Ethylene-vinyl alcohol copolymer resin particle composition, ethylene-vinyl alcohol copolymer film formed therefrom, and multilayer structure
By preparing the EVOH resin particle composition with a specific void volume range of the core surface, the problem of insufficient appearance and gas barrier properties of the thermoformed body of the EVOH material is solved, and multiple performance improvements of the thermoformed body are achieved.
Patent Information
- Application Number
- CN202210692339.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-06-16
- Filing Date
- 2022-06-16
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-06-16
AI Technical Summary
The thermoformed bodies made of existing EVOH materials have shortcomings in appearance, thermoformability and gas barrier properties, and have failed to effectively meet industrial needs.
By preparing an EVOH resin particle composition with a specific surface core void volume range, including the first EVOH resin particles and the second EVOH resin particles, a thin film with good ethylene content uniformity is formed, thereby enhancing the appearance and gas barrier of the thermoformed body. sex.
The thermoformed body made of EVOH material has good thermoforming properties, appearance and gas barrier properties, and meets the industry's multiple performance requirements for thermoformed bodies.
Smart Images

Figure CN115477805B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an ethylene-vinyl alcohol (EVOH) copolymer composition; in particular, to an ethylene-vinyl alcohol copolymer resin particle composition, a film and a multilayer structure formed from the EVOH resin particle composition. Background Art
[0002] EVOH resin is widely used in multilayer bodies for preserving perishable items. For example, EVOH resin and multilayer bodies made therefrom are commonly used in the food packaging industry, medical equipment and consumables industry, pharmaceutical industry, electronics industry and agricultural chemical industry. Specifically, EVOH resin is commonly used to be added to multilayer bodies as a unique layer to serve as an oxygen barrier layer. Furthermore, multilayer bodies made of EVOH can also be made into various types of containers by thermoforming.
[0003] In practice, the industry usually has requirements for the appearance, thermoforming properties, and gas barrier properties of the thermoformed bodies made of EVOH materials. For example, in terms of appearance, if there is no gelling, roughness, or yellowing after production, it can be said that it has excellent appearance characteristics; if the thickness difference between different areas of the thermoformed body is kept within a certain range, it can be said that it has good thermoforming properties; and if the oxygen permeability after thermoforming is kept below a certain level, it can be said that it has ideal gas barrier properties. Summary of the invention
[0004] However, the background art has never proposed a concept or means that can effectively meet the above requirements. In response to this technical problem, the inventors have found through research that when two EVOH resin particles contained in an EVOH resin particle composition each have a specific surface core void volume (Vvc) value range, the film formed by the EVOH resin particle composition has good ethylene content uniformity, and the subsequent thermoformed body can have good thermoforming, appearance and gas barrier properties.
[0005] Accordingly, the present invention provides an ethylene vinyl alcohol copolymer (EVOH) resin particle composition, which includes: a first EVOH resin particle having a surface core void volume (Vvc) of 0.002-14 μm 3 / um 2 , and a second EVOH resin particle having a surface core void volume (Vvc) of 0.010 to 48 μm 3 / um 2 .
[0006] According to some embodiments of the present invention, the Vvc of the second EVOH resin particle is greater than the Vvc of the first EVOH resin particle.
[0007] According to some embodiments of the present invention, the melting point of the first EVOH resin particles is 135-179°C, and the melting point of the second EVOH resin particles is 180-198°C.
[0008] According to some embodiments of the present invention, the ethylene content of the first EVOH resin particles is 36 to 50 mol percent.
[0009] According to some embodiments of the present invention, the ethylene content of the second EVOH resin particles is 20 to 35 mol percent.
[0010] According to some embodiments of the present invention, the EVOH resin particles are shaped like cylinders, elliptical cylinders, angular cylinders, spheres, ellipsoids or go shapes, and their major diameter / height is 1-5 mm, and their minor diameter is 1-5 mm.
[0011] According to some embodiments of the present invention, the weight percentage of the first EVOH resin particles to the second EVOH resin particles is 5:95 to 75:25.
[0012] According to some embodiments of the present invention, the EVOH resin particle composition has a boron content of 5 to 550 ppm.
[0013] According to some embodiments of the present invention, the EVOH resin particle composition has an alkali metal content of 10 to 550 ppm.
[0014] According to some embodiments of the present invention, the first EVOH resin particle has a surface core portion entity volume (Vmc) of 0.001 to 12 μm. 3 / um 2 ; and the second EVOH resin particle has a surface core entity volume (Vmc) of 0.022 to 55 um 3 / um 2 .
[0015] According to some embodiments of the present invention, the first EVOH resin particle has a root mean square height (Sq) surface parameter of 0.001 to 25 um; and the second EVOH resin particle has a root mean square height (Sq) surface parameter of 0.020 to 65 um.
[0016] According to some embodiments of the present invention, the first EVOH resin particle has a surface parameter of a maximum height (Sz) of 0.030 to 28 um; and the second EVOH resin particle has a surface parameter of a maximum height (Sz) of 0.120 to 65 um.
[0017] According to some embodiments of the present invention, the first EVOH resin particle has a core height difference (Sk) surface parameter of 0.010-25 um; and the second EVOH resin particle has a core height difference (Sk) surface parameter of 0.030-65 um.
[0018] According to some embodiments of the present invention, the first EVOH resin particle has a linear arithmetic mean height (Ra) surface parameter of 0.001 to 0.600 um; and the second EVOH resin particle has a linear arithmetic mean height (Ra) surface parameter of 0.012 to 0.800 um.
[0019] According to some embodiments of the present invention, the first EVOH resin particle has a line maximum height (Rz) surface parameter of 0.005-7 um; and the second EVOH resin particle has a line maximum height (Rz) surface parameter of 0.080-7.500 um.
[0020] Another aspect of the present invention provides an ethylene-vinyl alcohol copolymer film, which is formed from the above EVOH resin particle composition.
[0021] In another aspect, the present invention provides a multilayer structure comprising: (a) at least one layer of ethylene-vinyl alcohol copolymer film formed from the EVOH resin particle composition; (b) at least one polymer layer; and (c) at least one adhesive layer.
[0022] According to some embodiments of the present invention, the polymer layer is selected from the group consisting of a low-density polyethylene layer, a polyethylene grafted maleic anhydride layer, a polypropylene layer, and a nylon layer, and the adhesive layer is a tie layer.
[0023] According to some embodiments of the present invention, the multi-layer structure is polymer layer / adhesive layer / ethylene-vinyl alcohol copolymer film / adhesive layer / polymer layer.
[0024] The ethylene vinyl alcohol copolymer (EVOH) resin particle composition, the ethylene vinyl alcohol copolymer film formed therefrom and the multilayer structure comprising the film provided by the present invention can make the thermoformed body made of EVOH material have good thermoformability, appearance and gas barrier properties without being limited by a specific theory. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The following is an exemplary description of the present invention with reference to the accompanying drawings, in which:
[0026] Figure 1 is a schematic diagram illustrating the void volume of the surface core portion used in the present invention;
[0027] Figure 2 Schematic diagram of the appearance of a thermoformed container according to the present invention.
[0028] It should be understood that aspects of the present invention are not limited to the configurations, instrumentalities, and characteristics shown in the drawings. DETAILED DESCRIPTION
[0029] The present invention relates to an ethylene vinyl alcohol copolymer (EVOH) resin particle composition, comprising: a first EVOH resin particle having a surface core void volume (Vvc) of 0.002 to 14 μm. 3 / um 2 , and a second EVOH resin particle having a surface core void volume (Vvc) of 0.010 to 48 μm 3 / um 2 .
[0030] As used herein, the surface core void volume (Vvc) refers to the difference between the void volume at a load area ratio of p% and the void volume at a load area ratio of q%, and its definition is based on ISO 25178:2012. In addition, the size of the core, the protruding peak, and the protruding trough can also be quantified by volume parameters. Figure 1 As shown, Vmp represents the volume of the protruding peak part, Vmc represents the volume of the core part, Vvc represents the volume of the core space, and Vvv represents the load area ratio of the protruding trough part. Figure 1 The example preset specifies that 10% to 80% is the interval of the core part. The Vvc of the first EVOH resin particle is 0.002 to 14 um 3 / um 2 , for example: 0.002, 0.005, 0.010, 0.050, 0.100, 0.500, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13 or 14. The Vvc of the second EVOH resin particle is 0.010-48 um 3 / um 2 , for example: 0.010, 0.050, 0.100, 0.500, 1, 5, 10, 15, 20, 25, 30, 35, 40, 45, 46, 47 or 48. According to a preferred embodiment of the present invention, the Vvc of the second EVOH resin particle is greater than the Vvc of the first EVOH resin particle.
[0031] According to some embodiments of the present invention, the melting point of the first EVOH resin particles is 135-179° C., for example, 135, 140, 145, 150, 155, 160, 165, 170, 175 or 179° C. On the other hand, the melting point of the second EVOH resin particles is 180-198° C., for example, 180, 182, 184, 186, 188, 190, 192, 194, 196 or 198° C.
[0032] According to some embodiments of the present invention, the ethylene content of the first EVOH resin particles may be about 36-50 mole percent (mole%), for example, 36, 38, 40, 42, 44, 46, 48 or 50 mole%. On the other hand, the ethylene content of the second EVOH resin particles is 20-35 mole%, for example, 20, 21, 23, 25, 27, 29, 31, 33 or 35 mole%.
[0033] Additionally or alternatively, the EVOH may have a saponification degree of 90 mole % or higher, preferably 95 mole % or higher, preferably 97 mole % or higher, preferably 99.5 mole % or higher.
[0034] The EVOH particles described herein refer to the form and / or shape of one or more particles formed by granulation of EVOH resin. Although the present invention is described as forming one or more EVOH particles by granulation, the EVOH particles can be processed into beads, cubes, fragments, shavings, etc.; according to some embodiments of the present invention, the shape of the EVOH resin particles is cylindrical, elliptical, angular, spherical, elliptical or go-shaped, and its major diameter or height is 1 to 5 mm, for example: 1, 2, 3, 4 or 5 mm; and its minor diameter is 1 to 5 mm, for example: 1, 2, 3, 4 or 5 mm. As used herein, the "major diameter / height" refers to the longest outer diameter of an object whose surface is composed of a closed curved surface; and the "minor diameter" refers to the smallest diameter in a cross section perpendicular to the major diameter or height and having the largest area. As used herein, the “object having a surface composed of a closed curved surface” may be understood as an object whose entire surface is composed of curved surfaces; an object formed by the intersection of multiple faces without edges and corners; or an object whose cross-section at any position is not rectangular.
[0035] Specifically, when the EVOH resin particles are cylindrical or elliptical, the height range is between 1 and 5 mm, for example: 1.5 to 5.0 mm, 1.7 to 5.0 mm, 2.2 to 5.0 mm, 2.4 to 5.0 mm, 2.6 to 5.0 mm, 2.8 to 5.0 mm, 3.0 to 5.0 mm, 3.2 to 5.0 mm, 3.4 to 5.0 mm, 3.6 to 5.0 mm, 3.8 to 5.0 mm, 4.0 to 5.0 mm, 1.7 to 4.5 mm, 1.7 to 4.4 mm, 1.7 to 4.2 mm, 1.7 to 4.0 mm, 1.7 to 3.8 mm, 1.7 to 3.6 mm, 1.7 to 3.4 mm, 1.7 to 3.2 mm, 1.7~3.0mm; its minor diameter range is between 1~5mm, for example: 1.5~5.0mm, 1.7~5.0mm, 2.2~5.0mm, 2.4~5.0mm, 2.6~5.0mm, 2.8~5.0mm, 3.0~5.0mm, 3.2~5.0mm, 3.4~5.0mm, 3.6~5.0mm, 3.8~5.0mm, 4.0~5.0mm, 1.7~4.5mm, 1.7~4.4mm, 1.7~4.2mm, 1.7~4.0mm, 1.7~3.8mm, 1.7~3.6mm, 1.7~3.4mm, 1.7~3.2mm, 1.7~3.0mm.
[0036] When the EVOH particles are spherical, such as spherical, elliptical or go-shaped, the range of their major diameter is between 1 and 5 mm, for example: 1.5-5.0 mm, 2.2-5.0 mm, 2.4-5.0 mm, 2.6-5.0 mm, 2.8-5.0 mm, 3.0-5.0 mm, 3.2-5.0 mm, 3.4-5.0 mm, 3.6-5.0 mm, 3.8-5.0 mm, 4.0-5.0 mm, 2.0-4.5 mm, 2.0-4.4 mm, 2.0-4.2 mm, 2.0-4.0 mm, 2.0-3.8 mm, 2.0-3.6 mm, 2.0-3.4 mm, 2.0-3 .2mm, 2.0~3.0mm; the range of its short diameter is between 1~5mm, for example: 1.5~5.0mm, 1.8~4.6mm, 2.4~4.6mm, 2.6~4.6mm, 2.8~4.6mm, 3.0~4.6mm, 3.2~4.6mm, 3.4~4.6mm, 3.6~4.6mm, 3.8~4.6mm, 4.0~4.6mm, 1.6~4.5mm, 1.6~4.4mm, 1.6~4.2mm, 1.6~4.0mm, 1.6~3.8mm, 1.6~3.6mm, 1.6~3.4mm, 1.6~3.2mm, 1.6~3.0mm.
[0037] According to some embodiments of the present invention, the weight percentage of the first EVOH resin particles to the second EVOH resin particles is 5:95 to 75:25, for example: 5:95, 15:85, 25:75, 35:65, 45:55, 55:45, 65:35 or 75:25.
[0038] According to some embodiments of the present invention, the EVOH resin particle composition may contain a boron compound and / or boric acid and / or cinnamic acid and / or an alkali metal and / or a conjugated polyene and / or a lubricant and / or an alkaline earth metal in some cases. The above substances can give the EVOH resin particle composition better properties.
[0039] According to some embodiments of the present invention, the EVOH resin particle composition may include a boron compound, wherein the boron content is 5 to 550 ppm. In some cases, the boron content of the EVOH resin particle composition may be 10 to 450 ppm, 10 to about 400 ppm, 10 to about 350 ppm, 10 to about 300 ppm, 10 to about 275 ppm, 10 to about 250 ppm, 10 to about 225 ppm, 10 to about 200 ppm, 10 to about 175 ppm, about 20 to 450 ppm, about 20 to about 400 ppm, about 20 to about 350 ppm, about 20 to about 300 ppm, about 10 to about 275 ppm, about 10 to about 250 ppm, about 10 to about 225 ppm, about 10 to about 200 ppm, about 175 ppm, about 20 to 450 ppm, about 20 to about 400 ppm, about 20 to about 350 ppm, about 20 to about 300 ppm, about 1 ... 00ppm, about 20 to about 275ppm, about 20 to about 250ppm, about 20 to about 225ppm, about 20 to about 200ppm, about 20 to about 175ppm, about 60 to 450ppm, about 60 to about 400ppm, about 60 to about 350ppm, about 60 to about 300ppm, about 60 to about 275ppm, about 60 to about 250ppm, about 60 to about 225ppm, about 60 to about 200ppm, about 60 to about 175ppm, about 10 ... ppm, about 100 to about 400 ppm, about 100 to about 350 ppm, about 100 to about 300 ppm, about 100 to about 275 ppm, about 100 to about 250 ppm, about 100 to about 225 ppm, about 100 to about 200 ppm, about 100 to about 175 ppm, about 140 to 450 ppm, about 140 to about 400 ppm, about 140 to about 350 ppm, about 140 to about 300 ppm, about 140 to about 275 ppm, about 140 to about 250 ppm m, about 140 to about 225ppm, about 140 to about 200ppm, about 180 to about 450ppm, about 180 to about 400ppm, about 180 to about 350ppm, about 180 to about 300ppm, about 180 to about 275ppm, about 180 to about 250ppm, about 180 to about 225ppm, about 220 to 450ppm, about 220 to about 400ppm, about 220 to about 350ppm, about 220 to about 300ppm, about 220 to about 275ppm. When the boron content of the EVOH resin particle composition is within a certain range, the viscosity of the EVOH resin particle composition can be increased and the chance of the EVOH resin particle composition adhering to the screw can be reduced, or the EVOH on the screw can be removed, so that the material has a self-cleaning function, which can further improve the uniformity of film thickness. According to a preferred embodiment of the present invention, in addition to the boron compound, the EVOH resin particle composition may also contain cinnamic acid, alkali metals, conjugated polyenes, alkaline earth metals, their salts and / or mixtures thereof; the above substances are common substances usually present in the EVOH resin particle composition, making it have better properties.If the content of the above-mentioned conjugated polyene structure compound is 1 to 30,000 ppm per unit weight of the EVOH resin particle composition, the coloring after heating can be further suppressed, and the thermal stability is more excellent. If the content of the alkali metal compound or alkaline earth metal compound per unit weight of the EVOH resin composition is 10 to 550 ppm in terms of metal conversion, the long-term operation formability can be better; the content can be, for example, between 10-550 ppm, between about 10-500 ppm, between about 10-450 ppm, between about 10-400 ppm, between about 10-350 ppm, between about 10-300 ppm, between about 10-250 ppm, depending on different situations. ppm, between about 10-200 ppm, between about 10-150 ppm, between about 10-100 ppm, between about 10-50 ppm, between about 50-550 ppm, between about 50-500 ppm, between about 50-450 ppm, between about 50-400 ppm, between about 50-350 ppm, between about 50-300 ppm, between about 50-250 ppm, between about 50-200 ppm, between about 50-150 ppm, between about 50-1 00ppm, between about 100-550ppm, between about 100-500ppm, between about 100-450ppm, between about 100-400ppm, between about 100-350ppm, between about 100-300ppm, between about 100-250ppm, between about 100-200ppm, between about 100-150ppm, between about 200-550ppm, between about 200-500ppm, between about 200-450ppm, between about 2 ppm, between about 200-350 ppm, between about 200-300 ppm, between about 200-250 ppm, between about 300-550 ppm, between about 300-500 ppm, between about 300-450 ppm, between about 300-400 ppm, between about 300-350 ppm, between about 400-550 ppm, between about 400-500 ppm, between about 400-450 ppm, or between about 500-550 ppm.
[0040] According to some embodiments of the present invention, the boron compound may include boric acid or a metal salt thereof. Examples of metal salts include, but are not limited to, calcium borate, cobalt borate, zinc borate (e.g., zinc tetraborate, zinc metaborate), potassium aluminum borate, ammonium borate (e.g., ammonium metaborate, ammonium tetraborate, ammonium pentaborate, ammonium octaborate), cadmium borate (e.g., cadmium orthoborate, cadmium tetraborate), potassium borate (e.g., potassium metaborate, potassium tetraborate, potassium pentaborate, potassium hexaborate, potassium octaborate), silver borate (e.g., silver metaborate, silver tetraborate), copper borate (e.g., copper (II) borate, copper metaborate, copper tetraborate), sodium borate (e.g., sodium metaborate, sodium diborate, tetraborate), The borate minerals may include, for example, sodium borate, sodium pentaborate, sodium hexaborate, sodium octaborate), lead borate (e.g., lead metaborate, lead hexaborate), nickel borate (e.g., nickel orthoborate, nickel diborate, nickel tetraborate, nickel octaborate), barium borate (e.g., barium orthoborate, barium metaborate, barium diborate, barium tetraborate), bismuth borate, magnesium borate (e.g., magnesium orthoborate, magnesium diborate, magnesium metaborate, trimagnesium tetraborate, pentamagnesium tetraborate), manganese borate (e.g., manganese (I) borate, manganese metaborate, manganese tetraborate), lithium borate (e.g., lithium metaborate, lithium tetraborate, lithium pentaborate), salts thereof, or combinations thereof. Borate minerals may include, for example, borax, kainite, kainite, suanite, and szaibelyite. Among them, borax, boric acid and sodium borate (eg, sodium metaborate, sodium diborate, sodium tetraborate, sodium pentaborate, sodium hexaborate and sodium octaborate) are preferably used.
[0041] According to some embodiments of the present invention, the first EVOH resin particle has a surface core volume (Vmc, which can be referred to as Figure 1 As shown) is about 0.001~12um 3 / um 2 , for example: between about 0.001 and 12 um 3 / um 2 , between about 0.010~12um 3 / um 2 , between about 0.100~12um 3 / um 2 , between about 1~12um 3 / um 2 , between about 3~12um 3 / um 2 , between about 3~10um 3 / um 2 , between about 5~10um 3 / um 2 Or between about 5~7um 3 / um 2 On the other hand, the second EVOH resin particle has a surface core volume (Vmc) of 0.022-55 μm.3 / um 2 , for example: between about 0.220 and 55um 3 / um 2 , between about 2.200~55um 3 / um 2 , between about 22~55um 3 / um 2 , between about 22~48um 3 / um 2 , between about 22~40um 3 / um 2 , between about 22~36um 3 / um 2 , between about 30~55um 3 / um 2 Or between about 38~55um 3 / um 2 .
[0042] According to some embodiments of the present invention, the first EVOH resin particle has a root mean square height (Sq) surface parameter of 0.001-25um, for example, between about 0.001-25um, between about 0.010-25um, between about 0.100-25um, between about 1-25um, between about 1-23.30um, between about 1-20um, between about 1-15um, between about 5-15um, or between about 7-10um. On the other hand, the second EVOH resin particle has a root mean square height (Sq) surface parameter of 0.020-65um, for example, between about 0.020-65um, between about 0.200-65um, between about 2-65um, between about 2-61.30um, between about 10-61.30um, between about 20-50um, between about 25-40um, between about 30-40um, or between about 30-36um.
[0043] As used in this article, the definition of the "root mean square height (Sq) surface parameter" refers to ISO25178:2012; it can be understood as the root mean square value of the distance (Z-axis distance, i.e., height) of each point on the contour surface relative to the reference plane within a sampling range, which is equivalent to the standard deviation of the object height.
[0044] According to some embodiments of the present invention, the first EVOH resin particle has a surface parameter of a maximum height (Sz) of 0.030-28 um, for example, between about 0.300-28 um, between about 0.300-25 um, between about 1-28 um, between about 1-25 um, between about 1-23 um, between about 1-20 um, between about 1-15 um, between about 5-15 um, or between about 7-10 um. On the other hand, the second EVOH resin particle has a surface parameter of a maximum height (Sz) of 0.120-65 um, for example, between about 0.120-65 um, between about 1.200-65 um, between about 2-65 um, between about 2-61.30 um, between about 10-61.30 um, between about 20-50 um, between about 25-40 um, between about 30-40 um, or between about 30-36 um.
[0045] As used herein, the definition of the "surface maximum height (Sz) surface parameter" refers to ISO25178:2012, which can be understood as the distance (Z-axis distance, i.e., height) value between the maximum peak and the maximum trough relative to the reference surface within a sampling range.
[0046] According to some embodiments of the present invention, the first EVOH resin particle has a core height difference (Sk) surface parameter of 0.010-25um, for example, between about 0.100-25um, between about 1-25um, between about 1-23um, between about 1-20um, between about 1-15um, between about 5-15um, or between about 7-10um. On the other hand, the second EVOH resin particle has a core height difference (Sk) surface parameter of 0.030-65um, for example, between about 0.300-65um, between about 1-65um, between about 2-65um, between about 3-61.30um, between about 10-61.30um, between about 20-50um, between about 25-40um, between about 30-40um, or between about 30-36um.
[0047] As used herein, the definition of the "core height difference (Sk) surface parameter" refers to ISO 25178:2012, which can be understood as the value of the maximum height minus the minimum height within a core range.
[0048] According to some embodiments of the present invention, the first EVOH resin particles have a linear arithmetic mean height (Ra) surface parameter of 0.001 to 0.990 um, for example: between about 0.001 to 0.990 um, between about 0.001 to 0.700 um, between about 0.001 to 0.500 um, between about 0.001 to 0.300 um, between about 0.010 to 0.100 um, between about 0.050 to 0.990 um, between about 0.050 to 0.700 um, between about 0.050 to 0.500 um, between about 0.050 to 0.300 um or between about 0.050 to 0.100 um. On the other hand, the second EVOH resin particles have a linear arithmetic average height (Ra) surface parameter of 0.001 to 0.990 um, for example, between about 0.010 to 0.990 um, between about 0.010 to 0.700 um, between about 0.010 to 0.500 um, between about 0.010 to 0.300 um, between about 0.010 to 0.100 um, between about 0.050 to 0.990 um, between about 0.050 to 0.700 um, between about 0.050 to 0.500 um, between about 0.050 to 0.300 um or between about 0.050 to 0.100 um.
[0049] As used herein, the “line arithmetic mean height (Ra) surface parameter” is a parameter for defining surface roughness, and its definition may refer to JIS B 0601. Specifically, it may be understood as the average absolute value of a profile curve over a reference length.
[0050] According to some embodiments of the present invention, the first EVOH resin particle has a line maximum height (Rz) surface parameter of 0.0010 to 9.9000 um, for example: between about 0.0010 to 9 um, between about 0.0010 to 7 um, between about 0.0010 to 5 um, between about 0.0100 to 3 um, between about 0.0500 to 5 um, between about 0.0500 to 3 um, between about 0.0500 to 1 um or between about 0.0500 to 0.0800 um. On the other hand, the second EVOH resin particles have a line maximum height (Rz) surface parameter of 0.0010 to 9.9000 um, for example, between about 0.0800 to 9 um, between about 0.1000 to 9 um, between about 0.1500 to 9 um, between about 0.1500 to 7 um, between about 0.5000 to 5 um, between about 0.5000 to 2.5000 um or between about 1 to 2.5000 um.
[0051] As used herein, the "line maximum height (Rz) surface parameter" is a parameter for defining surface roughness, and its definition can refer to JIS B 0601. Specifically, it can be understood as the distance between the highest peak and the lowest valley of a profile curve relative to a reference length.
[0052] In another aspect, the present invention provides an ethylene-vinyl alcohol copolymer film, which is formed from the above EVOH resin particle composition. Specifically, the ethylene-vinyl alcohol copolymer film is a single-layer film.
[0053] In yet another aspect, the present invention provides a multilayer structure comprising: (a) at least one ethylene-vinyl alcohol copolymer film formed from the EVOH resin particle composition; (b) at least one polymer layer; and (c) at least one adhesive layer.
[0054] According to some embodiments of the present invention, the polymer layer is selected from the group consisting of a low-density polyethylene layer, a polyethylene grafted maleic anhydride layer, a polypropylene layer and a nylon layer, and the adhesive layer is a tie layer, such as ARKEMA OREVAC 18729 of ARKEMA. Specifically, the stacked structure of the multilayer structure is a polymer layer, an adhesive layer, an ethylene-vinyl alcohol copolymer film, an adhesive layer and a polymer layer in sequence. According to some embodiments of the present invention, the thickness of the polymer layer is 100-500um, preferably 200-400um, and more preferably 300um; the thickness of the adhesive layer is 10-40um, preferably 20-30um, and more preferably 25um; the thickness of the ethylene-vinyl alcohol copolymer film is 20-80um, preferably 40-60um, and more preferably 50um.
[0055] Without being limited by any theory, it is believed that the core area of the 10% to 80% void volume of the Vvc core part accounts for a large proportion, which is the main factor affecting friction and will affect the melting and mixing of the first EVOH resin particles and the second EVOH resin particles. For the first EVOH resin particles with a lower melting point, when the Vvc is smaller, the surface friction between the particles is smaller, the friction heat is lower, the particles melt later, and the melting zone is backward; while the second EVOH resin particles with a higher melting point are controlled to have a larger Vvc, the surface friction between the particles is larger, the friction heat is higher, the particles melt earlier, and the melting zone is forward; therefore, the composition formed by the two different EVOH particles with controlled Vvc ranges has close melting zones of the particles in the components and better mixing, thereby improving the thermoforming properties of the EVOH composition.
[0056] Example
[0057] The following non-limiting examples of various aspects of the present invention are provided primarily to illustrate various aspects of the present invention and the benefits achieved thereby. The EVOH formulation of each embodiment and comparative example is prepared from at least two components. More specifically, the two components of the EVOH resin particle composition of the embodiment and comparative example are two kinds of EVOH resin particles.
[0058] Preparation of EVOH resin pellet composition
[0059] The following provides a non-limiting method for preparing EVOH resin particle compositions. Five non-limiting example EVOH resin particle compositions (Examples EVOH 1-5) and six comparative example EVOH resin particle compositions (Comparative Examples EVOH 1-6) were prepared according to methods similar to those disclosed below. However, the specific methods for preparing Example EVOH 1-5 and Comparative Examples EVOH 1-6 will generally differ from the methods disclosed below in one or more aspects.
[0060] First EVOH resin pellets of Example 1
[0061] 500 kg of vinyl acetate, 100 kg of methanol, 0.0585 kg of acetyl peroxide, and 0.015 kg of citric acid were added to a polymerization reactor equipped with a cooling coil. The polymerization reactor was temporarily purged with nitrogen and then purged with ethylene and pressed until the ethylene pressure reached 45 kg / cm 2 . Under ethylene pressure environment, the temperature was raised to 67°C while stirring to start polymerization. 6 hours after the start of polymerization, when the polymerization rate reached 60%, 0.0525 kg of sorbic acid conjugated polyene was added as an inhibitor. Thus, an ethylene-vinyl acetate copolymer with an ethylene structural unit content of 44 mole% was obtained. Then, the reaction solution containing the ethylene-vinyl acetate copolymer was supplied to a distillation tower, and methanol vapor was introduced from the lower part of the tower to remove unreacted vinyl acetate, thereby obtaining a methanol solution of ethylene-vinyl acetate copolymer.
[0062] In this embodiment, EVOH is formed by saponifying a component formed by polymerizing ethylene monomer and vinyl acetate monomer (ethylene-vinyl acetate copolymer, hereinafter referred to as "EVAC" polymer) with a saponification degree of 99.5%. Subsequently, EVOH is dissolved in an alcohol aqueous solution with a ratio of methanol to water of 70:30. The EVOH / methanol / water solution is placed at 60°C for 1 hour to promote the dissolution of EVOH in the EVOH / methanol / water solution. The solid content of the EVOH / methanol / water solution is 41wt%.
[0063] Then, the solution of methanol, water and EVOH is granulated by strip cutting. Specifically, a pump is used to pump the solution of methanol, water and EVOH into a feed pipe at a flow rate of 120L / min, and then fed into a circular opening mold with a diameter of 0.5mm, and the EVOH solution is extruded into a 5°C water / methanol mixed solution (water / methanol mass ratio = 9 / 1) to precipitate into strands, and then cut with a rotating knife at a speed of 500rpm to obtain EVOH particles. At the same time, 5°C circulating condensed water is used to cool the EVOH particles. Subsequently, the EVOH particles are centrifuged to separate the EVOH particles. After the EVOH particles are separated by water washing, the first dehydrator speed is 5000rpm in the centrifugal and washing steps; the water / wet particle ratio during transportation is 10; the type of the centrifugal pump for transportation is open; the transportation pump speed is 3000rpm; the water / wet particle weight ratio during water washing is 5; the water flow rate during water washing is 2m / min; the second dehydrator speed is 2000rpm, and then the EVOH particles are immersed in a boric acid / sodium acetate solution, the concentration of which is adjusted according to the boron content and alkali metal content of the final product, and finally dried by three different dryers to obtain EVOH cylindrical particles with a height of 5mm and a short diameter of 1mm.
[0064] The conditions of the above three drying stages are as follows: the first drying stage uses a belt dryer and is dried at 80°C for 2 hours; the second drying stage uses a belt dryer and is dried at 100°C for 20 hours; the third drying stage uses a flow dryer and is dried at 120°C for 20 hours. Finally, the particles are transported and stored. The transportation is carried out under the following conditions: the transportation form is air transportation, the pipeline diameter is 6 inches, the number of elbows is 4, the pipeline length is 30 meters, and the transportation speed is 40m / min.
[0065] Second EVOH resin pellets of Example 1
[0066] In this embodiment, compared with the first EVOH resin pellet of Example 1, the difference is that here, ethylene-vinyl acetate copolymer (hereinafter referred to as "EVAC") with an ethylene content of 32 mole% is saponified with a saponification degree of 99.5% to prepare EVOH polymer. And it is sent into a circular opening mold with a diameter of 2mm, and the EVOH solution is extruded into a 5°C water / methanol mixed solution (water / methanol mass ratio = 9 / 1) to precipitate into strands, and is cut with a rotating knife at a speed of 2000rpm. Subsequently, it is dried by three different dryers to obtain EVOH cylindrical pellets with a height of 2mm and a short diameter of 3mm.
[0067] The conditions of the above three drying stages are as follows: the first drying stage uses a microwave dryer and is dried at 70°C for 3 hours; the second drying stage uses a cylindrical stirring dryer and is dried at 110°C for 20 hours; the third drying stage uses a box dryer and is dried at 115°C for 30 hours.
[0068] For subsequent further preparation, the first EVOH resin particles and the second EVOH resin particles are further mixed in a ratio of 25 and 75 wt % respectively to form the EVOH resin particle composition of Example 1, and mixed using a conical screw mixer (model: CM-2, purchased from Xiehui Machinery Industry Co., Ltd.) at 10 rpm for 5 minutes.
[0069] The first and second EVOH resin particles of Example 2
[0070] The first and second EVOH methanol aqueous solutions used in Example 2 were prepared using a similar preparation method to the EVOH resin pellets of Example 1. However, when preparing the first EVOH methanol aqueous solution of Example 2, its ethylene content was 48 mole%; and the granulation step granulated the aforementioned methanol, water and EVOH solution by underwater pelletization. Specifically, the aforementioned methanol, water and EVOH solution was pumped into a feed pipe at a flow rate of 120L / min using a pump, and then fed into an input pipe with a diameter of 1mm, and cut using a rotating knife at 1500rpm to obtain EVOH pellets. At the same time, circulating condensed water at 5°C was used to cool the EVOH pellets. Subsequently, the EVOH pellets were centrifuged to separate the EVOH particles, and the separated EVOH particles were washed with water; the above-mentioned centrifugal dehydration step was performed a second time, and then the EVOH particles were immersed in a boric acid / sodium acetate solution, and then a drying step was performed and calcium stearate was added to obtain the final product of EVOH resin pellets. The three-stage drying conditions are as follows: the first stage drying is carried out in a box dryer at 60°C for 4 hours; the second stage drying is carried out in a microwave dryer at 80°C for 15 hours; the third stage drying is carried out in a flow dryer at 110°C for 30 hours; after drying, EVOH ellipsoidal particles with a long diameter of 3 mm and a short diameter of 2 mm are obtained. On the other hand, when preparing the second EVOH methanol aqueous solution of Example 2, its ethylene content is 27 mole%; and a similar preparation method is used as the first EVOH resin particles of Example 2; and the diameter of the input pipe is 2 mm: and the three-stage drying conditions are as follows: the first stage drying is carried out in a flow dryer at 60°C for 3 hours; the second stage drying is carried out in a belt dryer at 70°C for 30 hours; the third stage drying is carried out in a belt dryer at 100°C for 30 hours; after drying, EVOH spherical particles with a short diameter of 3 mm are obtained. Furthermore, the first EVOH resin particles and the second EVOH resin particles are further mixed in a ratio of 10 wt % and 90 wt % respectively to form the EVOH resin particle composition of Example 2.
[0071] The first and second EVOH resin particles of Example 3
[0072] The first and second EVOH methanol aqueous solutions used in Example 3 were prepared using a similar preparation method to the EVOH resin pellets of Example 2. However, when preparing the first EVOH methanol aqueous solution of Example 3, its ethylene content was 38 mole%; and the granulation step granulated the aforementioned methanol, water and EVOH solution by underwater pelletization. Specifically, the aforementioned methanol, water and EVOH solution was pumped into the feed pipe at a flow rate of 120L / min using a pump, and then fed into an input pipe with a diameter of 0.5mm, and cut using a rotating knife at 3000rpm to obtain EVOH pellets. At the same time, circulating condensed water at 5°C was used to cool the EVOH pellets. Subsequently, the EVOH pellets were centrifuged to separate the EVOH particles, and the separated EVOH particles were washed with water; the above-mentioned centrifugal dehydration step was performed a second time, and then the EVOH particles were immersed in a boric acid / sodium acetate solution, and then a drying step was performed and calcium stearate was added to obtain the final product of EVOH resin pellets. The three-stage drying conditions are as follows: the first stage drying is carried out using a belt dryer at 75°C for 2 hours; the second stage drying is carried out using a ventilated rotary dryer at 80°C for 15 hours; the third stage drying is carried out using an infrared dryer at 115°C for 20 hours; and after drying, EVOH spherical particles with a short diameter of 1 mm are obtained. On the other hand, when preparing the second EVOH methanol aqueous solution of Example 3, its ethylene content is 29 mole%; a similar preparation method as that of the EVOH resin particles of Example 1 is used, and the diameter of the opening die for strip cutting is 4 mm, and the rotating speed of the rotary knife is 3000 rpm; and the three-stage drying conditions are as follows: the first stage drying is carried out using a microwave dryer at 80°C for 2 hours; the second stage drying is carried out using a flow type dryer at 100°C for 20 hours; the third stage drying is carried out using a drum stirring type dryer at 105°C for 15 hours; and after drying, EVOH cylindrical particles with a height of 1 mm and a short diameter of 5 mm are obtained. Furthermore, the first EVOH resin particles and the second EVOH resin particles are further mixed in a ratio of 50 wt % and 50 wt % respectively to form the EVOH resin particle composition of Example 3.
[0073] The first and second EVOH resin particles of Example 4
[0074] The first and second EVOH methanol aqueous solutions used in Example 4 were prepared using a similar preparation method to the EVOH resin particles of Example 2. However, when preparing the first EVOH methanol aqueous solution of Example 4, its ethylene content was 48 mole%; and the granulation step was performed by granulating the aforementioned methanol, water and EVOH solution by underwater pelletization. Specifically, a pump was used to pump the aforementioned methanol, water and EVOH solution into a feed pipe at a flow rate of 120 L / min, and then fed into an input pipe with a diameter of 0.5 mm, and cut with a rotating knife at 500 rpm to obtain EVOH particles. At the same time, circulating condensed water at 5°C was used to cool the EVOH particles. Subsequently, the EVOH particles were centrifuged to separate the EVOH particles, and the separated EVOH particles were washed with water; the above-mentioned centrifugal dehydration step was performed a second time, and then the EVOH particles were immersed in a boric acid / sodium acetate solution, and then a drying step was performed and calcium stearate was added to obtain the final product of EVOH resin particles. The three-stage drying conditions are as follows: the first stage drying is carried out using a belt dryer at 80°C for 3 hours; the second stage drying is carried out using a microwave dryer at 90°C for 20 hours; the third stage drying is carried out using a ventilated rotary dryer at 110°C for 25 hours; after drying, EVOH ellipsoidal spherical particles with a long diameter of 5 mm and a short diameter of 1 mm are obtained. On the other hand, when preparing the second EVOH methanol aqueous solution of Example 4, its ethylene content is 32 mole%; and the preparation method similar to that of the first EVOH resin particles of Example 1 is used; and the diameter of the opening die for strip cutting is 2 mm, and the rotating speed of the rotary knife is 1500 rpm; and the three-stage drying conditions are as follows: the first stage drying is carried out using a flow type dryer at 70°C for 2 hours; the second stage drying is carried out using an infrared dryer at 90°C for 20 hours; the third stage drying is carried out using a box dryer at 100°C for 30 hours; after drying, EVOH cylindrical particles with a height of 3 mm and a short diameter of 3 mm are obtained. Furthermore, the first EVOH resin particles and the second EVOH resin particles are further mixed in a ratio of 15 wt % and 85 wt % respectively to form the EVOH resin particle composition of Example 4.
[0075] The first and second EVOH resin particles of Example 5
[0076] The first and second EVOH methanol aqueous solutions used in Example 5 were prepared using a similar preparation method to the EVOH resin pellets of Example 2. However, when preparing the first EVOH methanol aqueous solution of Example 5, its ethylene content was 38 mole%; and the granulation step granulated the aforementioned methanol, water and EVOH solution by underwater pelletization. Specifically, the aforementioned methanol, water and EVOH solution was pumped into the feed pipe at a flow rate of 120L / min using a pump, and then fed into an input pipe with a diameter of 1mm, and cut using a rotating knife at 1000rpm to obtain EVOH pellets. At the same time, circulating condensed water at 5°C was used to cool the EVOH pellets. Subsequently, the EVOH pellets were centrifuged to separate the EVOH particles, and the separated EVOH particles were washed with water; the above-mentioned centrifugal dehydration step was performed a second time, and then the EVOH particles were immersed in a boric acid / sodium acetate solution, and then a drying step was performed and calcium stearate was added to obtain the final product of EVOH resin pellets. The three-stage drying conditions are as follows: the first stage drying uses a flow type dryer and is dried at 60°C for 3 hours; the second stage drying uses a belt dryer and is dried at 100°C for 10 hours; the third stage drying uses a drum stirring type dryer and is dried at 110°C for 20 hours; after drying, EVOH ellipsoidal spheres with a long diameter of 4 mm and a short diameter of 2 mm are obtained. On the other hand, when preparing the second EVOH methanol aqueous solution of Example 5, its ethylene content is 24 mole%; the same preparation method as the first EVOH resin particle of Example 2 is used, the input tube diameter is 0.5 mm, and the cutting is performed at 1000 rpm using a rotary knife, and the three-stage drying conditions are as follows: the first stage drying uses an infrared dryer and is dried at 70°C for 2 hours; the second stage drying uses a ventilated rotary dryer and is dried at 95°C for 15 hours; the third stage drying uses a flow type dryer and is dried at 115°C for 30 hours; after drying, EVOH ellipsoidal spheres with a long diameter of 4 mm and a short diameter of 1 mm are obtained. Furthermore, the first EVOH resin particles and the second EVOH resin particles are further mixed in a ratio of 35 wt % and 65 wt % respectively to form the EVOH resin particle composition of Example 5.
[0077] The first and second EVOH resin pellets of Comparative Example 1
[0078] The first and second EVOH methanol aqueous solutions for Comparative Example 1 were prepared using a similar preparation method to the EVOH resin pellets of Example 2. However, when preparing the first EVOH methanol aqueous solution of Comparative Example 1, its ethylene content was 44 mole%; and the granulation step granulated the aforementioned methanol, water and EVOH solution by underwater pelletization. Specifically, the aforementioned methanol, water and EVOH solution was pumped into a feed pipe at a flow rate of 120 L / min using a pump, and then fed into an input pipe with a diameter of 2.5 mm, and cut using a rotating knife at 1200 rpm to obtain EVOH pellets. At the same time, circulating condensed water at 5°C was used to cool the EVOH pellets. Subsequently, the EVOH pellets were centrifuged to separate the EVOH particles, and the separated EVOH particles were washed with water; the above-mentioned centrifugal dehydration step was performed a second time, and then the EVOH particles were immersed in a boric acid / sodium acetate solution, and then a drying step was performed and calcium stearate was added to obtain the final product of EVOH resin pellets. The three-stage drying conditions are as follows: the first stage drying is carried out using a belt dryer at 80°C for 1 hour; the second stage drying is carried out using a belt dryer at 110°C for 2 hours; the third stage drying is carried out using a microwave dryer at 120°C for 10 hours; after drying, EVOH spherical particles with a short diameter of 3.5 mm are obtained. On the other hand, the second EVOH methanol aqueous solution of Comparative Example 1 is prepared, and its ethylene content is 29 mole%; a similar preparation method is used as the first EVOH resin particles of Example 1, the diameter of the open die for strip cutting is 3.5 mm, and the rotating knife speed is 500 rpm; and the three-stage drying conditions are as follows: the first stage drying is carried out using an infrared dryer at 85°C for 2 hours; the second stage drying is carried out using a box dryer at 105°C for 25 hours; the third stage drying is carried out using a microwave dryer at 130°C for 10 hours; after drying, EVOH cylindrical particles with a height of 5 mm and a short diameter of 4.5 mm are obtained. Furthermore, the first EVOH resin particles and the second EVOH resin particles are further mixed in a ratio of 5 wt % and 95 wt % respectively to form the EVOH resin particle composition of Comparative Example 1.
[0079] The first and second EVOH resin pellets of Comparative Example 2
[0080] The first and second EVOH methanol aqueous solutions for Comparative Example 2 were prepared using a similar preparation method to the EVOH resin pellets of Example 2. However, when preparing the first EVOH methanol aqueous solution of Comparative Example 2, its ethylene content was 35 mole%; and the granulation step granulated the aforementioned methanol, water and EVOH solution by underwater pelletization. Specifically, the aforementioned methanol, water and EVOH solution was pumped into a feed pipe at a flow rate of 120L / min using a pump, and then fed into an input pipe with a diameter of 1mm, and cut using a rotating knife at 1500rpm to obtain EVOH pellets. At the same time, circulating condensed water at 5°C was used to cool the EVOH pellets. Subsequently, the EVOH pellets were centrifuged to separate the EVOH particles, and the separated EVOH particles were washed with water; the above-mentioned centrifugal dehydration step was performed a second time, and then the EVOH particles were immersed in a boric acid / sodium acetate solution, and then a drying step was performed and calcium stearate was added to obtain the final product of EVOH resin pellets. The three-stage drying conditions are as follows: the first stage drying is carried out using an infrared dryer at 80°C for 4 hours; the second stage drying is carried out using a belt dryer at 110°C for 20 hours; the third stage drying is carried out using a microwave dryer at 105°C for 10 hours; and after drying, EVOH ellipsoidal spherical particles with a long diameter of 3 mm and a short diameter of 2 mm are obtained. On the other hand, when the second EVOH methanol aqueous solution of Comparative Example 2 is prepared, its ethylene content is 24 mole%; and a similar preparation method is used as the EVOH resin particles of Example 1, the diameter of the opening die for strip cutting is 1 mm, and the rotating knife speed is 1000 rpm; and the three-stage drying conditions are as follows: the first stage drying is carried out using a cylindrical stirring type dryer at 110°C for 3 hours; the second stage drying is carried out using a flow type dryer at 110°C for 30 hours; the third stage drying is carried out using a ventilated rotary dryer at 120°C for 50 hours; and after drying, EVOH cylindrical particles with a height of 4 mm and a short diameter of 2 mm are obtained. Furthermore, the first EVOH resin particles and the second EVOH resin particles are further mixed in a ratio of 75 wt % and 25 wt % respectively to form the EVOH resin particle composition of Comparative Example 2.
[0081] The first and second EVOH resin pellets of Comparative Example 3
[0082] The first and second EVOH methanol aqueous solutions used in Comparative Example 3 were prepared by a similar method to the EVOH resin pellets of Example 1. However, when the first EVOH methanol aqueous solution of Comparative Example 3 was prepared, its ethylene content was 48 mole%; and the same method as the EVOH resin pellets of Example 1 was used, the diameter of the open die for strip cutting was 3 mm, and the rotation speed of the rotary knife was 1700 rpm; and the three-stage drying state was: the first stage drying used a flow type dryer, and dried at 90°C for 3 hours; the second stage drying used a ventilated rotary dryer, and dried at 100°C for 25 hours; the third stage drying used a drum stirring type dryer, and dried at 110°C for 40 hours; after drying, EVOH cylindrical pellets with a height of 2.5 mm and a short diameter of 4 mm were obtained. On the other hand, when the second EVOH methanol aqueous solution of Comparative Example 3 was prepared, its ethylene content was 32 mole%; and the same method as the EVOH resin pellets of Example 1 was used, the diameter of the open die for strip cutting was 2 mm, and the rotation speed of the rotary knife was 1200 rpm. The three-stage drying process is as follows: the first stage drying uses a flow-type dryer at 80°C for 4 hours; the second stage drying uses a ventilated rotary dryer at 110°C for 30 hours; the third stage drying uses a flow-type dryer at 115°C for 30 hours; after drying, EVOH cylindrical particles with a height of 3.5 mm and a short diameter of 3 mm are obtained. Furthermore, the first EVOH resin particles and the second EVOH resin particles are further mixed at a weight percentage of 15 and 85 wt % respectively to form the EVOH resin particle composition of Comparative Example 3.
[0083] The first and second EVOH resin pellets of Comparative Example 4
[0084] The first and second EVOH methanol aqueous solutions for Comparative Example 4 were prepared using a similar preparation method to the EVOH resin pellets of Example 2. However, when preparing the first EVOH methanol aqueous solution of Comparative Example 4, its ethylene content was 38 mole%; and the granulation step granulated the aforementioned methanol, water and EVOH solution by underwater pelletization. Specifically, the aforementioned methanol, water and EVOH solution was pumped into a feed pipe at a flow rate of 120L / min using a pump, and then fed into an input pipe with a diameter of 0.5mm, and cut using a rotating knife at 3000rpm to obtain EVOH pellets. At the same time, circulating condensed water at 5°C was used to cool the EVOH pellets. Subsequently, the EVOH pellets were centrifuged to separate the EVOH particles, and the separated EVOH particles were washed with water; the above-mentioned centrifugal dehydration step was performed a second time, and then the EVOH particles were immersed in a boric acid / sodium acetate solution, and then a drying step was performed and calcium stearate was added to obtain the final product of EVOH resin pellets. The three-stage drying conditions are as follows: the first stage drying is carried out in a box dryer at 60°C for 2 hours; the second stage drying is carried out in a drum stirring dryer at 80°C for 30 hours; the third stage drying is carried out in a microwave dryer at 105°C for 20 hours; and after drying, EVOH spherical particles with a short diameter of 1 mm are obtained. On the other hand, when the second EVOH methanol aqueous solution of Comparative Example 4 is prepared, its ethylene content is 27 mole%; a preparation method similar to that of the first EVOH resin particles of Example 2 is used, the diameter of the input pipe is 3 mm during cutting, and a rotary knife is used to cut at 1000 rpm, and the three-stage drying conditions are as follows: the first stage drying is carried out in a drum stirring dryer at 100°C for 4 hours; the second stage drying is carried out in a ventilated rotary dryer at 90°C for 40 hours; the third stage drying is carried out in a flow dryer at 110°C for 30 hours; and after drying, EVOH spherical particles with a short diameter of 4 mm are obtained. Furthermore, the first EVOH resin particles and the second EVOH resin particles are further mixed in a ratio of 10 wt % and 90 wt % respectively to form the EVOH resin particle composition of Comparative Example 4.
[0085] The first and second EVOH resin pellets of Comparative Example 5
[0086] The first and second EVOH methanol aqueous solutions for Comparative Example 5 were prepared using a similar preparation method to the EVOH resin pellets of Example 2. However, when preparing the first EVOH methanol aqueous solution of Comparative Example 5, its ethylene content was 44 mole%; and the granulation step granulated the aforementioned methanol, water and EVOH solution by underwater pelletization. Specifically, the aforementioned methanol, water and EVOH solution was pumped into a feed pipe at a flow rate of 120L / min using a pump, and then fed into an input pipe with a diameter of 2.5mm, and cut using a rotating knife at 1000rpm to obtain EVOH pellets. At the same time, circulating condensed water at 5°C was used to cool the EVOH pellets. Subsequently, the EVOH pellets were centrifuged to separate the EVOH particles, and the separated EVOH particles were washed with water; the above-mentioned centrifugal dehydration step was performed a second time, and then the EVOH particles were immersed in a boric acid / sodium acetate solution, and then a drying step was performed and calcium stearate was added to obtain the final product of EVOH resin pellets. The three-stage drying conditions are as follows: the first stage drying is carried out using an infrared dryer at 60°C for 5 hours; the second stage drying is carried out using a belt dryer at 80°C for 10 hours; the third stage drying is carried out using an infrared dryer at 105°C for 20 hours; and after drying, EVOH ellipsoidal particles with a long diameter of 4 mm and a short diameter of 3.5 mm are obtained. On the other hand, when the second EVOH methanol aqueous solution of Comparative Example 5 is prepared, its ethylene content is 29 mole %; a similar preparation method is used as the first EVOH resin particle of Example 2, the diameter of the input tube is 0.5 mm during cutting, and a rotary knife is used to cut at 1700 rpm, and the three-stage drying conditions are as follows: the first stage drying is carried out using a belt dryer at 80°C for 2 hours; the second stage drying is carried out using a flow type dryer at 100°C for 10 hours; the third stage drying is carried out using an infrared dryer at 110°C for 15 hours; and after drying, EVOH ellipsoidal particles with a long diameter of 2.5 mm and a short diameter of 1 mm are obtained. Furthermore, the first EVOH resin particles and the second EVOH resin particles are further mixed in a ratio of 20 wt % and 80 wt % respectively to form the EVOH resin particle composition of Comparative Example 5.
[0087] The first and second EVOH resin pellets of Comparative Example 6
[0088] The first and second EVOH methanol aqueous solutions for Comparative Example 6 were prepared using a similar preparation method to the EVOH resin pellets of Example 2. However, when preparing the first EVOH methanol aqueous solution of Comparative Example 6, its ethylene content was 38 mole%; and the granulation step granulated the aforementioned methanol, water and EVOH solution by underwater pelletization. Specifically, the aforementioned methanol, water and EVOH solution was pumped into a feed pipe at a flow rate of 120L / min using a pump, and then fed into an input pipe with a diameter of 1.5mm, and cut using a rotating knife at 1700rpm to obtain EVOH pellets. At the same time, circulating condensed water at 5°C was used to cool the EVOH pellets. Subsequently, the EVOH pellets were centrifuged to separate the EVOH particles, and the separated EVOH particles were washed with water; the above-mentioned centrifugal dehydration step was performed a second time, and then the EVOH particles were immersed in a boric acid / sodium acetate solution, and then a drying step was performed and calcium stearate was added to obtain the final product of EVOH resin pellets. The three-stage drying conditions are as follows: the first stage drying is carried out using a cylindrical stirring type dryer at 105°C for 4 hours; the second stage drying is carried out using a ventilated rotary dryer at 110°C for 30 hours; the third stage drying is carried out using a flow type dryer at 105°C for 40 hours; and after drying, EVOH spherical particles with a short diameter of 2.5 mm are obtained. On the other hand, when the second EVOH resin methanol aqueous solution of Comparative Example 6 is prepared, its ethylene content is 32 mole%; and a similar preparation method is used as the first EVOH resin particles of Example 2; and the diameter of the input tube is 0.5 mm, and a rotary knife is used to cut at 1000 rpm: and the three-stage drying conditions are as follows: the first stage drying is carried out using a box dryer at 60°C for 3 hours; the second stage drying is carried out using a ventilated rotary dryer at 100°C for 20 hours; the third stage drying is carried out using a microwave dryer at 110°C for 30 hours; and after drying, EVOH elliptical spherical particles with a long diameter of 4 mm and a short diameter of 1 mm are obtained. Furthermore, the first EVOH resin particles and the second EVOH resin particles are further mixed in a ratio of 35 wt % and 65 wt % respectively to form the EVOH resin particle composition of Comparative Example 6.
[0089] The aforementioned box dryers, belt dryers, microwave dryers and infrared dryers are "static dryers"; flow dryers are "disturbance dryers"; drum stirring dryers and ventilated rotary dryers are "strong disturbance dryers". A brief description of disturbance dryers and strong disturbance dryers is as follows:
[0090] The disturbance type dryer means that the particles only move in one direction or slightly during drying. Among them, the flow type dryer is similar to a hot air oven, but the air volume is larger than that of a hot air oven, which will cause the particles to be slightly blown upward by the wind.
[0091] Strong disturbance type dryer refers to the dryer in which particles move in more than two dimensions or move violently during drying. Among them, drum stirring type dryer: using external force to stir, so particles will collide in the front, back, left and right directions; ventilation type rotary dryer: particles will collide in the tube wall during drying.
[0092] Parameters of EVOH resin pellets
[0093] The parameters of the EVOH resin pellets of the present invention and their evaluation / analysis methods are provided below.
[0094] Particle surface roughness
[0095] In order to evaluate / analyze the surface roughness of the EVOH resin particles in the embodiment, the EVOH resin particles are placed flat on a plate to measure the surface roughness of the particles; the data with an inclination greater than 0.5 must be excluded during measurement to ensure that the scanning plane is in a relatively horizontal state (inclination = maximum surface height Sz / side length of the analysis range 129μm). The laser microscope is LEXT OLS5000-SAF manufactured by Olympus, and the image is made at an air temperature of 24±3°C and a relative humidity of 63±3%. The filter is set to no filtering. The light source is a 405nm-wavelength light source. The objective lens is 100x magnification (MPLAPON-100xLEXT). The optical zoom is set to 1.0x. The image area is set to 129μm x 129μm (when measuring Rz, the center line of the image area is taken). The resolution is set to 1024 pixels x 1024 pixels. The values of 100 particles are measured and the average value is taken. Among them, Vvc, Vmc, Sq, Sz and Sk are measured using the ISO 25178:2012 method; Ra and Rz are measured using the JIS B 0601 (2001) method.
[0096] Ethylene content analysis
[0097] In order to evaluate / analyze the ethylene content of the EVOH resin particles of the embodiment, the present invention uses a Raman spectrometer manufactured by UniDRON, and uses a laser light source with a wavelength of 473nm to randomly measure the ethylene content of 5 points on each EVOH resin particle, and takes the average value as the ethylene content value of the EVOH resin particle sample.
[0098] Melting point analysis
[0099] Here, the melting point temperature of the EVOH resin pellets is measured according to ISO 11357-3-2011 method using a DSC Q200 device (TZERO TECHNOLOGIES, INC.; the lid (Tzero lid) is TA Instruments T170607, and the pan (Tzero pan) is TA Instruments T170620).
[0100] In practice, without being limited by a specific theory, when there are a large number of EVOH resin particles, 100 EVOH resin particles can be taken first and their individual ethylene contents can be obtained by the above-mentioned ethylene content analysis method. Then, for those with an ethylene content between 35 and 48 mole%, they are pre-classified as low-melting-point EVOH resin particles with a melting point of about 135 to 179°C; and for those with an ethylene content between 24 and 34 mole%, they are pre-classified as high-melting-point EVOH resin particles with a melting point of about 180 to 198°C. Furthermore, 10 EVOH resin particles are randomly taken out from the groups of low-melting-point EVOH resin particles and high-melting-point EVOH resin particles, and their surface roughness is obtained by the above-mentioned surface parameter measurement method, and then the melting points of these EVOH resin particles are determined by the above-mentioned melting point measurement method.
[0101] Preparation and analysis of EVOH single-layer film
[0102] The EVOH resin particle compositions of Examples 1 to 5 and Comparative Examples 1 to 6 were formed into films according to the following method. The EVOH resin particle compositions of Examples 1 to 5 and Comparative Examples 1 to 6 were fed into a single screw extruder (model ME25 / 5800V4, brand OCS) to extrude and prepare a single-layer film. The thickness of the films formed by the EVOH resin particle compositions of Examples 1 to 5 and Comparative Examples 1 to 6 was 20 μm. The temperature of the extruder was set to 220° C.; and the rotation frequency of the screw was set to 7 rpm (rotations / minutes).
[0103] Furthermore, the uniformity of the ethylene content of the single-layer films of the above-mentioned Examples 1 to 5 and Comparative Examples 1 to 6 can be analyzed. Specifically, the analysis method is to use a Raman spectrometer manufactured by UniDRON and use a laser light source with a wavelength of 473nm to randomly measure the ethylene content of 5 points on each film, and then calculate the standard deviation. When the standard deviation is less than 1, it is judged as "0"; when the standard deviation is between 1 and 2, it is judged as "△"; when the standard deviation is greater than 2, it is judged as "X".
[0104] Preparation of multilayer structures
[0105] Here, the EVOH resin particle compositions, polypropylene and adhesive layers (e.g. 18729, Arkema Co., Ltd.) were co-extruded to form the respective multilayer films of Examples 1 to 5 and Comparative Examples 1 to 6. The multilayer film has 5 layers. Specifically, EVOH particles (I), polypropylene (II) and adhesive resin (III) were fed to a five-layer co-extrusion film forming machine to prepare a multilayer sheet having the following structure: (II) / (III) / (I) / (III) / (II), with thicknesses of 300 / 25 / 50 / 25 / 300 (um), respectively.
[0106] Preparation and analysis of thermoformed bodies
[0107] Next, the multilayer films of Examples 1 to 5 and Comparative Examples 1 to 6 are thermoformed to form a container shape (e.g., a cup and / or a cup-shaped container, such as a fruit cup), thereby obtaining a thermoformed body in the form of a multilayer container (e.g., Figure 2 As shown), its height H is 10 cm, the upper end diameter R1 is 10 cm, and the bottom diameter R2 is 7 cm. Further, in order to evaluate the thermoformability of Examples 1 to 5 and Comparative Examples 1 to 6, the thermoformed bodies of Examples 1 to 5 and Comparative Examples 1 to 6 were cut with a razor, and the thickness of the EVOH layer in the standing surface area A1 and the corner surface area A2 was measured with an optical microscope. Specifically, when the difference in the thickness of the EVOH layer between the standing surface area A1 and the corner surface area A2 is less than 20%, it is judged as "O"; when the difference in the thickness of the EVOH layer between the standing surface area A1 and the corner surface area A2 is 20-40%, it is judged as "△"; when the difference in the thickness of the EVOH layer between the standing surface area A1 and the corner surface area A2 is greater than 40%, it is judged as "X".
[0108] On the other hand, the appearance of the thermoformed body is judged by the naked eye to see whether there are rough surfaces. Specifically, if there are no rough surfaces, it is judged as "O", and if there are rough surfaces, it is judged as "X".
[0109] Furthermore, the present invention evaluates the gas barrier properties of the thermoformed body by measuring the oxygen transmission rate (OTR) of the thermoformed body. The present invention uses an OX-TRAN Model 2 / 22 oxygen transmission rate tester (mocon company) to measure the OTR of the thermoformed bodies of Examples 1 to 5 and Comparative Examples 1 to 6, respectively, according to the ISO 14663-2 method. The OTR test is carried out under the conditions of a relative humidity of 65% and 23°C, and the unit is cc / pkg*day. Specifically, when the OTR is less than 0.01cc / pkg*day, it is judged as "O"; when the OTR is 0.01~0.5cc / pkg*day, it is judged as "△"; when the OTR is greater than 0.5cc / pkg*day, it is judged as "X".
[0110] Results Analysis of Examples and Comparative Examples
[0111] In this section, the EVOH resin pellet compositions of Examples 1 to 5 and Comparative Examples 1 to 6 are compared in terms of the uniformity of the ethylene content of the films made therefrom, as well as the subsequent thermoformability, appearance of the thermoformed bodies, and OTR of the thermoformed bodies. The results are shown in Tables 1 and 2, respectively.
[0112] Table 1
[0113]
[0114] Table 2
[0115]
[0116] As can be seen from Table 1 and Table 2, the surface core void volume (Vvc) of the first EVOH resin particles contained in the EVOH resin particle compositions of Examples 1 to 5 is 0.002 to 14 μm. 3 / um 2 At the same time, the surface core void volume (Vvc) of the second EVOH resin particle is 0.010-48um 3 / um 2 ; and the film made thereof has good ethylene content uniformity and ideal thermoformability, and the thermoformed body made therefrom has excellent appearance and gas barrier properties. In contrast, the EVOH resin particle compositions of Comparative Examples 1 to 6 do not meet the numerical range of the surface core void volume (Vvc) of the first and second EVOH resin particles; and the film made therefrom has poor ethylene content uniformity and unsatisfactory thermoformability, and the thermoformed body made therefrom has poor appearance and gas barrier properties. Preferably, the Vvc of the second EVOH resin particle of the first EVOH resin particle is greater than the Vvc of the first EVOH resin particle. Preferably, the melting point of the first EVOH resin particle is 135 to 179°C, and the melting point of the second EVOH resin particle is 180 to 198°C. Preferably, the ethylene content of the first EVOH resin particle is 36 to 50 mole percent, and the ethylene content of the second EVOH resin particle is 20 to 35 mole percent.
[0117] Further comparison of Table 1 and Table 2 shows that although the first EVOH resin particles contained in the EVOH resin particle composition of Comparative Example 4, the second EVOH resin particles contained in the EVOH resin particle composition of Comparative Example 5, and the second EVOH resin particles contained in the EVOH resin particle composition of Comparative Example 6 respectively fall within the Vvc numerical range of the first or second EVOH resin particles defined in the present invention, the other EVOH resin particles contained in these EVOH resin particle compositions are not within the corresponding Vvc numerical range. It can be understood that only when the two EVOH resin particles contained in the EVOH resin particle composition meet the Vvc numerical range defined in this case, the two EVOH resins can have better miscibility, and thus the film made thereof has good ethylene content uniformity, and has ideal thermoforming properties, and the thermoformed body made therefrom has excellent appearance and gas barrier properties.
[0118] In addition, the inventors have found that by adjusting the combination of multiple variables in the three-stage drying used in the processing of EVOH pellets, the desired Vvc of the present invention can be controlled and obtained, namely: A. The first stage of drying cannot use a strongly disturbed dryer. B. The second and third stages of drying cannot all use a strongly disturbed dryer. C. It is better not to use a static dryer for all three stages of drying.
[0119] Assuming that the above three situations are not involved in the processing, it is further recommended that the temperature range of the first drying stage is 60-80°C, and the drying time is 2-4 hours; the temperature range of the second drying stage is 70-110°C, and the drying time is 15-30 hours; the temperature range of the third drying stage is 100-120°C, and the drying time is 15-30 hours.
[0120] Herein, all ranges provided are intended to include each specific range within a given range and combinations of sub-ranges between the given ranges. In addition, unless otherwise stated, all ranges provided herein include the endpoints of the ranges. Thus, ranges 1-5 specifically include 1, 2, 3, 4, and 5, as well as sub-ranges such as 2-5, 3-5, 2-3, 2-4, 1-4, etc.
[0121] All publications and patent applications cited in this specification are incorporated herein by reference, and each individual publication or patent application is specifically and individually indicated to be incorporated herein by reference for any and all purposes. In the event of any inconsistency between this document and any publication or patent application incorporated herein by reference, this document controls.
[0122] As used herein, the terms "include", "have" and "comprises" have an open, non-restrictive meaning. The terms "a", "an" and "the" are to be understood to cover the plural as well as the singular. The term "one or more" means "at least one", and thus may include a single feature or a mixture / combination of features. The term "between" includes its endpoint values.
[0123] Except in the operating examples or where otherwise indicated, all numbers indicating amounts of ingredients and / or reaction conditions may in all cases be modified by the term "about", meaning within ±5% of the indicated number. As used herein, the terms "substantially free" or "substantially free" refer to less than about 2% of a particular feature. All elements or features that are positively described herein may be negatively excluded from the claims.
Claims
1. An ethylene vinyl alcohol copolymer (EVOH) resin particle composition comprising: A first EVOH resin particle having a surface core void volume (Vvc) of 0.002 to 14 μm 3 / um 2 , and the ethylene content of the first EVOH resin particles is 36 to 50 mol percent, and A second EVOH resin particle having a surface core void volume (Vvc) of 0.010 to 48 μm 3 / um 2 , and the ethylene content of the second EVOH resin particles is 20 to 35 mol percent; The Vvc of the second EVOH resin particles is greater than the Vvc of the first EVOH resin particles.
2. The EVOH resin particle composition according to claim 1, wherein the melting point of the first EVOH resin particles is 135 to 179°C, and wherein the melting point of the second EVOH resin particles is 180 to 198°C.
3. The EVOH resin particle composition according to claim 1 or 2, wherein the EVOH resin particles are in the shape of a cylinder, an elliptical cylinder, an angular cylinder, a sphere, an elliptical sphere or a go shape, and have a major diameter / height of 1 to 5 mm and a minor diameter of 1 to 5 mm. 4 . The EVOH resin particle composition according to claim 1 , wherein the weight percentage of the first EVOH resin particles to the second EVOH resin particles is 5:95 to 75:
25.
5. The EVOH resin pellet composition according to claim 1 or 2, which has a boron content of 5 to 550 ppm.
6. The EVOH resin pellet composition according to claim 1 or 2, which has an alkali metal content of 10 to 550 ppm.
7. The EVOH resin particle composition according to claim 1 or 2, wherein: The first EVOH resin particle has a surface core volume (Vmc) of 0.001-12 μm. 3 / um 2 ;and The second EVOH resin particle has a surface core volume (Vmc) of 0.022-55 μm. 3 / um 2 .
8. The EVOH resin particle composition according to claim 1 or 2, wherein: The first EVOH resin particles have a root mean square height (Sq) surface parameter of 0.001 to 25 um; and The second EVOH resin particles have a root mean square height (Sq) surface parameter of 0.020 to 65 um.
9. The EVOH resin particle composition according to claim 1 or 2, wherein: The first EVOH resin particles have a surface parameter of maximum height (Sz) of 0.030 to 28 μm; and The second EVOH resin particles have a surface parameter of a maximum height (Sz) of 0.120 to 65 μm.
10. The EVOH resin particle composition according to claim 1 or 2, wherein: The first EVOH resin particles have a core height difference (Sk) surface parameter of 0.010 to 25 um; and The second EVOH resin particles have a core height difference (Sk) surface parameter of 0.030-65 um.
11. The EVOH resin particle composition according to claim 1 or 2, wherein: The first EVOH resin particles have a surface parameter of a linear arithmetic average height (Ra) of 0.001 to 0.990 um; and The second EVOH resin particles have a surface parameter of a linear arithmetic average height (Ra) of 0.001 to 0.990 um.
12. The EVOH resin particle composition according to claim 1 or 2, wherein: The first EVOH resin particles have a line maximum height (Rz) surface parameter of 0.0010 to 9.9000 um; and The second EVOH resin particles have a line maximum height (Rz) surface parameter of 0.0010 to 9.9000 um.
13. An ethylene-vinyl alcohol copolymer film, which is formed from the EVOH resin particle composition according to any one of claims 1 to 12.
14. A multilayer structure comprising: (a) at least one layer of an ethylene-vinyl alcohol copolymer film formed from the EVOH resin particle composition according to any one of claims 1 to 12; (b) at least one polymer layer; and (c) at least one adhesive layer.
15. The multilayer structure of claim 14, wherein the polymer layer is selected from the group consisting of a low density polyethylene layer, a polyethylene grafted maleic anhydride layer, a polypropylene layer, and a nylon layer, and the adhesive layer is a tie layer.
16. The multilayer structure according to claim 14 or 15, wherein the multilayer structure is polymer layer / adhesive layer / ethylene-vinyl alcohol copolymer film / adhesive layer / polymer layer.