A method for evaluating the permeability of the tuyere whirlpool zone of a raw coal blast furnace

By using the softening temperature of the ash cone in the blast furnace tuyere whirling area to evaluate the air permeability, the problem that existing technology cannot accurately describe local air permeability is solved, and a reasonable description of the tuyere whirling area and simulation of the actual production environment are achieved.

CN115468974BActive Publication Date: 2024-10-08SHENHUA SHENDONG COAL GRP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211110565.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-13
Publication Date
2024-10-08
Estimated Expiration
2042-09-13

AI Technical Summary

Technical Problem

The existing technology cannot accurately describe and evaluate the local air permeability of the blast furnace tuyere convolution zone. It mainly describes it through the overall air permeability index. It cannot simulate the actual production environment and cannot make accurate evaluations in emergencies.

Method used

Raw coal is used as raw material, volatile matter is removed in an oxygen-free environment, and coke ash and unburned coal fly ash are obtained by burning, which are mixed to form an ash cone. The softening temperature of the ash cone in a reducing atmosphere is tested as the permeability of the blast furnace tuyere whirling zone. Evaluation indicators.

Benefits of technology

The softening temperature of the ash cone can accurately simulate the local permeability of the tuyere whirling zone of the blast furnace. Compared with the existing technology, the description of the tuyere whirling zone is more reasonable and can provide stable simulation and evaluation in the actual production environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004985074180000071
    Figure GDA0004985074180000071
  • Figure GDA0004985074180000081
    Figure GDA0004985074180000081
Patent Text Reader

Abstract

The present invention provides a method for evaluating the air permeability of a tuyere whirlpool zone of a raw coal blast furnace. The evaluation method comprises: step S1, using raw coal as raw material, removing volatiles from the raw coal in an oxygen-free environment to prepare unburned coal powder; step S2, burning coke and unburned coal powder as raw materials to obtain coke ash and unburned coal powder ash; step S3, mixing coke ash and unburned coal powder ash to form an ash cone, testing the softening temperature of the ash cone under a reducing atmosphere, and using the softening temperature as an evaluation index for the air permeability of the tuyere whirlpool zone of the blast furnace. The present application uses an ash cone to simulate the actual production environment of the tuyere whirlpool zone, and uses the softening temperature of the ash cone as an evaluation index for the air permeability of the tuyere whirlpool zone of the blast furnace, which can accurately simulate the local air permeability of the tuyere whirlpool zone of the blast furnace. Compared with the description of the overall air permeability of the blast furnace in the prior art, the evaluation method of the present application describes the situation of the tuyere whirlpool zone more reasonably.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ironmaking production, and in particular to a method for evaluating the air permeability of a tuyere whirlpool zone of a raw coal blast furnace. Background Art

[0002] The technology of pulverized coal injection in blast furnace is an important foundation and key link to maintain the stability and durability of blast furnace ironmaking. At the current stage of blast furnace ironmaking, increasing the amount of pulverized coal injection and reducing the amount of coke fed into the furnace are of great significance for reducing the cost of pig iron, improving the working condition of the furnace, reducing the pollution of coking production, and alleviating the shortage of high-quality coking coal resources. However, too much coal injection will affect the combustion efficiency of pulverized coal, the coal-coke replacement ratio, the permeability of the furnace, and the stability of the blast furnace. When the amount of coal injection reaches a certain level, the carbon content in the blast furnace dust will show an increasing trend. Therefore, it is of great significance to study a method to evaluate the permeability of the tuyere whirlpool zone caused by the injection of high-calcium bituminous coal.

[0003] A large amount of research on coal powder combustion and blast furnace coal injection practices at home and abroad have shown that under the conditions of blast furnace coal injection, it is impossible for the coal powder to be 100% gasified in the short period of time from the outlet of the spray gun to the combustion zone before leaving the tuyere. Not only can some coal powder fail to complete the three stages of gasification, but the gasified coal powder will inevitably produce carbon black particles with high resistance to surface oxidation during the gasification process. These unburned coal powder and the generated carbon black particles rise with the coal gas leaving the combustion zone and enter the dripping zone, soft melting zone and even the block zone.

[0004] A large amount of unburned coal powder and carbon black are retained in the soft melting zone and the dripping zone, which reduces their air permeability and liquid permeability, resulting in the premature appearance of liquid flooding and difficulty in moving the lower part or suspended materials.

[0005] During the blast furnace ironmaking process, fine dust in ore, coke, and flux will be carried out of the furnace by the blast furnace gas, and then captured and removed by the gas dust removal and purification system outside the furnace. It contains a large amount of carbon in the form of coal powder and coke. As the demand for reducing blast furnace smelting costs becomes stronger, large-scale coal injection technology has become one of the effective means to reduce the coke ratio. However, with the increase in coal injection, the content of unburned coal powder in blast furnace gas is also increasing, which not only deteriorates the permeability of the blast furnace, but also worsens the effect of reducing the coke ratio, resulting in economic irrationality.

[0006] At present, the blast furnace permeability index is mainly used to comprehensively reflect the blast furnace operation status. There are three main permeability index prediction models:

[0007] The first method is to predict the blast furnace permeability index by combining the wavelet analysis method with the support vector machine technology. Combining the advantages of the above two technologies can well realize the prediction of the permeability index. Support vector machine: Support vector machine is known for its modeling accuracy based on small amounts of data and excellent generalization ability. Its essence is to convert the low-dimensional non-linearly divisible space to a high-dimensional space through kernel operations and finally make it linearly separable. It ensures excellent generalization performance through the principle of minimum structured risk. At present, it has been widely used in pattern recognition, predictive regression, control and other fields; Wavelet analysis: Wavelet transform is a time-frequency analysis method for signals. The signal can be decomposed into sub-signals of different frequencies and scales by changing the scale and frequency of the mother wave function.

[0008] The second blast furnace permeability index prediction model based on the improved multi-layer excessive learning machine first analyzes the relevant operating parameters that affect the blast furnace permeability index. Considering that the blast furnace production data contains a lot of noise, the wavelet denoising method is used to eliminate the noise interference of the data. Then a blast furnace permeability index prediction model is established. In the modeling process, the partial least squares is combined with the multi-layer excessive learning machine algorithm to eliminate the multicollinearity of the last hidden layer of the multi-layer excessive learning machine, thereby improving the prediction accuracy of the model.

[0009] The third method uses feature selection methods such as Spearman, MIC (maximum information coefficient) and random forest feature elimination to select feature variables from the standardized data, and uses the Xgboost model for prediction. Based on the actual production data of a domestic blast furnace, by collecting and integrating relevant historical data of the blast furnace, the correlation between data is deeply explored, and a blast furnace permeability index prediction model is established to accurately predict the blast furnace permeability index in the next hour, timely guide the blast furnace production, and ensure the stable and smooth operation of the blast furnace.

[0010] The above three prediction methods for blast furnace permeability index research are all based on computer modeling, and a large amount of actual production data is used for simulation training, and the quality of the model is judged by the accuracy of the simulation results. The permeability index obtained by the above methods mainly predicts the overall permeability of the blast furnace, and cannot reasonably describe the local permeability of the blast furnace tuyere whirlpool area. Summary of the invention

[0011] The main purpose of the present invention is to provide a method for evaluating the permeability of the tuyere vortex zone of a raw coal blast furnace, so as to solve the problem that the prior art can only describe the overall permeability of the blast furnace but cannot describe the local permeability of the tuyere vortex zone of the blast furnace.

[0012] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, there is provided a method for evaluating the air permeability of the vortex zone of the tuyere of a raw coal blast furnace, the evaluation method comprising: step S1, using raw coal as raw material, removing volatile matter in the raw coal in an oxygen-free environment to prepare unburned coal powder; step S2, burning coke and unburned coal powder as raw materials to obtain coke ash and unburned coal powder ash; step S3, mixing the coke ash and the unburned coal powder ash to form an ash cone, testing the softening temperature of the ash cone under a reducing atmosphere, and taking the softening temperature as an evaluation index for the air permeability of the tuyere vortex zone of the blast furnace.

[0013] Furthermore, the softening temperature is divided into five levels, the temperature range of level I is 0-1000℃, the temperature range of level II is 1100-1250℃, the temperature range of level III is 1250-1350℃, the temperature range of level IV is 1350-1500℃, the temperature of level V is greater than 1500℃, and the permeability of the blast furnace tuyere convolution zone deteriorates from level I to level V according to the softening temperature.

[0014] Furthermore, the raw coal is one or more of Shenhua high-calcium coal, Russian coal, Taoqing coal, Qifengdu coal, Heqi coal, and Pingshi coal; the preferred coke is one or more of blast furnace coke, Russian coke, Hunan 2# coke, and Shaoguan Iron and Steel's self-produced coke.

[0015] Furthermore, in step S3, the mass ratio of unburned coal fly ash to coke ash is 2:1 to 3:1.

[0016] Furthermore, in step S3, the preparation method of the ash cone includes: using dextrin solution to mix unburned coal fly ash and coke ash into a paste to obtain a paste ash cone; putting the paste ash cone into an ash cone mold for extrusion molding to obtain an ash cone.

[0017] Furthermore, step S1 comprises: placing the raw coal in a reaction vessel of a high-temperature heating furnace, introducing nitrogen or an inert gas and heating, maintaining dry distillation after the temperature stabilizes, and cooling the reaction vessel to room temperature while continuing to introduce nitrogen or an inert gas to obtain unburned coal powder; preferably, the dry distillation time is 1 to 2 hours.

[0018] Further, the heating includes: heating to 300° C. at a heating rate of 5° C. / min, and then heating to 1100° C. at a heating rate of 10° C. / min.

[0019] Furthermore, step S2 comprises: placing the unburned coal powder and coke in two ash dishes which have been pre-burned to a constant mass, respectively, and placing the ash dishes in a muffle furnace for burning to obtain coke ash and unburned coal powder ash.

[0020] Furthermore, when the ash content is higher than 15%, step S2 further includes: inspectively burning the ash tray.

[0021] Furthermore, in step S2, the burning includes: heating the ash dish to 500°C to 550°C in 30 to 60 minutes, maintaining the temperature at 500°C to 550°C for 30 to 50 minutes; and then continuing to heat to (815±10)°C and maintaining the temperature for 1 to 2 hours.

[0022] By applying the technical solution of the present invention, the present application utilizes ash cones to simulate the actual production environment of the tuyere whirlpool zone, and utilizes the softening temperature of the ash cones as an evaluation index for the air permeability of the tuyere whirlpool zone of the blast furnace. This can accurately simulate the local air permeability of the tuyere whirlpool zone of the blast furnace. Compared with the description of the overall air permeability of the blast furnace in the prior art, the evaluation method of the present application is more reasonable in describing the situation of the tuyere whirlpool zone. DETAILED DESCRIPTION

[0023] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0024] As analyzed in the background technology of this application, the existing blast furnace permeability index evaluation method can only describe the overall permeability of the blast furnace, and cannot accurately reflect the permeability of the blast furnace tuyere whirlpool area, nor can it simulate the actual production environment of the tuyere bird's nest area. In addition, the existing blast furnace permeability index requires a large amount of actual production data as support, and cannot make an accurate evaluation of emergencies in actual production, and cannot provide enterprises with a method for stably simulating the actual on-site tuyere permeability. In order to solve these problems, the present application provides an evaluation method for the permeability of the tuyere whirlpool area of ​​a raw coal blast furnace.

[0025] In a typical embodiment of the present application, a method for evaluating the air permeability of a vortex zone in a raw coal blast furnace tuyere is provided, and the evaluation method comprises: step S1, using raw coal as raw material, removing volatile matter in the raw coal in an oxygen-free environment to prepare unburned coal powder; step S2, burning coke and unburned coal powder as raw materials to obtain coke ash and unburned coal powder ash; step S3, mixing coke ash and unburned coal powder ash to form an ash cone, testing the softening temperature of the ash cone under a reducing atmosphere, and using the softening temperature as an evaluation index for the air permeability of the vortex zone in the tuyere of the blast furnace.

[0026] The present application utilizes ash cones to simulate the actual production environment of the tuyere whirlpool zone, and utilizes the softening temperature of the ash cones as an evaluation index for the air permeability of the tuyere whirlpool zone of the blast furnace. This can accurately simulate the local air permeability of the tuyere whirlpool zone of the blast furnace. Compared with the description of the overall air permeability of the blast furnace in the prior art, the evaluation method of the present application is more reasonable in describing the situation of the tuyere whirlpool zone.

[0027] In some embodiments, the test methods for the deformation temperature, softening temperature, hemisphere temperature and flow temperature of the ash cone in a reducing atmosphere are as follows:

[0028] A small amount of coal ash (coke ash and unburned coal fly ash) is mixed into a paste with dextrin solution, and the above-mentioned paste coal ash is made into a triangular cone shape using a mold. After the paste coal ash solidifies and takes shape in the mold, it is fixed in the triangular pit of the ash cone support plate, and the ash cone is perpendicular to the surface of the support plate. The support plate with the ash cone is placed on the corundum boat. Open the lid of the high-temperature furnace, and slowly push the corundum boat into the furnace until the ash cone is located in the high-temperature zone and close to the hot end of the thermocouple (about 2 mm apart). Close the furnace lid, introduce reducing gas carbon monoxide into the equipment to start heating and control the heating rate to: below 900℃, 15-20℃ / min; 900℃ and above, (5±1)℃ / min. Observe the morphological changes of the ash cone at any time, and record the four melting characteristic temperatures of the ash cone-deformation temperature, softening temperature, hemispherical temperature and flow temperature. The experiment is terminated when all ash cones reach the flow temperature or the furnace temperature rises to 1450℃. The determination method of coal ash fusibility adopts the Chinese national standard method (GB219 Determination method of coal ash fusibility). The definitions of the four temperatures are as follows:

[0029] (1) Deformation temperature DT is the temperature at which the tip of the ash cone begins to round or bend;

[0030] (2) Softening temperature ST is the temperature at which the cone of the ash cone bends until the tip touches the support plate and the ash cone begins to become spherical;

[0031] (3) Hemispherical temperature HT is the temperature at which the ash cone melts completely into a hemispherical shape;

[0032] (4) Flow temperature FT is the temperature at which the ash cone melts into liquid or spreads into a thin layer with a height of less than 1.5 mm.

[0033] In this application, the temperature when the ash cone shrinks by 10% can be used as the deformation temperature, the temperature when it shrinks by 30% can be used as the softening temperature, the temperature when it shrinks by 50% can be used as the hemispherical temperature, and the temperature when it shrinks by 80% can be used as the flow temperature. During the test, the photos of the ash melting at different temperatures are saved, and the shapes of the ash at different temperatures are calibrated with a ruler to read the different temperatures of the ash.

[0034] In some embodiments, the present application divides the softening temperature into five levels, the temperature range of level I is 0-1000°C, the temperature range of level II is 1100-1250°C, the temperature range of level III is 1250-1350°C, the temperature range of level IV is 1350-1500°C, and the temperature of level V is greater than 1500°C. The air permeability of the blast furnace tuyere cyclone zone deteriorates in sequence from level I to level V according to the softening temperature, as shown in Table 1. The present application adopts a comparative relationship to express the degree of air permeability, wherein good>better>medium>poor>poor.

[0035] Table 1

[0036] Serial number Level Name Code Classification range ST / ℃ Breathability 1 Low softening temperature ash Ⅰ ≤1000 good 2 Lower softening temperature ash Ⅱ >1100~1250 better 3 Medium softening temperature gray Ⅲ >1250~1350 medium 4 Medium to high softening temperature gray Ⅳ >1350~1500 Poor 5 High softening temperature ash Ⅴ >1500 Difference

[0037] The main factor affecting the air permeability of the blast furnace tuyere cyclotron zone is that the unburned coal fly ash and part of the coke ash block the coke window in the blast furnace bird's nest area, resulting in a decrease in air permeability. The lower the softening temperature of the ash cone, the better the air permeability of the active blast furnace tuyere cyclotron zone. The low softening temperature of the ash cone is conducive to softening and melting, thereby avoiding the unmelted ash cone blocking the coke window of the tuyere cyclotron zone, thereby improving the air permeability of the active blast furnace tuyere cyclotron zone. On the contrary, if the softening temperature of the ash cone is high, the ash cone is not easy to soften and melt, and the ash formed will block the coke window of the tuyere cyclotron zone, forming a high melting point compound with coke, thereby affecting the air permeability of the tuyere cyclotron zone. Therefore, the present application can determine the strength of the air permeability of the blast furnace tuyere cyclotron zone by the difference in softening temperature.

[0038] This application can also well describe the local permeability of the blast furnace tuyere cyclotron zone when changing coal or coke in actual production, which is more stable and efficient. In some embodiments, the raw coal is preferably one or more of Shendong high-calcium coal, Russian coal, Taoqing coal, Qifengdu coal, Heqi coal, and Pingshi coal; the coke is preferably one or more of blast furnace coke, Russian coke, Hunan 2# coke, and Shaoguan Iron and Steel's self-produced coke.

[0039] The trend of unburned coal powder in the blast furnace is: in vertical comparison, the content of unburned coal powder is high in the upper part and low in the lower part; in horizontal comparison, the content of unburned coal powder is low in the center of the blast furnace and high at the edge. Although the changes in the unburned coal powder at the edge vary greatly according to the characteristics of the coal powder airflow and the changes in the furnace type of blast furnace nodules, the rules are still the same. For coke powder, the content of coke powder and the content of unburned coal powder show an opposite trend. The content of coke in the blast furnace is less in the upper part and more in the lower part, and more in the center of the blast furnace than at the edge. According to the above-mentioned trend of the content of unburned coal powder and coke in the blast furnace, the ratio of unburned coal fly ash and coke ash is adjusted. In some embodiments, in step S3, the mass ratio of unburned coal fly ash and coke ash is 2:1 to 3:1. In order to restore the composition ratio of the real blast furnace tuyere area and make the experiment more convincing, the mass ratio of unburned coal fly ash and coke ash is preferably 7:3. There are more low-melting-point substances in unburned coal fly ash, and fewer low-melting-point substances in coke. If the coke content is too high, the softening temperature will increase, thereby affecting the permeability of the vortex zone of the blast furnace tuyere.

[0040] The present application has no particular restrictions on the preparation method of the ash cone, as long as it can be extruded in an ash cone mold. In some embodiments, in step S3, the preparation method of the ash cone includes: using a dextrin solution to mix unburned coal fly ash and coke ash into a paste to obtain a paste ash cone; putting the paste ash cone into an ash cone mold and extruding it to obtain an ash cone.

[0041] The present application prepares unburned coal powder according to the conditions in the actual production environment. In some embodiments, step S1 includes: placing the raw coal in a reaction vessel of a high-temperature heating furnace, introducing nitrogen or an inert gas and heating, maintaining dry distillation after the temperature stabilizes, and cooling the reaction vessel to room temperature while continuing to introduce nitrogen or an inert gas to obtain unburned coal powder; preferably, the dry distillation time is 1 to 2 hours. The above heating includes: heating to 300°C at a heating rate of 5°C / min, and then heating to 1100°C at a heating rate of 10°C / min.

[0042] In order to ensure that the volatile matter in the coal powder can be fully removed and the nitrogen at the bottom of the container can be kept flowing smoothly, in some embodiments, a layer of corundum balls with a thickness of about 100 mm is required to be laid on the bottom of the reaction container of the above-mentioned high-temperature heating furnace, and the amount of raw coal put in each time is about 10 g, and the raw coal powder is spread flat in the reaction container.

[0043] In some embodiments, before step S1, the raw coal needs to be dried in an oven at 110° C. for 3 hours to remove moisture; then the raw coal is ball-milled to a size of less than 200 meshes and sealed for later use.

[0044] The present application adopts the muffle furnace method to detect the ash content of unburned coal powder and coke. In some embodiments, step S2 includes: placing the unburned coal powder in an ash dish that has been pre-burned to a constant mass, placing the ash dish in a muffle furnace for burning, and obtaining coke ash and unburned coal powder ash. Specifically including: in the ash dish that has been pre-burned to a constant mass, weigh (1±0.1)g of the above-mentioned unburned coal powder with a particle size of less than 0.2mm, weigh to 0.0002g, and evenly spread it in the ash dish so that its mass per square centimeter does not exceed 0.15g. Send the ash dish into the constant temperature zone of the muffle furnace with a furnace temperature not exceeding 100℃, close the furnace door and leave a gap of about 15mm in the furnace door. Slowly raise the furnace temperature to 500℃ in no less than 30min, and maintain it at this temperature for 30min. Continue to heat up to (815±10)℃ and burn at this temperature for 1h. Take out the ash dish from the furnace, place it on a heat-resistant porcelain plate or asbestos board, cool it in the air for about 5 minutes, move it into a dryer and cool it to room temperature (about 20 minutes) before weighing. Use an X-ray fluorescence spectrometer to test the ash composition of unburned coal powder and coke.

[0045] In some embodiments, when the ash content is higher than 15%, step S2 further includes: performing inspection burning on the ash dish. The present application has no particular limitation on the method of inspection burning, and the inspection burning methods commonly used in the art can be applied to the present application. For example: the time for inspection burning is 20 minutes each time, until the mass change after two consecutive burnings does not exceed 0.0010g. When the ash content is lower than 15.00%, inspection burning is not necessary. The mass after the last burning is used as the calculation basis, and the percentage of the mass of the residue to the mass of the coal sample is used as the ash content of the coal sample.

[0046] The present application has no particular restrictions on the conditions for burning. In order to fully convert the coke and raw coal into ash, in some embodiments, in step S2, the burning step includes: heating the ash pan to 500°C to 550°C in 30 to 60 minutes, maintaining the temperature at 500°C to 550°C for 30 to 50 minutes; then continuing to heat the ash pan to (815±10)°C and maintaining the temperature for 1 to 2 hours.

[0047] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0048] Example 1

[0049] (1) The raw coal (Shendong high-calcium coal) was dried in an oven at 110°C for three hours to remove moisture. Then the raw coal was ground to less than 200 meshes using a ball mill and sealed for standby use. The ground Shendong high-calcium coal was placed in the reactor of a new high-temperature heating furnace. To ensure that the reactor was an oxygen-free environment, nitrogen protection was passed throughout the experiment. In addition, to ensure that the volatile matter in the coal powder was fully removed and the nitrogen flow at the bottom of the container was smooth, a layer of corundum balls about 100 mm thick was laid at the bottom of the reaction container, and the amount of raw coal placed each time was about 10 g, and the raw coal powder was spread flat in the reaction container. The high-temperature heating furnace was heated at a rate of 5°C / min when it was below 300°C, and then heated to 1100°C at 10°C / min. After the temperature stabilized, it was kept for dry distillation for 1 hour. Then the power was turned off, and the reaction container was cooled to room temperature while continuing to pass nitrogen to obtain unburned coal powder.

[0050] (2) In an ash dish that has been pre-burned to a constant mass, weigh 1g of air-dried coal sample and coke with a particle size of less than 0.2mm, weigh to 0.0002g, and evenly spread them in the ash dish so that the mass per square centimeter does not exceed 0.15g. Place the ash dish in the constant temperature zone of a muffle furnace with a furnace temperature not exceeding 100℃, close the furnace door and leave a gap of about 15mm. Slowly raise the furnace temperature to 500℃ in no less than 30 minutes and maintain it at this temperature for 30 minutes. Continue to raise the temperature to 815℃ and burn at this temperature for 1h. Remove the ash dish from the furnace, place it on a heat-resistant porcelain plate or asbestos board, cool it in the air for about 5 minutes, move it into a desiccator and cool it to room temperature (about 20 minutes) before weighing. Perform inspection burning for 20 minutes each time until the mass change after two consecutive burnings does not exceed 0.0010g.

[0051] (3) Prepare ash cones according to the content of unburned coal powder and coke in the blast furnace tuyere raceway: weigh 1g of coal ash and coke ash according to the mass ratio of unburned coal powder to coke ash of 7:3 and place them on a porcelain plate or glass plate, moisten them with a few drops of dextrin solution and adjust them into a plastic state, then use a small sharp knife to shovel them into an ash cone mold and extrude them into shape. Use a small sharp knife to carefully push the ash cone in the mold onto a porcelain plate or glass, and air-dry it in the air or at 60°C for later use.

[0052] Use dextrin solution to make a small amount of coal ash into a paste, and use it to fix the ash cone in the triangular pit of the ash cone support plate, and make the side of the ash cone perpendicular to the bottom surface and perpendicular to the support plate surface. Place the support plate with the ash cone on the corundum boat. Open the lid of the high-temperature furnace, slowly push the corundum boat into the furnace until the ash cone is located in the high-temperature zone and close to the hot end of the thermocouple (about 2mm apart). Close the furnace cover, introduce reducing gas carbon monoxide into the equipment to start heating and control the heating rate to: below 900℃, 15℃ / min; 900℃ and above, 5℃ / min. Observe the morphological changes of the ash cone at any time, and record the deformation temperature, softening temperature, hemispherical temperature and flow temperature of the ash cone. The experiment ends when all ash cones reach the flow temperature or the furnace temperature rises to 1450℃. The determination method of coal ash fusibility adopts the Chinese national standard method (GB219 Determination method of coal ash fusibility).

[0053] During the test, photographs of the coal ash melting at different temperatures were saved, and the shapes of the coal ash at different temperatures were calibrated with a ruler to read the different temperatures of the coal ash.

[0054] Example 2

[0055] The difference from Example 1 is that the raw coal is Russian coal.

[0056] Example 3

[0057] The difference from Example 1 is that the raw coal is Taoqing coal.

[0058] Example 4

[0059] The difference from Example 1 is that the raw coal is Qifengdu coal.

[0060] Example 5

[0061] The difference from Example 1 is that the raw coal is Heqi coal.

[0062] Example 6

[0063] The difference from Example 1 is that the raw coal is Pingshi coal.

[0064] Example 7

[0065] Different from Example 1, the mass ratio of unburned coal fly ash to coke ash is 3.5:1.

[0066] Example 8

[0067] Different from Example 1, the mass ratio of unburned coal fly ash to coke ash is 1:1.

[0068] The internal pressure of the blast furnace in each of the above embodiments is tested using a pressure detection device (such as a pressure transmitter of model EJA530A-DBS4N-02NN / HAC) to obtain the maximum pressure difference. The melting temperature, air permeability and maximum pressure difference measured in each of the above embodiments are shown in Table 2.

[0069] Table 2

[0070]

[0071]

[0072] It can be seen from the above embodiments that poor air permeability leads to a larger maximum pressure difference, which is in line with the air permeability law, indicating that the evaluation method of the present application is accurate and reliable.

[0073] From the above description, it can be seen that the above-mentioned embodiments of the present invention achieve the following technical effects: the present application utilizes ash cones to simulate the actual production environment of the tuyere whirlpool zone, and utilizes the softening temperature of the ash cones as an evaluation index for the air permeability of the tuyere whirlpool zone of the blast furnace, thereby accurately simulating the local air permeability of the tuyere whirlpool zone of the blast furnace. Compared with the description of the overall air permeability of the blast furnace in the prior art, the evaluation method of the present application is more reasonable in describing the situation of the tuyere whirlpool zone.

[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for evaluating the air permeability of the tuyere whirlpool zone of a raw coal blast furnace, characterized in that: The evaluation method includes: Step S1, using raw coal as raw material, removing volatile matter from the raw coal in an oxygen-free environment to prepare unburned coal powder; Step S2, burning the coke and the unburned coal powder as raw materials to obtain coke ash and unburned coal powder ash; Step S3, mixing the coke ash and the unburned coal fly ash to form an ash cone, testing the softening temperature of the ash cone under a reducing atmosphere, and using the softening temperature as an evaluation index for the air permeability of the blast furnace tuyere raceway; The softening temperature is divided into five levels, the temperature range of level I is 0-1000°C, the temperature range of level II is 1100-1250°C, the temperature range of level III is 1250-1350°C, the temperature range of level IV is 1350-1500°C, and the temperature of level V is greater than 1500°C. The air permeability of the blast furnace tuyere raceway zone deteriorates in sequence from level I to level V according to the softening temperature; In the step S3, the mass ratio of the unburned coal fly ash to the coke ash is 2:1 to 3:

1.

2. The evaluation method according to claim 1, characterized in that: The raw coal is one or more of Shenhua high-calcium coal, Russian coal, Taoqing coal, Qifengdu coal, Heqi coal, and Pingshi coal.

3. The evaluation method according to claim 2, characterized in that: The coke is one or more of blast furnace coke, Russian coke, Hunan No. 2 coke, and Shaoguan Iron and Steel's self-produced coke.

4. The evaluation method according to claim 1, characterized in that: In step S3, the method for preparing the ash cone includes: The unburned coal fly ash and the coke ash are mixed into a paste by using a dextrin solution to obtain a paste ash cone; The paste-like ash cone is placed in an ash cone mold for extrusion molding to obtain the ash cone.

5. The evaluation method according to claim 1, characterized in that: The step S1 comprises: The raw coal is placed in a reaction vessel of a high-temperature heating furnace, and nitrogen or inert gas is introduced and heated. After the temperature is stabilized, dry distillation is maintained, and the reaction vessel is cooled to room temperature while continuing to introduce nitrogen or inert gas to obtain the unburned coal powder.

6. The evaluation method according to claim 5, characterized in that: The dry distillation time is 1 to 2 hours.

7. The evaluation method according to claim 6, characterized in that: The heating includes: heating to 300° C. at a heating rate of 5° C. / min, and then heating to 1100° C. at a heating rate of 10° C. / min.

8. The evaluation method according to claim 1, characterized in that: The step S2 comprises: placing the unburned coal powder and the coke in two ash dishes which have been pre-burned to a constant mass, respectively, and placing the ash dishes in a muffle furnace for burning to obtain the coke ash and the unburned coal powder ash.

9. The evaluation method according to claim 8, characterized in that: When the ash content is higher than 15%, the step S2 further comprises: inspectively burning the ash tray.

10. The evaluation method according to claim 8, characterized in that: In the step S2, the burning comprises: The ash dish is heated to 500°C to 550°C within 30 to 60 minutes, and maintained at 500°C to 550°C for 30 to 50 minutes; Then continue to raise the temperature to (815±10)℃ and maintain for 1 to 2 hours.

Citation Information

Patent Citations

  • Method for detecting calorific value characteristic of raw material fire coal

    CN108956364A

  • Detecting method and system for rapidly determining proportion of cokes in furnace ash of blast furnace

    CN109187260A

  • Blast furnace tuyere raceway test simulation technology and method

    CN112322813A

  • Blast furnace pulverized coal integral heater

    CN112762742A

  • Method for producing coke for blast furnace

    JP2011213827A