Transparent resin laminate, and transparent substrate material and transparent protective material using the same
A resin laminate with closely matched glass transition temperatures and a hard coating layer addresses thermoformability issues in acrylic-polycarbonate laminates, ensuring low-temperature thermoforming without cracking or interference fringes, suitable for transparent substrates and protective materials.
Patent Information
- Application Number
- CN202080052701.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-08-20
- Filing Date
- 2020-07-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-07-01
AI Technical Summary
Existing laminates of acrylic and polycarbonate resins face issues with thermoformability at low temperatures, leading to interface peeling, whitening, and cracking during thermoforming, and rebounding that prevents accurate mold reproduction.
A resin laminate comprising a polycarbonate-based resin layer with a thermoplastic resin layer containing methacrylic resin and styrene copolymer, where the glass transition temperatures are closely matched, and a hard coating layer, allowing for thermoforming without cracking or interference fringes.
The laminate achieves excellent thermoformability at low temperatures, preventing cracking and interference fringes, while maintaining a good appearance, suitable for transparent substrates and protective materials.
Smart Images

Figure BDA0003480518160000031 
Figure BDA0003480518160000051 
Figure BDA0003480518160000052
Abstract
Description
Technical Field
[0001] The present invention relates to a resin laminate used for a transparent substrate material or a protective material, and more specifically, to a resin laminate having excellent thermoformability at low temperatures, and having a good appearance and capable of suppressing the generation of interference fringes. Background Art
[0002] Acrylic resins are excellent in surface hardness, transparency, scratch resistance, weather resistance, etc. On the other hand, polycarbonate resins are excellent in impact resistance, etc. Therefore, a laminate having an acrylic resin layer and a polycarbonate resin layer is excellent in surface hardness, transparency, scratch resistance, weather resistance, impact resistance, etc., and can be used for automobile parts, home appliances, electronic equipment, and display windows of portable information terminals.
[0003] In recent years, along with the diversification of design requirements, the front panel of display equipment and the like also need products with improved design through thermoforming such as vacuum forming or air pressure forming. Laminated bodies having acrylic resin layers and polycarbonate resin layers have been tried for use in front panels because of their excellent performance as described above. However, when thermoforming the laminated body having acrylic resin layers and polycarbonate resin layers, the sheet needs to be heated to a temperature at which the polycarbonate resin is fully extended, which will apply too much heat to the acrylic resin, so that sometimes the interface between the acrylic resin layer and the polycarbonate resin layer peels off, and the surface whitens or cracks. On the other hand, when the molding temperature is lowered in order to suppress the occurrence of whitening / cracking, "rebound" that cannot reproduce the mold shape sometimes occurs.
[0004] Patent Document 1 discloses a molding resin sheet of a polycarbonate resin having a specific terminal group and an acrylic resin as a molding resin sheet suitable for thermoforming such as vacuum molding or gas pressure molding. The resin sheet can suppress whitening / cracking during bending processing by thermoforming. However, when the surface of the acrylic resin layer of the resin sheet is hard-coated, there is a problem of cracking during bending processing by thermoforming.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2016 / 060100 Summary of the invention
[0008] Technical problem to be solved by the invention
[0009] The present invention provides a resin laminate having excellent thermoformability at low temperatures, in which the generation of interference fringes can be suppressed and which has a good appearance.
[0010] Technical solutions for solving technical problems
[0011] In order to solve the above technical problems, the inventors of the present invention have repeatedly conducted in-depth research and finally completed the present invention. The specific contents of the present invention are as follows.
[0012] [1] A resin laminate comprising a layer comprising a thermoplastic resin (B) on at least one surface of a layer comprising a polycarbonate-based resin (A), and a hard coating layer on at least one surface of the layer comprising the thermoplastic resin (B),
[0013] The glass transition temperature of the polycarbonate resin (A) is 115°C to 140°C.
[0014] The thermoplastic resin (B) contains a methacrylic resin (C) and a styrene copolymer (D), wherein the content of the methacrylic resin (C) is 5 to 70 parts by mass and the content of the styrene copolymer (D) is 95 to 30 parts by mass, based on 100 parts by mass of the total content of the methacrylic resin (C) and the styrene copolymer (D).
[0015] The styrene copolymer (D) is a copolymer containing 68 to 84% by mass of a vinyl aromatic monomer unit (d1) and 16 to 32% by mass of a cyclic acid anhydride monomer unit (d2).
[0016] [2] The resin laminate according to the above [1], wherein the thermoplastic resin (B) consists only of the methacrylic resin (C) and the styrene copolymer (D).
[0017] [3] The resin laminate according to [1] or [2] above, wherein the polycarbonate resin (A) has a glass transition temperature of 115°C or higher and lower than 130°C.
[0018] [4] The resin laminate according to any one of [1] to [3] above, wherein no cracks are generated after being thermoformed to a thickness of 50 mmR using a hot press.
[0019] [5] The resin laminate according to any one of [1] to [4] above, wherein springback does not occur after being thermoformed to a thickness of 50 mmR using a hot press.
[0020] [6] The resin laminate according to any one of [1] to [5] above, wherein the difference between the glass transition temperature of the polycarbonate resin (A) and the glass transition temperature of the thermoplastic resin (B) is in the range of 0 to 15°C.
[0021] [7] The resin laminate according to any one of [1] to [6] above, wherein the thermoplastic resin (B) is a polymer alloy of a methacrylic resin (C) and a styrene copolymer (D).
[0022] [8] The resin laminate according to any one of [1] to [7] above, wherein the vinyl aromatic monomer unit (d1) contained in the styrene copolymer (D) is styrene.
[0023] [9] The resin laminate according to any one of [1] to [8] above, wherein the cyclic acid anhydride monomer unit (d2) contained in the styrene copolymer (D) is maleic anhydride.
[0024]
[10] The resin laminate according to any one of [1] to [9] above, wherein the polycarbonate resin (A) has a terminal structure derived from a monohydric phenol represented by the following general formula (1) and a structural unit derived from a dihydric phenol.
[0025]
[0026] (In the formula, R1 represents an alkyl group having 8 to 36 carbon atoms or an alkenyl group having 8 to 36 carbon atoms, and R2 to R5 each represent hydrogen, a halogen, or an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 12 carbon atoms which may have a substituent, and the substituent is a halogen, an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 12 carbon atoms.)
[0027]
[11] The resin laminate as described in any one of [1] to
[10] above, wherein the thickness of the layer containing the thermoplastic resin (B) is in the range of 10 to 250 μm, and the thickness of the entire resin laminate is in the range of 0.4 to 4.0 mm.
[0028]
[12] The resin laminate as described in any one of [1] to
[11] above, wherein at least one of the layer comprising the polycarbonate resin (A), the layer comprising the thermoplastic resin (B), and the hard coat layer contains a UV absorber.
[0029]
[13] The resin laminate according to any one of [1] to
[12] above, wherein the hard coat layer is an acrylic hard coat layer.
[0030]
[14] A resin laminate as described in any one of [1] to
[13] above, wherein one or both sides of the resin laminate are subjected to at least one of anti-fingerprint treatment, anti-reflection treatment, anti-glare treatment, weather resistance treatment, antistatic treatment and anti-fouling treatment.
[0031]
[15] A thermoformed body formed by subjecting the resin laminate according to any one of [1] to
[14] above to a heat-bending process.
[0032]
[16] A transparent substrate material comprising the resin laminate according to any one of [1] to
[14] above, or the thermoformed product according to
[15] above.
[0033]
[17] A transparent protective material comprising the resin laminate described in any one of [1] to
[14] above, or the thermoformed product described in
[15] above.
[0034]
[18] A touch panel front protection plate comprising the resin laminate according to any one of [1] to
[14] above, or the thermoformed body according to
[15] above.
[0035]
[19] A front panel for a car navigation system, OA equipment or a portable electronic device, comprising the resin laminate described in any one of [1] to
[14] above, or the thermoformed product described in
[15] above.
[0036] Effects of the Invention
[0037] According to the present invention, a resin laminate is provided that can form a thermoformed product having excellent thermoformability at low temperature and suppressing the generation of interference fringes. That is, the resin laminate of the present invention can obtain a molded product having good appearance while suppressing the generation of whitening / cracking during thermoforming.
[0038] The resin laminate can be used as a transparent substrate material or a transparent protective material. Specifically, it is suitable for use as, for example, a front panel for protecting portable display devices such as mobile phone terminals, portable electronic game consoles, portable information terminals, and mobile PCs, and display devices such as notebook PCs, desktop PC liquid crystal monitors, car navigation liquid crystal monitors, and liquid crystal televisions. DETAILED DESCRIPTION
[0039] Hereinafter, the present invention will be described in detail with reference to production examples and embodiments, but the present invention is not limited to the production examples and embodiments, and can be carried out by changing to any method within the scope not greatly exceeding the scope of the present invention.
[0040] <Polycarbonate resin (A)>
[0041] The polycarbonate resin (A) used in the present invention is a polycarbonate resin (A) with polycarbonate resin as the main component. Here, "with polycarbonate resin as the main component" means that the content of polycarbonate resin exceeds 50% by mass. The polycarbonate resin (A) preferably contains more than 75% by mass of polycarbonate resin, more preferably contains more than 90% by mass of polycarbonate resin, and further preferably is substantially composed of polycarbonate resin. The polycarbonate resin (A) contains a carbonate bond in the main chain of the molecule. That is, as long as it contains -[O-R-OCO]- units (wherein R represents a group containing an aliphatic group, an aromatic group, or both an aliphatic group and an aromatic group, and having a branched structure or a branched structure), there is no particular limitation, and it is particularly preferred to use a polycarbonate containing a structural unit of the following formula (2). By using such a polycarbonate, a resin laminate with excellent impact resistance can be obtained.
[0042]
[0043] The polycarbonate resin (A) is preferably synthesized using a monohydric phenol represented by the following general formula (1) as a terminal terminator.
[0044]
[0045] (In the formula, R1 represents an alkyl group having 8 to 36 carbon atoms or an alkenyl group having 8 to 36 carbon atoms, and R2 to R5 each represent hydrogen, a halogen, or an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 12 carbon atoms which may have a substituent, and the substituent is a halogen, an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 12 carbon atoms.)
[0046] The monohydric phenol of the general formula (1) is more preferably a monohydric phenol represented by the following general formula (3).
[0047]
[0048] (In the formula, R1 represents an alkyl group having 8 to 36 carbon atoms, or an alkenyl group having 8 to 36 carbon atoms.)
[0049] It is more preferred that the number of carbon atoms of R1 in the general formula (1) or the general formula (3) is within a specific numerical range. Specifically, the upper limit of the number of carbon atoms of R1 is preferably 36, more preferably 22, and particularly preferably 18. In addition, the lower limit of the number of carbon atoms of R1 is preferably 8, and more preferably 12.
[0050] Among the monohydric phenols (terminator) represented by the general formula (1) or (3), it is particularly preferred to use either or both of hexadecyl p-hydroxybenzoate and 2-hexyldecyl p-hydroxybenzoate as the terminator.
[0051] When a monophenol (terminator) having, for example, an alkyl group having 16 carbon atoms is used as R1 in the general formula (1) or the general formula (3), the glass transition temperature, melt fluidity, moldability, sag resistance, and solvent solubility of the monophenol when producing the polycarbonate resin are excellent, and it is particularly preferred as a terminator used for the polycarbonate resin used in the present invention.
[0052] On the other hand, when the number of carbon atoms of R1 in the general formula (1) or (3) is too large, the solubility of the monohydric phenol (terminator) in an organic solvent tends to decrease, and productivity in producing a polycarbonate resin may decrease.
[0053] For example, when the carbon number of R1 is 36 or less, the productivity is high and the economic efficiency is good when manufacturing polycarbonate resin. When the carbon number of R1 is 22 or less, the organic solvent solubility of monohydric phenol is particularly excellent, which can make the productivity of manufacturing polycarbonate resin very high and the economic efficiency is also improved.
[0054] When the number of carbon atoms of R1 in the general formula (1) or (3) is too small, the glass transition temperature of the polycarbonate resin cannot be sufficiently low, and the thermoformability may be reduced.
[0055] As other resins contained in the polycarbonate resin (A), there are polyester resins. In the polyester resin, as a dicarboxylic acid component, terephthalic acid can be contained as the main component, and dicarboxylic acid components other than terephthalic acid can also be contained. For example, it is preferred that a polyester resin formed by polycondensation of a diol component containing 20 to 40 (molar ratio, total 100) of 1,4-cyclohexanedimethanol with respect to 80 to 60 (molar ratio) of the main component ethylene glycol and a dicarboxylic acid component, namely the so-called "PETG". In addition, the polycarbonate resin (A) may contain a polyester carbonate resin having an ester bond and a carbonate bond in the polymer skeleton.
[0056] In the present invention, the weight average molecular weight of the polycarbonate resin (A) affects the impact resistance and molding conditions of the resin laminate. That is, when the weight average molecular weight is too small, the impact resistance of the resin laminate is reduced, which is not preferred. When the weight average molecular weight is too high, sometimes an excessive heat source is required when laminating layers containing the polycarbonate resin (A), which is not preferred. Moreover, depending on the molding method, high temperature is sometimes required, so the polycarbonate resin (A) is exposed to high temperature, which sometimes has an adverse effect on its thermal stability. The weight average molecular weight of the polycarbonate resin (A) is preferably 10,000 to 75,000, and more preferably 15,000 to 60,000. More preferably, it is 20,000 to 50,000.
[0057] <Method for measuring weight average molecular weight of polycarbonate resin (A)>
[0058] The weight average molecular weight of the polycarbonate resin (A) can be measured according to the description in paragraphs 0061 to 0064 of JP-A-2007-179018. The details of the measurement method are as follows.
[0059] [Table 1]
[0060] Table 1: Determination conditions of weight average molecular weight
[0061] Device Waters manufactures "Aliance" Chromatographic columns Showa Denko "Shodex K-805L" (2 pieces) Detector UV detector: 254nm Eluent Chloroform
[0062] After using polystyrene (PS) as a standard polymer for measurement, the relationship between the dissolution time and the molecular weight of polycarbonate (PC) is obtained by the universal calibration method, and a standard curve is prepared. Then, the dissolution curve (chromatogram) of PC is measured under the same conditions as the standard curve, and each average molecular weight is obtained from the dissolution time (molecular weight) and the peak area (number of molecules) of the dissolution time. When the number of molecules of the molecular weight Mi is set to Ni, the weight average molecular weight is expressed as follows. And the conversion formula uses the following formula.
[0063] (Weight average molecular weight)
[0064] Mw=Σ(NiMi 2 ) / Σ(NiMi)
[0065] (Conversion formula)
[0066] MPC=0.47822MPS1.01470
[0067] Here, MPC represents the molecular weight of PC, and MPS represents the molecular weight of PS.
[0068] The glass transition temperature of the polycarbonate resin (A) used in the present invention is preferably 115 to 140°C, more preferably 120 to 135°C, and even more preferably 120 to 130°C. In particular, in order to make the thermoformability of the resin laminate good, the upper limit of the glass transition temperature is preferably lower than 130°C, for example, 129°C or 128°C. The glass transition temperature of the polycarbonate resin (A) in this specification refers to the temperature measured at a heating rate of 10°C / min using a differential scanning calorimeter and calculated at the intersection of the tangent line of the baseline and the inflection point.
[0069] The melt flow rate of the polycarbonate resin (A) is preferably in the range of 1 to 30 g / 10 minutes, more preferably in the range of 8 to 20 g / 10 minutes, and further preferably in the range of 11 to 15 g / 10 minutes. When the melt flow rate is in the range of 1 to 30 g / 10 minutes, the stability of the heated melt molding is good. The melt flow rate of the polycarbonate resin (A) in this specification refers to the value measured using a melt indexer at a temperature of 300°C and a load of 1.2 kg.
[0070] The method for producing the polycarbonate resin (A) used in the present invention can be appropriately selected from a known phosgene method (interfacial polymerization method), an ester exchange method (melt method), and the like according to the monomers used.
[0071] <Thermoplastic resin (B)>
[0072] The thermoplastic resin (B) used in the present invention contains a methacrylic resin (C) and a styrene copolymer (D), but it is particularly preferred to consist of only the methacrylic resin (C) and the styrene copolymer (D) because of good compatibility.
[0073] <Methacrylic resin (C)>
[0074] The methacrylic resin (C) contained in the thermoplastic resin (B) of the present invention includes a structural unit derived from a methacrylic acid ester monomer.
[0075] Examples of the methacrylic acid ester monomer of the methacrylic acid resin (C) include alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, pentyl methacrylate, hexyl methacrylate, heptyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, decyl methacrylate, and dodecyl methacrylate; cycloalkyl methacrylates such as 1-methylcyclopentyl methacrylate, cyclohexyl methacrylate, cycloheptyl methacrylate, cyclooctyl methacrylate, and tricyclo[5.2.1.02,6]dec-8-yl methacrylate; aryl methacrylates such as phenyl methacrylate; and aralkyl methacrylates such as benzyl methacrylate. From the viewpoint of availability, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, and tert-butyl methacrylate are preferred, and methyl methacrylate is most preferred.
[0076] From the viewpoint of heat resistance, the methacrylic resin preferably contains 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, of a structural unit derived from MMA.
[0077] Furthermore, the methacrylic resin (C) may further contain structural units derived from other monomers other than methacrylic acid esters. Examples of such other monomers include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, hexyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, decyl acrylate, dodecyl acrylate, stearyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, cyclohexyl acrylate, 2-methoxyethyl acrylate, 3-methoxybutyl acrylate, trifluoromethyl acrylate, trifluoroethyl acrylate, pentafluoroethyl acrylate, glycidyl acrylate, allyl acrylate, phenyl acrylate, toluene acrylate, benzyl acrylate, isobornyl acrylate, 3-dimethylaminoethyl acrylate and other acrylates. From the viewpoint of availability, acrylates such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, and tert-butyl acrylate are preferred, methyl acrylate and ethyl acrylate are more preferred, and methyl acrylate is most preferred. The total content of structural units derived from these other monomers in the methacrylic resin (C) is preferably 20% by mass or less, more preferably 10% by mass or less, and further preferably 5% by mass or less.
[0078] The methacrylic resin (C) preferably has a triad-expressed syndiotacticity (rr) of 50 mol% or more, more preferably 51 mol% or more, and further preferably 52 mol% or more. When the lower limit of the content of this structure is 50 mol% or more, the heat resistance is excellent.
[0079] Here, the syndiotacticity (rr) expressed by the triad (hereinafter sometimes referred to as "syndiotacticity (rr)") is the ratio of two chains (two chains, diad) of a chain of three consecutive structural units (three-unit group, triad) to be racemic (referred to as rr). Among them, the chains (two-unit group, diad) of structural units in the polymer molecule with the same stereo configuration are called meso, and the opposite is called racemo, and these are respectively referred to as m and r.
[0080] The syndiotacticity (rr) (%) of the methacrylic resin (C) can be calculated as follows: 1 The H-NMR spectrum was measured by measuring the area (X) of the 0.6 to 0.95 ppm region and the area (Y) of the 0.6 to 1.35 ppm region when tetramethylsilane (TMS) was set to 0 ppm, and the result was calculated using the formula: (X / Y)×100.
[0081] The weight average molecular weight of the methacrylic resin (C) is determined by the ease of mixing (dispersion) with the styrene copolymer (D) and the ease of manufacturing these thermoplastic resins (B). That is, when the weight average molecular weight of the methacrylic resin (C) is too large, the difference in melt viscosity with the styrene copolymer (D) becomes too large, so the mixing (dispersion) of the two becomes poor, and the transparency of the thermoplastic resin (B) becomes poor, or it is impossible to continue to perform stable melt kneading. On the contrary, when the weight average molecular weight of the methacrylic resin (C) is too small, the strength of the thermoplastic resin (B) decreases, which may cause problems such as decreased impact resistance of the resin laminate. The weight average molecular weight of the methacrylic resin (C) is preferably in the range of 50,000 to 700,000, more preferably in the range of 60,000 to 500,000, and further preferably in the range of 70,000 to 200,000. The above weight average molecular weight is a weight average molecular weight converted to standard polystyrene measured by gel permeation chromatography (GPC).
[0082] The glass transition temperature of the methacrylic resin (C) is preferably 100°C or higher, more preferably 105°C or higher, and even more preferably 108°C or higher. When the glass transition temperature is 100°C or higher, the laminate provided by the present invention is less likely to deform or crack under a thermal environment. The glass transition temperature of the methacrylic resin (C) in this specification is a temperature measured at a heating rate of 10°C / min using a differential scanning calorimeter and calculated at the intersection of the tangent line of the baseline and the inflection point.
[0083] The melt flow rate of the above-mentioned methacrylic resin (C) is preferably in the range of 1 to 10 g / 10 minutes. The lower limit of the melt flow rate is more preferably 1.2 g / 10 minutes or more, and more preferably 1.5 g / 10 minutes. In addition, the upper limit of the melt flow rate is more preferably 7.0 g / 10 minutes or less, and more preferably 4.0 g / 10 minutes or less. When the melt flow rate is in the range of 1 to 10 g / 10 minutes, the stability of heated melt molding is good. Among them, the melt flow rate of the methacrylic resin (C) in this specification is a value measured using a melt indexer at a temperature of 230°C and a load of 3.8 kg.
[0084] <Styrene copolymer (D)>
[0085] The styrene copolymer (D) contained in the thermoplastic resin (B) of the present invention is characterized in that it contains vinyl aromatic monomer units (d1) and cyclic acid anhydride monomer units (d2), and the total ratio of the vinyl aromatic monomer units (d1) and the cyclic acid anhydride monomer units (d2) is 92 to 100% by mass relative to the total of all monomer units in the above-mentioned styrene copolymer (D).
[0086] The vinyl aromatic monomer unit (d1) of the styrene copolymer (D) is not particularly limited, and any known aromatic vinyl monomer can be used. From the perspective of ease of use, styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, tert-butylstyrene, etc. can be cited. Among them, styrene is particularly preferred from the perspective of compatibility. Two or more of these aromatic vinyl monomers can be mixed.
[0087] The cyclic acid anhydride monomer unit (d2) of the styrene copolymer (D) includes anhydrides of maleic acid, itaconic acid, citraconic acid, aconitic acid, etc. Maleic anhydride is preferred from the viewpoint of compatibility with acrylic resin. Two or more of these unsaturated dicarboxylic anhydride monomers may be mixed.
[0088] In the above-mentioned styrene copolymer (D) used in the present invention, the total ratio of the above-mentioned vinyl aromatic monomer unit (d1) and the above-mentioned cyclic acid anhydride monomer unit (d2) is 92 to 100% by mass, preferably 95 to 100% by mass, and more preferably 98 to 100% by mass relative to the total of all monomer units in the above-mentioned styrene copolymer (D).
[0089] That is, the styrene copolymer (D) may contain monomer units other than the vinyl aromatic monomer units (d1) and the cyclic anhydride monomer units (d2) in an amount of 8% by weight or less relative to the total of all monomer units. Examples of monomer units other than the vinyl aromatic monomer units (d1) and the cyclic anhydride monomer units (d2) include methacrylate monomer units, N-substituted maleimide monomers, and the like.
[0090] Examples of the methacrylic acid ester monomer unit in the styrene copolymer (D) include alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, pentyl methacrylate, hexyl methacrylate, heptyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, decyl methacrylate, and dodecyl methacrylate; cycloalkyl methacrylates such as 1-methylcyclopentyl methacrylate, cyclohexyl methacrylate, cycloheptyl methacrylate, cyclooctyl methacrylate, and tricyclo[5.2.1.02,6]dec-8-yl methacrylate; aryl methacrylates such as phenyl methacrylate; and aralkyl methacrylates such as benzyl methacrylate. Methyl methacrylate is preferred from the viewpoint of compatibility with the methacrylic acid resin. Two or more of these methacrylic acid ester monomers may be mixed.
[0091] As the N-substituted maleimide monomer in the styrene copolymer (D), N-phenylmaleimide, N-chlorophenylmaleimide, N-methylphenylmaleimide, N-naphthylmaleimide, N-hydroxyphenylmaleimide, N-methoxyphenylmaleimide, N-carboxyphenylmaleimide, N-nitrophenylmaleimide, N-tribromophenylmaleimide and other N-arylmaleimides can be listed, and N-phenylmaleimide is preferred from the viewpoint of compatibility with methacrylic resin. Two or more of these N-substituted maleimide monomers can be mixed.
[0092] The proportion of the vinyl aromatic monomer unit (d1) is 68 to 84% by mass, preferably 70 to 82% by mass, more preferably 74 to 80% by mass, and further preferably 76 to 79% by mass, relative to the total of all monomer units in the styrene copolymer (D). The proportion of the cyclic anhydride monomer unit (d2) is 16 to 32% by mass, preferably 18 to 30% by mass, more preferably 20 to 26% by mass, and further preferably 21 to 24% by mass, relative to the total of all monomer units in the styrene copolymer (D).
[0093] When the ratio of the vinyl aromatic monomer unit (d1) to the total monomer units in the styrene copolymer (D) is other than 68 to 84% by mass, the compatibility with the methacrylic resin (C) is poor. When the ratio of the cyclic acid anhydride monomer unit (d2) to the total monomer units in the styrene copolymer (D) is other than 16 to 32% by mass, the compatibility with the methacrylic resin (C) is poor.
[0094] The weight average molecular weight of the styrene copolymer (D) is not particularly limited, but is preferably 30,000 to 400,000, more preferably 40,000 to 300,000, and particularly preferably 50,000 to 200,000 from the viewpoint of compatibility with the methacrylic resin (C). The weight average molecular weight is a weight average molecular weight in terms of standard polystyrene measured by gel permeation chromatography (GPC).
[0095] The glass transition temperature of the above-mentioned styrene copolymer (D) is preferably in the range of 120 to 190°C, and more preferably in the range of 130 to 170°C. By having a glass transition temperature of 120°C or higher, the laminate provided by the present invention is less likely to deform or crack under a thermal environment. In addition, by being below 190°C, the processability is excellent by continuous heat shaping using a mirror roll or a shaping roll, or batch heat shaping using a mirror mold or a shaping mold. Among them, the glass transition temperature of the styrene copolymer (D) in this specification is the temperature measured using a differential scanning calorimeter at a heating rate of 10°C / min and calculated at the intersection of the baseline and the tangent line of the inflection point.
[0096] The melt flow rate of the above-mentioned styrene copolymer (D) is preferably in the range of 1 to 10 g / 10 minutes, more preferably in the range of 4 to 9 g / 10 minutes, and further preferably in the range of 6 to 8 g / 10 minutes. When the melt flow rate is in the range of 1 to 10 g / 10 minutes, the stability of heat-melt molding is good. Among them, the melt flow rate of the styrene copolymer (D) of the present invention in this specification is a value measured using a melt indexer at a temperature of 230°C and a load of 3.8 kg.
[0097] The method for producing the styrene copolymer (D) is not particularly limited, and a known solution polymerization method, bulk polymerization method, suspension polymerization method, or the like can be appropriately selected.
[0098] The above-mentioned styrene copolymer (D) is a binary copolymer or a multi-component copolymer containing a vinyl aromatic monomer unit (d1) and a cyclic acid anhydride monomer unit (d2), but by using a methacrylic resin (C) in combination, the hardness is higher than when only the styrene copolymer (D) is used, and a resin laminate with better thermoformability than when only the methacrylic resin (C) is used can be obtained.
[0099] In the present invention, regarding the mass ratio of the methacrylic resin (C) and the styrene copolymer (D), it is preferred that the methacrylic resin (C) is 5 to 70 parts by mass and the styrene copolymer (D) is 95 to 30 parts by mass, based on 100 parts by mass of the total content of the methacrylic resin (C) and the styrene copolymer (D). It is more preferred that the methacrylic resin (C) is 10 to 65 parts by mass and the styrene copolymer (D) is 90 to 35 parts by mass, further preferred that the methacrylic resin (C) is 15 to 60 parts by mass and the styrene copolymer (D) is 85 to 40 parts by mass, and particularly preferred that the methacrylic resin (C) is 20 to 55 parts by mass and the styrene copolymer (D) is 80 to 45 parts by mass. By setting the mass ratio within this range, an excellent thermoplastic resin (B) can be obtained that maintains transparency, has excellent heat resistance, has a high refractive index, and has a good appearance.
[0100] The glass transition temperature of the thermoplastic resin (B) is preferably in the range of 120 to 165°C, more preferably in the range of 120 to 155°C. When the glass transition temperature is above 120°C, the laminate provided by the present invention is less likely to deform or crack under a thermal environment. In addition, by being below 165°C, the processability is excellent by continuous heat forming using a mirror roll or a shaping roll, or batch heat forming using a mirror mold or a shaping mold. The glass transition temperature of the thermoplastic resin (B) in this specification is the temperature measured at a heating rate of 10°C / min using a differential scanning calorimeter and calculated at the intersection of the tangent line of the baseline and the inflection point.
[0101] The melt flow rate of the thermoplastic resin (B) is preferably in the range of 1 to 10 g / 10 minutes, more preferably in the range of 1.5 to 7 g / 10 minutes, and further preferably in the range of 2 to 5 g / 10 minutes. When the melt flow rate is in the range of 1 to 10 g / 10 minutes, the stability of the heated melt molding is good. The melt flow rate of the thermoplastic resin (B) in this specification is a value measured using a melt indexer at a temperature of 230°C and a load of 3.8 kg.
[0102] In the present invention, the method for producing the thermoplastic resin (B) is not particularly limited, and the following known methods can be used: for example, the required components are pre-mixed using a mixer such as a tumbler or Henschel mixer, a super mixer, and then melt-kneaded using a machine such as a Banbury mixer, a roll, a Brabender mixer, a single-screw extruder, a twin-screw extruder, a pressure kneader, etc.
[0103] One of the characteristics of the thermoplastic resin (B) used in the present invention is that the glass transition temperature is relatively high, preferably in the range of 115 to 170°C, more preferably in the range of 120 to 160°C, and particularly preferably in the range of 125 to 150°C. Since the glass transition temperature of the thermoplastic resin (B) used in the present invention is relatively high and the difference between the glass transition temperature of the thermoplastic resin (B) and the above-mentioned polycarbonate resin (A) is small, it has the advantage that even when the glass transition temperature of the polycarbonate resin (A) is approached during hot press molding or hot bending, the layer containing the thermoplastic resin (B) has few problems of poor appearance. The difference between the glass transition temperature of the polycarbonate resin (A) and the glass transition temperature of the thermoplastic resin (B) is preferably in the range of 0 to 15°C, and more preferably in the range of 0 to 10°C.
[0104] <Hard coating>
[0105] There may be a further layer between the hard coating layer of the present invention and the layer containing the thermoplastic resin (B), but it is preferred that the hard coating layer is laminated on the front or both sides of the layer containing the thermoplastic resin (B). The hard coating layer is preferably an acrylic hard coating layer. In this specification, "acrylic hard coating layer" means a coating film having a cross-linked structure formed by polymerizing a monomer, oligomer or prepolymer containing a (meth)acryloyl group as a polymerizing group. As a composition of the acrylic hard coating layer, it is preferred to contain 2 to 98% by mass of a (meth)acrylic monomer, 2 to 98% by mass of a (meth)acrylic oligomer and 0 to 15% by mass of a surface modifier, and more preferably to contain 0.001 to 7 parts by mass of a photopolymerization initiator relative to 100 parts by mass of the total of the (meth)acrylic monomer, the (meth)acrylic oligomer and the surface modifier.
[0106] The hard coat layer more preferably contains 5 to 50% by mass of a (meth)acrylic monomer, 50 to 95% by mass of a (meth)acrylic oligomer, and 1 to 10% by mass of a surface modifier, and particularly preferably contains 20 to 40% by mass of a (meth)acrylic monomer, 60 to 80% by mass of a (meth)acrylic oligomer, and 2 to 5% by mass of a surface modifier.
[0107] The amount of the photopolymerization initiator is more preferably 0.01 to 5 parts by mass, particularly preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the total of the (meth)acrylic monomer, the (meth)acrylic oligomer, and the surface modifier.
[0108] As the (meth)acrylic monomer, any monomer having a (meth)acryloyl group as a functional group in the molecule can be used, and any monomer may be a monofunctional monomer, a difunctional monomer, or a trifunctional or higher-functional monomer.
[0109] As monofunctional monomers, (meth)acrylic acid and (meth)acrylates can be exemplified. Specific examples of bifunctional and / or trifunctional (meth)acrylic monomers include diethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, bisphenol A diglycidyl ether di(meth)acrylate, tetraethylene glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol diacrylate, neopentyl glycol di(meth)acrylate, 1,4-butanediol diacrylate, 1,3-butanediol di(meth)acrylate, dicyclopentyl di(meth)acrylate, acrylate, polyethylene glycol diacrylate, 1,4-butanediol oligoacrylate, neopentyl glycol oligoacrylate, 1,6-hexanediol oligoacrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane ethoxy tri(meth)acrylate, trimethylolpropane propoxy tri(meth)acrylate, pentaerythritol tri(meth)acrylate, glyceryl propoxy tri(meth)acrylate, trimethylolpropane trimethacrylate, trimethylolpropane ethylene oxide adduct triacrylate, glycerol propylene oxide adduct triacrylate, pentaerythritol tetraacrylate, etc.
[0110] The hard coat layer may contain one or two or more (meth)acrylic monomers.
[0111] Examples of (meth)acrylic oligomers include polyfunctional polyurethane (meth)acrylate oligomers having two or more functions (hereinafter also referred to as polyfunctional polyurethane (meth)acrylate oligomers), polyfunctional polyester (meth)acrylate oligomers having two or more functions (hereinafter also referred to as polyfunctional polyester (meth)acrylate oligomers), polyfunctional epoxy (meth)acrylate oligomers having two or more functions (hereinafter also referred to as polyfunctional epoxy (meth)acrylate oligomers), etc. The hard coat layer may contain one or more (meth)acrylic oligomers.
[0112] Examples of the multifunctional urethane (meth)acrylate oligomer include: a urethanization reaction product of a (meth)acrylate monomer having at least one (meth)acryloyloxy group and hydroxyl group in one molecule and a polyisocyanate; and a urethanization reaction product of an isocyanate compound obtained by reacting a polyol with a polyisocyanate and a (meth)acrylate monomer having at least one (meth)acryloyloxy group and hydroxyl group in one molecule.
[0113] Examples of the (meth)acrylate monomer having at least one (meth)acryloyloxy group and a hydroxyl group in one molecule used in the urethanization reaction include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, glycerol di(meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate.
[0114] Examples of the polyisocyanate used in the polyurethane reaction include hexamethylene diisocyanate, lysine diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, toluene diisocyanate, xylylene diisocyanate, diisocyanates obtained by hydrogenating aromatic isocyanates among these diisocyanates (for example, diisocyanates such as hydrogenated toluene diisocyanate and hydrogenated xylylene diisocyanate), di- or tri-polyisocyanates such as triphenylmethane triisocyanate and dimethylene triphenyl triisocyanate, or polyisocyanates obtained by polymerizing diisocyanates.
[0115] As polyols used in the polyurethane reaction, in addition to common aromatic, aliphatic and alicyclic polyols, polyester polyols, polyether polyols, etc. can also be used. Usually, as aliphatic and alicyclic polyols, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, ethylene glycol, propylene glycol, trimethylolethane, trimethylolpropane, dimethylolheptane, dimethylolpropionic acid, dimethylolbutyric acid, glycerin, hydrogenated bisphenol A, etc. can be listed.
[0116] As polyester polyol, the material obtained by the dehydration condensation reaction of the above-mentioned polyols and polycarboxylic acids can be cited. As the specific compound of polycarboxylic acids, succinic acid, adipic acid, maleic acid, trimellitic acid, hexahydrophthalic acid, phthalic acid, isophthalic acid, terephthalic acid, etc. can be cited. These polycarboxylic acids can be acid anhydrides. In addition, as polyether polyol, in addition to polyalkylene glycol, polyoxyalkylene modified polyols obtained by the reaction of the above-mentioned polyols or phenols with alkylene oxides can also be cited.
[0117] In addition, the multifunctional polyester (meth) acrylate oligomer can be obtained by a dehydration condensation reaction using (meth) acrylic acid, a polycarboxylic acid and a polyol. As the polycarboxylic acid used in the dehydration condensation reaction, succinic acid, adipic acid, maleic acid, itaconic acid, trimellitic acid, pyromellitic acid, hexahydrophthalic acid, phthalic acid, isophthalic acid, terephthalic acid, etc. can be listed. These polycarboxylic acids can be acid anhydrides. In addition, as the polyol used in the dehydration condensation reaction, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, triethylene glycol, propylene glycol, neopentyl glycol, dimethylol heptane, dimethylol propionic acid, dimethylol butyric acid, trimethylol propane, ditrimethylol propane, pentaerythritol, dipentaerythritol, etc. can be listed.
[0118] The polyfunctional epoxy (meth)acrylate oligomer can be obtained by the addition reaction of polyglycidyl ether and (meth)acrylic acid. Examples of the polyglycidyl ether include ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, and bisphenol A diglycidyl ether.
[0119] The surface modifier used in the present invention is a substance that changes the surface properties of the hard coating layer, such as a leveling agent, an antistatic agent, a surfactant, a water-repellent and an oil-repellent, an inorganic particle, and an organic particle.
[0120] Examples of the leveling agent include polyether-modified polyalkylsiloxane, polyether-modified silicone, polyester-modified hydroxyl-containing polyalkylsiloxane, polyether-modified polydimethylsiloxane having an alkyl group, modified polyether, and silicone-modified acrylic.
[0121] Examples of the antistatic agent include glycerin fatty acid ester monoglyceride, glycerin fatty acid ester organic acid monoglyceride, polyglycerin fatty acid ester, sorbitan fatty acid ester, cationic surfactants, and anionic surfactants.
[0122] Examples of the inorganic particles include silica particles, alumina particles, zirconia particles, silicon particles, silver particles, and glass particles.
[0123] Examples of the organic particles include acrylic particles and silicone particles.
[0124] Examples of the surfactant and water- and oil-repellent agent include fluorine-containing surfactants and water- and oil-repellent agents such as oligomers having a fluorine-containing group and a lipophilic group and oligomers having a fluorine-containing group, a hydrophilic group, a lipophilic group, and a UV reactive group.
[0125] The hard coat layer may contain a photopolymerization initiator. In the present specification, the photopolymerization initiator means a photo radical generator.
[0126] Examples of the monofunctional photopolymerization initiator that can be used in the present invention include: 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone [Darocur-2959, produced by Merck]; α-hydroxy-α,α'-dimethylacetophenone [Darocur-1173, produced by Merck]; acetophenone-based initiators such as methoxyacetophenone, 2,2'-dimethoxy-2-phenylacetophenone [Irgacure-651], and 1-hydroxy-cyclohexyl phenyl ketone; benzoin ether-based initiators such as benzoin ethyl ether and benzoin isopropyl ether; and halogenated ketones, acylphosphine oxides, acylphosphonates, and the like.
[0127] The method for forming the hard coat layer is not particularly limited, and the hard coat layer can be formed, for example, by applying a hard coat liquid on a layer located below the hard coat layer and then photopolymerizing the hard coat liquid.
[0128] The method for applying the hard coating liquid (polymerizable composition) is not particularly limited, and a known method can be used, for example, spin coating, dipping, spraying, oblique plate coating, rod coating, roller coating, gravure coating, meniscus coating, flexographic printing, screen printing, pat coating, brush coating, etc.
[0129] As the lamp used for irradiating light during photopolymerization, a lamp having a light emission distribution at a wavelength of 420 nm or less is used, and examples thereof include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, chemical lamps, black light lamps, microwave-excited mercury lamps, metal halide lamps, etc. Among them, high-pressure mercury lamps or metal halide lamps are preferred because they can efficiently emit light in the active wavelength range of the initiator, and do not emit a large amount of short-wavelength light that reduces the viscoelastic properties of the obtained polymer due to crosslinking, or long-wavelength light that heats and evaporates the reaction composition.
[0130] The irradiation intensity of the lamp is a factor affecting the polymerization degree of the obtained polymer, and can be appropriately controlled according to the performance of each target product. When a conventional cleavage initiator having an acetophenone group is used, the irradiation intensity is preferably 0.1 to 300 mW / cm 2 It is particularly preferred to use a metal halide lamp and set the illumination to 10 to 40 mW / cm 2 .
[0131] The photopolymerization reaction is inhibited by oxygen in the air or dissolved oxygen in the reactive composition. Therefore, light irradiation is preferably carried out by a method that can eliminate the reaction inhibition caused by oxygen. As one of such methods, there is a method of covering the reactive composition with a film made of polyethylene terephthalate or Teflon to block contact with oxygen, and irradiating light to the reactive composition through the film. It is also possible to irradiate light to the composition through a light-transmitting window in an inert atmosphere in which oxygen is replaced with an inert gas such as nitrogen or carbon dioxide.
[0132] In the case of light irradiation under an inert atmosphere, a certain amount of inert gas is always introduced in order to keep the atmospheric oxygen concentration at a low level. By introducing the inert gas, an airflow is formed on the surface of the reactive composition, and monomer evaporation occurs. In order to suppress the level of monomer evaporation, the airflow velocity of the inert gas is preferably less than 1 m / sec, more preferably less than 0.1 m / sec, as measured by the relative velocity relative to the laminate coated with the hard coating liquid moving under the inert gas atmosphere. By setting the airflow velocity within the above range, the monomer evaporation caused by the airflow can be substantially suppressed.
[0133] In order to improve the adhesion of the hard coat layer, the coated surface is sometimes pre-treated. Examples of treatments include sandblasting, solvent treatment, corona discharge treatment, chromic acid treatment, flame treatment, hot air treatment, ozone treatment, ultraviolet treatment, and primer treatment using a resin composition.
[0134] The hard coating was irradiated with UV light (254 nm) at an output of 20 mW / cm 2 When ultraviolet irradiation is performed using a metal halide lamp, the pencil hardness is preferably 2H or more.
[0135] The film thickness of the hard coating is preferably 1 μm to 40 μm, and more preferably 2 μm to 10 μm. With a film thickness of 1 μm or more, sufficient hardness can be obtained. In addition, with a film thickness of 40 μm or less, cracks can be suppressed during bending. The film thickness of the hard coating can be measured by observing the cross section using a microscope or the like and measuring from the coating interface to the surface.
[0136] In order to improve the adhesion of the hard coating layer, the coating surface is sometimes pre-treated before hard coating. Examples of the treatment include sandblasting, solvent treatment, corona discharge treatment, chromic acid treatment, flame treatment, hot air treatment, ozone treatment, ultraviolet treatment, and primer treatment using a resin composition.
[0137] <Haze>
[0138] The resin laminate before having a hard coat layer of the present invention preferably has a haze of ≤1.0%, more preferably ≤0.8%, and particularly preferably ≤0.7%. When the haze exceeds 1.0%, the resin laminate may appear white when viewed visually.
[0139] <Resin laminate>
[0140] In the present invention, the thickness of the layer containing the thermoplastic resin (B) affects the surface hardness and impact resistance of the resin laminate. That is, when the thickness of the layer containing the thermoplastic resin (B) is too thin, the surface hardness decreases and is not preferred. When the thickness of the layer containing the thermoplastic resin (B) is too large, the impact resistance deteriorates and is not preferred. The thickness of the layer containing the thermoplastic resin (B) is preferably 10 to 250 μm, more preferably 20 to 200 μm, and further preferably 30 to 150 μm.
[0141] In the present invention, if the total thickness of the layer containing the polycarbonate resin (A), the layer containing the thermoplastic resin (B) and the hard coating layer is too thin or too thick, molding will be difficult. The overall thickness of the resin laminate is preferably 0.4 to 4.0 mm, more preferably 0.5 to 3.5 mm, and even more preferably 0.5 to 3.0 mm.
[0142] In the present invention, the refractive index difference between the polycarbonate resin (A) and the thermoplastic resin (B) is preferably in the range of 0 to 0.07, more preferably in the range of 0 to 0.06, and even more preferably in the range of 0 to 0.05. When the difference in glass transition temperature between the polycarbonate resin (A) and the refractive index of the thermoplastic resin (B) is greater than 0.07, the reflected light intensity at the interface of the layer containing the polycarbonate resin (A) / the layer containing the thermoplastic resin (B) is large, and interference fringes and other undesirable conditions may occur.
[0143] The resin laminate of the present invention may be subjected to any one or more of anti-fingerprint treatment, anti-reflection treatment, anti-fouling treatment, anti-static treatment, weather resistance treatment and anti-glare treatment on one side or both sides. The methods of anti-reflection treatment, anti-fouling treatment, anti-static treatment, weather resistance treatment and anti-glare treatment are not particularly limited, and known methods may be used. For example, a method of applying a reflection-reducing coating, a method of evaporating a dielectric film, a method of applying an anti-static coating, etc. may be cited.
[0144] <Optional additives>
[0145] In the present invention, the polycarbonate resin (A) forming the substrate layer and / or the thermoplastic resin (B) forming the surface layer may contain components other than the above-mentioned main components.
[0146] For example, a UV absorber can be mixed in the polycarbonate resin (A) and / or the thermoplastic resin (B) for use. In addition, in the present invention, the hard coat layer may also contain a UV absorber. When the content of the UV absorber is too much, depending on the molding method, the excess UV absorber is scattered due to the application of high temperature, polluting the molding environment, and thus sometimes causing adverse conditions. Therefore, the content ratio of the UV absorber is preferably 0 to 5% by mass, more preferably 0 to 3% by mass, and further preferably 0 to 1% by mass. Examples of the ultraviolet absorber include benzophenone-based ultraviolet absorbers such as 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-n-octyloxybenzophenone, 2-hydroxy-4-dodecyloxybenzophenone, 2-hydroxy-4-octadecyloxybenzophenone, 2,2′-dihydroxy-4-methoxybenzophenone, 2,2′-dihydroxy-4,4′-dimethoxybenzophenone, and 2,2′,4,4′-tetrahydroxybenzophenone; 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-(2-hydroxy-3,5-diphenyl)benzotriazole, and the like. Benzotriazole-based UV absorbers such as benzoyl)benzotriazole, 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)benzotriazole, (2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol; benzoate-based UV absorbers such as phenyl salicylate and 2,4-di-tert-butylphenyl-3,5-di-tert-butyl-4-hydroxybenzoate; hindered amine-based UV absorbers such as bis(2,2,6,6-tetramethylpiperidin-4-yl)sebacate; 2,4-diphenyl-6-(2-hydroxy-4-methoxyphenyl)-1,3,5- Triazine, 2,4-diphenyl-6-(2-hydroxy-4-ethoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-(2-hydroxy-4-propoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-(2-hydroxy-4-butoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-butoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-hexyloxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-octyloxyphenyl)-1,3,5 triazine-based ultraviolet absorbers such as 2-[2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl]ethyl methacrylate, 2-[2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl]ethyl acrylate, 3-[2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl]ethyl acrylate, 2-[2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl]ethyl acrylate, 2-[2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl]ethyl acrylate, 2-[2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl]ethyl acrylate, 2-[2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl]ethyl acrylate, 2-[2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl]ethyl acrylate, 2-[2-(6-hydroxybenzo[1,3-[2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl]propyl-methacrylate, 3-[2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl]propyl-acrylate, 4-[2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl]butyl-methacrylate, 4-[2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl]butyl-acrylate, 2-[2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl]butyl-acrylate Benzotriazol-5-yloxy]ethyl methacrylate, 2-[2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yloxy]ethyl acrylate, 2-[3-{2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl}propionyloxy]ethyl methacrylate, 2-[3-{2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl}propionyloxy]ethyl acrylate, 4-[3-{2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl}propionyloxy]ethyl acrylate 2-[3-{2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl}propionyloxy]butyl-methacrylate, 2-[3-{2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl}propionyloxy]ethyl-methacrylate, 2-[3-{2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl}propionyloxy]ethyl-acrylate, 2-(methacryloyloxy)ethyl 2-( Sesamol-type benzotriazole ultraviolet absorbers such as 2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazole-5-carboxylate, 2-(acryloyloxy)ethyl 2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazole-5-carboxylate, 4-(methacryloyloxy)butyl 2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazole-5-carboxylate, and 4-(acryloyloxy)butyl 2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazole-5-carboxylate. The mixing method is not particularly limited, and a method of mixing the entire amount, a method of dry blending a masterbatch, and a method of dry blending the entire amount can be used. ,
[0147] In the present invention, in addition to the above-mentioned ultraviolet absorber, various additives can be mixed in the polycarbonate resin (A) forming the substrate layer and / or the thermoplastic resin (B) forming the surface layer. As such additives, for example, antioxidants and anti-coloring agents, antistatic agents, mold release agents, lubricants, dyes, pigments, plasticizers, flame retardants, resin modifiers, compatibilizers, organic fillers, inorganic fillers and other reinforcing materials can be listed. The mixing method is not particularly limited, and a method of mixing the whole amount, a method of dry blending the masterbatch, a method of dry blending the whole amount, etc. can be used.
[0148] The materials of the layer containing the polycarbonate resin (A), the layer containing the thermoplastic resin (B), and the hard coating layer of the present invention, such as the polycarbonate resin (A) and the thermoplastic resin (B), are preferably filtered and purified by a filter treatment. By refining or laminating through a filter, a resin laminate with less appearance defects such as foreign matter and defects can be obtained. The filtration method is not particularly limited, and melt filtration, solution filtration, or a combination thereof can be used.
[0149] The filter used is not particularly limited, and a known filter can be used, and it can be appropriately selected according to the use temperature, viscosity, and filtering accuracy of each material. As the filter medium, there is no particular limitation, and non-woven fabrics or rovings of polypropylene, cotton, polyester, viscose and glass fibers, cellulose impregnated with phenolic resin, sintered metal fiber non-woven fabrics, sintered metal powders, porous plates, or combinations thereof can all be used. In particular, when considering heat resistance, durability, and pressure resistance, the type formed by sintering metal fiber non-woven fabrics is preferred.
[0150] Regarding the filtration accuracy, for polycarbonate resin (A) and thermoplastic resin (B), it is 50 μm or less, preferably 30 μm or less, and more preferably 10 μm or less. In addition, from the perspective of coating on the outermost layer of the resin laminate, the filtration accuracy of the hard coating agent is 20 μm or less, preferably 10 μm or less, and more preferably 2 μm or less.
[0151] For filtering the polycarbonate resin (A) and the thermoplastic resin (B), it is preferred to use a polymer filter used for melt filtration of thermoplastic resins, for example. Polymer filters are classified into leaf disk filters, candle filters, laminated disk filters, cylindrical filters, etc. according to their structure, and leaf disk filters having a large effective filtration area are particularly preferred.
[0152] <Hot Bending>
[0153] The heat bending process of the resin laminate of the present invention is not particularly limited. For example, there are: "hot press forming" in which a punch (male mold) and a die (female mold) are installed on a press machine, and the two molds are used to clamp the heat-softened laminated sheet; "vacuum forming" in which the heat-softened laminated sheet and the punch (male mold) are formed into a vacuum state, so that the laminated sheet and the mold are tightly fitted and processed into the desired shape; "air pressure forming" in which a pressure greater than atmospheric pressure is applied to the heat-softened laminated sheet and the punch (male mold) mold, so that the laminated sheet and the mold are tightly fitted and processed into the desired shape. The resin laminate of the present invention can obtain a thermoformed body that does not rebound even when subjected to heat bending processing at low temperatures (for example, 120 to 130°C).
[0154] <Thermoformed body>
[0155] When a laminated sheet using existing polycarbonate resin (e.g., Iupilon S-2000, Iupilon S-1000, and Iupilon E-2000 purchased from Mitsubishi Engineering-Plastics Corporation) is subjected to hot press molding, the sheet needs to be heated at 135 to 145°C until the polycarbonate resin is fully stretched. As a result, excessive heat is applied to the thermoplastic resin, and sometimes peeling occurs at the interface between the thermoplastic resin layer and the polycarbonate resin layer, causing surface whitening or cracking. On the other hand, in order to suppress poor hot forming, if hot press molding is performed at a low temperature of 120 to 130°C, the shape of the mold may not be reproduced, and "rebound" may occur, in which the shape of the mold is restored to a flat state.
[0156] In contrast, the resin laminate according to the embodiment of the present invention uses a specific polycarbonate resin (A), so springback does not occur even when hot press molding is performed at a low temperature of 120°C to 130°C, and a thermoformed body with excellent design properties at low temperature can be obtained.
[0157] In addition, when a resin laminate having a layer containing a thermoplastic resin on a layer containing a polycarbonate resin and a hard coating layer on the surface of the layer containing the thermoplastic resin is heat-pressed at a low temperature of 120°C to 130°C, cracks sometimes occur in the bent portion of the resin laminate.
[0158] In contrast, since the resin laminate of the embodiment of the present invention uses a specific thermoplastic resin (B), even if the resin laminate having a hard coating layer on the surface of the thermoplastic resin layer is hot-pressed at a low temperature of 120°C to 130°C, cracks will not occur in the bent portion of the resin laminate, and a thermoformed body with excellent design properties at low temperatures can be obtained.
[0159] <Application>
[0160] The molded article (eg, thermoformed article) of the embodiment is a molded article including the resin laminate of the present invention including the above-mentioned various preferred forms and structures. The shape, style, color, dimensions, etc. of the molded article are not limited and can be arbitrarily set according to its use.
[0161] The resin laminate and thermoformed body of the embodiment have excellent thermoformability at low temperatures (e.g., 120 to 130° C.), and can suppress the generation of interference fringes. Therefore, it is suitable for use as a transparent substrate material or a transparent protective material, etc. Specifically, it can be used as a transparent substrate material and a transparent protective material (e.g., a front panel) for portable display devices such as mobile phone terminals, portable electronic game consoles, portable information terminals, and mobile PCs, and for display devices such as notebook PCs, desktop PC liquid crystal monitors, car navigation liquid crystal monitors, and liquid crystal televisions. Among them, it is suitable for use as a front protective plate for a touch panel that requires high design, and a front panel for car navigation, OA equipment, or portable electronic devices.
[0162] Example
[0163] Hereinafter, the present embodiment will be described in more detail using examples, but the present embodiment is not limited to these examples.
[0164] <Composition ratio of monomer units in styrene copolymer>
[0165] Using JNM-AL400 manufactured by JEOL Ltd., according to 1 H-NMR and 13 The results were calculated based on the measured values of C-NMR (400 MHz, solvent: CDCl3).
[0166] <Glass transition temperature>
[0167] A differential scanning calorimeter DSC6200 manufactured by Seiko Instruments Co., Ltd. was used. Under the condition of nitrogen gas flowing at 30 ml / min., the temperature was raised from 30°C to 200°C at 10°C / min., then lowered from 200°C to 30°C at 50°C / min., and then raised from 30°C to 200°C at 10°C / min. again. The intersection of the baseline at the second temperature increase and the tangent line of the inflection point was taken as the glass transition temperature.
[0168] <Appearance of pellets>
[0169] When making pellets, visually evaluate the appearance of the pellets. The appearance of the pellets is judged to be qualified according to the following criteria, and 0 is regarded as qualified.
[0170] ○: transparent;
[0171] ×: Translucent or turbid.
[0172] <Refractive Index>
[0173] The test piece was made by injection molding machine and cut into 40 mm in length, 10 mm in width and 3 mm in thickness. The refractive index of the sample was measured by multi-wavelength Abbe refractometer DR-M2 manufactured by ATAGO Co., Ltd. The measurement temperature was 20°C, the measurement wavelength was 589 nm, and monobromonaphthalene was used as the intermediate liquid.
[0174] <Total light transmittance>
[0175] The total light transmittance of the resin laminate was measured using a reflectance / transmittance meter Model HR-100 (manufactured by Murakami Color Research Laboratory Co., Ltd.) in accordance with JIS K7361-1.
[0176] <Haze>
[0177] The haze of the resin laminate was measured in accordance with JIS K7136 using a reflectance / transmittance meter HR-100 (manufactured by Murakami Color Research Laboratory Co., Ltd.).
[0178] <Pencil hardness>
[0179] In accordance with JIS K 5600-5-4, a pencil is pressed against the surface of the layer containing the thermoplastic resin (B) near the center of the resin laminate or the surface of the hard coating layer on the layer containing the thermoplastic resin (B) at an angle of 45 degrees and a load of 750 g, and the hardness is gradually increased. The hardest pencil hardness that does not cause scratches is evaluated as the pencil hardness.
[0180] <Interference fringes>
[0181] A black tape (black vinyl tape model 117BLA manufactured by 3M Japan) was attached to one side of the layer containing the polycarbonate resin (A) or the layer containing the thermoplastic resin (B) of the resin laminate, and the interference fringes were evaluated by irradiating the surface of the layer containing the thermoplastic resin (B) with a three-wavelength fluorescent lamp (Technica Inverter Light 60AL-60231 manufactured by Technica Co., Ltd.). The interference fringes were judged to be acceptable according to the following criteria, and 0 was regarded as acceptable.
[0182] ○: No interference fringes are visible, or the interference fringes appear very weak;
[0183] ×: Interference fringes appear strong.
[0184] <Hot press molding processability>
[0185] A mold is prepared in which a 1 mmt resin laminate is bent into a convex mold (male mold) and a concave mold (female mold) of 50 mmR. The resin laminate is preheated at 90°C for 1 minute before molding, and is placed in the mold in such a way that the thermoplastic resin (B) surface is convex before hard coating / the hard coating surface is convex after hard coating, and is pressed at a mold temperature of 120°C for 3 minutes, and cooled naturally to prepare a hot press molded body.
[0186] <Cracks in the bent portion>
[0187] The cracks in the bent portion of the hot press formed body were visually evaluated. The cracks in the bent portion were judged to be acceptable according to the following criteria, and 0 was regarded as acceptable.
[0188] ○: No cracks are observed in the bent portion of the hot press-formed body;
[0189] ×: Cracks were observed in the bent portion of the hot press-formed body.
[0190] <Rebound>
[0191] The hot press molded body was made to follow a cylinder of 50 mmR, and the springback was judged to be qualified according to the following criteria, and 0 was regarded as qualified.
[0192] ○: Along the cylinder. (No rebound);
[0193] ×: Not along the cylinder. (There is rebound).
[0194] In the examples, the following materials were used as polycarbonate resin (A-1), thermoplastic resin (B-1) to (B-4), methacrylic resin (C-1) to (C-2), styrene copolymer (D-1), and hard coating agent (J-1), but the materials are not limited thereto. On the other hand, in the comparative examples, the following polycarbonate resin (G-1), thermoplastic resin (F-1) to (F-9), styrene copolymer (E-1) to (E-2), thermoplastic resin before hard coating (I-1) to (I-42), and thermoplastic resin after hard coating (L-1) to (L-42) were used, respectively.
[0195] <Methacrylic resin (C-1) to (C-2), styrene copolymer (D-1), styrene copolymer (E-1) to (E-2), and polycarbonate resin (G-1)>
[0196] Methacrylic resin (C-1): ALTUGLAS (registered trademark) V020 manufactured by Arkema (weight average molecular weight: 127,000, glass transition temperature: 134° C., melt flow rate at 230° C. and 3.8 kg load: 1.8 g / 10 min., refractive index 1.49, mm / mr / rr=7.4 mol % / 37.4 mol % / 55.2 mol %).
[0197] Methacrylic resin (C-2): ALTUGLAS (registered trademark) V040 manufactured by Arkema (weight average molecular weight: 84,100, glass transition temperature: 109° C., melt flow rate at 230° C. and 3.8 kg load: 3.5 g / 10 min., refractive index 1.49).
[0198] Styrene copolymer (D-1): XIBOND160 manufactured by Polyscope ((d1) / (d2)=styrene / maleic anhydride=78 mass % / 22 mass %, weight average molecular weight: 69,500, glass transition temperature: 143°C, melt flow rate at 230°C and 3.8 kg load: 7.6 g / 10 min, refractive index: 1.58).
[0199] Styrene copolymer (E-1): XIBOND140 manufactured by Polyscope ((d1) / (d2)=styrene / maleic anhydride=85% by mass / 15% by mass, weight average molecular weight: 134,000, glass transition temperature: 129°C, melt flow rate at 230°C and 3.8 kg load: 6.9 g / 10 min, refractive index: 1.59).
[0200] Styrene copolymer (E-2): XIBOND180 manufactured by Polyscope ((d1) / (d2)=styrene / maleic anhydride=67 mass % / 33 mass %, weight average molecular weight: 50,100, glass transition temperature: 157°C, melt flow rate at 230°C and 3.8 kg load: 1.0 g / 10 min, refractive index: 1.59).
[0201] Polycarbonate resin (G-1): Iupilon S-1000 manufactured by Mitsubishi Engineering-Plastics Corporation (weight average molecular weight: 33,000, glass transition temperature: 147° C., melt flow rate at 300° C. and 1.2 kg load: 7.5 g / 10 min., refractive index: 1.59).
[0202] <Synthesis of polycarbonate resin (A-1)>
[0203] Synthesis Example 1〔Synthesis of polycarbonate resin terminal terminator〕
[0204] According to Handbook of Organic Chemistry, P143 to 150, 4-hydroxybenzoic acid produced by Tokyo Chemical Industry Co., Ltd. and 1-hexadecanol produced by Tokyo Chemical Industry Co., Ltd. were used to carry out esterification by a dehydration reaction to obtain cetyl p-hydroxybenzoate (CEPB).
[0205] Synthesis Example 2〔Production of polycarbonate resin (A-1) pellets〕
[0206] 7.1 kg (31.14 mol) of bisphenol A (hereinafter referred to as BPA) manufactured by Nippon Steel Sumitomo Chemical Co., Ltd. and 30 g of sodium dithionite were added to 57.2 kg of 9 w / w% sodium hydroxide aqueous solution and dissolved. 40 kg of dichloromethane was added thereto, and 4.33 kg of phosgene was blown in over 30 minutes while stirring the solution at a temperature of 15°C to 25°C. After the blowing of phosgene was completed, 6 kg of 9 w / w% sodium hydroxide aqueous solution, 11 kg of dichloromethane, and a solution obtained by dissolving 443 g (1.22 mol) of hexadecyl parahydroxybenzoate (CEPB) as a terminal terminator in 10 kg of dichloromethane were added, and the mixture was emulsified by vigorous stirring. Then, 10 ml of triethylamine was added to the solution as a polymerization catalyst, and polymerization was carried out for about 40 minutes.
[0207] The polymer solution was separated into an aqueous phase and an organic phase, and the organic phase was neutralized with phosphoric acid and repeatedly washed with pure water until the pH of the washing liquid reached neutrality. The organic solvent was distilled off from the purified polycarbonate resin solution to obtain a polycarbonate resin powder.
[0208] The obtained polycarbonate resin powder was melt-kneaded at a cylinder temperature of 260° C. using a twin-screw extruder having a screw diameter of 35 mm, extruded into a strand shape, and formed into pellets using a pelletizer.
[0209] The polycarbonate resin (A-1) had a weight average molecular weight of 29,000, a glass transition temperature of 127° C., a melt flow rate at a temperature of 300° C. and a load of 1.2 kg of 12.1 g / 10 minutes, and a refractive index of 1.59.
[0210] Production Example 1A [Production of Thermoplastic Resin (B-1) Pellets]
[0211] 500 ppm of phosphorus additive PEP-36 (manufactured by ADEKA Co., Ltd.) and 0.2% by mass of stearic acid monoglyceride (product name: H-100, manufactured by RIKEN VITAMIN CO., LTD.) were added to 100 parts by mass of 50 parts by mass of methacrylic resin (C-1) and 50 parts by mass of styrene copolymer (D-1), mixed for 20 minutes by a mixer, and then melt-kneaded at a barrel temperature of 240° C. using a twin-screw extruder (TEM-26SS, manufactured by Toshiba Machine Co., Ltd., L / D≈40) with a polymer filter having a mesh of 10 μm, extruded into strands, and pelletized by a pelletizer. Pellets of the thermoplastic resin (B-1) can be stably produced.
[0212] The pellets of the thermoplastic resin (B-1) had an appearance of 0 (transparent), a glass transition temperature of 121° C., a melt flow rate at a temperature of 230° C. and a load of 3.8 kg: 2.5 g / 10 min, and a refractive index of 1.54.
[0213] Production Example 2A [Production of Thermoplastic Resin (B-2) Pellets]
[0214] 500 ppm of phosphorus additive PEP-36 and 0.2% by mass of stearic acid monoglyceride were added to 100 parts by mass of a total of 25 parts by mass of methacrylic resin (C-1) and 75 parts by mass of styrene copolymer (D-1), and mixed in the same manner as in Production Example 1A to prepare pellets. Pellets of thermoplastic resin (B-2) can be stably produced.
[0215] The pellets of the thermoplastic resin (B-2) had an appearance of 0 (transparent), a glass transition temperature of 132° C., a melt flow rate at a temperature of 230° C. and a load of 3.8 kg: 3.5 g / 10 min, and a refractive index of 1.56.
[0216] Production Example 3A [Production of Thermoplastic Resin (B-3) Pellets]
[0217] 500 ppm of phosphorus additive PEP-36 and 0.2% by mass of stearic acid monoglyceride were added to 100 parts by mass of a total of 50 parts by mass of methacrylic resin (C-2) and 50 parts by mass of styrene copolymer (D-1), and mixed in the same manner as in Production Example 1A to prepare pellets. Pellets of thermoplastic resin (B-3) can be stably produced.
[0218] The pellets of the thermoplastic resin (B-3) had an appearance of 0 (transparent), a glass transition temperature of 125° C., a melt flow rate at a temperature of 230° C. and a load of 3.8 kg: 4.0 g / 10 minutes, and a refractive index of 1.54.
[0219] Production Example 4A [Production of Thermoplastic Resin (B-4) Pellets]
[0220] 500 ppm of phosphorus additive PEP-36 and 0.2% by mass of stearic acid monoglyceride were added to 100 parts by mass of a total of 25 parts by mass of methacrylic resin (C-2) and 75 parts by mass of styrene copolymer (D-1), and mixed in the same manner as in Production Example 1A to prepare pellets. Pellets of thermoplastic resin (B-4) can be stably produced.
[0221] The pellets of the thermoplastic resin (B-4) had an appearance of 0 (transparent), a glass transition temperature of 136° C., a melt flow rate at a temperature of 230° C. and a load of 3.8 kg of 4.6 g / 10 minutes, and a refractive index of 1.56.
[0222] Comparative Production Example 1A [Production of Thermoplastic Resin (F-1) Pellets]
[0223] 500 ppm of phosphorus additive PEP-36 and 0.2% by mass of stearic acid monoglyceride were added to 100 parts by mass of 75 parts by mass of methacrylic resin (C-1) and 25 parts by mass of styrene copolymer (D-1), and mixed in the same manner as in Production Example 1A to prepare pellets. Pellets of thermoplastic resin (F-1) can be stably produced.
[0224] The pellets of the thermoplastic resin (F-1) had an appearance of 0 (transparent), a glass transition temperature of 113° C., a melt flow rate at a temperature of 230° C. and a load of 3.8 kg: 2.0 g / 10 min, and a refractive index of 1.51.
[0225] Comparative Production Example 2A [Production of Thermoplastic Resin (F-2) Pellets]
[0226] 500 ppm of phosphorus additive PEP-36 and 0.2% by mass of stearic acid monoglyceride were added to 100 parts by mass of 75 parts by mass of methacrylic resin (C-2) and 25 parts by mass of styrene copolymer (D-1), and mixed in the same manner as in Production Example 1A to prepare pellets. Pellets of thermoplastic resin (F-2) can be stably produced.
[0227] The pellets of the thermoplastic resin (F-2) had an appearance of 0 (transparent), a glass transition temperature of 117° C., a melt flow rate at a temperature of 230° C. and a load of 3.8 kg: 3.7 g / 10 min, and a refractive index of 1.51.
[0228] Comparative Production Example 3A [Production of Thermoplastic Resin (F-3) Pellets]
[0229] 500 ppm of phosphorus additive PEP-36 and 0.2% by mass of stearic acid monoglyceride were added to 100 parts by mass of methacrylic resin (C-1), and the mixture was mixed in the same manner as in Production Example 1A to prepare pellets. Pellets of thermoplastic resin (F-3) were stably produced.
[0230] The pellets of the thermoplastic resin (F-3) had an appearance of 0 (transparent), a glass transition temperature of 109° C., a melt flow rate at a temperature of 230° C. and a load of 3.8 kg: 1.8 g / 10 min, and a refractive index of 1.49.
[0231] Comparative Production Example 4A [Production of Thermoplastic Resin (F-4) Pellets]
[0232] 500 ppm of phosphorus additive PEP-36 and 0.2% by mass of stearic acid monoglyceride were added to 100 parts by mass of methacrylic resin (C-2), and the mixture was mixed in the same manner as in Production Example 1A to prepare pellets. Pellets of thermoplastic resin (F-4) were stably produced.
[0233] The pellets of the thermoplastic resin (F-4) had an appearance of 0 (transparent), a glass transition temperature of 111° C., a melt flow rate at a temperature of 230° C. and a load of 3.8 kg: 3.5 g / 10 min, and a refractive index of 1.49.
[0234] Comparative Production Example 5A [Production of Thermoplastic Resin (F-5) Pellets]
[0235] 500 ppm of phosphorus additive PEP-36 and 0.2 mass % of stearic acid monoglyceride were added to 100 parts by mass of styrene copolymer (D-1), and mixed in the same manner as in Production Example 1A to prepare pellets. Pellets of thermoplastic resin (F-5) were stably produced.
[0236] The pellets of the thermoplastic resin (F-5) had an appearance of 0 (transparent), a glass transition temperature of 143° C., a melt flow rate at a temperature of 230° C. and a load of 3.8 kg of 7.6 g / 10 minutes, and a refractive index of 1.58.
[0237] Comparative Production Example 6A [Production of Thermoplastic Resin (F-6) Pellets]
[0238] 500 ppm of phosphorus additive PEP-36 and 0.2% by mass of stearic acid monoglyceride were added to 100 parts by mass of a total of 50 parts by mass of methacrylic resin (C-1) and 50 parts by mass of styrene copolymer (E-1), and mixed in the same manner as in Production Example 1A to prepare pellets. Pellets of thermoplastic resin (F-6) can be stably produced.
[0239] Appearance of the pellets of the thermoplastic resin (F-6): × (translucent).
[0240] Comparative Production Example 7A [Production of Thermoplastic Resin (F-7) Pellets]
[0241] 500 ppm of phosphorus additive PEP-36 and 0.2% by mass of stearic acid monoglyceride were added to 100 parts by mass of a total of 50 parts by mass of methacrylic resin (C-2) and 50 parts by mass of styrene copolymer (E-1), and mixed in the same manner as in Production Example 1A to prepare pellets. Pellets of thermoplastic resin (F-7) can be stably produced.
[0242] Appearance of the pellets of the thermoplastic resin (F-7): × (translucent).
[0243] Comparative Production Example 8A [Production of Thermoplastic Resin (F-8) Pellets]
[0244] 500 ppm of phosphorus additive PEP-36 and 0.2% by mass of stearic acid monoglyceride were added to 100 parts by mass of a total of 50 parts by mass of methacrylic resin (C-1) and 50 parts by mass of styrene copolymer (E-2), and mixed in the same manner as in Production Example 1A to prepare pellets. Pellets of thermoplastic resin (F-8) can be stably produced.
[0245] The appearance of the pellets of the thermoplastic resin (F-8) was: × (white turbidity).
[0246] Comparative Production Example 9A [Production of Thermoplastic Resin (F-9) Pellets]
[0247] 500 ppm of phosphorus additive PEP-36 and 0.2% by mass of stearic acid monoglyceride were added to 100 parts by mass of a total of 50 parts by mass of methacrylic resin (C-2) and 50 parts by mass of styrene copolymer (E-2), and mixed in the same manner as in Production Example 1A to prepare pellets. Pellets of thermoplastic resin (F-9) can be stably produced.
[0248] The appearance of the pellets of the thermoplastic resin (F-9) was: × (white turbidity).
[0249] [Table 2]
[0250]
[0251] Production Example 1B [Production of resin laminate (H-1)]
[0252] A resin laminate was formed by a multilayer extrusion device, wherein the multilayer extruder had a single screw extruder with a screw diameter of 32 mm, a single screw extruder with a screw diameter of 65 mm, a feed block connected to the full extruder, and a 650 mm wide T-die connected to the feed block, and had a multi-manifold die connected to each extruder. The thermoplastic resin (B-1) obtained in Manufacturing Example 1A was continuously introduced into the single screw extruder with a screw diameter of 32 mm, and extruded at a barrel temperature of 240°C and a discharge rate of 2.0 kg / h. In addition, the polycarbonate resin (A-1) obtained in Synthesis Example 2 was continuously introduced into the single screw extruder with a screw diameter of 65 mm, and extruded at a barrel temperature of 280°C and a discharge rate of 31.8 kg / h. The feed block connected to the full extruder was equipped with two types of two-layer distribution pins, and the temperature was set to 270° C., and the thermoplastic resin (B-1) and the polycarbonate resin (A-1) were introduced and laminated.
[0253] The resin laminate (H-1) of thermoplastic resin (B-1) and polycarbonate resin (A-1) was obtained by extruding it in a sheet form using a T-die connected to its front end at a temperature of 270°C, and mirror transfer was performed using three mirror-finished rollers set to temperatures of 110°C, 105°C, and 165°C from the upstream side, while cooling. The resin laminate (H-1) obtained had an overall thickness of 1000 μm in the central portion, and a thickness of 60 μm in the surface layer (layer containing thermoplastic resin (B)). The resin laminate (H-1) had a total light transmittance of 90.9%, a haze of 0.3%, a pencil hardness of H, interference fringes of 0, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0254] Production Example 2B [Production of resin laminate (H-2)]
[0255] A resin laminate (H-2) of a thermoplastic resin (B-1) and a polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-1) of manufacturing example 1B, except that the discharge rate of the single screw extruder with a screw diameter of 32 mm was changed to 3.4 kg / h and the discharge rate of the single screw extruder with a screw diameter of 65 mm was changed to 28.6 kg / h. The obtained resin laminate (H-2) had an overall thickness of 1000 μm in the central portion and a surface thickness of 100 μm. The resin laminate (H-2) had a total light transmittance of 90.9%, a haze of 0.5%, a pencil hardness of 2H, interference fringes of 0, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0256] Production Example 3B [Production of resin laminate (H-3)]
[0257] The discharge rate of the single screw extruder with a screw diameter of 32 mm was changed to 3.9 kg / h, the discharge rate of the single screw extruder with a screw diameter of 65 mm was changed to 28.1 kg / h, the two-layer distribution pins were changed to two-layer distribution pins, and the cooling was changed to mirror transfer using three mirror-finished rollers set to 110°C, 105°C, and 110°C from the upstream side. The same operation as the resin laminate (H-1) of Manufacturing Example 1B was performed to obtain a resin laminate (H-3) of a thermoplastic resin (B-1) and a polycarbonate resin (A-1). The obtained resin laminate (H-3) had an overall thickness of 1000 μm in the central portion and a surface thickness of 60 μm and 60 μm. The resin laminate (H-3) had a total light transmittance of 90.9%, a haze of 0.5%, a pencil hardness of H, interference fringes of 0, cracks in a bent portion of hot press molding processability of 0, and springback of hot press molding processability of 0.
[0258] Production Example 4B [Production of resin laminate (H-4)]
[0259] A resin laminate (H-4) of thermoplastic resin (B-2) and polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-1) of manufacturing example 1B except that thermoplastic resin (B-2) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (H-4) was 1000 μm, and the thickness of the surface layer was 60 μm. The resin laminate (H-4) had a total light transmittance of 90.7%, a haze of 0.5%, a pencil hardness of H, interference fringes of 0, cracks in the bending part of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0260] Production Example 5B [Production of resin laminate (H-5)]
[0261] A resin laminate (H-5) of thermoplastic resin (B-2) and polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-2) of manufacturing example 2B except that thermoplastic resin (B-2) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (H-5) was 1000 μm, and the thickness of the surface layer was 100 μm. The resin laminate (H-5) had a total light transmittance of 90.5%, a haze of 0.6%, a pencil hardness of H, interference fringes of 0, cracks in the bending part of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0262] Production Example 6B [Production of resin laminate (H-6)]
[0263] A resin laminate (H-6) of thermoplastic resin (B-2) and polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-3) of manufacturing example 3B except that thermoplastic resin (B-2) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (H-6) was 1000 μm, and the surface thicknesses were 60 μm and 60 μm. The resin laminate (H-6) had a total light transmittance of 90.5%, a haze of 0.6%, a pencil hardness of H, interference fringes of 0, cracks in the bending part of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0264] Production Example 7B [Production of resin laminate (H-7)]
[0265] A resin laminate (H-7) of thermoplastic resin (B-3) and polycarbonate resin (A-1) was obtained in the same manner as the resin laminate (H-1) of Manufacturing Example 1B except that thermoplastic resin (B-3) was used instead of thermoplastic resin (B-1). The obtained resin laminate (H-7) had an overall thickness of 1000 μm in the central portion and a surface thickness of 60 μm. The resin laminate (H-7) had a total light transmittance of 90.9%, a haze of 0.3%, a pencil hardness of H, interference fringes of 0, cracks in the bending portion of hot press molding processability of 0, and springback of hot press molding processability of 0.
[0266] Production Example 8B [Production of resin laminate (H-8)]
[0267] A resin laminate (H-8) of thermoplastic resin (B-3) and polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-2) of manufacturing example 2B except that thermoplastic resin (B-3) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (H-8) was 1000 μm, and the thickness of the surface layer was 100 μm. The resin laminate (H-8) had a total light transmittance of 90.9%, a haze of 0.5%, a pencil hardness of H, interference fringes of 0, cracks in the bending part of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0268] Production Example 9B [Production of resin laminate (H-9)]
[0269] A resin laminate (H-9) of thermoplastic resin (B-3) and polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-3) of manufacturing example 3B except that thermoplastic resin (B-3) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (H-9) was 1000 μm, and the surface thicknesses were 60 μm and 60 μm. The resin laminate (H-9) had a total light transmittance of 90.9%, a haze of 0.5%, a pencil hardness of H, interference fringes of 0, cracks in the bending part of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0270] Production Example 10B [Production of resin laminate (H-10)]
[0271] A resin laminate (H-10) of thermoplastic resin (B-4) and polycarbonate resin (A-1) was obtained in the same manner as the resin laminate (H-1) of manufacturing example 1B except that thermoplastic resin (B-4) was used instead of thermoplastic resin (B-1). The obtained resin laminate (H-10) had an overall thickness of 1000 μm in the central portion and a surface thickness of 60 μm. The resin laminate (H-10) had a total light transmittance of 90.7%, a haze of 0.5%, a pencil hardness of H, interference fringes of 0, cracks in the bending portion of hot press molding processability of 0, and springback of hot press molding processability of 0.
[0272] Production Example 11B [Production of resin laminate (H-11)]
[0273] A resin laminate (H-11) of thermoplastic resin (B-4) and polycarbonate resin (A-1) was obtained in the same manner as the resin laminate (H-2) of manufacturing example 2B except that thermoplastic resin (B-4) was used instead of thermoplastic resin (B-1). The obtained resin laminate (H-11) had an overall thickness of 1000 μm in the central portion and a surface thickness of 100 μm. The resin laminate (H-11) had a total light transmittance of 90.5%, a haze of 0.6%, a pencil hardness of H, interference fringes of 0, cracks in the bending portion of hot press molding processability of 0, and springback of hot press molding processability of 0.
[0274] Production Example 12B [Production of resin laminate (H-12)]
[0275] A resin laminate (H-12) of thermoplastic resin (B-4) and polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-3) of manufacturing example 3B except that thermoplastic resin (B-4) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (H-12) was 1000 μm, and the surface thicknesses were 60 μm and 60 μm. The resin laminate (H-12) had a total light transmittance of 90.5%, a haze of 0.6%, a pencil hardness of H, interference fringes: 0, cracks in the bending part of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0276] Comparative Manufacturing Example 1B [Manufacture of Resin Laminated Body (I-1)]
[0277] A resin laminate (I-1) of thermoplastic resin (F-1) and polycarbonate resin (A-1) was obtained in the same manner as the resin laminate (H-1) of manufacturing example 1B except that thermoplastic resin (F-1) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-1) had an overall thickness of 1000 μm in the central portion and a surface thickness of 60 μm. The resin laminate (I-1) had a total light transmittance of 91.2%, a haze of 0.5%, a pencil hardness of 2H, interference fringes of 0, cracks in the bending portion of hot press molding processability of 0, and springback of hot press molding processability of 0.
[0278] Comparative Manufacturing Example 2B [Manufacture of Resin Laminated Body (I-2)]
[0279] A resin laminate (I-2) of thermoplastic resin (F-1) and polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-2) of manufacturing example 2B except that thermoplastic resin (F-1) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (I-2) was 1000 μm, and the thickness of the surface layer was 100 μm. The resin laminate (I-2) had a total light transmittance of 91.1%, a haze of 0.6%, a pencil hardness of 2H, interference fringes: 0, cracks in the bending part of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0280] Comparative Manufacturing Example 3B [Manufacture of Resin Laminated Body (I-3)]
[0281] A resin laminate (I-3) of thermoplastic resin (F-1) and polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-3) of manufacturing example 3B except that thermoplastic resin (F-1) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (I-3) was 1000 μm, and the surface thicknesses were 60 μm and 60 μm. The resin laminate (I-3) had a total light transmittance of 91.1%, a haze of 0.6%, a pencil hardness of 2H, interference fringes: 0, cracks in the bending part of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0282] Comparative Manufacturing Example 4B [Manufacture of Resin Laminated Body (I-4)]
[0283] A resin laminate (I-4) of thermoplastic resin (F-2) and polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-1) of manufacturing example 1B except that thermoplastic resin (F-2) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (I-4) was 1000 μm, and the thickness of the surface layer was 60 μm. The resin laminate (I-4) had a total light transmittance of 91.2%, a haze of 0.5%, a pencil hardness of 2H, interference fringes: 0, cracks in the bending part of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0284] Manufacturing Comparative Example 5B [Manufacture of Resin Laminated Body (I-5)]
[0285] A resin laminate (I-5) of thermoplastic resin (F-2) and polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-2) of manufacturing example 2B except that thermoplastic resin (F-2) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (I-5) was 1000 μm, and the thickness of the surface layer was 100 μm. The resin laminate (I-5) had a total light transmittance of 91.1%, a haze of 0.6%, a pencil hardness of 2H, interference fringes: 0, cracks in the bending part of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0286] Comparative Manufacturing Example 6B [Manufacture of Resin Laminated Body (I-6)]
[0287] A resin laminate (I-6) of thermoplastic resin (F-2) and polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-3) of manufacturing example 3B except that thermoplastic resin (F-2) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (I-6) was 1000 μm, and the surface thicknesses were 60 μm and 60 μm. The resin laminate (I-6) had a total light transmittance of 91.1%, a haze of 0.6%, a pencil hardness of 2H, interference fringes: 0, cracks in the bending part of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0288] Comparative Manufacturing Example 7B [Manufacture of Resin Laminated Body (I-7)]
[0289] The resin laminate (I-7) of thermoplastic resin (F-3) and polycarbonate resin (A-1) was obtained in the same manner as the resin laminate (H-1) of manufacturing example 1B except that thermoplastic resin (F-3) was used instead of thermoplastic resin (B-1). The total thickness of the central portion of the obtained resin laminate (I-7) was 1000 μm, and the thickness of the surface layer was 60 μm. The resin laminate (I-7) had a total light transmittance of 91.6%, a haze of 0.2%, a pencil hardness of 3H, interference fringes: ×, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0290] Manufacturing Comparative Example 8B [Manufacture of Resin Laminated Body (I-8)]
[0291] A resin laminate (I-8) of thermoplastic resin (F-3) and polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-2) of manufacturing example 2B except that thermoplastic resin (F-3) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (I-8) was 1000 μm, and the thickness of the surface layer was 100 μm. The resin laminate (I-8) had a total light transmittance of 91.6%, a haze of 0.2%, a pencil hardness of 3H, interference fringes: ×, cracks in the bending part of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0292] Manufacturing Comparative Example 9B [Manufacture of Resin Laminated Body (I-9)]
[0293] A resin laminate (I-9) of thermoplastic resin (F-3) and polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-3) of manufacturing example 3B except that thermoplastic resin (F-3) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (I-9) was 1000 μm, and the surface thicknesses were 60 μm and 60 μm. The resin laminate (I-9) had a total light transmittance of 91.6%, a haze of 0.2%, a pencil hardness of 3H, interference fringes: ×, cracks in the bending part of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0294] Comparative Manufacturing Example 10B [Manufacture of Resin Laminated Body (I-10)]
[0295] A resin laminate (I-10) of thermoplastic resin (F-4) and polycarbonate resin (A-1) was obtained in the same manner as the resin laminate (H-1) of manufacturing example 1B except that thermoplastic resin (F-4) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-10) had an overall thickness of 1000 μm in the central portion and a surface thickness of 60 μm. The resin laminate (I-10) had a total light transmittance of 91.6%, a haze of 0.2%, a pencil hardness of 3H, interference fringes: ×, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0296] Comparative Manufacturing Example 11B [Manufacture of Resin Laminated Body (I-11)]
[0297] A resin laminate (I-11) of thermoplastic resin (F-4) and polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-2) of manufacturing example 2B except that thermoplastic resin (F-4) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (I-11) was 1000 μm, and the thickness of the surface layer was 100 μm. The resin laminate (I-11) had a total light transmittance of 91.6%, a haze of 0.2%, a pencil hardness of 3H, interference fringes: ×, cracks in the bending part of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0298] Manufacturing Comparative Example 12B [Manufacture of Resin Laminated Body (I-12)]
[0299] A resin laminate (I-12) of thermoplastic resin (F-4) and polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-3) of manufacturing example 3B except that thermoplastic resin (F-4) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (I-12) was 1000 μm, and the surface thicknesses were 60 μm and 60 μm. The resin laminate (I-12) had a total light transmittance of 91.6%, a haze of 0.2%, a pencil hardness of 3H, interference fringes: ×, cracks in the bending part of hot press molding processability: 0, and springback of hot press molding processability: 0.
[0300] Manufacturing Comparative Example 13B [Manufacture of Resin Laminated Body (I-13)]
[0301] The resin laminate (I-13) of thermoplastic resin (F-5) and polycarbonate resin (A-1) was obtained in the same manner as the resin laminate (H-1) of manufacturing example 1B except that thermoplastic resin (F-5) was used instead of thermoplastic resin (B-1). The total thickness of the central portion of the obtained resin laminate (I-13) was 1000 μm, and the thickness of the surface layer was 60 μm. The resin laminate (I-13) had a total light transmittance of 90.6%, a haze of 0.6%, a pencil hardness of F, interference fringes: 0, cracks in the bending portion of hot press molding processability: ×, and springback of hot press molding processability: 0.
[0302] Manufacturing Comparative Example 14B [Manufacture of Resin Laminated Body (I-14)]
[0303] A resin laminate (I-14) of thermoplastic resin (F-5) and polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-2) of manufacturing example 2B except that thermoplastic resin (F-5) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (I-14) was 1000 μm, and the thickness of the surface layer was 100 μm. The resin laminate (I-14) had a total light transmittance of 90.5%, a haze of 0.7%, a pencil hardness of H, interference fringes of 0, cracks in the bending part of hot press molding processability: ×, and springback of hot press molding processability: 0.
[0304] Manufacturing Comparative Example 15B [Manufacture of Resin Laminated Body (I-15)]
[0305] The resin laminate (I-15) of thermoplastic resin (F-5) and polycarbonate resin (A-1) was obtained by the same operation as the resin laminate (H-3) of manufacturing example 3B except that thermoplastic resin (F-5) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (I-15) was 1000 μm, and the surface thicknesses were 60 μm and 60 μm. The resin laminate (I-15) had a total light transmittance of 90.5%, a haze of 0.7%, a pencil hardness of F, interference fringes: 0, cracks in the bending part of hot press molding processability: ×, and springback of hot press molding processability: 0.
[0306] Manufacturing Comparative Example 16B [Manufacture of Resin Laminated Body (I-16)]
[0307] A resin laminate (I-16) of thermoplastic resin (B-1) and polycarbonate resin (G-1) was obtained by using a polycarbonate resin (G-1) instead of a polycarbonate resin (A-1), and changing the method to mirror transfer while cooling using three mirror-finished rollers set at temperatures of 130°C, 140°C, and 180°C from the upstream side. The same operation as the resin laminate (H-1) of Manufacturing Example 1B was performed. The obtained resin laminate (I-16) had an overall thickness of 1000 μm in the central portion and a surface thickness of 60 μm. The resin laminate (I-16) had a total light transmittance of 90.9%, a haze of 0.3%, a pencil hardness of H, interference fringes: 0, cracks in the bent portion of hot press molding processability: 0, and rebound of hot press molding processability: ×. Manufacturing Comparative Example 17B [Manufacture of Resin Laminate (I-17)]
[0308] A resin laminate (I-17) of thermoplastic resin (B-1) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (H-2) of manufacturing example 2B, except that polycarbonate resin (G-1) was used instead of polycarbonate resin (A-1) and cooling was performed while mirror transfer was performed using three mirror-finished rollers set to 130°C, 140°C, and 180°C from the upstream side. The obtained resin laminate (I-17) had an overall thickness of 1000 μm in the central portion and a surface thickness of 100 μm. The resin laminate (I-17) had a total light transmittance of 90.9%, a haze of 0.5%, a pencil hardness of 2H, interference fringes of 0, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0309] Manufacturing Comparative Example 18B [Manufacture of resin laminate (I-18)]
[0310] A resin laminate (I-18) of thermoplastic resin (B-1) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (H-3) of manufacturing example 3B, except that polycarbonate resin (G-1) was used instead of polycarbonate resin (A-1) and cooling was performed while mirror transfer was performed using three mirror-finished rollers set to 130°C, 140°C, and 110°C from the upstream side. The obtained resin laminate (I-18) had an overall thickness of 1000 μm in the central portion and a surface thickness of 60 μm and 60 μm. The resin laminate (I-18) had a total light transmittance of 90.9%, a haze of 0.5%, a pencil hardness of H, interference fringes of 0, cracks in the bending portion of hot press molding processability of 0, and springback of hot press molding processability of ×.
[0311] Manufacturing Comparative Example 19B [Manufacture of Resin Laminated Body (I-19)]
[0312] The resin laminate (I-19) of thermoplastic resin (B-2) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-16) of Comparative Example 16B except that thermoplastic resin (B-2) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (I-19) was 1000 μm, and the thickness of the surface layer was 60 μm. The resin laminate (I-19) had a total light transmittance of 90.7%, a haze of 0.5%, a pencil hardness of H, interference fringes: 0, cracks in the bending part of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0313] Manufacturing Comparative Example 20B [Manufacture of Resin Laminated Body (I-20)]
[0314] A resin laminate (I-20) of thermoplastic resin (B-2) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-17) of Comparative Example 17B except that thermoplastic resin (B-2) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-20) had an overall thickness of 1000 μm in the central portion and a surface thickness of 100 μm. The resin laminate (I-20) had a total light transmittance of 90.5%, a haze of 0.6%, a pencil hardness of H, interference fringes of 0, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0315] Manufacturing Comparative Example 21B [Manufacture of Resin Laminated Body (I-21)]
[0316] A resin laminate (I-21) of thermoplastic resin (B-2) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-18) of Comparative Example 18B except that thermoplastic resin (B-2) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-21) had an overall thickness of 1000 μm in the central portion and surface thicknesses of 60 μm and 60 μm. The resin laminate (I-21) had a total light transmittance of 90.5%, a haze of 0.6%, a pencil hardness of H, interference fringes of 0, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0317] Manufacturing Comparative Example 22B [Manufacture of Resin Laminated Body (I-22)]
[0318] The resin laminate (I-22) of thermoplastic resin (B-3) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-16) of Comparative Example 16B except that thermoplastic resin (B-3) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (I-22) was 1000 μm, and the thickness of the surface layer was 60 μm. The resin laminate (I-22) had a total light transmittance of 90.9%, a haze of 0.3%, a pencil hardness of H, interference fringes: 0, cracks in the bending part of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0319] Manufacturing Comparative Example 23B [Manufacture of Resin Laminated Body (I-23)]
[0320] A resin laminate (I-23) of thermoplastic resin (B-3) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-17) of Comparative Example 17B except that thermoplastic resin (B-3) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-23) had an overall thickness of 1000 μm in the central portion and a surface thickness of 100 μm. The resin laminate (I-23) had a total light transmittance of 90.9%, a haze of 0.5%, a pencil hardness of 2H, interference fringes of 0, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0321] Manufacturing Comparative Example 24B [Manufacture of Resin Laminated Body (I-24)]
[0322] A resin laminate (I-24) of thermoplastic resin (B-3) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-18) of Comparative Example 18B except that thermoplastic resin (B-3) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-24) had an overall thickness of 1000 μm in the central portion and surface thicknesses of 60 μm and 60 μm. The resin laminate (I-24) had a total light transmittance of 90.9%, a haze of 0.5%, a pencil hardness of H, interference fringes of 0, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0323] Manufacturing Comparative Example 25B [Manufacture of Resin Laminated Body (I-25)]
[0324] A resin laminate (I-25) of thermoplastic resin (B-4) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-16) of Comparative Example 16B except that thermoplastic resin (B-4) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-25) had an overall thickness of 1000 μm in the central portion and a surface thickness of 60 μm. The resin laminate (I-25) had a total light transmittance of 90.7%, a haze of 0.5%, a pencil hardness of H, interference fringes of 0, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0325] Manufacturing Comparative Example 26B [Manufacture of Resin Laminated Body (I-26)]
[0326] A resin laminate (I-26) of thermoplastic resin (B-4) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-17) of Comparative Example 17B except that thermoplastic resin (B-4) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-26) had an overall thickness of 1000 μm in the central portion and a surface thickness of 100 μm. The resin laminate (I-26) had a total light transmittance of 90.5%, a haze of 0.6%, a pencil hardness of H, interference fringes of 0, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0327] Manufacturing Comparative Example 27B [Manufacture of Resin Laminated Body (I-27)]
[0328] A resin laminate (I-27) of thermoplastic resin (B-4) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-18) of Comparative Example 18B except that thermoplastic resin (B-4) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-27) had an overall thickness of 1000 μm in the central portion and surface thicknesses of 60 μm and 60 μm. The resin laminate (I-27) had a total light transmittance of 90.5%, a haze of 0.6%, a pencil hardness of H, interference fringes of 0, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0329] Manufacturing Comparative Example 28B [Manufacture of resin laminate (I-28)]
[0330] A resin laminate (I-28) of thermoplastic resin (F-1) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-16) of Comparative Example 16B except that thermoplastic resin (F-1) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-28) had an overall thickness of 1000 μm in the central portion and a surface thickness of 60 μm. The resin laminate (I-28) had a total light transmittance of 91.2%, a haze of 0.5%, a pencil hardness of 2H, interference fringes of 0, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0331] Manufacturing Comparative Example 29B [Manufacture of Resin Laminated Body (I-29)]
[0332] A resin laminate (I-29) of thermoplastic resin (F-1) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-17) of Comparative Example 17B except that thermoplastic resin (F-1) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-29) had an overall thickness of 1000 μm in the central portion and a surface thickness of 100 μm. The resin laminate (I-29) had a total light transmittance of 91.1%, a haze of 0.6%, a pencil hardness of 2H, interference fringes of 0, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0333] Manufacturing Comparative Example 30B [Manufacture of Resin Laminated Body (I-30)]
[0334] A resin laminate (I-30) of thermoplastic resin (F-1) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-18) of Comparative Example 18B except that thermoplastic resin (F-1) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-30) had an overall thickness of 1000 μm in the central portion and surface thicknesses of 60 μm and 60 μm. The resin laminate (I-30) had a total light transmittance of 91.1%, a haze of 0.6%, a pencil hardness of 2H, interference fringes of 0, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0335] Manufacturing Comparative Example 31B [Manufacture of Resin Laminated Body (I-31)]
[0336] A resin laminate (I-31) of thermoplastic resin (F-2) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-16) of Comparative Example 16B except that thermoplastic resin (F-2) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-31) had an overall thickness of 1000 μm in the central portion and a surface thickness of 60 μm. The resin laminate (I-31) had a total light transmittance of 91.2%, a haze of 0.5%, a pencil hardness of 2H, interference fringes of 0, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0337] Manufacturing Comparative Example 32B [Manufacture of Resin Laminated Body (I-32)]
[0338] A resin laminate (I-32) of thermoplastic resin (F-2) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-17) of Comparative Example 17B except that thermoplastic resin (F-2) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-32) had an overall thickness of 1000 μm in the central portion and a surface thickness of 100 μm. The resin laminate (I-32) had a total light transmittance of 91.1%, a haze of 0.6%, a pencil hardness of 2H, interference fringes of 0, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0339] Manufacturing Comparative Example 33B [Manufacture of Resin Laminated Body (I-33)]
[0340] A resin laminate (I-33) of thermoplastic resin (F-2) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-18) of Comparative Example 18B except that thermoplastic resin (F-2) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-33) had an overall thickness of 1000 μm in the central portion and surface thicknesses of 60 μm and 60 μm. The resin laminate (I-33) had a total light transmittance of 91.1%, a haze of 0.6%, a pencil hardness of 2H, interference fringes of 0, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0341] Manufacturing Comparative Example 34B [Manufacture of Resin Laminated Body (I-34)]
[0342] A resin laminate (I-34) of thermoplastic resin (F-3) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-16) of Comparative Example 16B except that thermoplastic resin (F-3) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-34) had an overall thickness of 1000 μm in the central portion and a surface thickness of 60 μm. The resin laminate (I-34) had a total light transmittance of 91.6%, a haze of 0.2%, a pencil hardness of 3H, interference fringes: ×, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0343] Manufacturing Comparative Example 35B [Manufacture of Resin Laminated Body (I-35)]
[0344] A resin laminate (I-35) of thermoplastic resin (F-3) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-17) of Comparative Example 17B except that thermoplastic resin (F-3) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-35) had an overall thickness of 1000 μm in the central portion and a surface thickness of 100 μm. The resin laminate (I-35) had a total light transmittance of 91.6%, a haze of 0.2%, a pencil hardness of 3H, interference fringes: ×, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0345] Manufacturing Comparative Example 36B [Manufacture of Resin Laminated Body (I-36)]
[0346] A resin laminate (I-36) of thermoplastic resin (F-3) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-18) of Comparative Example 18B except that thermoplastic resin (F-3) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-36) had an overall thickness of 1000 μm in the central portion and surface thicknesses of 60 μm and 60 μm. The resin laminate (I-36) had a total light transmittance of 91.6%, a haze of 0.2%, a pencil hardness of 3H, interference fringes: ×, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0347] Manufacturing Comparative Example 37B [Manufacture of Resin Laminated Body (I-37)]
[0348] A resin laminate (I-37) of thermoplastic resin (F-4) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-16) of Comparative Example 16B except that thermoplastic resin (F-4) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-37) had an overall thickness of 1000 μm in the central portion and a surface thickness of 60 μm. The resin laminate (I-37) had a total light transmittance of 91.6%, a haze of 0.2%, a pencil hardness of 3H, interference fringes: ×, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0349] Manufacturing Comparative Example 38B [Manufacture of Resin Laminated Body (I-38)]
[0350] A resin laminate (I-38) of thermoplastic resin (F-4) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-17) of Comparative Example 17B except that thermoplastic resin (F-4) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-38) had an overall thickness of 1000 μm in the central portion and a surface thickness of 100 μm. The resin laminate (I-38) had a total light transmittance of 91.6%, a haze of 0.2%, a pencil hardness of 3H, interference fringes: ×, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0351] Manufacturing Comparative Example 39B [Manufacture of Resin Laminated Body (I-39)]
[0352] A resin laminate (I-39) of thermoplastic resin (F-4) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-18) of Comparative Example 18B except that thermoplastic resin (F-4) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-39) had an overall thickness of 1000 μm in the central portion and surface thicknesses of 60 μm and 60 μm. The resin laminate (I-39) had a total light transmittance of 91.6%, a haze of 0.2%, a pencil hardness of 3H, interference fringes: ×, cracks in the bending portion of hot press molding processability: 0, and springback of hot press molding processability: ×.
[0353] Manufacturing Comparative Example 40B [Manufacture of Resin Laminated Body (I-40)]
[0354] A resin laminate (I-40) of thermoplastic resin (F-5) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-16) of Comparative Example 16B except that thermoplastic resin (F-5) was used instead of thermoplastic resin (B-1). The total thickness of the central part of the obtained resin laminate (I-40) was 1000 μm, and the thickness of the surface layer was 60 μm. The resin laminate (I-40) had a total light transmittance of 90.6%, a haze of 0.6%, a pencil hardness of F, interference fringes: 0, cracks in the bending part of hot press molding processability: ×, and springback of hot press molding processability: ×.
[0355] Manufacturing Comparative Example 41B [Manufacture of Resin Laminated Body (I-41)]
[0356] A resin laminate (I-41) of thermoplastic resin (F-5) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-17) of Comparative Example 17B except that thermoplastic resin (F-5) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-41) had an overall thickness of 1000 μm in the central portion and a surface thickness of 100 μm. The resin laminate (I-41) had a total light transmittance of 90.5%, a haze of 0.7%, a pencil hardness of H, interference fringes of 0, cracks in the bending portion of hot press molding processability: ×, and springback of hot press molding processability: ×.
[0357] Manufacturing Comparative Example 42B [Manufacture of Resin Laminated Body (I-42)]
[0358] A resin laminate (I-42) of thermoplastic resin (F-5) and polycarbonate resin (G-1) was obtained by the same operation as the resin laminate (I-18) of Comparative Example 18B except that thermoplastic resin (F-5) was used instead of thermoplastic resin (B-1). The obtained resin laminate (I-42) had an overall thickness of 1000 μm in the central portion and surface thicknesses of 60 μm and 60 μm. The resin laminate (I-42) had a total light transmittance of 90.5%, a haze of 0.7%, a pencil hardness of F, interference fringes of 0, cracks in the bending portion of hot press molding processability: ×, and springback of hot press molding processability: ×.
[0359] [Table 3]
[0360] Table 3
[0361]
[0362] Example 1 [Manufacturing of resin laminate (K-1)]
[0363] A coating was prepared by adding 1% by mass of a photopolymerization initiator (product name: I-184 [compound name: 1-hydroxy-cyclohexyl phenyl ketone] manufactured by BASF Corporation) to 100 parts by mass of a total of 60 parts by mass of a hexafunctional urethane acrylate oligomer (product name: U6HA, manufactured by Shin-Nakamura Chemical Co., Ltd.), 35 parts by mass of PEG200# diacrylate (product name: 4EG-A, manufactured by Kyoeisha Chemical Co., Ltd.), and 5 parts by mass of an oligomer containing a fluorine-containing group, a hydrophilic group, a lipophilic group, and a UV-reactive group (product name: RS-90, manufactured by DIC Corporation). The coating was applied to the surface of the thermoplastic resin (B-1) of the resin laminate (H-1) obtained in Production Example 1B using a bar coater, and irradiated with a metal halide lamp (20 mW / cm 2 ) for 5 seconds to cure the hard coat layer, thereby producing a resin laminate (K-1). The film thickness of the hard coat layer (J-1) was 6 μm.
[0364] The resin laminate (K-1) had a total light transmittance of 90.8%, a haze of 0.3%, a pencil hardness of 3H, interference fringes of 0, cracks in a bent portion of hot press molding processability of 0, and springback of hot press molding processability of 0.
[0365] Example 2〔Manufacturing of resin laminate (K-2)〕
[0366] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (B-1) of the resin laminate (H-2) obtained in Production Example 2B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (K-2). The film thickness of the hard coat layer (J-1) was 6 μm.
[0367] The resin laminate (K-2) had a total light transmittance of 90.8%, a haze of 0.5%, a pencil hardness of 3H, interference fringes of 0, cracks in the bent portion of the hot press molding processability of 0, and springback of the hot press molding processability of 0.
[0368] Example 3〔Manufacturing of resin laminate (K-3)〕
[0369] The same coating as in Example 1 was applied to one side of the thermoplastic resin (B-1) of the resin laminate (H-3) obtained in Production Example 3B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (K-3). The film thickness of the hard coat layer (J-1) was 6 μm.
[0370] The resin laminate (K-3) had a total light transmittance of 90.8%, a haze of 0.5%, a pencil hardness of 3H, interference fringes of 0, cracks in the bent portion of the hot press molding processability of 0, and springback of the hot press molding processability of 0.
[0371] Example 4 [Manufacturing of resin laminate (K-4)]
[0372] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (B-2) of the resin laminate (H-4) obtained in Production Example 4B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (K-4). The film thickness of the hard coat layer (J-1) was 6 μm.
[0373] The resin laminate (K-4) had a total light transmittance of 90.6%, a haze of 0.5%, a pencil hardness of 2H, interference fringes of 0, cracks in the bent portion of the hot press molding processability of 0, and springback of the hot press molding processability of 0.
[0374] Example 5〔Manufacturing of resin laminate (K-5)〕
[0375] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (B-2) of the resin laminate (H-5) obtained in Production Example 5B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (K-5). The film thickness of the hard coat layer (J-1) was 6 μm.
[0376] The resin laminate (K-5) had a total light transmittance of 90.4%, a haze of 0.6%, a pencil hardness of 3H, interference fringes of 0, cracks in the bent portion of the hot press molding processability of 0, and springback of the hot press molding processability of 0.
[0377] Example 6 [Manufacturing of resin laminate (K-6)]
[0378] The same coating as in Example 1 was applied to one side of the thermoplastic resin (B-2) of the resin laminate (H-6) obtained in Production Example 6B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (K-6). The film thickness of the hard coat layer (J-1) was 6 μm.
[0379] The resin laminate (K-6) had a total light transmittance of 90.4%, a haze of 0.6%, a pencil hardness of 2H, interference fringes of 0, cracks in a bent portion of hot press molding processability of 0, and springback of hot press molding processability of 0.
[0380] Example 7 [Manufacturing of resin laminate (K-7)]
[0381] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (B-3) of the resin laminate (H-7) obtained in Production Example 7B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (K-7). The film thickness of the hard coat layer (J-1) was 6 μm.
[0382] The resin laminate (K-7) had a total light transmittance of 90.8%, a haze of 0.3%, a pencil hardness of 3H, interference fringes of 0, cracks in the bent portion of the hot press molding processability of 0, and springback of the hot press molding processability of 0.
[0383] Example 8 [Manufacturing of resin laminate (K-8)]
[0384] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (B-3) of the resin laminate (H-8) obtained in Production Example 8B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (K-8). The film thickness of the hard coat layer (J-1) was 6 μm.
[0385] The resin laminate (K-8) had a total light transmittance of 90.8%, a haze of 0.5%, a pencil hardness of 3H, interference fringes of 0, cracks in the bent portion of the hot press molding processability of 0, and springback of the hot press molding processability of 0.
[0386] Example 9 [Manufacturing of resin laminate (K-9)]
[0387] The same coating as in Example 1 was applied to one side of the thermoplastic resin (B-3) of the resin laminate (H-9) obtained in Production Example 9B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (K-9). The film thickness of the hard coat layer (J-1) was 6 μm.
[0388] The resin laminate (K-9) had a total light transmittance of 90.8%, a haze of 0.5%, a pencil hardness of 3H, interference fringes of 0, cracks in the bent portion of the hot press molding processability of 0, and springback of the hot press molding processability of 0.
[0389] Example 10 [Manufacturing of resin laminate (K-10)]
[0390] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (B-4) of the resin laminate (H-10) obtained in Production Example 10B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (K-10). The film thickness of the hard coat layer (J-1) was 6 μm.
[0391] The resin laminate (K-10) had a total light transmittance of 90.6%, a haze of 0.5%, a pencil hardness of 2H, interference fringes of 0, cracks in a bent portion of hot press molding processability of 0, and springback of hot press molding processability of 0.
[0392] Example 11 [Manufacturing of resin laminate (K-11)]
[0393] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (B-4) of the resin laminate (H-11) obtained in Production Example 11B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (K-11). The film thickness of the hard coat layer (J-1) was 6 μm.
[0394] The resin laminate (K-11) had a total light transmittance of 90.4%, a haze of 0.6%, a pencil hardness of 3H, interference fringes of 0, cracks in a bent portion of hot press molding processability of 0, and springback of hot press molding processability of 0.
[0395] Example 12 [Manufacturing of resin laminate (K-12)]
[0396] The same coating as in Example 1 was applied to one side of the thermoplastic resin (B-4) of the resin laminate (H-12) obtained in Production Example 12B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (K-12). The film thickness of the hard coat layer (J-1) was 6 μm.
[0397] The resin laminate (K-12) had a total light transmittance of 90.4%, a haze of 0.6%, a pencil hardness of 2H, interference fringes of 0, cracks in a bent portion of hot press molding processability of 0, and springback of hot press molding processability of 0.
[0398] Comparative Example 1〔Manufacturing of resin laminate (L-1)〕
[0399] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-1) of the resin laminate (I-1) obtained in Comparative Example 1B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-1). The film thickness of the hard coat layer (J-1) was 6 μm.
[0400] The resin laminate (L-1) had a total light transmittance of 91.1%, a haze of 0.5%, a pencil hardness of 3H, interference fringes of 0, cracks in the bent portion of the hot press molding processability of x, and springback of the hot press molding processability of 0.
[0401] Comparative Example 2〔Manufacturing of resin laminate (L-2)〕
[0402] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-1) of the resin laminate (I-2) obtained in Comparative Example 2B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-2). The film thickness of the hard coat layer (J-1) was 6 μm.
[0403] The resin laminate (L-2) had a total light transmittance of 91.0%, a haze of 0.6%, a pencil hardness of 4H, interference fringes of 0, cracks in the bent portion of the hot press molding processability of x, and springback of the hot press molding processability of 0.
[0404] Comparative Example 3〔Manufacturing of resin laminate (L-3)〕
[0405] The same coating as in Example 1 was applied to one side of the thermoplastic resin (F-1) of the resin laminate (I-3) obtained in Comparative Example 3B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-3). The film thickness of the hard coat layer (J-1) was 6 μm.
[0406] The resin laminate (L-3) had a total light transmittance of 91.0%, a haze of 0.6%, a pencil hardness of 3H, interference fringes of 0, cracks in the bent portion of the hot press molding processability of x, and springback of the hot press molding processability of 0.
[0407] Comparative Example 4 [Manufacture of resin laminate (L-4)]
[0408] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-2) of the resin laminate (I-4) obtained in Comparative Example 4B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-4). The film thickness of the hard coat layer (J-1) was 6 μm.
[0409] The resin laminate (L-4) had a total light transmittance of 91.1%, a haze of 0.5%, a pencil hardness of 3H, interference fringes of 0, cracks in the bent portion of the hot press molding processability of x, and springback of the hot press molding processability of 0.
[0410] Comparative Example 5〔Manufacturing of resin laminate (L-5)〕
[0411] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-2) of the resin laminate (I-5) obtained in Comparative Example 5B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-5). The film thickness of the hard coat layer (J-1) was 6 μm.
[0412] The resin laminate (L-5) had a total light transmittance of 91.0%, a haze of 0.6%, a pencil hardness of 4H, interference fringes of 0, cracks in the bent portion of the hot press molding processability of x, and springback of the hot press molding processability of 0.
[0413] Comparative Example 6 [Manufacture of resin laminate (L-6)]
[0414] The same coating as in Example 1 was applied to one side of the thermoplastic resin (F-2) of the resin laminate (I-6) obtained in Comparative Example 6B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-6). The film thickness of the hard coat layer (J-1) was 6 μm.
[0415] The resin laminate (L-6) had a total light transmittance of 91.0%, a haze of 0.6%, a pencil hardness of 3H, interference fringes of 0, cracks in the bent portion of the hot press molding processability of x, and springback of the hot press molding processability of 0.
[0416] Comparative Example 7〔Manufacturing of resin laminate (L-7)〕
[0417] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-3) of the resin laminate (I-7) obtained in Comparative Example 7B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-7). The film thickness of the hard coat layer (J-1) was 6 μm.
[0418] The resin laminate (L-7) had a total light transmittance of 91.5%, a haze of 0.2%, a pencil hardness of 4H, interference fringes of ×, cracks in the bent portion of hot press molding processability of ×, and springback of hot press molding processability of 0.
[0419] Comparative Example 8 [Manufacture of resin laminate (L-8)]
[0420] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-3) of the resin laminate (I-8) obtained in Comparative Example 8B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-8). The film thickness of the hard coat layer (J-1) was 6 μm.
[0421] The resin laminate (L-8) had a total light transmittance of 91.5%, a haze of 0.2%, a pencil hardness of 4H, interference fringes of ×, cracks in the bent portion of hot press molding processability of ×, and springback of hot press molding processability of 0.
[0422] Comparative Example 9〔Manufacturing of resin laminate (L-9)〕
[0423] The same coating as in Example 1 was applied to one side of the thermoplastic resin (F-3) of the resin laminate (I-9) obtained in Comparative Example 9B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-9). The film thickness of the hard coat layer (J-1) was 6 μm.
[0424] The resin laminate (L-9) had a total light transmittance of 91.5%, a haze of 0.2%, a pencil hardness of 4H, interference fringes of ×, cracks in the bending portion of hot press molding processability of ×, and springback of hot press molding processability of 0.
[0425] Comparative Example 10 [Manufacture of resin laminate (L-10)]
[0426] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-4) of the resin laminate (I-10) obtained in Comparative Example 10B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-10). The film thickness of the hard coat layer (J-1) was 6 μm.
[0427] The resin laminate (L-10) had a total light transmittance of 91.5%, a haze of 0.2%, a pencil hardness of 4H, interference fringes of ×, cracks in the bent portion of hot press molding processability of ×, and springback of hot press molding processability of 0.
[0428] Comparative Example 11 [Manufacture of resin laminate (L-11)]
[0429] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-4) of the resin laminate (I-11) obtained in Comparative Example 11B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-11). The film thickness of the hard coat layer (J-1) was 6 μm.
[0430] The resin laminate (L-11) had a total light transmittance of 91.5%, a haze of 0.2%, a pencil hardness of 4H, interference fringes of ×, cracks in the bent portion of hot press molding processability of ×, and springback of hot press molding processability of 0.
[0431] Comparative Example 12 [Manufacture of resin laminate (L-12)]
[0432] The same coating as in Example 1 was applied to one side of the thermoplastic resin (F-4) of the resin laminate (I-12) obtained in Comparative Example 12B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-12). The film thickness of the hard coat layer (J-1) was 6 μm.
[0433] The resin laminate (L-12) had a total light transmittance of 91.5%, a haze of 0.2%, a pencil hardness of 4H, interference fringes of ×, cracks in the bent portion of hot press molding processability of ×, and springback of hot press molding processability of 0.
[0434] Comparative Example 13〔Manufacturing of resin laminate (L-13)〕
[0435] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-5) of the resin laminate (I-13) obtained in Comparative Example 13B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-13). The film thickness of the hard coat layer (J-1) was 6 μm.
[0436] The resin laminate (L-13) had a total light transmittance of 90.5%, a haze of 0.6%, a pencil hardness of H, interference fringes of 0, cracks in a bent portion of hot press molding processability of x, and springback of hot press molding processability of 0.
[0437] Comparative Example 14 [Manufacture of resin laminate (L-14)]
[0438] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-5) of the resin laminate (I-14) obtained in Comparative Example 14B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-14). The film thickness of the hard coat layer (J-1) was 6 μm.
[0439] The resin laminate (L-14) had a total light transmittance of 90.4%, a haze of 0.7%, a pencil hardness of 2H, interference fringes of 0, cracks in the bent portion of the hot press molding processability of x, and springback of the hot press molding processability of 0.
[0440] Comparative Example 15〔Manufacturing of resin laminate (L-15)〕
[0441] The same coating as in Example 1 was applied to one side of the thermoplastic resin (F-5) of the resin laminate (I-15) obtained in Comparative Example 15B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-15). The film thickness of the hard coat layer (J-1) was 6 μm.
[0442] The resin laminate (L-15) had a total light transmittance of 90.4%, a haze of 0.7%, a pencil hardness of H, interference fringes of 0, cracks in a bent portion of hot press molding processability of ×, and springback of hot press molding processability of 0.
[0443] Comparative Example 16 [Manufacture of resin laminate (L-16)]
[0444] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (B-1) of the resin laminate (I-16) obtained in Comparative Example 16B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-16). The film thickness of the hard coat layer (J-1) was 6 μm.
[0445] The resin laminate (L-16) had a total light transmittance of 90.8%, a haze of 0.3%, a pencil hardness of 3H, interference fringes of 0, cracks in a bent portion of hot press molding processability of 0, and springback of hot press molding processability of ×.
[0446] Comparative Example 17 [Manufacture of resin laminate (L-17)]
[0447] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (B-1) of the resin laminate (I-17) obtained in Comparative Example 17B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-17). The film thickness of the hard coat layer (J-1) was 6 μm.
[0448] The resin laminate (L-17) had a total light transmittance of 90.8%, a haze of 0.5%, a pencil hardness of 3H, interference fringes of 0, cracks in a bent portion of hot press molding processability of 0, and springback of hot press molding processability of ×.
[0449] Comparative Example 18 [Manufacture of resin laminate (L-18)]
[0450] The same coating as in Example 1 was applied to one side of the thermoplastic resin (B-1) of the resin laminate (I-18) obtained in Comparative Example 18B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-18). The film thickness of the hard coat layer (J-1) was 6 μm.
[0451] The resin laminate (L-18) had a total light transmittance of 90.8%, a haze of 0.5%, a pencil hardness of 3H, interference fringes of 0, cracks in a bent portion of hot press molding processability of 0, and springback of hot press molding processability of ×.
[0452] Comparative Example 19 [Manufacture of resin laminate (L-19)]
[0453] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (B-2) of the resin laminate (I-19) obtained in Comparative Example 19B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-19). The film thickness of the hard coat layer (J-1) was 6 μm.
[0454] The resin laminate (L-19) had a total light transmittance of 90.6%, a haze of 0.5%, a pencil hardness of 2H, interference fringes of 0, cracks in a bent portion of hot press molding processability of 0, and springback of hot press molding processability of ×.
[0455] Comparative Example 20〔Manufacture of resin laminate (L-20)〕
[0456] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (B-2) of the resin laminate (I-20) obtained in Comparative Example 20B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-20). The film thickness of the hard coat layer (J-1) was 6 μm.
[0457] The resin laminate (L-20) had a total light transmittance of 90.4%, a haze of 0.6%, a pencil hardness of 3H, interference fringes of 0, cracks in a bent portion of hot press molding processability of 0, and springback of hot press molding processability of ×.
[0458] Comparative Example 21 [Manufacture of resin laminate (L-21)]
[0459] The same coating as in Example 1 was applied to one side of the thermoplastic resin (B-2) of the resin laminate (I-21) obtained in Comparative Example 21B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-21). The film thickness of the hard coat layer (J-1) was 6 μm.
[0460] The resin laminate (L-21) had a total light transmittance of 90.4%, a haze of 0.6%, a pencil hardness of 2H, interference fringes of 0, cracks in a bent portion of hot press molding processability of 0, and springback of hot press molding processability of ×.
[0461] Comparative Example 22〔Manufacturing of resin laminate (L-22)〕
[0462] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (B-3) of the resin laminate (I-22) obtained in Comparative Example 22B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-22). The film thickness of the hard coat layer (J-1) was 6 μm.
[0463] The resin laminate (L-22) had a total light transmittance of 90.8%, a haze of 0.3%, a pencil hardness of 3H, interference fringes of 0, cracks in a bent portion of hot press molding processability of 0, and springback of hot press molding processability of ×.
[0464] Comparative Example 23〔Manufacturing of resin laminate (L-23)〕
[0465] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (B-3) of the resin laminate (I-23) obtained in Comparative Example 23B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-23). The film thickness of the hard coat layer (J-1) was 6 μm.
[0466] The resin laminate (L-23) had a total light transmittance of 90.8%, a haze of 0.5%, a pencil hardness of 3H, interference fringes of 0, cracks in a bent portion of hot press molding processability of 0, and springback of hot press molding processability of ×.
[0467] Comparative Example 24 [Manufacture of resin laminate (L-24)]
[0468] The same coating as in Example 1 was applied to one side of the thermoplastic resin (B-3) of the resin laminate (I-24) obtained in Comparative Example 24B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-24). The film thickness of the hard coat layer (J-1) was 6 μm.
[0469] The resin laminate (L-24) had a total light transmittance of 90.8%, a haze of 0.5%, a pencil hardness of 3H, interference fringes of 0, cracks in a bent portion of hot press molding processability of 0, and springback of hot press molding processability of ×.
[0470] Comparative Example 25〔Manufacture of resin laminate (L-25)〕
[0471] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (B-4) of the resin laminate (I-25) obtained in Comparative Example 25B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-25). The film thickness of the hard coat layer (J-1) was 6 μm.
[0472] The resin laminate (L-25) had a total light transmittance of 90.6%, a haze of 0.5%, a pencil hardness of 2H, interference fringes of 0, cracks in a bent portion of hot press molding processability of 0, and springback of hot press molding processability of ×.
[0473] Comparative Example 26 [Manufacture of resin laminate (L-26)]
[0474] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (B-4) of the resin laminate (I-26) obtained in Comparative Example 26B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-26). The film thickness of the hard coat layer (J-1) was 6 μm.
[0475] The resin laminate (L-26) had a total light transmittance of 90.4%, a haze of 0.6%, a pencil hardness of 3H, interference fringes of 0, cracks in the bending portion of the hot press molding processability of 0, and springback of the hot press molding processability of ×.
[0476] Comparative Example 27 [Manufacture of resin laminate (L-27)]
[0477] The same coating as in Example 1 was applied to one side of the thermoplastic resin (B-4) of the resin laminate (I-27) obtained in Comparative Example 27B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-27). The film thickness of the hard coat layer (J-1) was 6 μm.
[0478] The resin laminate (L-27) had a total light transmittance of 90.4%, a haze of 0.6%, a pencil hardness of 2H, interference fringes of 0, cracks in the bent portion of the hot press molding processability of 0, and springback of the hot press molding processability of ×.
[0479] Comparative Example 28 [Manufacture of resin laminate (L-28)]
[0480] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-1) of the resin laminate (I-28) obtained in Comparative Example 28B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-28). The film thickness of the hard coat layer (J-1) was 6 μm.
[0481] The resin laminate (L-28) had a total light transmittance of 91.1%, a haze of 0.5%, a pencil hardness of 3H, interference fringes of 0, cracks in a bent portion of hot press molding processability of ×, and springback of hot press molding processability of ×.
[0482] Comparative Example 29 [Manufacture of resin laminate (L-29)]
[0483] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-1) of the resin laminate (I-29) obtained in Comparative Example 29B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-29). The film thickness of the hard coat layer (J-1) was 6 μm.
[0484] The resin laminate (L-29) had a total light transmittance of 91.0%, a haze of 0.6%, a pencil hardness of 4H, interference fringes of 0, cracks in a bent portion of hot press molding processability of ×, and springback of hot press molding processability of ×.
[0485] Comparative Example 30〔Manufacturing of resin laminate (L-30)〕
[0486] The same coating as in Example 1 was applied to one side of the thermoplastic resin (F-1) of the resin laminate (I-30) obtained in Comparative Example 30B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-30). The film thickness of the hard coat layer (J-1) was 6 μm.
[0487] The resin laminate (L-30) had a total light transmittance of 91.0%, a haze of 0.6%, a pencil hardness of 3H, interference fringes of 0, cracks in a bent portion of hot press molding processability of ×, and springback of hot press molding processability of ×.
[0488] Comparative Example 31〔Manufacture of resin laminate (L-31)〕
[0489] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-2) of the resin laminate (I-31) obtained in Comparative Example 31B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-31). The film thickness of the hard coat layer (J-1) was 6 μm.
[0490] The resin laminate (L-31) had a total light transmittance of 91.1%, a haze of 0.5%, a pencil hardness of 3H, interference fringes of 0, cracks in a bent portion of hot press molding processability of ×, and springback of hot press molding processability of ×.
[0491] Comparative Example 32〔Manufacturing of resin laminate (L-32)〕
[0492] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-2) of the resin laminate (I-32) obtained in Comparative Example 32B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-32). The film thickness of the hard coat layer (J-1) was 6 μm.
[0493] The resin laminate (L-32) had a total light transmittance of 91.0%, a haze of 0.6%, a pencil hardness of 4H, interference fringes of 0, cracks in a bent portion of hot press molding processability of ×, and springback of hot press molding processability of ×.
[0494] Comparative Example 33〔Manufacturing of resin laminate (L-33)〕
[0495] The same coating as in Example 1 was applied to one side of the thermoplastic resin (F-2) of the resin laminate (I-33) obtained in Comparative Example 33B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-33). The film thickness of the hard coat layer (J-1) was 6 μm.
[0496] The resin laminate (L-33) had a total light transmittance of 91.0%, a haze of 0.6%, a pencil hardness of 3H, interference fringes of 0, cracks in a bent portion of hot press molding processability of ×, and springback of hot press molding processability of ×.
[0497] Comparative Example 34 [Manufacture of resin laminate (L-34)]
[0498] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-3) of the resin laminate (I-34) obtained in Comparative Example 34B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-34). The film thickness of the hard coat layer (J-1) was 6 μm.
[0499] The resin laminate (L-34) had a total light transmittance of 91.5%, a haze of 0.2%, a pencil hardness of 4H, interference fringes of ×, cracks in a bent portion of hot press molding processability of ×, and springback of hot press molding processability of ×.
[0500] Comparative Example 35〔Manufacturing of resin laminate (L-35)〕
[0501] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-3) of the resin laminate (I-35) obtained in Comparative Example 35B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-35). The film thickness of the hard coat layer (J-1) was 6 μm.
[0502] The resin laminate (L-35) had a total light transmittance of 91.5%, a haze of 0.2%, a pencil hardness of 4H, interference fringes of ×, cracks in a bent portion of hot press molding processability of ×, and springback of hot press molding processability of ×.
[0503] Comparative Example 36 [Manufacture of resin laminate (L-36)]
[0504] The same coating as in Example 1 was applied to one side of the thermoplastic resin (F-3) of the resin laminate (I-36) obtained in Comparative Example 36B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-36). The film thickness of the hard coat layer (J-1) was 6 μm.
[0505] The resin laminate (L-36) had a total light transmittance of 91.5%, a haze of 0.2%, a pencil hardness of 4H, interference fringes of ×, cracks in the bending portion of hot press molding processability of ×, and springback of hot press molding processability of ×.
[0506] Comparative Example 37〔Manufacturing of resin laminate (L-37)〕
[0507] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-4) of the resin laminate (I-37) obtained in Comparative Example 37B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-37). The film thickness of the hard coat layer (J-1) was 6 μm.
[0508] The resin laminate (L-37) had a total light transmittance of 91.5%, a haze of 0.2%, a pencil hardness of 4H, interference fringes of ×, cracks in the bending portion of hot press molding processability of ×, and springback of hot press molding processability of ×.
[0509] Comparative Example 38 [Manufacture of resin laminate (L-38)]
[0510] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-4) of the resin laminate (I-38) obtained in Comparative Example 38B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-38). The film thickness of the hard coat layer (J-1) was 6 μm.
[0511] The resin laminate (L-38) had a total light transmittance of 91.5%, a haze of 0.2%, a pencil hardness of 4H, interference fringes of ×, cracks in a bent portion of hot press molding processability of ×, and springback of hot press molding processability of ×.
[0512] Comparative Example 39〔Manufacturing of resin laminate (L-39)〕
[0513] The same coating as in Example 1 was applied to one side of the thermoplastic resin (F-4) of the resin laminate (I-39) obtained in Comparative Example 39B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-39). The film thickness of the hard coat layer (J-1) was 6 μm.
[0514] The resin laminate (L-39) had a total light transmittance of 91.5%, a haze of 0.2%, a pencil hardness of 4H, interference fringes of ×, cracks in the bending portion of hot press molding processability of ×, and springback of hot press molding processability of ×.
[0515] Comparative Example 40 [Manufacture of resin laminate (L-40)]
[0516] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-5) of the resin laminate (I-40) obtained in Comparative Example 40B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-40). The film thickness of the hard coat layer (J-1) was 6 μm.
[0517] The resin laminate (L-40) had a total light transmittance of 90.5%, a haze of 0.6%, a pencil hardness of H, interference fringes of 0, cracks in a bent portion of hot press molding processability of ×, and springback of hot press molding processability of ×.
[0518] Comparative Example 41 [Manufacture of resin laminate (L-41)]
[0519] The same coating as in Example 1 was applied to the surface of the thermoplastic resin (F-5) of the resin laminate (I-41) obtained in Comparative Example 41B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-41). The film thickness of the hard coat layer (J-1) was 6 μm.
[0520] The resin laminate (L-41) had a total light transmittance of 90.4%, a haze of 0.7%, a pencil hardness of 2H, interference fringes of 0, cracks in a bent portion of hot press molding processability of ×, and springback of hot press molding processability of ×.
[0521] Comparative Example 42〔Manufacture of resin laminate (L-42)〕
[0522] The same coating as in Example 1 was applied to one side of the thermoplastic resin (F-5) of the resin laminate (I-42) obtained in Comparative Example 42B using a bar coater, and the hard coat layer was cured in the same manner as in Example 1 to produce a resin laminate (L-42). The film thickness of the hard coat layer (J-1) was 6 μm.
[0523] The resin laminate (L-42) had a total light transmittance of 90.4%, a haze of 0.7%, a pencil hardness of H, interference fringes of 0, cracks in a bent portion of hot press molding processability of ×, and springback of hot press molding processability of ×.
[0524] [Table 4]
[0525] Table 4
[0526]
[0527] As described above, by satisfying the conditions of the present invention, there is obtained the advantageous effect of being able to obtain a resin laminate having excellent thermoformability at low temperatures, suppressed generation of interference fringes and a good appearance.
[0528] That is, as shown in Table 2, when comparing Production Examples 1A to 4A in which a methacrylic resin (C) and a specific styrene copolymer (D) were blended into a pelletized thermoplastic resin (B) with Production Comparative Examples 3A to 4A in which only the methacrylic resin (C) was used, the refractive index of Production Examples 1A to 4A was higher.
[0529] In comparison between Production Examples 1A to 4A and Comparative Production Examples 6A to 9A in which a styrene copolymer (E) other than the methacrylic resin (C) and the specific styrene copolymer (D) was blended, Production Examples 1A to 4A were transparent and had good appearance.
[0530] As shown in Table 3, regarding the resin laminate before hard coating, the interference fringes of the resin laminates of Manufacturing Examples 1B to 12B, which are obtained by laminating a thermoplastic resin (B) and a specific polycarbonate resin (A) after blending and pelletizing a methacrylic resin (C) having a high refractive index and a specific styrene copolymer (D), and Manufacturing Comparative Examples 7B to 12B, which are obtained by laminating a thermoplastic resin after pelletizing the methacrylic resin (C) alone and a specific polycarbonate resin (A), are good.
[0531] In addition, when compared with manufacturing examples 1B to 12B and manufacturing comparison examples 13B to 15B in which a thermoplastic resin obtained by pelletizing a specific styrene copolymer (D) and a specific polycarbonate resin (A) are laminated separately, the resin laminates of manufacturing examples 1B to 12B suppress cracks in the bent portion during hot press molding.
[0532] Furthermore, when manufacturing examples 1B to 12B are compared with manufacturing comparative examples 16B to 42B in which a polycarbonate resin (G) other than the specific polycarbonate resin (A) is laminated, the resin laminates of manufacturing examples 1B to 12B suppress springback during hot press molding.
[0533] As shown in Table 4, regarding the resin laminate after hard coating, Examples 1 to 12 in which a thermoplastic resin (B) and a specific polycarbonate resin (A) were laminated after blending and pelletizing a methacrylic resin (C) and a specific styrene copolymer (D), and a hard coating layer was provided on one side of the thermoplastic resin (B) were compared with Comparative Examples 7 to 12 in which a thermoplastic resin (A) and a specific polycarbonate resin (A) were laminated after pelletizing a methacrylic resin (C) alone, and a hard coating layer was provided on one side of the thermoplastic resin. The resin laminates of Examples 1 to 12 had good interference fringes as before hard coating.
[0534] In addition, when comparing Examples 1 to 12 with Comparative Examples 13 to 15 in which a thermoplastic resin obtained by pelletizing a specific styrene copolymer (D) and a specific polycarbonate resin (A) are laminated separately and a hard coating layer is provided on one side of the thermoplastic resin, the resin laminates of Examples 1 to 12 suppress cracks in the bent portion during hot press molding processing, as before the hard coating.
[0535] Furthermore, when Examples 1 to 12 are compared with Comparative Examples 16 to 42 in which a polycarbonate resin (G) other than a specific polycarbonate resin (A) is laminated and a hard coating is provided on one side surface of the thermoplastic resin, the resin laminates of Examples 1 to 12 suppress springback during hot press molding processing in the same manner as before hard coating.
[0536] In addition, when Examples 1 to 12 were compared with Comparative Examples 1 to 6 in which a thermoplastic resin in which a methacrylic resin (C) and a specific styrene copolymer (D) were blended and pelletized at a ratio other than a specific ratio and a specific polycarbonate resin (A) were laminated and a hard coating layer was provided on one side of the thermoplastic resin, the resin laminates of Examples 1 to 12 suppressed cracking of the bent portion during hot press molding, unlike before the hard coating.
Claims
1. A resin laminate, Features: A layer comprising a thermoplastic resin (B) is provided on at least one surface of a layer comprising a polycarbonate-based resin (A), and a hard coating layer is provided on at least one surface of the layer comprising the thermoplastic resin (B). The polycarbonate resin (A) has a glass transition temperature of 115° C. or higher and lower than 130° C., The difference between the glass transition temperature of the polycarbonate resin (A) and the glass transition temperature of the thermoplastic resin (B) is in the range of 0 to 15° C., The thermoplastic resin (B) contains a methacrylic resin (C) and a styrene copolymer (D), wherein the content of the methacrylic resin (C) is 15 to 60 parts by mass, and the content of the styrene copolymer (D) is 85 to 40 parts by mass, based on 100 parts by mass of the total content of the methacrylic resin (C) and the styrene copolymer (D). The styrene copolymer (D) is a copolymer consisting of only 68 to 84 mass % of styrene and 16 to 32 mass % of maleic anhydride. The hard coating layer is an acrylic hard coating layer.
2. The resin laminate according to claim 1, Features: The thermoplastic resin (B) consists only of the methacrylic resin (C) and the styrene copolymer (D).
3. The resin laminate according to claim 1 or 2, Features: No cracks were generated after 50 mmR hot forming using a hot press.
4. The resin laminate according to claim 1 or 2, Features: No springback occurs after 50mmR thermoforming using a hot press.
5. The resin laminate according to claim 1 or 2, Features: The thermoplastic resin (B) is a polymer alloy of a methacrylic resin (C) and a styrene copolymer (D).
6. The resin laminate according to claim 1 or 2, Features: The polycarbonate resin (A) has a terminal structure derived from a monohydric phenol represented by the following general formula (1) and a structural unit derived from a dihydric phenol. In the formula, R 1 represents an alkyl group having 8 to 36 carbon atoms or an alkenyl group having 8 to 36 carbon atoms, R 2 ~R 5 Each of them represents hydrogen, halogen, or an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 12 carbon atoms which may have a substituent, and the substituent is halogen, an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 12 carbon atoms.
7. The resin laminate according to claim 1 or 2, Features: The thickness of the layer containing the thermoplastic resin (B) is in the range of 10 to 250 μm, and the thickness of the entire resin laminate is in the range of 0.4 to 4.0 mm.
8. The resin laminate according to claim 1 or 2, Features: At least one of the layer containing the polycarbonate-based resin (A), the layer containing the thermoplastic resin (B), and the hard coat layer contains a UV absorber.
9. The resin laminate according to claim 1 or 2, Features: One or both sides of the resin laminate are subjected to at least one of anti-fingerprint treatment, anti-reflection treatment, anti-glare treatment, weather resistance treatment, antistatic treatment and antifouling treatment.
10. A thermoformed body, Features: The resin laminate according to any one of claims 1 to 9 is formed by heat bending.
11. A transparent substrate material, Features: The present invention comprises the resin laminate according to any one of claims 1 to 9 or the thermoformed body according to claim 10.
12. A transparent protective material, Features: The present invention comprises the resin laminate according to any one of claims 1 to 9 or the thermoformed body according to claim 10.
13. A touch panel front protection plate, Features: The present invention comprises the resin laminate according to any one of claims 1 to 9 or the thermoformed body according to claim 10.
14. A front panel for car navigation, OA equipment or portable electronic equipment, Features: The present invention comprises the resin laminate according to any one of claims 1 to 9 or the thermoformed body according to claim 10.
Citation Information
Patent Citations
Polycarbonate resin composition for light diffusion plate and light diffusion plate
JP2007179018A
Synthetic resin laminated sheet
WO2016060100A1
Process for producing extruded resin sheet, and extruded resin sheet
CN106715078A
Magneto-optic disc substrate
JP2000153535A
Polycarbonate resin laminate sheet for punching and its manufacturing method
JP2008049623A