By hot-pressing polyethylene resin sheets to coat modified polypropylene foam moldings, and using compatibilizers and nucleating agents to improve surface adhesion, the problem of poor surface adhesion of polypropylene foam moldings is solved and achieved. Preparation of composite materials with high strength and aesthetics, suitable for new energy vehicles and military products.

CN115476564BActive Publication Date: 2024-10-18NANJING GIELI NEW MATERIAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211230074.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-08
Publication Date
2024-10-18
Estimated Expiration
2042-10-08

AI Technical Summary

Technical Problem

The surface adhesion of polypropylene foam moldings is poor, making it difficult to meet high strength and aesthetic requirements. The existing improvement process steps are complex and costly.

Method used

The modified polypropylene foam molding is hot-pressed and coated with polyethylene resin sheets, using compatibilizers, compound nucleating agents and antioxidants to improve surface adhesion, and extruded through a two-stage twin-screw supercritical gas Machines and special molds are used to prepare composite materials.

Benefits of technology

It improves the adhesion of polypropylene resin foam materials and the strength of composite materials, and prepares composite materials with smooth surfaces and good aesthetics, which are suitable for lightweight interior and exterior decoration parts and industrial parts in harsh environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115476564B_ABST
    Figure CN115476564B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of foaming materials, and in particular to a composite material with a modified polypropylene foaming molded body as a core layer and a preparation method thereof, wherein the composite material is composited by a polyethylene resin sheet and a modified polypropylene foaming molded body, and the structure thereof is that the polyethylene resin sheet is hot-pressed to cover the modified polypropylene foaming molded body. The present invention has a simple process, and uses a compatibilizer, a compound nucleating agent and an antioxidant to modify polypropylene, thereby improving the adhesion of the surface of the polypropylene resin foaming material, enhancing the composite ability of the polyethylene resin sheet, and making the composite material have high strength performance; the present invention uses a special mold to polymerize the polyethylene resin sheet, and the surface of the prepared composite material is smooth, without obvious air plugging marks, and has aesthetics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of foaming materials, in particular to a composite material with a modified polypropylene foaming molding as a core layer and a preparation method thereof. Background Art

[0002] Polypropylene resin has a low density and has excellent properties such as environmental protection, low odor, lightweight, high cushioning, high buoyancy, sound insulation, and heat insulation. It can be widely used in industrial fields such as automobiles, packaging, construction, military industry, EMC, etc. Polypropylene foam moldings can be made into different shapes according to the application field.

[0003] Polypropylene resin has the characteristics of non-polarity and low surface energy, which leads to poor surface adhesion. When the surface of polypropylene resin is treated by traditional spraying process, the sprayed ink easily falls off. Conventional polypropylene foam molding is made by foaming bead compression molding. The surface is only the fusion between particles. The film thickness is only 0.01-0.02mm. It has obvious granularity and is not scratch-resistant. It is easily punctured after being impacted by sharp objects. It is usually only used as an internal filler, or a layer of high-hardness material is added to the surface using a composite process to improve the surface strength of the polypropylene foam molding. At the same time, the mold has residual pores and cannot meet higher appearance requirements. The surface adhesion of polypropylene resin is even worse after spraying ink. The prior art also discloses changing the surface resin state through bonding and hot pressing processes, but such processes generally have complex steps and are expensive.

[0004] In recent years, some proposals for improving the surface strength of foamed molded products have emerged both at home and abroad.

[0005] Japanese patent JP2013022734A discloses a molding method for a resin molded product and a resin molded product. The molding method utilizes the heat of a resin sheet to melt the surface of a foamed core material, and simultaneously utilizes a mold to bond and mold the core material and the resin sheet to obtain a resin molded product.

[0006] Japanese patent JP2016030431A discloses a fiber-reinforced composite material and a method for manufacturing a fiber-reinforced composite material. The disclosed technical solution is

[0007] Spherical resin is introduced into a mold having multiple ventilation holes, and the spherical resin is heated to expand and fuse the resin volume. The resin is formed in the mold and simultaneously penetrates into the ventilation holes to form a multi-layer structure with multiple protrusions. The fiber layer is hot-pressed onto the surface of the resin foam to form a fiber-reinforced resin layer with a multi-layer structure.

[0008] Chinese patent CN110506072A discloses a foamed particle molded body covered with a skin material, wherein the skin material has a multilayer structure of an inner layer and an outer layer, and the inner layer is bonded to a polypropylene resin foamed particle molded body. The multilayered polypropylene resin molded body is a hollow blow molded body formed by blow molding a multilayered parison, and then the foamed particles are filled and heated by steam to form a foamed particle molded body, and at the same time, the inner surface of the hollow blow molded body is melt-bonded to the foamed particle molded body, and after steam is supplied, the mold is cooled, and the molding mold is opened to obtain a molded body.

[0009] The process steps provided by the above-mentioned prior art are relatively complicated. Although they can cover the surface of the sandwich structure with a skin material, they do not improve the non-polar properties of the surface of the polypropylene resin foam material, and there are problems such as poor adhesion. The surface of the obtained material is rough and has poor aesthetics. Summary of the invention

[0010] The object of the present invention is to provide a composite material with a modified polypropylene foamed molded body as a core layer and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0011] The present invention is achieved through the following technical solutions:

[0012] The present invention provides a composite material with a modified polypropylene foaming molded body as a core layer, wherein the composite material is composited by a polyethylene resin sheet and a modified polypropylene foaming molded body, and the structure thereof is that the polyethylene resin sheet is hot-pressed and coated with the modified polypropylene foaming molded body, specifically:

[0013] The outer layer is a polyethylene resin sheet, the thickness of the polyethylene resin sheet is 0.3 to 3 mm;

[0014] The modified polypropylene foam molding is used as the core layer, and the modified polypropylene foam molding comprises the following components in parts by mass:

[0015] 85-95 parts of copolymerized polypropylene resin;

[0016] 5 to 10 parts of a compatibilizer, wherein the compatibilizer includes PP-g-MAH, and the compatibilizer is used to improve the adhesion of the surface of the polypropylene resin foam material and enhance the composite ability of the reinforcement and polyethylene resin sheet;

[0017] 0.5 to 3 parts of compound nucleating agent is used to increase the crystallization speed and improve the uniformity of the pores;

[0018] Antioxidant 0.05-1 part.

[0019] Preferably, the polyethylene resin sheet is made of ultra-high molecular weight polyethylene resin, the average molecular weight of which is 1×10 6 ~5×10 6 , preferably 2×106 ~2.5×10 6 .

[0020] Preferably, the thickness of the polyethylene resin sheet includes two types: 0.3-1.5 mm and 1.5-3 mm.

[0021] Preferably, the copolymerized polypropylene resin is binary block polypropylene, and its MFR is 2-7 g / min and its melting point is 150-165°C.

[0022] Preferably, the composite nucleating agent is composed of polytetrafluoroethylene and boric acid metal salt, the mass ratio of polytetrafluoroethylene to boric acid metal salt is 1:6-9, the average particle size of the boric acid metal salt particles is 0.9-6 μm, and the boric acid metal salt includes zinc borate.

[0023] Preferably, the antioxidant is selected from β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate or tris[2,4-di-tert-butylphenyl]phosphite, preferably β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate.

[0024] The present invention also provides a method for preparing a composite material with a modified polypropylene foaming molding as a core layer, comprising the following steps:

[0025] (1) Extrusion foaming: copolymerized polypropylene resin, compatibilizer, compound nucleating agent and antioxidant are injected into a two-stage twin-screw supercritical gas extruder through an automatic feeding device, gas is injected in the first-stage twin-screw extruder, and then extruded through the second-stage twin-screw extruder, and modified polypropylene foam particles are obtained by using an underwater pelletizing system;

[0026] (2) Compression molding: the foamed particles obtained in step (1) are input into a special mold, and sequentially subjected to pressure loading, compression molding, and drying steps to obtain the modified polypropylene foamed molded body;

[0027] (3) Laminating: The polypropylene foamed molded body obtained in step (2) is positioned and placed in a special mold, and polyethylene resin sheets are respectively placed on the two sides of the mold cavity of the special mold, and a composite material with the modified polypropylene foamed molded body as the core layer is obtained through heating, mold closing, air cooling, shaping, and cutting; when the thickness of the polyethylene resin sheet is 0.3 to 1.5 mm, the sheet is heated at 80 to 90° C. for 10 to 50 seconds; when the thickness of the polyethylene resin sheet is 1.5 to 3 mm, the mold cavity temperature is heated to 110 to 120° C.

[0028] As a further embodiment of the present invention, in step (1), the gas injected into the first-stage twin-screw extruder is CO2 and / or N2, the gas pressure in the two-stage twin-screw supercritical gas extruder is 8 to 11 MPa, and the extrusion temperature of the extruder is 175 to 220°C.

[0029] As a further solution of the present invention, in step (1), the underwater pelletizing system uses a mixture of water and glycerol as the circulating medium, the pelletizing temperature is set to 30-60°C, and the die head pressure of the underwater pelletizing system is set to 0.1-0.2Mpa, so as to facilitate the adjustment and control of the foaming density.

[0030] As a further solution of the present invention, in steps (2) and (3), the special mold includes a mold cavity and a shell arranged on the periphery of the mold cavity, the surface of the shell is etched with surface grains, the depth of the surface grains is 0.05 to 0.2 mm, and the air plug penetrates the shell and connects the mold cavity with the steam chamber, which can ensure the smoothness of the surface of the foamed molded body without affecting the heating efficiency.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] The process of the invention is simple. The polypropylene is modified by using a compatibilizer, a compound nucleating agent and an antioxidant, so that the adhesion of the surface of the polypropylene resin foam material can be improved, the composite ability of the polyethylene resin sheet is enhanced, and the composite material has high strength performance. The invention utilizes a special mold to polymerize the polyethylene resin sheet, and the prepared composite material has a smooth surface, no obvious air plugging marks, and is aesthetically pleasing. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0034] Figure 1 This is a SEM scanning electron microscope image of the modified polypropylene foamed particles of the present invention;

[0035] Figure 2 It is a top cross-sectional view of the special mold of the present invention;

[0036] Figure 3 It is a surface schematic diagram of the modified polypropylene foamed molded body of the present invention;

[0037] Figure 4 It is a surface schematic diagram of a polypropylene foamed molded body made by a conventional mold of the present invention;

[0038] Figure 5 Schematic diagram of the cross section of the composite material. DETAILED DESCRIPTION

[0039] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] Embodiment 1:

[0041] This embodiment provides a composite material with a modified polypropylene foaming molded body as a core layer. The composite material is composited by a polyethylene resin sheet and a modified polypropylene foaming molded body. The structure is that the polyethylene resin sheet is hot-pressed to cover the modified polypropylene foaming molded body. Specifically:

[0042] The outer layer is a polyethylene resin sheet with a thickness of 1.5 mm. The polyethylene resin sheet is made of ultra-high molecular weight polyethylene resin with an average molecular weight of 2×10 6 ~2.5×10 6 ;

[0043] The modified polypropylene foam molding is used as the core layer, and the modified polypropylene foam molding includes the following components in parts by weight:

[0044] 90 parts of binary block polypropylene resin, with MFR of 2-7 g / min and melting point of 150-165°C;

[0045] 8 parts of compatibilizer, PP-g-MAH is selected as the compatibilizer, which is used to improve the adhesion of the surface of polypropylene resin foam material and can enhance the composite ability of reinforcement and polyethylene resin sheet;

[0046] 1 part of a compound nucleating agent, the compound nucleating agent is composed of polytetrafluoroethylene and zinc borate in a mass ratio of 1:6, the average particle size of the zinc borate is 0.9-6 μm, and the compound nucleating agent is used to increase the crystallization speed and improve the uniformity of the pores;

[0047] 1 part of antioxidant, wherein the antioxidant is β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate.

[0048] This embodiment also provides a method for preparing the composite material, comprising the following steps:

[0049] (1) Extrusion foaming: inject binary block polypropylene resin, PP-g-MAH, a composite nucleating agent consisting of polytetrafluoroethylene-zinc borate and β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate into a two-stage twin-screw supercritical gas extruder through an automatic feeding device according to the above mass fractions, inject CO2 into the first-stage twin-screw extruder, control the temperature of the first-stage twin-screw extruder to be 190-220°C, and the pressure to be 9.5-11 MPa, and then extrude through a second-stage twin-screw extruder, the die head temperature of the second-stage twin-screw extruder close to the pelletizing system is 175°C, and the die head pressure is set to 8 MPa;

[0050] The underwater pelletizing system uses a mixture of water and glycerin as a circulating medium, the pelletizing temperature is set to 30-60°C, and the die head pressure of the underwater pelletizing system is set to 0.1-0.2Mpa, which is convenient for adjusting and controlling the foaming density. The modified polypropylene foam particles are prepared by using the above underwater pelletizing system. Figure 1 As shown in (magnification 200), the modified polypropylene foam particles obtained are oval in shape, with a particle size of 1 to 3 mm, a closed cell rate of more than 65%, and a density of 100 to 450 g / L;

[0051] (2) Compression molding: The foamed particles obtained in step (1) are input into a special mold, and sequentially subjected to pressure loading, compression molding, and drying steps to obtain a modified polypropylene foamed molded body;

[0052] (3) Laminating: The polypropylene foamed body obtained in step (2) is positioned and placed in a special mold, two polyethylene resin sheets with a thickness of 1.5 mm are taken, and the two polyethylene resin sheets are heated in an oven at 85° C. for 13 seconds, and then the polyethylene resin sheets are respectively placed on the left and right sides of the mold cavity of the special mold, and the positioned foamed body is quickly moved into the middle of the mold, and the left and right cavities are molded together for final shaping, and air cooling is performed for 8 seconds, and the mold is opened and taken out, and then the surrounding overflow burrs are cut off by a water jet cutting method to obtain a foamed body as shown in FIG. Figure 5 The composite material shown has a modified polypropylene resin foamed body as a core layer.

[0053] As attached Figure 2 It can be seen that the special mold includes a mold cavity 1 and a shell 2 arranged on the periphery of the mold cavity 1. The shell is made of aluminum alloy or cast aluminum. The surface of the shell 2 is laser-etched with a surface leather grain with a depth of 0.1 mm. The air plug 3 penetrates the shell 2 and connects the mold cavity 1 and the steam chamber 4. The aperture of the air plug 3 is 0.5 mm. The steam chamber 4 is connected to an external heat source through a pipeline. Figure 3 It can be seen that this embodiment can ensure that the surface of the foamed molded body arranged in the mold cavity 1 is flat and smooth without obvious traces of air blockage without affecting the heating efficiency.

[0054] Embodiment 2:

[0055] This embodiment provides a composite material with a modified polypropylene foaming molded body as a core layer. The composite material is composited by a polyethylene resin sheet with a thickness of 3 mm and a modified polypropylene foaming molded body, and its structure and raw material components are consistent with those in the embodiment.

[0056] In the composite material preparation method provided in this embodiment, during lamination, the polypropylene foamed molded body obtained in step (2) is positioned and placed in a special mold, two polyethylene resin sheets with a thickness of 3 mm are taken, the mold cavity is heated to 110°C, and then the polyethylene resin sheets are heated in an 85°C oven for 18 seconds, and then the polyethylene resin sheets are respectively placed on the left and right sides of the mold cavity of the special mold, and the positioned foamed molded body is quickly moved into the middle of the mold, the left and right cavities are molded together for final shaping, air cooled for 8 seconds, the mold is opened and taken out, and then the surrounding overflow burrs are cut off by water cutting to obtain the following. Figure 5 The composite material with the modified polypropylene resin foaming molding as the core layer is shown. The remaining preparation steps are consistent with those in Example 1.

[0057] Comparative Example 1:

[0058] Comparative Example 1 provides a composite material with a modified polypropylene foam molding as a core layer, the composite material is composed of a polyethylene resin sheet with a thickness of 1.5 mm and a modified polypropylene foam molding, and its structure is that the polyethylene resin sheet is hot-pressed and coated with the modified polypropylene foam molding. In the composite material provided in Comparative Example 1, the modified polypropylene foam molding includes the following components in parts by mass:

[0059] 98 parts of binary block polypropylene resin, with MFR of 2-7 g / min and melting point of 150-165°C;

[0060] 1 part of a compound nucleating agent, the compound nucleating agent is composed of polytetrafluoroethylene and zinc borate in a mass ratio of 1:6, the average particle size of the zinc borate is 0.9-6 μm, and the compound nucleating agent is used to increase the crystallization speed and improve the uniformity of the pores;

[0061] 1 part of antioxidant, wherein the antioxidant is β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate.

[0062] The remaining preparation steps are consistent with those in Example 1.

[0063] Comparative Example 2:

[0064] Comparative Example 2 provides a composite material with a modified polypropylene foaming molded body as a core layer, the composite material is composited by a polyethylene resin sheet with a thickness of 1.5 mm and a modified polypropylene foaming molded body, and its structure is that the polyethylene resin sheet is hot-pressed and coated with the modified polypropylene foaming molded body. In the composite material provided in Comparative Example 2, the modified polypropylene foaming molded body includes the following components in parts by mass:

[0065] 98 parts of binary block polypropylene resin, with MFR of 2-7 g / min and melting point of 150-165°C;

[0066] 1 part of nucleating agent, which is zinc borate with an average particle size of 0.9 to 6 μm, and is used to increase the crystallization rate and improve the uniformity of the pores;

[0067] 1 part of antioxidant, wherein the antioxidant is β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate.

[0068] The remaining preparation steps are consistent with those in Example 1.

[0069] Comparative Example 3:

[0070] Comparative Example 3 provides a composite material with a modified polypropylene foam molding as the core layer. The composite material is composed of a polyethylene resin sheet with a thickness of 1.5 mm and a modified polypropylene foam molding. Its structure is that the polyethylene resin sheet is hot-pressed to cover the modified polypropylene foam molding, and the raw material components are consistent with those in Example 1.

[0071] In the preparation method of the composite material provided in Comparative Example 3, a conventional mold with dense gas plug and large pore size is used to prepare the composite material as shown in FIG. Figure 4 The polypropylene foaming molding shown in the figure is consistent with the other steps in Example 1. Figure 4 As shown, the surface of the polypropylene foamed molded body prepared in Comparative Example 3 has obvious traces of air plugging.

[0072] Five test specimens with a size of 350 mm × 100 mm × 25 mm (the sample surface includes one side of the skin) were cut and taken from the composite materials prepared in Examples 1-2 and Comparative Examples 1-3, respectively. The distance between the fulcrums was set to 200 mm, the pressing speed was 20 mm / min, the temperature was 23°C, and the humidity was 50% relative humidity. The flexural strength of the above test specimens was measured based on GB / T8812.2 (2007). The test results are shown in the following table.

[0073]

[0074] As can be seen from the above table, the present invention utilizes a compatibilizer, a compound nucleating agent and an antioxidant to modify polypropylene, which can improve the adhesion of the surface of the polypropylene resin foam material, enhance the composite ability of the polyethylene resin sheet, and make the composite material have higher bending strength; the present invention utilizes a special mold to polymerize the polyethylene resin sheet, and the prepared composite material has uniform particle size, smooth surface, no obvious traces of air plugging, and has aesthetics, and can be applied to lightweight interior and exterior trims of new energy vehicles, protective packaging of military products with strict requirements on the use environment, and industrial parts with high requirements on appearance.

[0075] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A composite material with a modified polypropylene foamed body as a core layer, characterized in that: The composite material is composed of a polyethylene resin sheet and a modified polypropylene foaming molded body, and its structure is that the polyethylene resin sheet is hot-pressed and coated with the modified polypropylene foaming molded body, specifically: The polyethylene resin sheet is used as the outer layer, and the thickness of the polyethylene resin sheet is 0.3-3 mm; The modified polypropylene foam molding is used as the core layer, and the modified polypropylene foam molding comprises the following components in parts by mass: 85-95 parts of copolymerized polypropylene resin; 5-10 parts of a compatibilizer, wherein the compatibilizer comprises PP-g-MAH; 0.5-3 parts of a composite nucleating agent is used to increase the crystallization speed and improve the uniformity of the pores; the composite nucleating agent is composed of polytetrafluoroethylene and a metal borate, the mass ratio of the polytetrafluoroethylene to the metal borate is 1:6-9, the average particle size of the particles of the metal borate is 0.9-6 μm, and the metal borate includes zinc borate; 0.05-1 part of antioxidant; the antioxidant is selected from β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate or tris[2,4-di-tert-butylphenyl]phosphite; The polyethylene resin sheet is made of ultra-high molecular weight polyethylene resin, and the copolymerized polypropylene resin is binary block polypropylene; The method for preparing the composite material comprises the following steps: (1) Extrusion foaming: inject copolymerized polypropylene resin, compatibilizer, compound nucleating agent and antioxidant into a two-stage twin-screw supercritical gas extruder, inject gas in the first-stage twin-screw extruder, and then extrude through the second-stage twin-screw extruder, and use an underwater pelletizing system to obtain modified polypropylene foam particles; (2) Compression molding: the foamed particles obtained in step (1) are input into a special mold, and sequentially subjected to pressure loading, compression molding, and drying steps to obtain the modified polypropylene foamed molded body; (3) Laminating: The polypropylene foamed molded body obtained in step (2) is positioned and placed in a special mold, and polyethylene resin sheets are placed on both sides of the special mold respectively, and subjected to heating, mold closing, air cooling, shaping, and cutting to obtain a composite material with the modified polypropylene foamed molded body as the core layer; Wherein, in step (1), the gas pressure in the two-stage twin-screw supercritical gas extruder is 8-11 MPa, and the extrusion temperature of the second-stage twin-screw extruder is 175-220°C; In steps (2) and (3), the special mold includes a mold cavity and a shell arranged on the periphery of the mold cavity. The shell is made of aluminum alloy or cast aluminum. The surface of the shell is laser etched to have a surface leather texture with a depth of 0.1 mm. The air plug penetrates the shell and connects the mold cavity and the steam chamber. The aperture of the air plug is 0.5 mm. The steam chamber is connected to an external heat source through a pipeline.

2. The composite material with modified polypropylene foamed molding as the core layer according to claim 1, characterized in that: The average molecular weight of the ultra-high molecular weight polyethylene resin is 1×10 6 ~5×10 6 .

3. The composite material with modified polypropylene foamed molding as the core layer according to claim 1, characterized in that: The thickness of the polyethylene resin sheet includes two types: 0.3~1.5mm and 1.5~3mm.

4. The composite material with modified polypropylene foamed molding as the core layer according to claim 1, characterized in that: The binary block polypropylene has an MFR of 2-7 g / min and a melting point of 150-165° C.

5. The composite material with modified polypropylene foamed molding as the core layer according to claim 1, characterized in that: In step (1), the gas injected into the first-stage twin-screw extruder is CO2 and / or N2.

6. The composite material with modified polypropylene foamed molding as the core layer according to claim 1, characterized in that: In step (1), the underwater pelletizing system uses a mixture of water and glycerol as a circulating medium, the pelletizing temperature is set to 30-60° C., and the die head pressure of the underwater pelletizing system is set to 0.1-0.2 MPa.

Citation Information

Patent Citations

  • Surface-material-coated foamed particle molded body

    CN110506072A

  • Method of molding resin molded product and resin molded product

    JP2013022734A

  • Fiber-reinforced complex, and method for producing fiber-reinforced complex

    JP2016030431A

  • Low-forming energy consumption polypropylene foam particles and preparation method thereof

    CN110229372A

  • Hollow EPE particle preparation method and foam production process

    CN113201167A