether. The obtained solution was washed with 200 mL of water, dried over Na2SO4 and then evaporated to dryness. The solid formed was ground with 30 mL of cold n-hexane and the solid thus obtained was collected on a glass frit (G3). The product was dried under reduced pressure. Yield 18.9 g (73%) of a yellow-green solid. 1 H NMR(CDCl3): δ7.31-7.35(m,1H), δ7.23-7.25(m,2H),6.43(m,1H),6.10(br.s,1H),5.7 6(m,1H),3.71(s,3H),3.32(sept,J=6.94Hz,2H),2.26(s,3H),1.13(d,J=6.94Hz,12H).

[0624] 3-tert-butyl-2'-{4-[(2,6-diisopropylphenyl)amino]-1,6-dimethyl-1H-benzimidazol-2-yl}-5-methylbiphenyl-2-

[0625]

[0626] To a solution of 2.00 g (4.88 mmol) of 2-(3'-(tert-butyl)-2'-(methoxymethoxy)-5'-methyl-[1,1'-biphenyl]-2-yl)-4,4,5,5-tetramethyl-1,3,2-dioxaborolane and 1.69 g (4.75 mmol) of 2-chloro-N-(2,6-diisopropylphenyl)-1,6-dimethyl-1H-benzimidazol-4-amine in 30 mL of 1,4-dioxane was added 4.00 g (12.27 mmol) of cesium carbonate and 20 mL of water. After purging the resulting mixture with argon for 30 minutes, 370 mg (0.321 mmol) of Pd(PPh3)4 was added. This mixture was stirred at 95°C for 12 hours, then cooled to room temperature and diluted with 50 mL of water. 50 mL of diethyl ether was added to the obtained two-phase mixture. The organic layer is separated and washed with brine. The solution produced is dried by Na2SO4 and then evaporated to dryness. 40mL of tetrahydrofuran, 40mL of methanol and 1.9mL of 12N hydrochloric acid are added to the oil produced. The reaction mixture is stirred overnight at 60°C and then poured into 200mL of water. Sodium bicarbonate is added until pH~7. The mixture obtained is extracted with dichloromethane (3×50mL), and the organic extracts combined are dried and then evaporated to dryness by Na2SO4. The residue is purified by flash chromatography on silica gel 60 (40-63 microns, eluent: hexane-ethyl acetate-triethylamine=100:10:1 volume). Yield 950mg (36%) colorless glassy oil. 1 H NMR (CDCl3, 400MHz): δ7.55-7.59(m,1H),7.46-7.52(m,2H),7.42(dd,J1=7.6Hz ,J2=0.83Hz,1H),7.31–7.35(m,1H),7.23-7.25(m,2H),7.02(d,J=1.89Hz,1H),6 .79(d,J=2.2Hz,1H),6.43(s,1H),6.05(s,1H),5.77(d,J=0.89Hz,1H),3.47(s, 3H),3.21(br.s,2H),2.24(s,3H),2.23(s,3H),1.37(s,9H),1.05-1.18(m,12H).

[0627] Hafnium dimethyl[3-tert-butyl-2'-{4-[(2,6-diisopropylphenyl)amino]-1,6-dimethyl-1H-benzimidazol-2-yl}-5-methylbiphenyl-2-phenolate](CAT 5)

[0628]

[0629] 0.830mL (2.41mmol, 2.9M) of MeMgBr in diethyl ether was added to a suspension of 172mg (0.536mmol) of hafnium tetrachloride in 30mL of dry toluene at room temperature. The resulting suspension was stirred for 20 minutes, and a solution of 300mg (0.536mmol) of 3-tert-butyl-2'-{4-[(2,6-diisopropylphenyl)amino]-1,6-dimethyl-1H-benzimidazol-2-yl}-5-methylbiphenyl-2-phenol in 10mL of dry toluene was added dropwise over 5 minutes. The reaction mixture was stirred at room temperature overnight and then evaporated to near dryness. The solid obtained was extracted with 2×20mL of boiling methylcyclohexane, and the combined organic extracts were filtered through a thin pad of Cel i te 503. Next, the filtrate was evaporated to dryness. The resulting solid was washed with 5mL of n-pentane and then dried in a vacuum. Yield 204 mg (50%) of yellow solid. 40 H 49 Anal. Calcd. for HfN3O: C, 62.69, H, 6.45, N, 5.48. Found: C 62.92, H 6.57, N 5.36. 1 H NMR (C6D6, 400MHz): δ7.39-7.46 (m, 1H), 7.28-7.38 (m, 3H), 7.25 (d, J = 2.00Hz, 1H), 6.99-7.14 (m, 2H), 6 .95(dt,J=1.28,7.57Hz,1H),6.74(dd,J=0.67,2.33Hz,1H),6.25(dd,J=1.00,7.76Hz,1H),5.80-5.87(m ,2H),4.17(sept,J=6.76Hz,1H),3.54-3.68(m,1H),2.72(s,3H),2.21(s,3H),2.08-2.15(m,3H),1.64-1 .74(m,8H),1.49(d,J=6.88Hz,3H),1.35-1.42(m,6H),1.10(d,J=6.76Hz,3H),0.51(s,3H),0.35(s,3H). 13C NMR(C6D6,100MHz): δ159.49,152.24,149.37,146.50,146.01,145.79,143.08,1 39.21,137.42,134.27,133.56,132.32,131.90,131.77,130.46,129.69,128.89, 127.31,126.63,126.02,124.77,124.73,108.11,98.47,57.51,53.22,35.46,31.33,30.97,29.15,28.91,27.60,27.03,26.81,25.56,25.21,23.06,21.19,14.75.

[0630] Polymerization Example

[0631] Solvents, polymer-grade toluene and / or isohexane, were supplied by ExxonMobil Chemical Co. and purified by a series of columns: two 500 cm 3 Oxyclear cylinders, then filled with dry Two 500 cm molecular sieves (8-12 mesh, Aldrich Chemical Company) were connected in series. 3 Column and packed with dry Two 500 cm molecular sieves (8-12 mesh, Aldrich Chemical Company) were connected in series. 3 column.

[0632] 1-Octene (98%) (Aldrich Chemical Company) was dried by filtration through basic alumina (Aldrich Chemical Company, Brockman Basic 1) after stirring overnight on Na-K alloy. Tri(n-octyl)aluminum (TNOA) was purchased from Aldrich Chemical Company or Akzo Nobel and used as received.

[0633] Polymerization grade ethylene was further purified by passing the ethylene through the following series of columns: 500 cm 3 Oxyclear cylinders, then filled with dry Molecular sieve (8-12 mesh, Aldrich Chemical Company) 500 cm 3 Column and packed with dry Molecular sieve (8-12 mesh, Aldrich Chemical Company) 500 cm 3 column.

[0634] Polymer grade propylene was further purified by passing the propylene through the following series of columns: 2,250 cm 3 Oxyclear cylinders, followed by Molecular sieve (8-12 mesh, Aldrich Chemical Company) 2,250 cm 3 Columns, then two in series are filled with Molecular sieve (8-12 mesh, Aldrich Chemical Company) 500 cm 3 Column, 500 cm packed with Selexsorb CD (BASF) 3 The column was then filled with Selexsorb COS (BASF) at 500 cm 3 column.

[0635] N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate (also referred to as Activator 1) was purchased from Albemarle Corporation. All complexes and activators were added to the reactor as diluent solutions in toluene. The concentrations of the solutions of activator, scavenger, and complex added to the reactor were selected so that between 40 microliters and 200 microliters of solution were added to the reactor to ensure accurate delivery.

[0636] Methylaluminoxane (MAO, also referred to as Activator 2) was purchased from Albemarle as a 10 wt % solution in toluene.

[0637] Reactor Description and Preparation. Polymerizations were performed in an inert atmosphere (N2) drybox using an autoclave equipped with an external heater for temperature control, a glass insert (internal volume of the reactor was 23.5 mL for C2 and C2 / C8 runs and 22.5 mL for C3 runs), a septum inlet, a regulated supply of nitrogen, ethylene and propylene and equipped with a disposable polyetheretherketone mechanical stirrer (800 RPM). The autoclave was prepared by purging with dry nitrogen at 110°C or 115°C for 5 hours and then at 25°C for 5 hours.

[0638] Ethylene polymerization or ethylene / 1-octene copolymerization

[0639] The reactor is prepared as described above and then purged with ethylene. Solvent (toluene, unless otherwise noted), optional 1-octene (0.1 mL when used), and optional MAO are added by syringe at room temperature and atmospheric pressure. The reactor is then brought to process temperature (typically 80°C) and ethylene is added to process pressure (typically 75 psig = 618.5 kPa or 200 psig = 1480.3 kPa) while stirring at 800 RPM. An optional scavenger solution (e.g., TNOA in isohexane) is then added to the reactor by syringe under process conditions. An optional non-coordinating activator (e.g., N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate) solution (in toluene) is added to the reactor by syringe under process conditions, followed by a precatalyst (e.g., complex or catalyst) solution (in toluene) added to the reactor by syringe under process conditions. A computer-controlled solenoid valve is used to allow ethylene to enter the autoclave to maintain the reactor gauge pressure (+ / -2 psi) during the polymerization process. The reactor temperature is monitored and typically maintained within + / -1°C. The polymerization was stopped by adding about 50 psi O2 / Ar (5 mol% O2) gas mixture to the autoclave for about 30 seconds. The polymerization was quenched after a predetermined cumulative amount of ethylene had been added or for a maximum polymerization time of 30 minutes. The reactor was cooled and vented. The polymer was separated after removing the solvent in a vacuum. The reported yield includes the total weight of the polymer and the residual catalyst. The catalyst activity is reported as grams of polymer / mmol transition metal compound / hour of reaction time (g / mmol / hr). The optional non-coordinating anion activator (e.g., N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate) solution (in toluene) was then added to the reactor by a syringe under process conditions, followed by the addition of a precatalyst (i.e., complex or catalyst) solution (in toluene) to the reactor by a syringe under process conditions. The reactor temperature was monitored and generally maintained within + / -1°C. The polymerization was stopped by adding about 50 psi O2 / Ar (5 mol% O2) gas mixture to the autoclave for about 30 seconds. The polymerization was quenched based on a predetermined pressure loss of about 8 psi or for a maximum polymerization time of 30 minutes. The reactor was cooled and vented. The polymer was isolated after removal of the solvent in vacuo. The reported yield includes the total weight of polymer and residual catalyst. The catalyst activity is reported as grams of polymer / mmol transition metal compound / hour of reaction time (gP.mmolcat -1 .h -1 ).

[0640] Propylene polymerization

[0641] The reactor was prepared as described above, then heated to 40°C and purged with propylene gas at atmospheric pressure. Solvent (toluene, unless otherwise noted), optional MAO and liquid propylene (1.0 mL) were added by syringe. The reactor was then heated to the process temperature (70°C or 100°C) while stirring at 800RPM. An optional scavenger solution (e.g., TNOA in isohexane) was then added to the reactor by syringe under process conditions. An optional non-coordinating activator (e.g., N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate) solution (in toluene) was then added to the reactor by syringe under process conditions, followed by a precatalyst (i.e., complex or catalyst) solution (in toluene) added to the reactor by syringe under process conditions. The reactor temperature was monitored and generally maintained within + / -1°C. The polymerization was stopped by adding a gas mixture of about 50psi O2 / Ar (5mol% O2) to the autoclave for about 30 seconds. The polymerization was quenched based on a predetermined pressure loss of about 8psi or a maximum polymerization time of 30 minutes. The reactor was cooled and vented. The polymer was separated after removing the solvent in a vacuum. The reported yield includes the total weight of polymer and residual catalyst. Catalyst activity is typically reported as grams of polymer per mmol of transition metal compound per hour of reaction time (g / mmol / hr).

[0642] Polymer characterization

[0643] For analytical testing, polymer sample solutions were prepared by dissolving the polymer in 1,2,4-trichlorobenzene (TCB, 99+% purity, from Sigma-Aldrich) containing 2,6-di-tert-butyl-4-methylphenol (BHT, 99%, from Aldrich) in a shaker oven at 165°C for approximately 3 hours. Typical concentrations of polymer in solution were between 0.1 mg / mL and 0.9 mg / mL, with a BHT concentration of 1.25 mg BHT / mL of TCB. Samples were cooled to 135°C for testing.

[0644] High temperature size exclusion chromatography was performed using an automated "Fast GPC" system as described in U.S. Patents 6,491,816; 6,491,823; 6,475,391; 6,461,515; 6,436,292; 6,406,632; 6,175,409; 6,454,947; 6,260,407 and 6,294,388, each of which is incorporated herein by reference. The molecular weight (weight average molecular weight (Mw) and number average molecular weight (Mn)) and molecular weight distribution (MWD = Mw / Mn), which is sometimes also referred to as the polydispersity (PDI) of the polymer, were measured by gel permeation chromatography using a Symyx Technology GPC equipped with an evaporative light scattering detector and calibrated using polystyrene standards (Polymer Laboratories: Polystyrene Calibration Kit SM-10: Mp (peak Mw) between 5,000 and 3,390,000). The samples were run using three Polymer Laboratories: PLgel 10 μm Mixed-B 300×7.5 mm columns in series at an eluent flow rate of 2.0 mL / min (135° C. sample temperature, 165° C. oven / column) (250 μL of the polymer solution in TCB was injected into the system). No column diffusion correction was used. The HPLC-MS / MS / MS / MS available from Symyx Technologies was used. Data analysis was performed using AutomationStudio software or AutomationStudio software available from Freeslate. Molecular weights obtained are relative to linear polystyrene standards.

[0645] Differential Scanning Calorimetry (DSC) measurements were performed on a TA-Q100 instrument to determine the melting points of the polymers. The samples were pre-annealed at 220°C for 15 minutes and then allowed to cool to room temperature overnight. The samples were then heated to 220°C at a rate of 100°C / min and then cooled at a rate of 50°C / min. The melting points were collected during the heating process.

[0646] Samples for infrared analysis were prepared by depositing a stabilized polymer solution onto a silanized wafer (Part No. S10860, Symyx). By this method, between approximately 0.12 and 0.24 mg of polymer were deposited on the wafer unit. The samples were subsequently analyzed on a Bruker Equinox 55 FTIR spectrometer equipped with a specular reflectance sample accessory from Pikes' MappIR. The 2 cm -1 Resolution: 32 scans were collected to cover 5,000 cm -1 Up to 500cm -1 Spectral range of the spectrum.

[0647] Tables 1, 2 and 3 illustrate the results obtained for catalysts 1 to 5 in polymerizations using N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate activator (ACT1) and methylaluminoxane (MAO) activator. Catalysts 1 to 5 are represented as follows:

[0648]

[0649] Table 1 describes the homopolymerization of ethylene using each catalyst and activator combination. General conditions for ACT 1: catalyst complex = 25 nmol, activator = 1.1 molar equivalents, 75 psig ethylene, Al(n-octyl)3 = 500 nmol, temperature = 80°C, total volume = 5 mL, solvent = toluene. General conditions for MAO: catalyst complex = 25 nmol, activator = 500 molar equivalents, 75 psig ethylene, temperature = 80°C, total volume = 5 mL, solvent = toluene.

[0650] In each case, a narrow PDI value range of 1.5-2.7 was observed for polyethylene and a high melting point temperature range of 135°C-138°C was also observed. Catalysts 2 and 3 were found to have higher average activities than the other catalysts. In particular, Catalyst 2 exhibited the highest catalyst activity with MAO (e.g., Run 10-12: 89,149 gP.mmolcat -1 .h -1 to 133,824 gP.mmolcat -1 .h -1 ) and also produced polyethylene with Mw values ​​ranging from 185,316 g / mol to 221,657 g / mol. Catalyst 3 with ACT 1 (Runs 13–15) also exhibited Mw values ​​ranging from 81,051 gP.mmolcat -1 .h -1 To 84,873 gP.mmolcat -1 .h -1 The high activity between 0.04 and 0.06 is consistent with higher values ​​of Mn, Mw, and Mz exhibited in the relative Catalyst 2 sample. As can be seen, each of the catalysts and activators appear to produce a range of high Mw, crystalline polyethylene products with high catalyst activity.

[0651] Table 1

[0652] Ethylene homopolymerization

[0653]

[0654]

[0655] Table 1 (continued)

[0656]

[0657] Table 2 describes the ethylene homopolymerization-octene copolymerization using each catalyst and activator combination. General conditions for ACT 1: 1-octene = 0.1 mL, catalyst complex = 25 nmol, activator = 1.1 molar equivalents, 75 psig ethylene, Al(n-octyl)3 = 500 nmol, temperature = 80°C, total volume = 5 mL, solvent = toluene. General conditions for MAO: 1-octene = 0.1 mL, catalyst complex = 25 nmol, activator = 500 molar equivalents, 75 psig ethylene, temperature = 80°C, total volume = 5 mL, solvent = toluene.

[0658] In each case described, a narrow range of PDI values ​​of 1.6-3.1 was observed for polyethylene-1-octene. Catalysts 2 and 5 were found to have higher average activities than the other catalysts. In particular, Catalyst 2 with MAO at both 75 psig and 200 psig reactor pressures, and Catalyst 2 with ACT 1 at 200 psig reactor pressure, exhibited a balance of high catalyst activities (e.g., Runs 40-48: 105,396 gP.mmolcat -1 .h -1 to 1,682,743 gP.mmolcat -1 .h -1 ) and produced polymers with Mw values ​​ranging from 174,145 g / mol to 1,808,674 g / mol. Catalyst 5 with ACT 1 at a reactor pressure of 75 psig produced copolymers with the highest octene levels ranging from 31 wt% to 33 wt%, based on the total weight of the copolymer. The molecular weights of these polymers ranged from 498,334 g / mol to 596,088 g / mol. In contrast, Catalyst 5 with ACT 1 at a reactor pressure of 200 psig produced copolymers with 741,795 gP.mmolcat. -1 .h -1 -1,272,240gP.mmolcat -1 .h -1 The activities of produced polymers with 13 wt% octene and Mw ranging from 932,277 g / mol to 1,147,464 g / mol. As can be seen in Table 2, each of the catalysts and activators were shown to produce a range of high Mw, crystalline or semi-crystalline products over a range of catalyst activities.

[0659] Table 2

[0660] Ethylene-octene copolymerization

[0661]

[0662]

[0663] Table 2 (continued)

[0664]

[0665]

[0666] Table 3 describes the homopolymerization of propylene using each catalyst and activator combination. General conditions for ACT 1: propylene = 1 mL, catalyst complex = 25 nmol, activator = 1.1 molar equivalents, Al(n-octyl)3 = 500 nmol, total volume = 5 mL, solvent = isohexane. General conditions for MAO: propylene = 1 mL, catalyst complex = 40 nmol, activator = 500 molar equivalents, total volume = 5 mL, solvent = toluene.

[0667] In each case, a narrow PDI value range of 1.5-3.4 was observed for polypropylene. Catalysts 2, 4 and 5 with ACT 1 produced crystalline or semi-crystalline polymers at both reactor temperatures of 70°C and 100°C. Catalyst 4 produced polymers with the highest melting point values ​​in the range of 136°C-147°C. In particular, Catalyst 4 had an activity range of 2,926 gP.mmolcat at 70°C reactor temperature. -1 .h -1 to 3,062 gP.mmolcat -1 .h -1 and produced polymers with molecular weights ranging from 152,804 g / mol to 162,181 g / mol. Catalyst 5 produced polymers with molecular weights ranging from 477,837 g / mol to 162,181 g / mol. -1 .h -1 -964,800gP.mmolcat -1 .h -1 The catalyst activity produced polymers having melting point values ​​ranging from 81°C to 84°C and Mw ranging from 411,768 g / mol to 627,072 g / mol.

[0668] Table 3

[0669] Propylene homopolymer

[0670]

[0671]

[0672]

[0673] Table 3. (Continued)

[0674]

[0675]

[0676] In general, the catalysts, catalyst systems and methods of the present disclosure can provide high temperature ethylene polymerization, propylene polymerization or copolymerization because the Lewis base catalyst is stable at high polymerization temperatures and has good activity at high polymerization temperatures. Stable catalysts with good activity can form polymers with one or more of the following compared to conventional catalysts: high melting point, high isotacticity, controllable molecular weight, and the ability to prepare increased amounts of polymers in a given reactor. The non-metallocene catalysts, catalyst systems and methods of the present disclosure can provide ethylene- or propylene-based polymers with high Tm values, which can provide harder and more thermally stable materials compared to materials formed using polymers with lower Tm values.

[0677] Unless otherwise specified, the phrases "consisting essentially of" and "consisting essentially of" do not exclude the presence of other steps, elements, or materials, whether or not specifically mentioned in the present specification, as long as such steps, elements, or materials do not affect the basic and novel characteristics of the present disclosure, and further, they do not exclude impurities and variations normally associated with the elements and materials used.

[0678] For the purpose of brevity, only some ranges are explicitly disclosed herein. However, the range from any lower limit can be combined with any upper limit to record the range that is not clearly recorded, and the range from any lower limit can be combined with any other lower limit to record the range that is not clearly recorded, and in the same way, the range from any upper limit can be combined with any other upper limit to record the range that is not clearly recorded. In addition, even if it is not clearly recorded, each point or individual value between its endpoints is included in the scope. Therefore, each point or individual value can serve as their own lower limit or upper limit, combined with any other point or individual value or any other lower limit or upper limit, so as to record the range that is not clearly recorded.

[0679] All documents described herein are incorporated herein by reference, including any priority documents and / or test procedures, as long as they do not contradict this article. As is apparent from the general description and specific embodiments above, although the form of the present disclosure has been set forth and described, various changes can be made without departing from the spirit and scope of the present disclosure. Therefore, it is not intended to limit the present disclosure thereby. Similarly, for the purposes of U.S. law, the term "comprising" is considered to be synonymous with the term "including". Similarly, whenever a composition, element or group of elements is preceded by the conjunction "comprising", it should be understood that we also consider the same composition or group of elements preceded by the conjunction "essentially consisting of...", "consisting of...", "selected from a group consisting of..." or "is", and vice versa.

[0680] Although the disclosure has been described with respect to a number of embodiments and examples, those skilled in the art, having benefit of this disclosure, will appreciate that other embodiments can be devised that do not depart from the scope and spirit of the disclosure.

Claims

1. A catalyst compound represented by formula (I): in: M is a Group 3, 4, 5 or 6 metal; A 1 and A 2 wherein each is independently selected from the group consisting of aryl, substituted aryl, heteroaryl, and substituted heteroaryl groups; J comprises a heterocyclic Lewis base; Each L is independently a Lewis base; Each X is independently an anionic ligand; n is 1, 2, or 3; m is 0, 1, or 2; n+m is not greater than 4; R 1 Select from the following: C1-C 40 Hydrocarbyl, substituted C1-C 40 Hydrocarbyl groups, heteroatom-containing groups and substituted heteroatom-containing groups; Any two L groups are optionally joined together to form a bidentate Lewis base; The X group is optionally joined to the L group to form a monoanionic bidentate group; and Any two X groups are optionally joined together to form a dianionic ligand group; E 1 is selected from the group consisting of a hydrocarbon group, a substituted hydrocarbon group, a silyl group, and a substituted silyl group, and J is represented by the following formula: Where R 2 , R 3 and R 4 Each of which is independently selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 Hydrocarbon groups, heteroatoms and groups containing heteroatoms, or R 2 and R 3 or R 3 and R 4 wherein one or more pairs are optionally joined to form one or more hydrocarbyl, substituted hydrocarbyl, heterocyclic or substituted heterocyclic rings, each having 5, 6, 7 or 8 ring atoms, and wherein substituents on the rings may join to form additional rings, or Where J and E 1 are joined to form a ring represented by the formula: Where E 2 Selected from O, S and N (R 10 ), where R 5 , R 6 , R 7 and R 10 Each of which is independently selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 A hydrocarbon group, a heteroatom, a group containing a heteroatom, and a substituted group containing a heteroatom, or R 5 and R 6 or R 6 and R 7 wherein one or more pairs are optionally joined to form one or more hydrocarbyl, substituted hydrocarbyl, heterocyclic or substituted heterocyclic rings, each having 5, 6, 7 or 8 ring atoms, and wherein substituents on the rings may join to form additional rings, or Where J and E 1 are joined to form a ring represented by the formula: Where R 5 , R 6 , R 7 , R 10 and R 15 Each of which is independently selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 Hydrocarbyl, heteroatom and heteroatom-containing groups, and substituted heteroatom-containing groups, or R 5 and R 6 or R 6 and R 7 or R 7 and R 10 or R 10 and R 15 One or more pairs of these are optionally joined to form one or more hydrocarbyl, substituted hydrocarbyl, heterocyclic or substituted heterocyclic rings, each having 5, 6, 7 or 8 ring atoms, and wherein substituents on the rings may join to form additional rings. 2 . The catalyst compound of claim 1 , wherein the catalyst compound comprises an eight-membered metallocycle ring and a five-membered metallocycle ring.

3. The catalyst compound according to claim 1, wherein E 1 Selected from C(R 8 )(R 9 ) and Si(R 8 )(R 9 ), where R 8 and R 9 Each of which is independently selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 A hydrocarbon group, a heteroatom, a group containing a heteroatom, and a substituted group containing a heteroatom, or R 8 and R 9 Optionally joined to form one or more C3-C 20 Alkyl groups, hydrocarbyl rings, substituted hydrocarbyl rings, heterocyclic rings, or substituted heterocyclic rings, each having 5, 6, 7, or 8 ring atoms, and wherein substituents on the rings may join to form additional rings.

4. The catalyst compound according to claim 1, wherein M is a Group 4 transition metal and A 1 It is an aryl group or a substituted aryl group.

5. The catalyst compound according to claim 1, wherein A 2 It is expressed by the following formula: Where R 11 , R 12 , R 13 and R 14 Each of which is independently selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 Hydrocarbyl groups, heteroatoms, heteroatom-containing groups, and substituted heteroatom-containing groups.

6. The catalyst compound according to claim 5, wherein R 11 It is C1-C 20 A hydrocarbon or substituted hydrocarbon group is tert-butyl, is di-tert-butylphenyl, or R 11 It is expressed by the following formula:

7. The catalyst compound according to claim 1, wherein E 2 Selected from the following: NH, C1-C 20 Alkyl-N and C4-C 20 Aryl-N.

8. The catalyst compound according to claim 1, wherein R 2 , R 3 and R 4 Each of which is independently selected from the following: hydrogen and C1-C 10 Alkyl, R 1 is di-tert-butylphenyl and E 1 is C(R 8 )(R 9 ), where R 8 is hydrogen and R 9 is tert-butylphenyl, or E 1 It is CH2.

9. The catalyst compound according to claim 1, wherein the catalyst compound is selected from the following:

10. The catalyst compound according to claim 1, wherein the catalyst compound is:

11. A catalyst system comprising an activator and the catalyst compound of any one of claims 1 to 10.

12. The catalyst system of claim 11, wherein the activator is represented by the formula: (From d+ )(A d- ) Where Z is (LH) or a reducible Lewis acid, L is a Lewis base; H is hydrogen, (LH) + is a Bronsted acid; A d- is a non-coordinating anion having a charge d-; and d is an integer from 1 to 3, or Among them A d- is a non-coordinating anion having a charge d-; d is an integer from 1 to 3 and Z is a reducible Lewis acid represented by the formula: (Ar3C + ), wherein Ar is an aromatic group or is substituted by a heteroatom, C1-C 40 Hydrocarbon or substituted C1-C 40 a hydrocarbyl-substituted aryl group; or The activator is represented by formula (AI): [R 1 R 2 R 3 EH] d + [M k+ Q n ] d- (AI) in: E is nitrogen or phosphorus; d is 1, 2 or 3; k is 1, 2 or 3; n is 1, 2, 3, 4, 5 or 6; nk = d; R 1 , R 2 and R 3 Each of which is independently hydrogen, C1-C 40 Alkyl or C5-C 50 -aryl, where R 1 , R 2 and R 3 Each of which is independently unsubstituted or substituted; wherein R 1 , R 2 and R 3 Contains 15 or more carbon atoms in total; M is an element selected from Group 13 of the Periodic Table; and Each Q is independently selected from the group consisting of hydrogen, bridged or unbridged dialkylamino, halo, alkoxy, substituted alkoxy, aryloxy, substituted aryloxy, hydrocarbyl, substituted hydrocarbyl, halohydrocarbyl, substituted halohydrocarbyl, and halo-substituted hydrocarbyl groups.

13. The catalyst system of claim 11, further comprising a metal hydrocarbenyl chain transfer agent represented by the formula: Al(R')3-v(R")v Wherein each R' is independently C1-C 30 Hydrocarbyl group; each R" is independently C4-C 20 a hydrocarbenyl group; and v is 0.1-3.

14. A method for preparing a polymer, comprising: polymerizing an olefin by contacting the olefin with a catalyst system comprising an activator and the catalyst compound of claim 1, The polymerization is carried out in one or more continuous stirred tank reactors or loop reactors connected in series or in parallel at a reactor pressure of 0.05 MPa to 1,500 MPa and a reactor temperature of 30° C. to 230° C.

15. The method of claim 14, wherein the polymer is homopolyethylene and the olefin is ethylene, wherein the homopolyethylene has a Mw value of 155,000 g / mol to 1,200,000 g / mol, a Mn value of 90,000 to 550,000, a Mz value of 350,000 to 4,000,000, and a PDI of 1.5 to 3.

16. The method according to claim 15, wherein The melting temperature of the polymer is 135°C to 138°C, and The catalyst compound is represented by: Where R 11 Selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 Hydrocarbyl groups, heteroatoms and groups containing heteroatoms; or in: The melting temperature of the polymer is 135°C to 138°C, and The catalyst compound is: or wherein the polymer is an ethylene-octene copolymer, The copolymer has an M w Value is 100,000-3,600,000, M n Value is 50,000-2,250,000, M z The value is 225,000-6,200,000, and the PDI is 1.5-3, The melting temperature of the polymer is 104°C-126°C, and The catalyst compound is represented by: Where R 11 Selected from the following: hydrogen, C1-C 40 Hydrocarbyl, substituted C1-C 40 Hydrocarbyl groups, heteroatoms and groups containing heteroatoms; or in: The olefin is propylene, The polymer is homopolypropylene, and The homopolypropylene has: M w The value is 85,000g / mol-750,000g / mol, M n The value is 55,000g / mol-400,000g / mol, M z Values ​​range from 165,000 g / mol to 1,600,000 g / mol, and PDI is 1.6-2.1, The reactor temperature is 60°C to 80°C, The melting temperature of the polymer is 146°C-147°C, and The catalyst compound is:

Citation Information

Patent Citations

  • Catalyst for olefin polymerization, and method for producing olefin polymer

    JP2015199919A

  • Method and apparatus for the production of solid polymers of olefins

    US3248179A

  • Fluidized bed reaction systems

    US4543399A

  • Method for fluidized bed polymerization

    US4588790A

  • Loop reactor settling leg system for separation of solid polymers and liquid diluent

    US4613484A