LED electrode and preparation method thereof
By sequentially evaporating a chromium layer, an aluminum-copper layer, a ruthenium-platinum alloy layer and a gold layer on the LED chip, the problem of heat loss and photon overflow of the LED chip under high current is solved, the hardness and toughness of the electrode is improved, and the life of the LED chip is extended. and improved its reliability.
Patent Information
- Application Number
- CN202211221466.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-10-08
AI Technical Summary
When high-power LED chips are driven by large currents, it is easy to damage the electrode structure due to heat loss and shorten the life. Some photons cannot escape, causing the junction temperature to rise, affecting the stability of the electrodes.
The LED electrode structure includes a chromium layer, an aluminum-copper layer, a ruthenium-platinum alloy layer and a gold layer. The ruthenium-platinum alloy layer enhances the hardness, toughness and corrosion resistance of the electrode through multiple repeated growth of titanium, platinum and ruthenium gold layers. Ability to reduce the evaporation rate of platinum and ruthenium to control the cavity temperature, avoid carbonization of the photoresist, and introduce nitrogen at high temperatures to prevent metal oxidation.
It improves the driving resistance and high-temperature stability of the LED electrode, extends the life of the high-power LED chip, enhances its reliable performance, and controls the cost.
Smart Images

Figure CN115458657B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor electronic technology, and in particular to an LED electrode and a preparation method thereof. Background Art
[0002] Gallium nitride-based light emitting diodes (LEDs) have the advantages of low functional loss, long life, and good reliability, and are widely used in signal lights, backlight displays, automotive lighting, and indoor lighting. With the popularization and application of high-power and high-efficiency LEDs, LEDs have a broader application market and their application value will be higher.
[0003] However, high-power LED chips must be able to withstand the test of high current. When LED chips are driven by high current, the PN junction cannot be extremely perfect, and the injection efficiency of the component will not reach 100%. That is, when the LED is working, in addition to the P region injecting charges (holes) into the N region, the N region will also inject charges (electrons) into the P region. Generally, the latter type of charge injection will not produce a photoelectric effect, but will be consumed in the form of heat. Even if the useful part of the injected charge is not all converted into light, a part of it will combine with impurities or defects in the junction area and eventually turn into heat.
[0004] At present, advanced material growth and component manufacturing processes have enabled most of the input electrical energy of LEDs to be converted into light radiation energy. However, since the refractive index of LED chip materials is much larger than that of the surrounding medium, most of the photons generated inside the chip cannot smoothly overflow the interface, but are totally reflected at the interface between the chip and the medium, returning to the inside of the chip and eventually being absorbed by the chip material or substrate through multiple internal reflections, and converted into heat in the form of lattice vibrations, causing the junction temperature to rise. The junction temperature of some LEDs is as high as 200°C, which will pose a great test to the electrode structure. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide an LED electrode and a preparation method thereof, which can stably drive under high current conditions and extend the life of a high-power LED chip.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0007] An LED electrode comprises a chromium layer, an aluminum-copper layer, a ruthenium-platinum alloy layer and a gold layer stacked in sequence;
[0008] The chromium layer is adhered to the LED chip, and the ruthenium-platinum alloy layer includes a titanium layer, a platinum layer, a ruthenium-gold layer and a platinum layer that are repeatedly grown, and the thickness of each platinum layer is The thickness of each ruthenium-gold layer is
[0009] In order to solve the above technical problems, another technical solution adopted by the present invention is:
[0010] A method for preparing an LED electrode, comprising the steps of:
[0011] A chromium layer, an aluminum-copper layer, a ruthenium-platinum alloy layer, and a gold layer are sequentially deposited on the LED chip;
[0012] The ruthenium-platinum alloy layer includes a titanium layer, a platinum-gold layer, a ruthenium-gold layer and a platinum-gold layer that are repeatedly grown, and the vapor deposition thickness of each platinum-gold layer is The evaporation thickness of each ruthenium-gold layer is
[0013] The beneficial effects of the present invention are as follows: a chromium layer, an aluminum-copper layer, a ruthenium-platinum alloy layer and a gold layer are sequentially evaporated on the LED chip, and the ruthenium-platinum alloy layer includes a titanium layer, a platinum-gold layer, a ruthenium-gold layer and a platinum-gold layer that are repeatedly grown, and the hardness and toughness of the LED electrode can be enhanced through the unique properties of the platinum-ruthenium alloy, and the platinum-ruthenium alloy has strong corrosion resistance and extremely high thermal stability. Under the drive of a large current, the LED chip can emit light stably; and the platinum-ruthenium atoms in the ruthenium-platinum alloy cannot completely penetrate each other, and the penetration depth is usually about Therefore, the thickness of the platinum layer and the ruthenium layer is designed to be On the one hand, it ensures the driving resistance of the LED electrode, and on the other hand, it controls the lower cost, thereby greatly improving the reliability of high-power LEDs. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 is a schematic diagram of an LED electrode according to an embodiment of the present invention;
[0015] Figure 2 The present invention is a flowchart of a method for preparing an LED electrode according to an embodiment of the present invention. DETAILED DESCRIPTION
[0016] In order to explain the technical content, achieved objectives and effects of the present invention in detail, the following is an explanation in combination with the implementation modes and the accompanying drawings.
[0017] Please refer to Figure 1 , an embodiment of the present invention provides an LED electrode, comprising a chromium layer, an aluminum-copper layer, a ruthenium-platinum alloy layer and a gold layer stacked in sequence;
[0018] The chromium layer is adhered to the LED chip, and the ruthenium-platinum alloy layer includes a titanium layer, a platinum layer, a ruthenium-gold layer and a platinum layer that are repeatedly grown, and the thickness of each platinum layer is The thickness of each ruthenium-gold layer is
[0019] From the above description, it can be seen that the beneficial effects of the present invention are: a chromium layer, an aluminum-copper layer, a ruthenium-platinum alloy layer and a gold layer are sequentially evaporated on the LED chip, and the ruthenium-platinum alloy layer includes a titanium layer, a platinum-gold layer, a ruthenium-gold layer and a platinum-gold layer that are repeatedly grown, and the hardness and toughness of the LED electrode can be enhanced through the unique properties of the platinum-ruthenium alloy, and the platinum-ruthenium alloy has strong corrosion resistance and extremely high thermal stability. Under the drive of a large current, the LED chip can emit light stably; and the platinum-ruthenium atoms in the ruthenium-platinum alloy cannot completely penetrate each other, and the penetration depth is usually about Therefore, the thickness of the platinum layer and the ruthenium layer is designed to be On the one hand, it ensures the driving resistance of the LED electrode, and on the other hand, it controls the lower cost, thereby greatly improving the reliability of high-power LEDs.
[0020] Furthermore, the thickness of the chromium layer is The thickness of the aluminum copper is The thickness of the gold layer is
[0021] From the above description, it can be seen that the thickness of the preparation is The chromium layer can achieve the first layer adhesion of the electrode and improve the ohmic contact of the electrode; the thickness of the preparation is The aluminum-copper layer can provide the reliability of the electrode.
[0022] Furthermore, the thickness of the titanium layer is
[0023] Furthermore, the ruthenium-platinum alloy layer includes a titanium layer, a platinum layer, a ruthenium-gold layer and a platinum-gold layer which are repeatedly grown three times.
[0024] From the above description, it can be seen that repeating the evaporation of titanium layer, platinum layer, ruthenium gold layer and platinum layer three times can increase the driving current of the LED, thereby improving the high-temperature driving stability of the LED and ensuring the driving resistance of the LED electrode.
[0025] Please refer to Figure 2 Another embodiment of the present invention provides a method for preparing an LED electrode, comprising the steps of:
[0026] A chromium layer, an aluminum-copper layer, a ruthenium-platinum alloy layer, and a gold layer are sequentially deposited on the LED chip;
[0027] The ruthenium-platinum alloy layer includes a titanium layer, a platinum-gold layer, a ruthenium-gold layer and a platinum-gold layer that are repeatedly grown, and the vapor deposition thickness of each platinum-gold layer is The evaporation thickness of each ruthenium-gold layer is
[0028] From the above description, it can be seen that the chromium layer, aluminum-copper layer, ruthenium-platinum alloy layer and gold layer are sequentially evaporated on the LED chip, and the ruthenium-platinum alloy layer includes a titanium layer, a platinum-gold layer, a ruthenium-gold layer and a platinum-gold layer that are repeatedly grown. The unique properties of the platinum-ruthenium alloy can enhance the hardness and toughness of the LED electrode. The platinum-ruthenium alloy has strong corrosion resistance and extremely high thermal stability. Under the drive of large current, the LED chip can emit light stably. In addition, the platinum-ruthenium atoms in the ruthenium-platinum alloy cannot completely penetrate each other, and the penetration depth is usually about Therefore, the thickness of the platinum layer and the ruthenium layer is designed to be On the one hand, it ensures the driving resistance of the LED electrode, and on the other hand, it controls the lower cost, thereby greatly improving the reliability of high-power LEDs.
[0029] Further, evaporating the ruthenium-platinum alloy layer comprises:
[0030] use The titanium layer was evaporated at a rate of The platinum layer and the ruthenium layer are evaporated at a rate of.
[0031] From the above description, we can know that adding platinum between titanium and ruthenium is to overcome the problem of high temperature in the cavity. When evaporating platinum and ruthenium, the cavity temperature will rise very quickly because the melting point of platinum and ruthenium is very high. However, before evaporating the LED electrode, the wafer needs to be covered with a layer of photoresist as a mask, and the temperature resistance of the photoresist is normally around 110°C. Too high a temperature will carbonize the photoresist, resulting in abnormal LED electrode patterns. Therefore, by reducing the evaporation rate of platinum and ruthenium to The temperature of the evaporation chamber can be controlled at about 100°C to avoid carbonization of the photoresist and cause abnormality of the LED electrode.
[0032] Furthermore, the step of sequentially evaporating a chromium layer, an aluminum-copper layer, a ruthenium-platinum alloy layer and a gold layer on the LED chip comprises:
[0033] A high-temperature furnace tube at 250° C. was used to introduce nitrogen into the LED chip.
[0034] From the above description, it can be seen that after evaporation, the alloying operation is carried out for 15 minutes in a high-temperature furnace tube at 250° C. and nitrogen is introduced to avoid oxidation of the metal during the alloying process.
[0035] The LED electrode and the preparation method thereof described above are suitable for preparing high-power LED electrodes, and are described below through specific implementation methods:
[0036] Embodiment 1
[0037] Please refer to Figure 1 , an LED electrode, comprising a chromium layer, an aluminum-copper layer, a ruthenium-platinum alloy layer and a gold layer stacked in sequence;
[0038] The chromium layer adheres to the LED chip, and the ruthenium-platinum alloy layer includes a titanium layer, a platinum layer, a ruthenium-gold layer, and a platinum layer that are repeatedly grown. The thickness of each platinum layer is The thickness of each Ru-Au layer is
[0039] The thickness of the chromium layer is The thickness of aluminum copper is The thickness of the gold layer is The thickness of the titanium layer is
[0040] In some embodiments, the ruthenium-platinum alloy layer includes a titanium layer, a platinum layer, a ruthenium-gold layer, and a platinum-gold layer that are repeatedly grown three times.
[0041] Therefore, the high-power LED driving current of the LED electrode of this embodiment can be increased by about 1.5 times, thereby improving the high-temperature driving stability of the LED.
[0042] Embodiment 2
[0043] Please refer to Figure 2 , a method for preparing an LED electrode, comprising the steps of:
[0044] S1. A chromium layer, an aluminum-copper layer, a ruthenium-platinum alloy layer and a gold layer are sequentially deposited on the LED chip.
[0045] S2, the ruthenium-platinum alloy layer includes a titanium layer, a platinum layer, a ruthenium-gold layer and a platinum-gold layer that are repeatedly grown, and the vapor deposition thickness of each of the platinum-gold layers is The evaporation thickness of each ruthenium-gold layer is
[0046] S3, using a high-temperature furnace tube at 250° C. to introduce nitrogen into the LED chip.
[0047] Wherein, evaporating the ruthenium-platinum alloy layer comprises:
[0048] use The titanium layer was evaporated at a rate of The platinum layer and the ruthenium layer are evaporated at a rate of.
[0049] In this embodiment, the electrode is placed in a high vacuum environment of 1.0E-6Torr or higher, the plating pot speed is set to 7-9rpm, preferably 8rpm in this embodiment; the plating pot inclination angle is 40-42°, preferably 41° in this embodiment, and the plating is repeated 3 times at room temperature to form a platinum-ruthenium alloy structure to enhance the high current driving stability. The specific steps are as follows:
[0050] Step 1: Chromium (Cr) evaporation: plating rate Thickness Preferably After evaporation, the plating source is cooled for 2 minutes to allow the functional first layer to adhere and improve ohmic contact.
[0051] Step 2: Aluminum-copper (AlCu) evaporation: plating rate Thickness Preferably After evaporation, the plating source is cooled for 5 minutes.
[0052] Step 3: Titanium (Ti) evaporation: plating rate Thickness Preferably After evaporation, the plating source is cooled for 10 minutes.
[0053] Step 4: Platinum (Pt) evaporation: plating rate Thickness Preferably After evaporation, the plating source is cooled for 10 minutes.
[0054] Step 5: Ruthenium (Ru) evaporation: plating rate Thickness Preferably After evaporation, the plating source was cooled for 17 minutes.
[0055] Step 6: Platinum (Pt) evaporation: plating rate Thickness Preferably After evaporation, the plating source is cooled for 10 minutes.
[0056] Step 7: Repeat steps 3 to 6 twice.
[0057] Step 8: Gold (Au) evaporation: plating rate Thickness Preferably After evaporation, the plating source is cooled for 15 minutes.
[0058] After evaporation, use a high-temperature furnace tube at 250°C to alloy for 15 minutes (13 to 17 minutes), and introduce nitrogen to prevent the metal from being oxidized during the alloying process. The alloying can enhance the ohmic contact between the electrode and the semiconductor layer, and also form an alloy structure between the metals, thereby improving the driving resistance of the electrode.
[0059] Among them, adding platinum between titanium and ruthenium is to overcome the problem of high temperature in the cavity. When evaporating platinum and ruthenium, the cavity temperature will rise very quickly because the melting point of platinum and ruthenium is very high, about 1768~2310℃. However, before evaporating the LED electrode, the wafer needs to be covered with a layer of photoresist as a mask, and the temperature resistance of the photoresist is normally around 110℃. Too high a temperature will carbonize the photoresist, resulting in abnormal LED electrode patterns. Therefore, in this embodiment, the cooling time of the target material is extended to 163min, the cooling water volume of the evaporation cavity is increased to 10.5L / min, and the evaporation rate of platinum and ruthenium is reduced to Thereby controlling the temperature of the evaporation chamber at about 100°C, avoiding carbonization of the photoresist and causing abnormality of the LED electrode.
[0060] Please refer to Table 1. When the chip size is about 850*400μm, the voltage rise is observed under constant temperature and humidity at different currents, i.e. 85℃, 85%RH, for 192H aging. The voltage rise indicates that the electrode begins to overload and deteriorate, which may easily lead to the situation that the lamp is not lit. When the voltage is 0.1V higher, the lamp starts to be dim, and when the voltage is 0.2V higher, the electrode finger is basically burned out.
[0061] Table 1 Voltage of different electrode structures at different currents
[0062]
[0063]
[0064] In summary, the present invention provides an LED electrode and a preparation method thereof, wherein a chromium layer, an aluminum-copper layer, a ruthenium-platinum alloy layer and a gold layer are sequentially evaporated on an LED chip, and the ruthenium-platinum alloy layer includes a titanium layer, a platinum-gold layer, a ruthenium-gold layer and a platinum-gold layer that are repeatedly grown. The hardness and toughness of the LED electrode can be enhanced by the unique properties of the platinum-ruthenium alloy, and the platinum-ruthenium alloy has strong corrosion resistance and extremely high thermal stability. Under the drive of a large current, the LED chip can emit light stably. Moreover, the platinum-ruthenium atoms in the ruthenium-platinum alloy cannot completely penetrate each other, and the penetration depth is usually about Therefore, the thickness of the platinum layer and the ruthenium layer is designed to be On the one hand, it ensures the driving resistance of the LED electrode, and on the other hand, it controls the lower cost, thereby greatly improving the reliability of high-power LEDs.
[0065] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention's specification and drawings, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. An LED electrode, characterized in that: It includes a chromium layer, an aluminum-copper layer, a ruthenium-platinum alloy layer and a gold layer stacked in sequence; The chromium layer is adhered to the LED chip, and the ruthenium-platinum alloy layer includes a titanium layer, a platinum layer, a ruthenium-gold layer and a platinum layer that are repeatedly grown, and the thickness of each platinum layer is The thickness of each ruthenium-gold layer is 2. The LED electrode according to claim 1, characterized in that: The thickness of the chromium layer is The thickness of the aluminum copper is The thickness of the gold layer is 3. The LED electrode according to claim 1, characterized in that: The thickness of the titanium layer is 4. The LED electrode according to claim 1, characterized in that: The ruthenium-platinum alloy layer includes a titanium layer, a platinum-gold layer, a ruthenium-gold layer and a platinum-gold layer which are repeatedly grown three times.
5. A method for preparing an LED electrode, characterized in that: Includes steps: A chromium layer, an aluminum-copper layer, a ruthenium-platinum alloy layer, and a gold layer are sequentially deposited on the LED chip; The ruthenium-platinum alloy layer includes a titanium layer, a platinum-gold layer, a ruthenium-gold layer and a platinum-gold layer that are repeatedly grown, and the vapor deposition thickness of each platinum-gold layer is The evaporation thickness of each ruthenium-gold layer is 6. The method for preparing an LED electrode according to claim 5, characterized in that: The evaporation of the ruthenium-platinum alloy layer comprises: use The titanium layer was evaporated at a rate of The platinum layer and the ruthenium layer are evaporated at a rate of.
7. The method for preparing an LED electrode according to claim 5, characterized in that: The step of sequentially evaporating a chromium layer, an aluminum-copper layer, a ruthenium-platinum alloy layer and a gold layer on the LED chip comprises: A high-temperature furnace tube at 250° C. was used to introduce nitrogen into the LED chip.
Citation Information
Patent Citations
Light-emitting diode and manufacturing method thereof
CN111048642A
Optical device and method of fabricating the same
WO2007069871A1