Carbon black and method for producing carbon black
Carbon black with tailored N2SA, DBP absorption, N2SA/IA, hydrogen content, and ΔD values addresses dispersibility and aggregation issues, enhancing rubber reinforcement and tensile properties in harsh environments.
Patent Information
- Application Number
- CN202180029456.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-04-02
- Filing Date
- 2021-08-13
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing carbon black formulations struggle to provide adequate reinforcement in rubber components, especially in harsh environments, due to issues with dispersibility and aggregation, which affect the tensile properties of rubber parts.
Carbon black with specific properties including nitrogen adsorption specific surface area (N2SA) of 25-60 m²/g, DBP absorption of 90-180 cm³/100g, N2SA to iodine adsorption ratio (N2SA/IA) of 1.10×10³-1.50×10³ m²/g, hydrogen content of 150-250/g, and Raman scattering peak half-maximum width (ΔD) of 260-290 cm⁻¹, enhancing both macroscopic and microscopic dispersibility and interaction with rubber.
The specified carbon black properties result in improved tensile product of rubber components, achieving better reinforcement and dispersibility, suitable for use in harsh environmental conditions.
Smart Images

Figure GDA0005040982600000171 
Figure GDA0005040982600000181 
Figure GDA0005040982600000191
Abstract
Description
Technical Field
[0001] The present invention relates to carbon black and a method for producing the same. Background Art
[0002] Carbon black is used for various purposes, and is mainly used as a filler for reinforcing rubber parts. As is well known, in order to give the rubber parts sufficient reinforcement, it is crucial to uniformly disperse the carbon black in the rubber parts.
[0003] At present, various technical improvements have been made to improve the dispersibility of carbon black and enhance the reinforcement of rubber parts. For example, Patent Document 1 discloses a carbon black having good dispersibility in a rubber mixture, thereby having a very high reinforcement effect and slight hysteresis. According to the invention described in Patent Document 1, the above-mentioned problems can be solved by using carbon black whose CTAB surface area, COAN, OAN and COAN sum are within a predetermined numerical range.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent document 1: Japanese Patent No. 6140915. Summary of the invention
[0007] Problems to be solved by the invention
[0008] In recent years, rubber parts are increasingly used in harsh environments. As a result, carbon black is also required to have a higher reinforcing property for rubber parts.
[0009] Therefore, an object of the present invention is to provide carbon black which can further strengthen a rubber component when mixed with the rubber component, and a method for producing the same.
[0010] Technical solutions to problems
[0011] The present inventors found that the nitrogen adsorption specific surface area (hereinafter referred to as N2SA), DBP absorption, the ratio of N2SA to iodine adsorption (hereinafter referred to as IA) (hereinafter referred to as N2SA / IA), hydrogen content ( / g) and the half-maximum full width ΔD (cm2) of the Raman scattering peak of carbon black can be used to calculate the carbon black adsorption specific surface area (hereinafter referred to as N2SA), DBP absorption, the ratio of N2SA to iodine adsorption (hereinafter referred to as IA) (hereinafter referred to as N2SA / IA), hydrogen content ( / g) and half-maximum full width ΔD (cm2) of the Raman scattering peak. -1 ) are limited to a specific range, which can solve the above problem.
[0012] That is, the present invention includes the following matters.
[0013] [1] A carbon black, wherein
[0014] Nitrogen adsorption specific surface area (N2SA) is 25~60m 2 / g,
[0015] DBP absorption is 90~180cm 3 / 100g,
[0016] The ratio of nitrogen adsorption specific surface area (N2SA) to iodine adsorption (IA) (N2SA / IA) is 1.10×10 3 ~1.50×10 3 m 2 / g,
[0017] When the nuclear magnetic resonance signal of the spin-spin relaxation process observed by the solid echo method is represented by the sum of a first signal and a second signal having a larger time constant than the first signal, the amount of hydrogen represented by the signal intensity per unit mass of the first signal at time 0 is 150 to 250 / g,
[0018] When the excitation wavelength is set to 532nm, the -1 The full width at half maximum of the Raman scattering peak in the range of 260 to 290 cm -1 .
[0019] [2] The carbon black according to [1], wherein the DBP absorption is 90 to 150 cm 3 / 100g.
[0020] [3] The carbon black according to [1] or [2], wherein the N2SA / IA is 1.20×10 3 ~1.50×10 3 m 2 / g.
[0021] [4] The carbon black according to any one of [1] to [3], which is used as a filler for rubber parts.
[0022] [5] The carbon black according to [4], wherein the carbon black is added in an amount of 10 to 170 parts by weight based on 100 parts by weight of the rubber component in the rubber member.
[0023] [6] A method for producing carbon black, comprising the following steps:
[0024] A reaction step in which hydrocarbons as raw materials are incompletely burned in a reaction furnace to generate carbon black raw materials;
[0025] a granulation step of granulating the carbon black raw material to a predetermined size; and
[0026] a drying step of dehydrating and drying the granulated carbon black raw material;
[0027] The reaction process is carried out in a reaction region between a position where the refrigerant is introduced and a position where the cooling liquid is introduced in the reaction furnace.
[0028] A refrigerant is introduced to make the temperature of the reaction zone 800-900°C,
[0029] A cooling liquid is introduced to make the residence time of the carbon black raw material in the reaction area become 20 to 30 milliseconds, and then the reaction of the carbon black raw material is stopped.
[0030] According to the present invention, it is possible to provide carbon black which, when mixed with a rubber component, can increase the tensile product of rubber compared with conventional methods, and a method for producing the same. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 is a diagram for explaining the method of calculating the amount of hydrogen;
[0032] Figure 2 is a diagram for explaining the method of calculating the amount of hydrogen;
[0033] Figure 3 is a diagram showing a method for calculating the full width at half maximum ΔD of a Raman scattering peak;
[0034] Figure 4 is a block diagram showing a sequence of processing steps used to manufacture carbon black;
[0035] Figure 5 This is a schematic diagram showing an example of a reactor. DETAILED DESCRIPTION
[0036] An embodiment of the present invention is described below.
[0037] The carbon black involved in this embodiment is used as a filler added to a rubber component. The carbon black involved in this embodiment is used to strengthen a rubber component. It should be noted that, in the following, "strengthening" a rubber component means increasing the product of the tensile strength and tensile elongation of the rubber component, that is, increasing the value of the tensile product of the rubber component.
[0038] Generally, it is expected that in order to improve the reinforcing effect of carbon black on rubber parts, the higher the surface activity of carbon black, the easier it is to interact with rubber, and the higher the reinforcing effect of rubber parts. However, in reality, if the surface activity of carbon black is increased, carbon blacks tend to aggregate in a homogeneous phase, making it difficult to evenly disperse carbon black. As a result, the reinforcing effect of carbon black cannot be fully exerted.
[0039] Therefore, the inventors focused on the "hydrogen content" and "crystallinity" of carbon black. These properties affect the ease of interaction between carbon black and rubber and the cohesiveness of carbon black. Therefore, it is believed that limiting them within a predetermined range can simultaneously improve the ease of interaction and high dispersibility.
[0040] In addition, the inventors focused on both macroscopic and microscopic dispersibility. In order to obtain good dispersibility at both macroscopic and microscopic scales, the values of "hydrogen content" and "crystallinity" were adjusted. As a result, it was found that carbon black with high surface activity but excellent dispersibility could be obtained, thereby further strengthening rubber parts.
[0041] Specifically, the carbon black according to the present embodiment has the following features.
[0042] (A) Nitrogen adsorption specific surface area (N2SA) is 25 to 60 m 2 / g.
[0043] (B) DBP absorption is 90 to 180 cm 3 / 100g.
[0044] (C) The ratio of nitrogen adsorption specific surface area (N2SA) to iodine adsorption (IA) (N2SA / IA) is 1.10×10 3 ~1.50×10 3 m 2 / g.
[0045] (D) When the nuclear magnetic resonance signal of the spin-spin relaxation process observed by the solid echo method is represented by the sum of a first signal and a second signal having a larger time constant than the first signal, the amount of hydrogen represented by the signal intensity per unit mass of the first signal at time 0 is 150 to 250 / g.
[0046] (E) When the excitation wavelength is set to 532 nm, the -1 The full width at half maximum of the Raman scattering peak in the range of 260 to 290 cm -1 .
[0047] Since the carbon black according to the present embodiment has the above features, when added as a filler to a rubber component, it is well dispersed both microscopically and macroscopically. As a result, the tensile product of the rubber component can be improved.
[0048] Next, matters limiting the carbon black according to the present embodiment will be described in detail.
[0049] (A) N2SA: 25-60m 2 / g
[0050] N2SA is the amount of nitrogen molecules adsorbed per unit mass of carbon black (m 2 In addition, N2SA can be obtained by the method described in "Test methods for basic properties of carbon black for rubber use" of JIS K6217-7:2013 (refer to ASTM D6556-16).
[0051] N2SA is preferably 25 to 60 m 2 / g. N2SA is 25m 2 / g or more, high reinforcement can be obtained. In addition, N2SA is 60m 2 / g or less, homogeneous aggregation of carbon blacks can be suppressed, thereby obtaining high dispersibility.
[0052] From the viewpoint of obtaining strengthening and dispersibility, N2SA is more preferably 30 m 2 / g~55m 2 / g.
[0053] (B) DBP absorption: 90-180 cm 3 / 100g
[0054] DBP absorption is the absorption of DBP (dibutyl phthalate) per 100g of carbon black (cm 3 / 100g) to express the value of the structure of carbon black.
[0055] The DBP absorption can be determined in accordance with JIS K6217-1997 "Test methods for basic properties of carbon black for rubber use".
[0056] The void ratio between carbon black aggregates is positively correlated with the structure of carbon black. Therefore, a larger value of DBP absorption means a more developed structure of carbon black.
[0057] The DBP absorption is preferably 90 to 180 cm 3 / 100g. DBP absorption is 90cm 3 / 100g or more, high dispersibility can be obtained. In addition, the DBP absorption is 180cm 3 / 100g or less, high reinforcement can be obtained.
[0058] From the viewpoint of obtaining good processability and high reinforcement, the DBP absorption is more preferably 150 cm 3 / 100g or less.
[0059] In addition, as long as a technical solution for solving the problem to be solved by the present invention is provided, the present invention can also be implemented by limiting the numerical range of the N2SA and DBP absorption amounts to predetermined values as shown below.
[0060] For example, the interaction between carbon black and rubber can be increased by setting the N2SA of carbon black slightly higher than the center of the above further preferred range, and the tensile product of the rubber component when added to rubber can be increased by setting the DBP absorption of carbon black slightly lower than the center of the above preferred range, thereby giving the rubber component a higher reinforcement. In this case, N2SA is preferably set to 49m 2 / g above 55m 2 / g or less, and the DBP absorption is preferably set to 115 cm 3 / 100g and above 135cm 3 / Range below 100g.
[0061] In addition, for example, by setting the N2SA of carbon black to near the center of the above further preferred range, homogeneous agglomeration of carbon black can be suppressed, and by setting the DBP absorption of carbon black to be slightly lower than the center of the above preferred range, the tensile product of the rubber component when added to the rubber can be increased, thereby achieving both good dispersibility of carbon black in the rubber and high reinforcement. In this case, N2SA is preferably set to 35 m / s. 2 / g above 47m 2 / g or less, and the DBP absorption is preferably set to 115 cm 3 / 100g and above 132cm 3 / Range below 100g.
[0062] In addition, for example, by setting the N2SA of carbon black to be slightly lower than the center of the above further preferred range, the homogeneous agglomeration of carbon blacks can be strongly suppressed, and by setting the DBP absorption of carbon black to be slightly higher than the center of the above preferred range, a larger shear force can be obtained when adding to rubber for kneading, so that good dispersibility of carbon black in rubber can be obtained. In this case, N2SA is preferably set to 28 m 2 / g above 34m 2 / g or less, and the DBP absorption is preferably set to 133 cm 3 / 100g and above 141cm 3 / Range below 100g.
[0063] (C)N2SA / IA:1.10×10 3 ~1.50×10 3 m 2 / g
[0064] IA is a value that represents the specific surface area of carbon black in terms of the amount of iodine molecules adsorbed per unit mass of carbon black in the liquid phase (mg / g). IA is an indicator of the specific surface area of carbon black, just like N2SA, but the value of IA also depends on the number of surface functional groups of carbon black (the more acidic functional groups there are, the less likely iodine molecules are to be adsorbed, resulting in a value slightly lower than N2SA).
[0065] IA can be determined in accordance with JIS K6217-1997 "Test methods for basic properties of carbon black for rubber use".
[0066] The value obtained by dividing the value of N2SA by the value of IA is an index of the surface activity of carbon black. The value of N2SA / IA is obtained by setting the unit of the value of N2SA to m 2 / g, and the unit of IA is set to mg / g and calculated. The larger the value of N2SA / IA, the more surface functional groups there are on the carbon black. If the number of surface functional groups on the carbon black is large, the surface of the carbon black is prone to chemical reactions via the surface functional groups and is prone to interacting with rubber. In other words, the value of the surface activity of carbon black is a value that quantitatively represents the ease of chemical reactions on the surface of the carbon black.
[0067] According to this embodiment, N2SA / IA is 1.10×10 3 m 2 / g or more, thereby achieving strengthening properties.
[0068] In addition, if N2SA / IA is 1.50×10 3 m 2 / g or less, it is also easy to manufacture. Carbon black can be manufactured, for example, by burning raw oil to obtain raw material pellets of carbon black and then granulating them, which will be described in detail later. Among them, the shorter the combustion reaction time, the greater the N2SA / IA. However, if the combustion reaction time is too short, unburned oil is likely to remain, making granulation difficult. If N2SA / IA is 1.50×10 3 m 2 / g or less, the reaction can be carried out under conditions where unburned oil is less likely to remain during production.
[0069] From the viewpoint of making carbon black and rubber more interactive and obtaining higher reinforcement, N2SA / IA is preferably 1.20×10 3 m 2 / g or above.
[0070] (D) Hydrogen content: 150-250 / g
[0071] The hydrogen amount indicates the amount of hydrogen obtained by NMR. The larger the value, the more hydrogen there is on the surface of the carbon black. The inventors believe that the amount of hydrogen on the surface of the carbon black is related to the ease of interaction between the carbon black and the rubber and the cohesion of the carbon black, which will affect the strengthening and dispersibility. The more hydrogen there is on the surface, the easier it is for the carbon black to interact with the rubber, that is, the easier it is for the carbon black and the rubber to coagulate (heterogeneous agglomeration), the dispersibility is improved, and thus the strengthening is improved. On the other hand, if there is too much hydrogen on the surface, the carbon blacks are likely to coagulate with each other (homogeneous agglomeration), the dispersibility is reduced, and thus the strengthening is reduced. Therefore, the inventors focused on this and studied the NMR hydrogen amount, and the result was determined to be in the range of 150 to 250.
[0072] From the viewpoint of obtaining ease of interaction between carbon black and rubber and good dispersibility, the amount of hydrogen is preferably 150 to 240 g.
[0073] The amount of hydrogen can be specifically determined by the following method.
[0074] (1) Minispec mq20 manufactured by Bruker Biosphinx was used as a pulsed nuclear magnetic resonance instrument. The carbon black to be measured was dried at 110°C for 30 minutes, and 0.2 g of the carbon black was filled into a glass sample tube as a measurement sample. The spin-spin relaxation time (transverse relaxation time) T2 was measured under the following measurement conditions to obtain a T2 relaxation curve (free induction decay curve).
[0075] <Measurement Conditions>
[0076] Detection nuclide: 1H
[0077] Pulse mode: solid echo method (90°×-τ-90°y)
[0078] 90° pulse width: 2.7μs
[0079] Measurement time: 2ms
[0080] Standby time: 500ms
[0081] Total times: 52 times
[0082] Measurement temperature: 40℃
[0083] Gain: 90
[0084] The mass of carbon black is constant at 0.2 g, and the device function is also constant (gain = 90), so the signal intensity of the obtained T2 relaxation curve (free induction decay curve) increases or decreases in proportion to the 1H concentration of the measurement object.
[0085] (2) Using the fitting software (TD-NMR-A for Windows 7) attached to the above-mentioned pulsed NMR equipment (Minispec mq20 from Bruker Biospec Co., Ltd.), the obtained free induction decay curve was fitted by the linear least squares method to obtain an approximate curve represented by the following formula f(t).
[0086] f(t)=A(1)exp(-t / T2(1))+A(2)exp(-t / T2(2))
[0087] [Wherein, T2(1) is the relaxation time of the short component of the relaxation time; T2(2) is the relaxation time of the long component of the relaxation time; A(1) is the signal intensity of the short component of the relaxation time at t=0; A(2) is the signal intensity of the long component of the relaxation time at t=0.]
[0088] (3) Divide the above signal intensity A(1) by the mass w(g) of the sample to be measured.
[0089] like Figure 1 As shown, it can be seen that when the time of 90° pulse excitation is set to t=0, a signal of magnetization (signal intensity) in the y-axis direction decaying with time will be obtained. It should be noted that Figure 1 The graph shown is for explaining the calculation method of the NMR hydrogen amount and is not the measurement result of the carbon black according to the present embodiment.
[0090] Figure 2 The solid line indicates Figure 1 The T2 relaxation curve (free induction decay curve) shown is the fitting curve when it is fitted by the linear least squares method. Figure 2 As shown, the obtained T2 relaxation curve (free induction decay curve) can be expressed as the sum of two exponential functions by fitting.
[0091] Since it is impossible to distinguish between liquid and solid by the difference in time constant, the signal intensity A(1) at t=0 (when excited by a 90° pulse) in the exponential function related to the short component of the relaxation time can be determined as hydrogen atoms (-COOH, -OH, -H on the surface, -H in the carbon skeleton, etc.) on the surface of carbon black. Similarly, in the exponential function related to the short component of the relaxation time, the signal intensity A(2) at t=0 (when excited by a 90° pulse) can be determined as water or liquid polycyclic aromatic hydrocarbons adsorbed on the surface of carbon black.
[0092] By dividing the above signal intensity A(1) (arbitrary unit) by the mass w (0.2 g) of the carbon black used for measurement, the amount of hydrogen per unit mass of carbon black "A(1) / w" can be calculated. The carbon black used as a reference in this measurement is seast 9 (trade name) manufactured by Tokai Carbon Co., Ltd., and its hydrogen content is 114 / g. That is, the hydrogen content of the sample to be measured is calculated on the basis of adjusting the measurement conditions that affect the signal intensity so that the hydrogen content of seast 9 (trade name) manufactured by Tokai Carbon Co., Ltd. becomes 114 / g.
[0093] Through research by the present inventors, it was found that the amount of hydrogen represented by A(1) / w is highly correlated with the amount of hydrogen obtained by the currently well-known method for measuring the amount of hydrogen on the surface of carbon black, namely the thermal decomposition method, and can therefore be preferably used as an indicator for representing the amount of hydrogen on the surface of carbon black.
[0094] (E) Raman scattering peak half-maximum width ΔD: 260-290 cm -1
[0095] ΔD is the value of the Raman spectrum at 1350±10cm in the Raman spectrum obtained by measuring with a laser Raman spectrometer at an excitation wavelength of 532nm. -1 The full width at half maximum of the peak with a peak top (cm -1 ).
[0096] In the above Raman spectrum, at 1350±10cm -1 The range has a peak with a peak top, which is equivalent to the peak on the D peak of the Raman spectrum.
[0097] According to the research conducted by the present inventors, the full width at half maximum of the D peak indicates the disorder of the crystal structure on the surface of carbon black, that is, the crystallinity. The larger the ΔD value, the more disordered the crystal structure (the lower the crystallinity).
[0098] In the case of a disordered crystal structure (low crystallinity), there will be many edges on the surface of carbon black, that is, the formation sites (active points) of functional groups that show affinity to rubber, and the ease of interaction between carbon black and rubber will increase. As a result, carbon black and rubber will easily agglomerate in a heterogeneous manner, and the dispersibility will be improved. On the other hand, if the crystallinity is too low, carbon blacks will easily agglomerate in a homogeneous manner, which will damage the dispersibility. Therefore, considering these circumstances, the inventors conducted research to obtain the best crystallinity and finally determined ΔD to be 260 to 290.
[0099] That is, when the ΔD value is 260 or more, heterogeneous aggregation is easy to occur, thereby obtaining high dispersibility and ultimately improving reinforcement. On the other hand, when the ΔD value is 290 or less, homogeneous aggregation is not easy to occur, thereby obtaining high dispersibility and still obtaining high reinforcement.
[0100] From the viewpoint of obtaining easy interaction between carbon black and rubber and good dispersibility, the ΔD value is more preferably 260 to 280 cm -1 .
[0101] Specifically, ΔD can be measured by the following method.
[0102] Figure 3 This is a diagram showing the calculation method of ΔD value. It should be noted that Figure 3 It is shown only for explaining the calculation method of ΔD and is not the measurement result of carbon black according to the present embodiment.
[0103] like Figure 3 As shown in the Raman spectrum of carbon black measured by laser Raman spectroscopy at an excitation wavelength of 532 nm, a peak at 1350 ± 10 cm -1 The range has a peak with a peak top.
[0104] Then, the measurement wavelength of the peak position is set as Dmax (cm -1 ), in the obtained ΔD spectrum, the detection position on the low wavelength (low Raman shift) side having a detection intensity half of the peak intensity of the above Dmax is set as D50 (cm -1 ), at this time, the value calculated by the following formula is taken as ΔD (cm -1 ).
[0105] ΔD value = (Dmax-D50) × 2
[0106] The carbon black used as a standard in this measurement is seast G-SO (trade name) manufactured by Tokai Carbon Co., Ltd., and its ΔD value is 249 cm -1 That is, the ΔD of the sample to be measured is obtained by adjusting the measurement conditions that affect the ΔD value so that the ΔD of seast 9 (trade name) manufactured by Tokai Carbon Co., Ltd. becomes 249 cm -1 Calculated on the basis of .
[0107] (F) Other specific matters
[0108] As described above, the carbon black according to the present embodiment is used as a filler for reinforcing a rubber component.
[0109] Here, the rubber parts are not particularly limited, for example, they can be used for the following rubbers: general-purpose rubbers such as natural rubber, styrene-butadiene rubber, butadiene rubber, butyl rubber, ethylene-propylene rubber, nitrile rubber, chloroprene rubber, etc.; or special rubbers such as acrylic rubber, chlorosulfonated polyethylene rubber, polyurethane rubber, silicone rubber, fluororubber, and rubber parts mixed with them. The use of the rubber parts in which the carbon black involved in this embodiment is used as a filler is preferably various rubber parts (weather strips, hoses, belts, shock-absorbing rubbers, boots, sealing and packaging materials, etc.) for general industries such as automobiles. In the automotive field, with the development of high performance, the use of rubber parts in harsh environments such as high temperature and high pressure has gradually increased. In addition, the compactness of automotive parts has led to the development of rubber parts towards miniaturization, while the lightweight of automotive parts has led to the development of rubber parts towards lightness and thinness. As a result, it is increasingly difficult for existing carbon black to satisfactorily give the required reinforcement to rubber parts. The carbon black involved in this embodiment can be used to meet these requirements for automotive rubber parts.
[0110] The carbon black is mixed in an amount of, for example, 10 to 170 parts by weight, preferably 20 to 160 parts by weight, based on 100 parts by weight of the rubber component.
[0111] (G) Method for producing carbon black
[0112] The carbon black according to the present embodiment can be obtained by incompletely burning a hydrocarbon raw material and appropriately adjusting the reaction conditions according to a common carbon black production method such as an oil furnace method. An example of the production method of the carbon black according to the present embodiment will be described below.
[0113] Figure 4 This is a block diagram showing the sequence of processing steps for producing carbon black according to one embodiment of the present invention. Figure 5 FIG. 1 is a schematic diagram showing an example of a reactor. Figure 4 As shown, the carbon black according to one embodiment of the present invention can be produced by sequentially performing the reaction step S1, the granulation step S2, and the drying step S3.
[0114] First, in the reaction step S1, a carbon black raw material is generated by a reaction furnace 10. Figure 5 As shown, the reactor 10 is cylindrical and has a fuel combustion area 4 , a raw material introduction area 6 and a reaction area 9 .
[0115] The fuel combustion zone 4 is a part that generates high-temperature combustion gas. The fuel combustion zone 4 is provided with an oxygen-containing gas inlet 1, a combustion burner 2, and an alkali metal salt·aqueous solution supply nozzle 3. Oxygen-containing gas (oxygen, air, etc.) is introduced into the fuel combustion zone 4 from the oxygen-containing gas inlet 1. In addition, fuel (FCC residual oil, hydrogen, carbon monoxide, natural gas, petroleum gas, etc.) is supplied to the fuel combustion zone 4 from the combustion burner 2. Thus, high-temperature combustion gas is generated. Carbonates, chlorides, hydroxides, etc. of sodium, potassium, etc. are supplied to the fuel combustion zone 4 from the alkali metal salt·aqueous solution supply nozzle 3 as an alkali metal salt·aqueous solution. By adding an alkali metal salt·aqueous solution, the structure of carbon black can be adjusted to be underdeveloped in the raw material introduction zone 6. The combustion gas generated in the fuel combustion zone 4 is supplied to the raw material introduction zone 6.
[0116] The raw material introduction area 6 is a part for introducing raw material oil. The diameter of the raw material introduction area 6 is smaller than that of the fuel combustion area 4. The raw material introduction area 6 is connected to the raw material introduction nozzle 5. The raw material oil is introduced into the raw material introduction area 6 via the raw material oil introduction nozzle 5 and mixed with the combustion gas. At this time, tiny nuclei of carbon black are generated by thermal decomposition, and a predetermined structure is formed by the collision of the nuclei, thereby generating carbon black raw materials, i.e., carbon black particles. As the raw material oil, the following hydrocarbons can be used: aromatic hydrocarbons such as naphthalene and anthracene; coal-based hydrocarbons such as creosote and tar; petroleum-based heavy oils such as FCC residual oil and ethylene heavy oil; aliphatic hydrocarbons such as acetylenic unsaturated hydrocarbons and hexane. The mixture of combustion gas and raw material oil is supplied to the reaction area 9.
[0117] The reaction area 9 is a part where the reaction is stopped after the carbon black particles generated in the raw material introduction area 6 are further fully grown in the gas phase. The diameter of the reaction area 9 is larger than the diameter of the fuel combustion area 4. The flow rate of the carbon black particles generated in the raw material introduction area 6 will be reduced in the reaction area 9 with a large pore size. At this time, the aromatic hydrocarbons in the gas phase will be carbonized, stacked and grown on the surface of the carbon black particles to generate carbon black raw materials. The reaction area 9 is provided with a refrigerant introduction nozzle 7 and a coolant introduction nozzle 8 for stopping the reaction. The refrigerant introduction nozzle 7 is arranged on the upstream side compared to the coolant introduction nozzle 8. A refrigerant is supplied from the refrigerant introduction nozzle 7 to the reaction area 9 to control the temperature of the reaction area 9. Cooling water is sprayed from the coolant introduction nozzle 8 to the reaction area 9. As a result, the generation reaction of the carbon black raw material is stopped.
[0118] The carbon black raw material generated in the reaction area 9 is transferred to a collection system (not shown) and collected by a collection device such as a cyclone separator and a bag filter.
[0119] Next, in the granulation step S2, the carbon black raw material is granulated so that the particles of the carbon black raw material become a predetermined size. The specific method of the granulation treatment is not particularly limited, and a known granulation method can be applied. As a known granulation method, for example, a wet granulation method can be cited. An example of a wet granulation method is a method in which a spiral shaft equipped with a plurality of special rod-shaped pins is rotated at a high speed in the center of a cylinder in a predetermined container, and carbon and water are continuously supplied into the container, and the mixture is stirred and mixed to form pelletized particles of a predetermined size.
[0120] Next, in the drying step S3, in order to dehydrate the granulated carbon black raw material, the granulated carbon black raw material is dried to obtain a dried carbon black raw material. The specific method of the drying treatment is not particularly limited, and a known drying method can be applied. As a known drying method, for example, an indirect heating drying method can be cited. An example of an indirect heating drying method uses an indirect heating rotary dryer. This method is to supply hot gas to the space between the outer cylinder and the inner cylinder of the double-tube structure of the rotary furnace-like indirect heating rotary dryer, and heat and dry the granulated carbon black raw material containing water arranged in the inner cylinder at a predetermined temperature.
[0121] After the above process, carbon black can be produced.
[0122] Here, for example, by adjusting the reaction conditions in the reaction step S1, the properties of the obtained carbon black can be controlled.
[0123] For example, in the reaction step S1, the DBP absorption value can be reduced by increasing the amount of the alkali metal salt·aqueous solution introduced. Therefore, the desired DBP absorption value can be obtained by adjusting the amount of the alkali metal salt·aqueous solution introduced.
[0124] In addition, in the reaction step S1, if the amount of oxygen-containing gas introduced is increased or the amount of feedstock oil introduced is reduced, the value of N2SA will increase. Therefore, by adjusting the amount of oxygen introduced or the amount of feedstock oil introduced, the desired N2SA can be obtained.
[0125] In addition, if the reaction time from the introduction of the feedstock oil to the termination of the reaction by rapid cooling is shortened, the value of N2SA / IA will increase. Therefore, by adjusting the reaction time, the desired N2SA / IA can be obtained.
[0126] In addition, the NMR hydrogen amount and ΔD (crystallinity) depend on the reaction temperature of the reaction region 9 and the residence time in the reaction region 9. Therefore, the refrigerant is introduced into the nozzle 7 while adjusting the addition amount. Figure 1Inert gases such as nitrogen, heavy oil with a specific gravity less than 1.0 (A heavy oil, B heavy oil or C heavy oil), light hydrocarbons (gasoline, light oil or kerosene, etc.), or refrigerants such as water vapor are introduced into the reaction area 9 (furnace temperature above 1000°C) between the raw material inlet area 6 and the coolant inlet nozzle 8, so that the reaction temperature of the reaction area 9 becomes 800-900°C, and then the reaction is stopped by sudden cooling (rapid cooling by water spray) so that the residence time (between nozzle 7 and nozzle 8) becomes 20-30 milliseconds, thereby obtaining the desired NMR hydrogen amount and ΔD.
[0127] Example
[0128] In order to explain the present invention in more detail, the following examples are described. However, the present invention should not be limited to the following examples for interpretation.
[0129] (Examples 1 to 12, Comparative Examples 1 to 10)
[0130] according to Figure 4 The carbon black according to one embodiment of the present invention is produced by the process sequence shown in FIG. Figure 5 The reactor of the structure shown generates carbon black raw materials with different properties by changing the following items: whether to introduce refrigerant into the reaction area 9 through the refrigerant introduction nozzle 7, the reaction temperature of the reaction area 9, and the residence time until the reaction stops.
[0131] (Examples 1 to 12)
[0132] Nitrogen is introduced into the reaction area 9 between the raw oil introduction nozzle 5 and the coolant introduction nozzle 8 through the refrigerant introduction nozzle 7, the reaction temperature is adjusted to 800-900°C, and the residence time until the reaction is stopped by the coolant introduction nozzle 8 is adjusted to 20-30 milliseconds, thereby producing carbon black.
[0133] (Comparative Example 1)
[0134] Nitrogen is introduced into the reaction area 9 between the crude oil introduction nozzle 5 and the coolant introduction nozzle 8 through the refrigerant introduction nozzle 7, the reaction temperature is adjusted to 800-900°C, and the residence time until the reaction is stopped by the coolant introduction nozzle 8 is adjusted to less than 20 milliseconds, thereby producing carbon black.
[0135] (Comparative Examples 2, 3, 7 to 9)
[0136] Carbon black was produced without introducing nitrogen gas into the reaction region 9 through the refrigerant introduction nozzle 7 .
[0137] (Comparative Example 4)
[0138] Nitrogen is introduced into the reaction area 9 between the crude oil introduction nozzle 5 and the coolant introduction nozzle 8 through the refrigerant introduction nozzle 7, the reaction temperature is adjusted to below 800°C, and the residence time until the reaction is stopped by the coolant introduction nozzle 8 is adjusted to 20 to 30 milliseconds, thereby producing carbon black.
[0139] (Comparative Example 5)
[0140] Nitrogen is introduced into the reaction area 9 between the crude oil introduction nozzle 5 and the coolant introduction nozzle 8 through the refrigerant introduction nozzle 7, the reaction temperature is adjusted to more than 900°C, and the residence time until the reaction is stopped by the coolant introduction nozzle 8 is adjusted to 20 to 30 milliseconds, thereby producing carbon black.
[0141] (Comparative Example 6)
[0142] Nitrogen is introduced into the reaction area 9 between the crude oil introduction nozzle 5 and the coolant introduction nozzle 8 through the refrigerant introduction nozzle 7, the reaction temperature is adjusted to 800-900°C, and the residence time until the reaction is stopped by the coolant introduction nozzle 8 is adjusted to more than 30 milliseconds, thereby producing carbon black.
[0143] (Comparative Example 10)
[0144] Nitrogen is introduced into the reaction zone 9 between the raw oil introduction nozzle 5 and the coolant introduction nozzle 8 through the refrigerant introduction nozzle 7, the reaction temperature is adjusted to 800-900°C, and the residence time until the reaction is stopped by the coolant introduction nozzle 8 is adjusted to 20-30 milliseconds, thereby producing a nitrogen adsorption specific surface area (N2SA) exceeding 60m by reducing the amount of raw hydrocarbon. 2 / g of carbon black.
[0145] Next, in the granulation step S2, each carbon black raw material obtained in the reaction step S1 was subjected to a wet granulation treatment under certain conditions. Thus, carbon blacks according to Examples 1 to 12 and Comparative Examples 1 to 10 were obtained.
[0146] For each of the obtained carbon blacks of Examples 1 to 12 and Comparative Examples 1 to 10, whether nitrogen was introduced through the refrigerant introduction nozzle 7, the temperature of the reaction region 9 at the intermediate point between the refrigerant introduction nozzle 7 and the coolant introduction nozzle 8, the residence time at the intermediate point between the refrigerant introduction nozzle 7 and the coolant introduction nozzle 8, N2SA, N2SA / IA, DPB absorption, NMR hydrogen amount, and ΔD were measured. The results are shown in Tables 1-1, 1-2, and 2.
[0147] Next, 40 parts by weight of carbon black according to each example and comparative example was added to 100 parts by weight of NBR rubber to prepare rubber compositions. The prepared rubber compositions were measured. The measured physical properties and measurement methods are as follows.
[0148] (Durometer hardness Hs)
[0149] The hardness Hs was measured using a type A durometer in accordance with JIS K6253-3-2012 (vulcanized rubber and thermoplastic rubber—method for determining hardness).
[0150] (Tensile strength TB)
[0151] The tensile strength TB (MPa) at break was measured in accordance with JIS K6251-2017 (vulcanized rubber and thermoplastic rubber—Determination of tensile properties).
[0152] (Elongation EB)
[0153] The elongation EB (%) at break was measured in accordance with JIS K6251-2017 (vulcanized rubber and thermoplastic rubber-method for determining tensile properties).
[0154] (Tensile product TB×EB)
[0155] From the TB and EB obtained above, the tensile product (TB×EB) was calculated.
[0156] (Payne Effect Value)
[0157] Using a viscoelasticity spectrometer VR-7110 (manufactured by Ueshima Seisakusho Co., Ltd.), the dynamic modulus [E'(0.1)] at a deformation of 0.1% was measured at 50 Hz and 60°C. In addition, the dynamic modulus [E'(2.0)] at a deformation of 2.0% was also measured. The difference between the two [E'(0.1)-E'(2.0)] was calculated as the Payne effect value. In the dynamic viscoelasticity of rubber mixed with carbon black, the dynamic modulus in the low deformation region is largely dependent on the cohesion of the carbon blacks; while the dynamic modulus in the high deformation region is less dependent on the cohesion of the carbon blacks because the carbon blacks are forced to be pulled apart by external forces due to the elongation of the rubber; and the dynamic modulus of the rubber itself in the state without carbon black mixing is highly dependent. Therefore, the smaller the difference in the dynamic modulus (Payne effect) between the low deformation region and the high deformation region, the lower the cohesion of the carbon blacks in the microscopic region of the rubber, in other words, the higher the dispersion of the carbon black in the microscopic region.
[0158] (Dispersion rate)
[0159] The area occupied by undispersed blocks of carbon black larger than 3 μm in a fixed field of view was measured using disperGRADERαview SR manufactured by Alpha Technology in accordance with ASTM D7723, and the dispersion rate (%) was calculated. This dispersion rate is different from the value of the Payne effect and indicates the dispersibility of carbon black in a macroscopic region. The smaller the value, the higher the dispersibility in the macroscopic region.
[0160] (Research)
[0161] The results are shown in Table 1-1, Table 1-2, and Table 2.
[0162] The nitrogen adsorption specific surface area (N2SA), N2SA / IA, DBP absorption, NMR hydrogen content and ΔD of Examples 1 to 12 are within the above-mentioned specific ranges. However, the manufacturing conditions of Comparative Examples 1 to 10, and / or at least one of the above-mentioned characteristics are outside the specific ranges.
[0163] Examples 1 to 12 have larger tensile products (TB×EB) than Comparative Examples 1 to 10. That is, it is understood that the rubber members mixed with the carbon black according to Examples 1 to 12 are easily stretched and have high strength.
[0164] In addition, Examples 1 to 12 have lower Payne effect values and higher dispersion rates than Comparative Examples 1 to 10. It is therefore believed that the carbon blacks of Examples 1 to 12 have high dispersibility not only in the macroscopic region but also in the microscopic region, thereby achieving high reinforcement.
[0165] In summary, by setting the nitrogen adsorption specific surface area (N2SA), DBP absorption, N2SA / IA, NMR hydrogen content and ΔD within a specific range, carbon black with excellent dispersibility in both macro and micro regions can be obtained, thereby greatly improving the tensile product of rubber parts compared to existing rubber parts.
[0166] [Table 1-1]
[0167]
[0168] [Table 1-2] Table 2
[0169]
[0170] [Table 2]
[0171]
[0172] Explanation of symbols
[0173] 1 Oxygen-containing gas inlet
[0174] 2 Combustion burner
[0175] 3. Alkali metal salt and aqueous solution supply nozzle
[0176] 4 Fuel combustion area
[0177] 5. Raw oil introduction nozzle
[0178] 6Raw material import area
[0179] 7Refrigerant inlet nozzle
[0180] 8Coolant inlet nozzle
[0181] 9 Reaction Area
[0182] 10 reactors.
Claims
1. A method for producing carbon black, comprising the following steps: A reaction step in which hydrocarbons as raw materials are incompletely burned in a reaction furnace to generate carbon black raw materials; a granulation step of granulating the carbon black raw material to a predetermined size; and a drying step of dehydrating and drying the granulated carbon black raw material; in, The reaction process is carried out in a reaction region between a position where the refrigerant is introduced and a position where the cooling liquid is introduced in the reaction furnace. A refrigerant is introduced to make the temperature of the reaction zone 800-900°C, A cooling liquid was introduced to stop the reaction by rapid cooling, so that the residence time became 20 to 30 milliseconds.
2. Carbon black produced by the production method according to claim 1.