A method for manufacturing a composite substrate from discarded bamboo fiber lunch boxes, a composite substrate and a damping composite floor and applications thereof

By using waste bamboo fiber lunch boxes to prepare regenerated bamboo fiber-rubber particle composite substrates, and combining them with melamine formaldehyde resin-impregnated adhesive film paper, the environmental pollution and performance problems of traditional disposable plastic lunch boxes and artificial boards have been solved, and efficient reduction has been achieved. Vibration damping performance and lightweight, high-strength composite substrate are suitable for ground paving and container floors.

CN115464897BActive Publication Date: 2024-10-18INT CENT FOR BAMBOO & RATTAN
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211132948.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-16
Publication Date
2024-10-18
Estimated Expiration
2042-09-16

AI Technical Summary

Technical Problem

Traditional disposable plastic lunch boxes are difficult to degrade and cause environmental pollution. At the same time, the processing and use of artificial boards have problems such as high cost, heavy weight, and poor vibration and damping performance.

Method used

By separating waste bamboo fiber lunch boxes into oil and water, soaking in hot water and crushing them, long and short bamboo fibers are sorted out, mixed with rubber particles and phenolic resin, and molded to prepare a regenerated bamboo fiber-rubber particle composite substrate. Melamine formaldehyde resin impregnated film paper is laminated to prepare damping composite flooring.

Benefits of technology

Efficient reuse of low-quality resources is achieved. The resulting composite substrate has good vibration damping properties, is lightweight, has high strength, has good wear resistance and weather resistance, and is suitable for ground paving and container flooring.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115464897B_ABST
    Figure CN115464897B_ABST
Patent Text Reader

Abstract

The present invention provides a method for manufacturing a composite substrate from a discarded bamboo fiber lunch box, a composite substrate and a damping composite floor and their applications, and relates to the technical field of composite materials. The method for manufacturing a regenerated bamboo fiber-rubber particle composite substrate from a discarded bamboo fiber lunch box provided by the present invention comprises the following steps: subjecting the discarded bamboo fiber lunch box to an oil-water separation treatment to obtain a clean lunch box; subjecting the clean lunch box to a hot water soaking treatment, crushing the clean lunch box in a wet state, and sorting out long bamboo fibers and short bamboo fibers; mixing the long bamboo fibers, short bamboo fibers, rubber particles and phenolic resin, and performing compression molding to obtain a regenerated bamboo fiber-rubber particle composite substrate. The present invention uses discarded bamboo fiber lunch boxes as raw materials to prepare composite substrates, thereby achieving efficient reuse of low-quality resources, and the obtained composite substrate not only has good vibration damping characteristics, but also has the advantages of lightweight and high strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite materials, and in particular to a method for manufacturing a composite substrate from discarded bamboo fiber lunch boxes, a composite substrate and a damping composite floor and applications thereof. Background Art

[0002] The growing development of the mobile Internet industry has brought many conveniences to our daily lives. The takeaway industry, which represents "Internet + catering", is gradually changing everyone's dining habits. "Ordering takeaway" has become an important dining form for the majority of office workers and students. While takeaways bring convenience to life, they are also accompanied by many problems. Traditional disposable plastic lunch boxes are difficult to degrade, generating a huge amount of white garbage, causing major environmental pollution problems.

[0003] my country has always attached great importance to environmental protection. In view of the fact that my country has abundant bamboo resources and advanced bamboo product development technology, the International Bamboo and Rattan Center has put forward the idea of ​​"replacing plastic with bamboo" in response to the current situation. By rationally using renewable and easily degradable green bamboo to replace plastic, the use of disposable plastic products can be reduced and the damage to the environment caused by the use of plastic products can be alleviated. Environmentally friendly products such as bagasse, corn starch, PLA and bamboo fiber disposable lunch boxes and containers have emerged as a substitute for plastic products. While providing convenience for people's daily lives, they have effectively reduced the negative effects on the environment.

[0004] As a traditional industrial material, wood-based panels are widely used in the fields of construction, transportation, aerospace, etc. However, there are many problems in the processing and use of wood-based panels: (1) The production of wood-based panels relies on imported raw materials, which is costly; (2) Pure wood-based panels have poor vibration damping performance and high weight, which limits their application areas. Summary of the invention

[0005] The purpose of the present invention is to provide a method for manufacturing a composite substrate from discarded bamboo fiber lunch boxes, a composite substrate and a damping composite floor and their applications. The present invention uses discarded bamboo fiber lunch boxes as raw materials to prepare the composite substrate, thereby achieving efficient recycling of low-quality resources. The obtained composite substrate not only has good vibration reduction and damping properties, but also has the advantages of light weight and high strength.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for manufacturing a regenerated bamboo fiber-rubber particle composite substrate from a discarded bamboo fiber lunch box, comprising the following steps:

[0008] The discarded bamboo fiber lunch box is subjected to oil-water separation treatment to obtain a clean lunch box; the bamboo fiber content of the discarded bamboo fiber lunch box is 85-98wt%;

[0009] The clean lunch box is soaked in hot water, crushed in a wet state, and sorted to obtain long bamboo fibers and short bamboo fibers; the long bamboo fibers have a length of 7 to 12 mm and an average diameter of 0.5 to 0.8 mm; the short bamboo fibers have a length of greater than or equal to 2 mm and less than 7 mm, and an average diameter of greater than or equal to 0.2 mm and less than 0.5 mm;

[0010] The long bamboo fibers, short bamboo fibers, rubber particles and phenolic resin are mixed and compression molded to obtain a regenerated bamboo fiber-rubber particle composite substrate.

[0011] Preferably, the oil-water separation process adopts micro-nano bubble technology.

[0012] Preferably, the particle size of the bubbles in the oil-water separation process is 100 nm to 50 μm.

[0013] Preferably, the washing solution used in the oil-water separation treatment is a surfactant solution; the flow rate of the washing solution is 3 to 4 L / min.

[0014] Preferably, the temperature of the hot water immersion treatment is 85-95° C.; the time of the hot water immersion treatment is 1.5-3 hours.

[0015] Preferably, the mass ratio of the long bamboo fibers, the short bamboo fibers, the rubber particles and the phenolic resin is (25-45): (25-45): (15-20): (8-15).

[0016] Preferably, the compression molding includes pre-pressing and hot pressing molding performed in sequence; the pre-pressing temperature is 130-140°C; the pre-pressing pressure is 0.8-1.5MPa; the holding time of the pre-pressing is 30s-1min; the hot pressing temperature is 145-155°C; the hot pressing pressure is 1-2MPa; the holding time of the hot pressing is 10-20min.

[0017] The present invention provides a regenerated bamboo fiber-rubber particle composite substrate prepared by the method described in the above technical solution.

[0018] The invention provides a damping composite floor, comprising a laminated composite substrate and melamine formaldehyde resin impregnated adhesive film paper; the composite substrate is the regenerated bamboo fiber-rubber particle composite substrate described in the above technical solution.

[0019] The present invention provides the application of the damping composite floor described in the above technical solution in ground laying and container bottom plate.

[0020] The present invention provides a method for manufacturing a regenerated bamboo fiber-rubber particle composite substrate from a discarded bamboo fiber lunch box. The present invention uses oil-water separation to remove oil stains on the discarded bamboo fiber lunch box to obtain a clean lunch box; during the hot water soaking process, the moisture content of the clean lunch box increases, and the structure becomes loose, which is conducive to subsequent crushing treatment; the present invention sorts out long bamboo fibers and short bamboo fibers, wherein the spatial mesh structure composed of the long bamboo fibers can improve the mechanical strength of the composite substrate, and the short bamboo fibers and rubber particles fill the gaps in the mesh structure, which can improve the vibration damping performance of the composite substrate. The present invention uses discarded bamboo fiber lunch boxes as raw materials, uses oil-water separation, hot water soaking, crushing, and sorting processes to obtain two types of regenerated bamboo fibers with different aspect ratios, and mixes the two types of regenerated bamboo fibers with rubber particles, and molds them to obtain a lightweight substrate with good vibration damping properties. The present invention realizes the efficient reuse of low-quality resources, and the obtained composite substrate not only has good vibration damping properties, but also has the advantages of lightweight and high strength.

[0021] The present invention also provides a damping composite floor, which is laminated with melamine formaldehyde resin impregnated adhesive film paper and a composite substrate to obtain a composite floor with good wear resistance and weather resistance. The damping composite floor provided by the present invention can be widely used in the field of ground paving and container bottom plates. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A schematic diagram of the structure of a recycled bamboo fiber-rubber particle composite substrate made from discarded bamboo fiber lunch boxes of the present invention;

[0023] Figure 2 It is a schematic structural diagram of the damping composite floor of the present invention. DETAILED DESCRIPTION

[0024] The present invention provides a method for manufacturing a regenerated bamboo fiber-rubber particle composite substrate from a discarded bamboo fiber lunch box, comprising the following steps:

[0025] The discarded bamboo fiber lunch box is subjected to oil-water separation treatment to obtain a clean lunch box; the bamboo fiber content of the discarded bamboo fiber lunch box is 85-98wt%;

[0026] The clean lunch box is soaked in hot water, crushed in a wet state, and sorted to obtain long bamboo fibers and short bamboo fibers; the long bamboo fibers have a length of 7 to 12 mm and an average diameter of 0.5 to 0.8 mm; the short bamboo fibers have a length of greater than or equal to 2 mm and less than 7 mm, and an average diameter of greater than or equal to 0.2 mm and less than 0.5 mm;

[0027] The long bamboo fibers, short bamboo fibers, rubber particles and phenolic resin are mixed and compression molded to obtain a regenerated bamboo fiber-rubber particle composite substrate.

[0028] The present invention performs oil-water separation on the discarded bamboo fiber lunch box to obtain a clean lunch box. In the present invention, the bamboo fiber content of the discarded bamboo fiber lunch box is 85-98wt%, preferably 90-95wt%. Before performing the oil-water separation, the present invention preferably further includes removing food residues on the surface of the discarded bamboo fiber lunch box.

[0029] In the present invention, the oil-water separation treatment preferably adopts micro-nano bubble technology. In the present invention, the particle size of the bubbles in the oil-water separation treatment process is preferably 100nm~50μm. In the present invention, the washing solution used in the oil-water separation treatment is preferably a surfactant solution, more preferably a cetyltrimethylammonium bromide (CTAB) solution. In the present invention, the concentration of the CTAB solution is preferably 250mg / L. In the present invention, the flow rate of the washing solution is preferably 3~4L / min, more preferably 3.5L / min. In the present invention, the temperature of the oil-water separation treatment is preferably 25~30℃, more preferably 26~29℃; the time of the oil-water separation treatment is preferably 50min~2h, more preferably 1h. In the present invention, after the oil-water separation treatment, the treated lunch box is preferably washed with clean water to obtain a clean lunch box.

[0030] After obtaining the clean lunch box, the present invention soaks the clean lunch box in hot water, performs crushing in a wet state, and sorts out long bamboo fibers and short bamboo fibers. In the present invention, the temperature of the hot water soaking treatment is preferably 85 to 95° C., more preferably 89 to 92° C.; the time of the hot water soaking treatment is preferably 1.5 to 3 hours, more preferably 2 hours. The present invention performs crushing in a wet state to improve the efficiency of mechanical crushing and reduce production time and energy consumption.

[0031] In the present invention, the crushing process is preferably carried out by using a wood fiber crusher. In the present invention, the crushing process is preferably followed by drying and then sorting.

[0032] In the present invention, the separation is preferably carried out by using an air separator to obtain long bamboo fibers and short bamboo fibers. In the present invention, the moisture content of the long bamboo fibers and short bamboo fibers is preferably 7-11wt%, more preferably 8-10wt%.

[0033] In the present invention, the length of the long bamboo fiber is 7-12 mm, and the average length is preferably 9 mm; the average diameter is 0.5-0.8 mm, and preferably 0.6-0.7 mm; the density of the long bamboo fiber is preferably 0.7-0.8 g / cm 3 , more preferably 0.78 g / cm 3In the present invention, the length of the short bamboo fiber is greater than or equal to 2 mm and less than 7 mm, and the average length is preferably 4 mm; the average diameter is greater than or equal to 0.2 mm and less than 0.5 mm, and preferably 0.3 mm; the density of the short bamboo fiber is preferably 0.7-0.8 g / cm 3 , more preferably 0.78 g / cm 3 .

[0034] After obtaining the long bamboo fibers and the short bamboo fibers, the present invention mixes the long bamboo fibers, the short bamboo fibers, the rubber particles and the phenolic resin, and performs compression molding to obtain a regenerated bamboo fiber-rubber particle composite substrate. In the present invention, the mass ratio of the long bamboo fibers, the short bamboo fibers, the rubber particles and the phenolic resin is preferably (25-45): (25-45): (15-20): (8-15), and more preferably 32:39:18:11. In the present invention, the particle size of the rubber particles is preferably 25-30 meshes; irregular shape. In the present invention, the solid content of the phenolic resin is preferably 30-55wt%, and more preferably 45wt%.

[0035] In the present invention, the compression molding preferably includes pre-pressing and hot pressing molding performed in sequence; the pre-pressing temperature is preferably 130-140°C; the pre-pressing pressure is preferably 0.8-1.5MPa, more preferably 1MPa; the holding time of the pre-pressing is preferably 30s-1min, more preferably 40s; the hot pressing temperature is preferably 145-155°C, more preferably 149-152°C; the hot pressing pressure is preferably 1-2MPa, more preferably 1.5MPa; the heat preservation and holding time of the hot pressing is preferably 10-20min, more preferably 15min.

[0036] In the present invention, after the compression molding, the obtained plate is preferably subjected to aging and sanding treatment in sequence. In the present invention, the aging time is preferably 1 day.

[0037] The present invention provides a regenerated bamboo fiber-rubber particle composite substrate prepared by the method described in the above technical solution. The regenerated bamboo fiber-rubber particle composite substrate prepared by the present invention is as follows Figure 1 As shown, long bamboo fibers are interwoven to form a spatial network structure, and short bamboo fibers and rubber particles are evenly dispersed and filled in the spatial network structure. The regenerated bamboo fiber-rubber particle composite substrate prepared by the present invention increases the internal friction absorption of energy and has good vibration damping properties.

[0038] In the present invention, the thickness of the regenerated bamboo fiber-rubber particle composite substrate is preferably 8 to 20 mm, and more preferably 10 to 15 mm.

[0039] The present invention provides a damping composite floor, such as Figure 2As shown, it comprises a laminated composite substrate and melamine formaldehyde resin impregnated film paper; the composite substrate is the recycled bamboo fiber-rubber particle composite substrate described in the above technical solution. In the present invention, the density of the melamine formaldehyde resin impregnated film paper is preferably 90g / cm 3 The preferred amount of impregnation is 135%, and the preferred degree of pre-curing is 45%. In the present invention, the melamine formaldehyde resin impregnated adhesive film paper can improve the mechanical properties and oil resistance of the board surface.

[0040] In the present invention, the preparation method of the damping composite floor preferably comprises: placing melamine formaldehyde resin impregnated adhesive film paper on the surface of the composite substrate, and hot pressing to obtain the damping composite floor. In the present invention, the pressure of the hot pressing is preferably 0.8 MPa, the temperature is preferably 125-130°C, more preferably 126-129°C; the heat preservation and pressure holding time is preferably 7 minutes.

[0041] The present invention provides the application of the damping composite floor described in the above technical solution in ground paving and container bottom plates. The damping composite floor provided by the present invention has the advantages of light weight, good damping and shock absorption characteristics, high structural strength, and good wear resistance and weather resistance, and can be widely used in the field of ground paving and container bottom plate load-bearing.

[0042] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] Example 1

[0044] Material:

[0045] Discarded bamboo fiber lunch boxes;

[0046] CTAB: domestic analytical grade;

[0047] Rubber particles: particle size 25-30 mesh, irregular shape;

[0048] Melamine formaldehyde resin film paper: 90g / cm 3 , dipping amount 135%, pre-curing degree 45%;

[0049] Phenolic resin: solid content 45wt%;

[0050] Preparation of recycled bamboo fiber-rubber particles composite substrate:

[0051] (1) Rinse the discarded bamboo fiber lunch box with running tap water until there is no obvious food residue attached to the surface; put the rinsed discarded bamboo fiber lunch box into a cleaning tank, and inject 250 mg / L CTAB aqueous solution until it covers the upper edge of the lunch box;

[0052] Turn on the micro-nano bubble generator and introduce micro-nano bubbles from the bottom of the cleaning tank. The bubble particle size is in the range of 100nm to 50μm. The water temperature is 29℃, the flow rate of the washing solution is 3.5L / min, and the washing is continued for 1h.

[0053] After washing, take out the lunch box and rinse it with clean water to obtain a clean lunch box;

[0054] (2) soaking the clean lunch box in hot water for 2 hours, with the water temperature maintained at 89° C.;

[0055] The wet discarded bamboo fiber lunch boxes were crushed by a wood fiber crusher and dried to a moisture content of 8wt%. The long bamboo fibers and short bamboo fibers were separated by a wind separator to obtain the long bamboo fibers with an average length of 9mm, an average diameter of 0.6mm and a density of 0.78g / cm 3 The average length of short bamboo fiber is 4mm, the average diameter is 0.3mm, and the density is 0.8g / cm 3 ;

[0056] (3) uniformly mixing rubber particles, long bamboo fibers, short bamboo fibers and phenolic resin, with the mixing mass ratio being: 18% of rubber particles, 32% of long bamboo fibers, 39% of short bamboo fibers and 11% of phenolic resin;

[0057] Paving; use a press to pre-press at a pressure of 1.0MPa for 40s;

[0058] The press was used for hot pressing, with a pressure of 1.5 MPa, a temperature of 149°C, a hot pressing time of 15 min, and a sheet thickness of 1.0 cm after pressing;

[0059] After being pressed and formed, the substrate was left to stand for 1 day and then sanded to obtain a regenerated bamboo fiber-rubber particle composite substrate.

[0060] The performance of the regenerated bamboo fiber-rubber particle composite substrate prepared in this embodiment was tested according to GB / T 17657-2013, and the surface bonding strength was 1.05 MPa, the static bending strength was 19.36 MPa, and the elastic modulus was 15.4 GPa.

[0061] Preparation of damping composite floor:

[0062] Melamine formaldehyde resin impregnated adhesive film paper is placed on the surface of the regenerated bamboo fiber-rubber particle composite substrate, and hot pressing is performed using a press with a pressure of 0.8 MPa, a temperature of 129° C., and a hot pressing time of 7 minutes to obtain a damping composite floor.

[0063] The performance of the damping composite floor prepared in this embodiment was tested according to GB / T 17657-2013 and GB / T 19889.3-2005. The thickness of the damping composite floor was 10 mm and the density was 0.95 g / cm 3 The wear value is 78.8mg / 100r, and the first three-order damping ratios are 3.14%, 3.56% and 3.44% respectively.

[0064] Comparative Example 1

[0065] Material:

[0066] Discarded bamboo fiber lunch boxes;

[0067] CTAB: domestic analytical grade;

[0068] Rubber particles: particle size 25-30 mesh, irregular shape;

[0069] Melamine formaldehyde resin film paper: 90g / cm 3 , dipping amount 135%, pre-curing degree 45%;

[0070] Phenolic resin: solid content 45wt%;

[0071] Preparation of recycled bamboo fiber-rubber particles composite substrate:

[0072] (1) Rinse the discarded bamboo fiber lunch box with running tap water until there is no obvious food residue attached to the surface; put the rinsed discarded bamboo fiber lunch box into a cleaning tank, and inject 250 mg / L CTAB aqueous solution until it covers the upper edge of the lunch box;

[0073] Turn on the micro-nano bubble generator and introduce micro-nano bubbles from the bottom of the cleaning tank. The bubble particle size is in the range of 100nm to 50μm. The water temperature is 29℃, the flow rate of the washing solution is 3.5L / min, and the washing is continued for 1h.

[0074] After washing, take out the lunch box and rinse it with clean water to obtain a clean lunch box;

[0075] (2) soaking the clean lunch box in hot water for 2 hours, with the water temperature maintained at 89° C.;

[0076] The wet discarded bamboo fiber lunch boxes were crushed with a wood fiber crusher and dried to a moisture content of 8wt% to obtain mixed fibers with an average length of 6mm, an average diameter of 0.5mm, and a density of 0.79g / cm 3;

[0077] (3) uniformly mixing rubber particles, long bamboo fibers, short bamboo fibers and phenolic resin, with the mixing mass ratio being: 18% of rubber particles, 71% of mixed bamboo fibers and 11% of phenolic resin;

[0078] Paving; use a press to pre-press at a pressure of 1.0MPa for 40s;

[0079] The press was used for hot pressing, with a pressure of 1.5 MPa, a temperature of 149°C, a hot pressing time of 15 min, and a sheet thickness of 1.0 cm after pressing;

[0080] After being pressed and formed, the substrate was left to stand for 1 day and then sanded to obtain a regenerated bamboo fiber-rubber particle composite substrate.

[0081] The performance of the regenerated bamboo fiber-rubber particle composite substrate prepared in this comparative example was tested according to GB / T 17657-2013, and the surface bonding strength was 0.96 MPa, the static bending strength was 17.02 MPa, and the elastic modulus was 13.2 GPa.

[0082] Preparation of damping composite floor:

[0083] Melamine formaldehyde resin impregnated adhesive film paper is placed on the surface of the regenerated bamboo fiber-rubber particle composite substrate, and hot pressing is performed using a press with a pressure of 0.8 MPa, a temperature of 129° C., and a hot pressing time of 7 minutes to obtain a damping composite floor.

[0084] The performance of the damping composite floor prepared in this comparative example was tested according to GB / T 17657-2013 and GB / T 19889.3-2005. The thickness of the damping composite floor was 10 mm and the density was 0.93 g / cm 3 The wear value is 77.9mg / 100r, and the first three-order damping ratios are 2.51%, 2.66% and 2.62% respectively.

[0085] Aiming at the shortcomings existing in the processing and utilization of bamboo-wood composite panels: (1) high density and heavy weight; (2) poor damping internal friction performance and poor vibration reduction effect; (3) high raw material cost and environmentally unfriendly production process; (4) low surface hardness, poor impact resistance and wear resistance, and single function. The composite substrate and damping composite floor prepared by the present invention have excellent vibration reduction and damping performance, are light and high-strength, and have excellent wear resistance. In addition, the present invention uses discarded bamboo fiber lunch boxes as raw materials, realizes the efficient application of low-quality resources, and has good economic and environmental benefits.

[0086] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for manufacturing a recycled bamboo fiber-rubber particle composite substrate from discarded bamboo fiber lunch boxes, comprising the following steps: The discarded bamboo fiber lunch box is subjected to oil-water separation treatment to obtain a clean lunch box; the bamboo fiber content of the discarded bamboo fiber lunch box is 85-98wt%; The clean lunch box is soaked in hot water, crushed in a wet state, and sorted to obtain long bamboo fibers and short bamboo fibers; the long bamboo fibers have a length of 7 to 12 mm and an average diameter of 0.5 to 0.8 mm; the short bamboo fibers have a length of greater than or equal to 2 mm and less than 7 mm, and an average diameter of greater than or equal to 0.2 mm and less than 0.5 mm; The long bamboo fibers, short bamboo fibers, rubber particles and phenolic resin are mixed and compression molded to obtain a regenerated bamboo fiber-rubber particle composite substrate; The mass ratio of the long bamboo fiber, the short bamboo fiber, the rubber particles and the phenolic resin is (25-45): (25-45): (15-20): (8-15); The compression molding includes pre-pressing and hot pressing molding performed in sequence; the pre-pressing temperature is 130-140°C; the pre-pressing pressure is 0.8-1.5MPa; the holding time of the pre-pressing is 30s-1min; the hot pressing temperature is 145-155°C; the hot pressing pressure is 1-2MPa; the heat preservation and holding time of the hot pressing is 10-20min.

2. The method according to claim 1, characterized in that The oil-water separation process adopts micro-nano bubble technology.

3. The method according to claim 2, characterized in that The particle size of the bubbles in the oil-water separation process is 100 nm to 50 μm.

4. The method according to claim 2 or 3, characterized in that: The washing solution used in the oil-water separation process is a surfactant solution; the flow rate of the washing solution is 3 to 4 L / min.

5. The method according to claim 1, characterized in that The temperature of the hot water soaking treatment is 85-95° C.; the time of the hot water soaking treatment is 1.5-3 hours.

6. The regenerated bamboo fiber-rubber particle composite substrate prepared by the method according to any one of claims 1 to 5.

7. A damping composite floor, characterized in that: It comprises a laminated composite substrate and melamine formaldehyde resin impregnated adhesive film paper; the composite substrate is the regenerated bamboo fiber-rubber particle composite substrate as claimed in claim 6.

8. Application of the damping composite floor according to claim 7 in ground paving and container bottom plates.

Citation Information

Patent Citations

  • Elastic layer with fibers

    EP3636835A1

  • Used paper board and method for manufacturing used paper board

    JP2001310310A