Preparation method of UV-resistant polylactic acid

By using metal complex catalysts in solvents to polymerize and lactide, covalent bonding between anti-UV molecules and polylactic acid is achieved, solving the problems of stability and complex process of anti-UV functional polylactic acid materials, significantly improving The durability and fastness of the material simplifies the process and reduces costs.

CN115477745BActive Publication Date: 2024-11-01SHANDONG UNIV OF TECH +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211046712.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-30
Publication Date
2024-11-01
Estimated Expiration
2042-08-30

AI Technical Summary

Technical Problem

The existing UV-resistant functional polylactic acid materials have poor stability, low crystallization performance, complex process and large energy consumption, which limits their large-scale application.

Method used

Under nitrogen protection, the metal complex catalyst and lactide are polymerized in a solvent to achieve covalent bonding between ultraviolet molecules and polylactic acid polymer chains, simplifying the process and improving the durability and fastness of the material.

Benefits of technology

It significantly improves the durability and fastness of UV-resistant functional polylactic acid, simplifies production processes, reduces industrial costs, and improves the uniformity and stability of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

The present invention belongs to the technical field of polylactic acid preparation, and specifically relates to a method for preparing anti-ultraviolet polylactic acid. Under nitrogen protection, a metal complex catalyst, ROH and lactide are polymerized in a solvent to obtain anti-ultraviolet polylactic acid. The present invention adopts a benzotriazole derivative with anti-ultraviolet function as a catalyst ligand, so that lactide directly links the anti-ultraviolet molecule with the polylactic acid polymer in the form of a covalent bond during the catalytic polymerization process, which can significantly improve the uniformity, stability and fastness performance of the anti-ultraviolet functional polylactic acid product, realize the one-step completion of polymer material preparation and functionalization, simplify the production process, reduce industrial costs, and expand the scope of use of polylactic acid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polylactic acid preparation, and particularly relates to a method for preparing UV-resistant polylactic acid. Background Art

[0002] Polylactic acid (PLA), also known as polylactide, is a completely biodegradable polyester polymer material; it is made by polycondensation of lactic acid. Currently, it is mostly made of starch-containing biomass such as corn or straw cellulose as raw materials, fermented to produce lactic acid, and lactic acid is prepared into cyclic dimer lactide, and then lactide is ring-opened and polymerized to produce polylactic acid; it does not use petroleum as raw material, but only uses biomass renewable resources formed by photosynthesis of plants as raw materials. About 2 tons of corn can produce 1 ton of polylactic acid, and about 3 tons of corn stalks and wheat straw can produce 1 ton of polylactic acid, which is inexhaustible. In theory, the waste of polylactic acid products can be decomposed into carbon dioxide and water by microorganisms in nature. Carbon dioxide and water form biomass through plant photosynthesis and continue to become raw materials for polylactic acid fermentation. Therefore, polylactic acid is currently recognized as an environmentally friendly material in the world.

[0003] Since excessive exposure to ultraviolet rays can cause many human diseases, the research and preparation of anti-ultraviolet textile materials has never stopped so far. Polylactic acid materials with anti-ultraviolet functionality not only have good ultraviolet absorption performance, but also meet the development needs of green environmental protection and easy degradation, but they have not yet been widely used. Researchers generally use anti-ultraviolet inorganic nanomaterials, such as titanium dioxide, silicon dioxide, etc., to dope polylactic acid oligomers to produce anti-ultraviolet functional polylactic acid. This method improves the anti-ultraviolet performance of polylactic acid, but the obtained anti-ultraviolet polylactic acid has poor stability, poor crystallization performance, and low fastness. Some researchers have also adopted the method of melt blending to prepare anti-ultraviolet functional polylactic acid. For example, Chinese patent CN109401250A discloses an anti-ultraviolet polylactic acid composite material and its preparation method. The anti-ultraviolet polylactic acid composite material is made by melt blending raw materials including the following components in parts by weight: 100 parts of poly-L-lactic acid; 5 to 25 parts of poly-D-lactic acid; 2 to 5 parts of anti-ultraviolet inorganic nanomaterials; the anti-ultraviolet inorganic nanomaterials include at least three of titanium dioxide, silicon dioxide, zinc oxide, cerium dioxide and cuprous oxide; the temperature of the melt blending is higher than the melting point of poly-L-lactic acid and poly-D-lactic acid, and lower than the melting point of stereocomplex polylactic acid. This patent adopts low-temperature melting processing. Once stereocomposite polylactic acid crystals are formed at this temperature, they will be dispersed in the polylactic acid resin in the form of a solid phase. The in-situ formed stereocomposite polylactic acid crystals collide with specific anti-ultraviolet inorganic nanomaterials added to the polylactic acid resin, so that these nanomaterials are evenly dispersed in the polylactic acid resin, which not only effectively improves the anti-ultraviolet performance of the composite material, but also accelerates the crystallization of poly-L-lactic acid and improves the crystallization performance of the composite material. However, this patent has high requirements on process conditions and equipment precision, and the operation process is relatively complicated.

[0004] In view of the common shortcomings of the production process of anti-ultraviolet polylactic acid, such as complicated process, high energy consumption, environmental pollution and poor stability, there is an urgent need to provide a preparation method of anti-ultraviolet polylactic acid with excellent performance, stable structure and simple process. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing UV-resistant polylactic acid, which realizes the covalent bond between the anti-UV molecules and the polylactic acid polymer chains, provides a more environmentally friendly and simple production process, significantly improves the durability and various fastnesses of the UV-resistant functional polylactic acid, and meets the market demand for UV-resistant functional polylactic acid textiles.

[0006] The preparation method of the anti-ultraviolet polylactic acid of the present invention is that under nitrogen protection, a metal complex catalyst, ROH and lactide are polymerized in a solvent to obtain the anti-ultraviolet polylactic acid.

[0007] The structural formula of the metal complex catalyst is as follows:

[0008] Anti-UV-M-Anti-UV

[0009] Wherein, M is a metal, Anti-UV is an anti-ultraviolet ligand, and the above structural formula represents that M is connected to Anti-UV.

[0010] The M is magnesium or zinc.

[0011] The structural formula of the Anti-UV is as follows:

[0012]

[0013] Wherein, R1 is -H, -C(CH3)2C6H5, -C(CH3)3, -C(CH3)2CH2CH3, -OCH3 or -O(CH2) n One of CH3, wherein 1≤n≤8, and n is an integer;

[0014] R2 is one of -CH3, -C(CH3)3, -C(CH3)2C6H5, -C(CH3)2CH2CH3, -C(CH3)2CH2C(CH3)3 or -OCH3;

[0015] R3 is -H or -Cl.

[0016] The structural formula of the Anti-UV is one of the following structural formulas:

[0017]

[0018]

[0019] The preparation method of the metal complex catalyst is that under nitrogen protection, Anti-UV reacts with a metal compound in a solvent to obtain the metal complex catalyst.

[0020] The metal compound is di-n-butyl magnesium or diethyl zinc.

[0021] The solvent is one or more of benzene, toluene, tetrahydrofuran or dichloromethane, preferably toluene or tetrahydrofuran.

[0022] The molar ratio of the Anti-UV to the metal compound is 2-2.5:1.

[0023] The mass ratio of the solvent to Anti-UV is 20-200:1.

[0024] The reaction is a stage temperature-raising reaction, wherein the reaction temperature of the first stage is 30-50° C., and the reaction temperature of the second stage is 70-125° C.; the reaction time is 3-12 hours.

[0025] The ROH is one of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, ethylene glycol, phenol, benzyl alcohol, phenylethyl alcohol, benzhydrol, triphenylmethanol, pyrogallol, triethanolamine, tetraethanolethylenediamine, cyclodextrin or allyl alcohol, preferably one of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol or benzyl alcohol.

[0026] The molar ratio of the metal complex catalyst, ROH and lactide is 1:1-1.2:500-10000.

[0027] The solvent is one or more of benzene, toluene, tetrahydrofuran or dichloromethane, preferably toluene or tetrahydrofuran.

[0028] The molar ratio of lactide to solvent is 1:2.5-10.

[0029] The polymerization reaction temperature is 100-180° C., and the polymerization reaction time is 2-24 hours.

[0030] The specific reaction equation of the present invention is as follows:

[0031]

[0032] The structural formula of the metal complex catalyst is as follows:

[0033]

[0034] Wherein, R1 is preferably one of -H, -C(CH3)3 or -C(CH3)2CH2CH3;

[0035] R2 is preferably one of -CH3, -C(CH3)3 or -C(CH3)2CH2CH3.

[0036] Anti-UV is a benzotriazole derivative with anti-ultraviolet function. The benzotriazole structure and hydroxyl structure containing coordinated N atoms in the benzotriazole derivative are half-enclosed, which provides excellent position conditions for the coordination reaction with the metal center.

[0037] The synthesis mechanism of anti-UV polylactic acid is that lactide coordinates with the metal center, resulting in electrophilic activation of lactide, which is then attacked by the nucleophilic attack of the metal center to form an intermediate, and ROH attacks the activated lactide monomer. The chemical bonds with higher energy in the intermediate are broken to achieve ring opening, forming a long chain of lactide monomers connected with Anti-UV ligands and -OR. The chain growth is accompanied by metal coordination, nucleophilic reaction, bond breaking and ring opening of lactide until the coordination bond undergoes cleavage and termination reaction.

[0038] The present invention creatively combines an anti-ultraviolet molecule with a metal complex catalyst for lactide ring-opening polymerization to prepare a new metal complex catalyst for lactide ring-opening polymerization, thereby enabling the anti-ultraviolet molecule to directly participate in the lactide ring-opening polymerization reaction process and achieve chemical bonding with the polylactic acid molecule.

[0039] The beneficial effects of the present invention are as follows:

[0040] Compared with the existing production process of anti-ultraviolet functional polylactic acid, the present invention adopts a benzotriazole derivative with anti-ultraviolet function as a catalyst ligand, thereby achieving direct covalent bonding of the anti-ultraviolet molecule with the polylactic acid polymer during the catalytic polymerization of lactide, which can significantly improve the uniformity, stability and fastness of the anti-ultraviolet functional polylactic acid product, achieve one-step completion of polymer material preparation and functionalization, simplify the production process, reduce industrial costs, and expand the scope of use of polylactic acid. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is the NMR spectrum of the light yellow metal complex catalyst prepared in Example 1.

[0042] Figure 2 It is the nuclear magnetic spectrum of the UV-resistant polylactic acid obtained in Example 1. DETAILED DESCRIPTION

[0043] The present invention is further described below with reference to the embodiments.

[0044] Example 1

[0045] Under nitrogen protection, 0.472g U1 was dissolved in 30ml toluene and reacted with 1ml 1mol / L diethylzinc solution at 30℃ for 5h. The mixed solution was slowly heated to 120℃ and heated for 1h. The solvent was removed by distillation under reduced pressure. The solid was washed with n-hexane and dried in vacuo. The product was recrystallized in benzene, washed and dried to obtain 0.49g of light yellow metal complex catalyst. The NMR spectrum of the metal complex catalyst is shown in Figure 1 , the structural formula of the metal complex catalyst is as follows:

[0046]

[0047] Under nitrogen protection, 14.4 g of lactide, 30 ml of purified toluene solution, 0.049 g of metal complex catalyst and 0.0108 g of benzyl alcohol were added to a Schlenk bottle, and then the polymerization reaction was carried out at 100° C. for 10 h. A 10% by volume hydrochloric acid ethanol solution was added thereto to terminate the reaction. The reaction solution was poured into n-hexane and allowed to stand for precipitation. The precipitate was filtered and dissolved with dichloromethane. An appropriate amount of n-hexane was added to precipitate the solid. This was repeated three times, and then the mixture was filtered and dried. The UV-resistant polylactic acid was obtained by vacuum drying. The NMR spectrum of the UV-resistant polylactic acid is shown in FIG. Figure 2 .

[0048] After testing, the anti-ultraviolet polylactic acid can block 99.9% of the UV-B band (280-315nm) and 92.5% of the UV-A band (315-400nm). After soap washing 10 times, it can still block 99.5% of the UV-B band (280-315nm) and 89.2% of the UV-A band (315-400nm). The blackboard temperature is set to (65±3)℃, the box humidity is (50±10)%, and the light intensity is 550W / m 2 The spraying cycle is (18±0.5) min, and the water-free time between two sprayings is (100±0.5) min. Under this condition, there is no yellowing after 240 hours of irradiation. After soaping 10 times, there is still no yellowing after continuing to irradiate for 240 hours.

[0049] Example 2

[0050] Under nitrogen protection, 0.540g U1 was dissolved in 40ml tetrahydrofuran and reacted with 1ml 1mol / L diethylzinc solution at 35°C for 4h. The mixed solution was slowly heated to 80°C and heated for 1h. The solvent was removed by distillation under reduced pressure. The solid was washed with n-hexane and dried in vacuo. The product was recrystallized in toluene, washed and dried to obtain 0.48g of a light yellow metal complex catalyst. The structural formula of the metal complex catalyst is as follows:

[0051]

[0052] Under nitrogen protection, 10 g of lactide, 40 ml of purified tetrahydrofuran solution, 0.051 g of metal complex catalyst and 0.0061 g of isopropanol were added to a Schlenk bottle, and then the polymerization reaction was carried out at 120°C for 9 hours. A 10% by volume solution of hydrochloric acid in ethanol was added to terminate the reaction. The reaction solution was poured into n-hexane and allowed to stand for precipitation. The precipitate was filtered and dissolved with dichloromethane. An appropriate amount of n-hexane was added to precipitate the solid. This was repeated three times, and then filtered and dried, and then vacuum dried to obtain UV-resistant polylactic acid.

[0053] After testing, the anti-ultraviolet polylactic acid can block 99.5% of the UV-B band (280-315nm) and 92.0% of the UV-A band (315-400nm). After soap washing 10 times, it can still block 99.0% of the UV-B band (280-315nm) and 88.9% of the UV-A band (315-400nm). The blackboard temperature is set to (65±3)℃, the box humidity is (50±10)%, and the light intensity is 550W / m 2 The spraying cycle is (18±0.5) min, and the water-free time between two sprayings is (100±0.5) min. Under this condition, there is no yellowing after 240 hours of irradiation. After soaping 10 times, there is still no yellowing after continuing to irradiate for 240 hours.

[0054] Example 3

[0055] Under nitrogen protection, 0.756g U2 was dissolved in 30ml toluene and reacted with 2ml 0.5mol / L di-n-butylmagnesium solution at 50°C for 5h. The mixed solution was slowly heated to 125°C and heated for 1h. The solvent was removed by distillation under reduced pressure. The solid was washed with n-hexane and dried in vacuo. The product was recrystallized in toluene, washed and dried to obtain 0.60g of yellow metal complex catalyst. The structural formula of the metal complex catalyst is as follows:

[0056]

[0057] Under nitrogen protection, 25 g of lactide, 40 ml of purified tetrahydrofuran solution, 0.067 g of metal complex catalyst and 0.0118 g of benzyl alcohol were added to a Schlenk bottle, and then the polymerization reaction was carried out at 130°C for 8 hours. A 10% by volume solution of hydrochloric acid in ethanol was added to terminate the reaction. The reaction solution was poured into n-hexane and allowed to stand for precipitation. The precipitate was filtered and dissolved with dichloromethane. An appropriate amount of n-hexane was added to precipitate the solid. This was repeated three times, and then filtered and dried, and then vacuum dried to obtain UV-resistant polylactic acid.

[0058] After testing, the anti-ultraviolet polylactic acid can block 99.6% of the UV-B band (280-315nm) and 93.5% of the UV-A band (315-400nm). After soap washing 10 times, it can still block 99.2% of the UV-B band (280-315nm) and 89.6% of the UV-A band (315-400nm). The blackboard temperature is set to (65±3)℃, the box humidity is (50±10)%, and the light intensity is 550W / m 2 The spraying cycle is (18±0.5) min, and the water-free time between two sprayings is (100±0.5) min. Under this condition, there is no yellowing after 240 hours of irradiation. After soaping 10 times, there is still no yellowing after continuing to irradiate for 240 hours.

Claims

1. A method for preparing UV-resistant polylactic acid, Features Under nitrogen protection, a metal complex catalyst, ROH and lactide are polymerized in a solvent to obtain UV-resistant polylactic acid; ROH is one of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, ethylene glycol, phenol, benzyl alcohol, phenylethyl alcohol, benzhydrol, triphenylmethanol, pyrogallol, triethanolamine, tetraethanolethylenediamine, cyclodextrin or propenol; the polymerization temperature is 100-180°C, and the polymerization time is 2-24h; The structural formula of the metal complex catalyst is as follows: Among them, M is metal, Anti-UV is anti-ultraviolet ligand; The M is magnesium or zinc; The structural formula of the Anti-UV is as follows: Among them, R 1 -H, -C(CH 3 ) 2 C 6 H 5 、-C(CH 3 ) 3 、-C(CH 3 ) 2 CH 2 CH 3 、-OCH 3 or -O(CH 2 ) n CH 3 One of , wherein 1≤n≤8, and n is an integer; R 2 -CH 3 、-C(CH 3 ) 3 、-C(CH 3 ) 2 C 6 H 5 、-C(CH 3 ) 2 CH 2 CH 3 、-C(CH 3 ) 2 CH 2 C(CH 3 ) 3 or -OCH 3 One of; R 3 is -H or -Cl; The preparation method of the metal complex catalyst is that under nitrogen protection, Anti-UV reacts with a metal compound in a solvent to obtain a metal complex catalyst. The reaction is a stage temperature increase reaction, wherein the first stage reaction temperature is 30-50°C and the second stage reaction temperature is 70-125°C.

2. The method for preparing the UV-resistant polylactic acid according to claim 1, Features The structural formula of the Anti-UV is one of the following structural formulas: 。 3. The method for preparing the UV-resistant polylactic acid according to claim 1, Features The metal compound is di-n-butyl magnesium or diethyl zinc, the solvent in the preparation method of the metal complex catalyst is one or more of benzene, toluene, tetrahydrofuran or dichloromethane, the molar ratio of Anti-UV to the metal compound is 2-2.5:1, and the mass ratio of the solvent to Anti-UV in the preparation method of the metal complex catalyst is 20-200:

1.

4. The method for preparing the UV-resistant polylactic acid according to claim 1, Features The reaction time is 3-12h.

5. The method for preparing the UV-resistant polylactic acid according to claim 1, Features The molar ratio of the metal complex catalyst, ROH and lactide is 1: 1-1.2:500-10000.

6. The method for preparing the UV-resistant polylactic acid according to claim 1, Features The solvent in the polymerization reaction is one or more of benzene, toluene, tetrahydrofuran or dichloromethane, and the molar ratio of lactide to the solvent in the polymerization reaction is 1:2.5-10.

Citation Information

Patent Citations

  • Uvioresistant polylactic acid compound material and preparation method thereof

    CN109401250A

  • Synthesis and application of propylamine morpholine hexa-coordinate dual-ligand zirconium metal complex