Nano-silver particle anchored plant fiber water purification composite material and preparation method and water purification device thereof
By loading nanosilver particles on plant fibers, forming nanosilver particles anchoring plant fiber water purification composite materials, the problem that existing water purification materials are prone to breed bacteria is solved, efficient sewage purification and toxic organic compounds are achieved, and significantly improved the The purification capacity of the water purification device.
Patent Information
- Application Number
- CN202211178435.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-26
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-09-26
AI Technical Summary
The water purification materials in existing water purification devices are prone to breed bacteria, leading to water pollution and health risks, and it is difficult to effectively remove toxic organic compounds in sewage.
By loading nanosilver particles on plant fibers, nanosilver particles anchor plant fiber water purification composite material is formed, and silver ions are activated in situ reduction into nanosilver particles using the hydrophilicity and antioxidant substances of plant fibers, and an antibacterial and Composite materials with efficient purification capabilities.
Effective control of bacteria in sewage is achieved, and the oil-water separation efficiency and adsorption capacity of toxic organic compounds are significantly improved. The purification effect is 99.95% dye removal rate and 99.89% polystyrene microsphere removal rate.
Smart Images

Figure CN115487783B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite material preparation, and more specifically, to a method for preparing a multifunctional composite material by using Caragana korshinskii and nano-silver particles through green chemistry, and belongs to the field of biomass resource utilization and sewage purification materials. Background Art
[0002] Drought and water shortage are prominent problems in my country's northern border and western regions. Purifying and recycling sewage is particularly important for the security of water resource supply and the sustainable development of the economy and society.
[0003] In the prior art, a water purification device includes a filter column and a water purification material filled in the filter column. Since sewage contains a large amount of organic compounds, the water purification material is prone to breed bacteria, which is not only harmful to water quality but also harmful to human health. Summary of the invention
[0004] The purpose of the present invention is to overcome the above-mentioned defects of the prior art and provide a nanosilver particle anchored plant fiber water purification composite material and its preparation method and water purification device, and by loading nanosilver particles on plant fibers, the water purification material has an antibacterial effect.
[0005] To achieve the above object, the technical solution of the present invention is as follows:
[0006] A nano-silver particle anchored plant fiber water purification composite material comprises plant fiber powder and nano-silver particles loaded on the plant fiber powder, wherein the fiber length of the plant fiber powder is 100-600 μm, and the particle size of the nano-silver particles is 3-5 nm.
[0007] The present invention also discloses a method for preparing the nano-silver particle anchored plant fiber water purification composite material, which comprises the following steps:
[0008] grinding the dried plant fiber into plant fiber powder;
[0009] Dissolving silver salt to obtain a silver ion solution, and mixing the plant fiber powder and the silver ion solution to obtain a mixed solution;
[0010] The mixed solution is heated to reduce the silver ions adsorbed on the plant fiber powder to nano-silver particles, thereby obtaining the nano-silver particle-anchored plant fiber water purification composite material.
[0011] The invention also discloses a water purification device, comprising a filter column and the above-mentioned nano-silver particle anchored plant fiber water purification composite material filled in the filter column.
[0012] Implementing the embodiments of the present invention will have the following beneficial effects:
[0013] The water purification composite material of the embodiment of the present invention uses plant fiber as a substrate. The fiber structure of the plant fiber has natural hydrophilicity, adsorption and degradability, and can be used for oil-water separation and adsorption of toxic organic compounds in sewage. The loaded nanosilver particles (AgNPs) are currently the most promising environmental bactericide, which makes the plant fiber substrate have antibacterial properties and avoids the growth of bacteria to pollute the water quality.
[0014] The mutual adsorption between nanosilver particles and plant fibers, on the one hand, the plant fibers adsorb nanosilver particles and realize the regulation of the release rate of nanosilver particles, thereby protecting the nanosilver particles from being rapidly oxidized and losing their antibacterial functions; on the other hand, the plant fibers can also act as a protective agent to adjust the size of nanosilver particles, thereby improving the antibacterial activity of nanosilver particles.
[0015] In addition, the size of the nanosilver particles and plant fibers makes the plant fibers loaded with nanosilver particles more hydrophilic, which can significantly improve the oil-water separation efficiency of the plant fibers and the adsorption capacity for dyes and toxic organic compounds, achieving unexpected and significant sewage purification capabilities.
[0016] The preparation method of the present invention uses a heating method to activate the antioxidant substances in the plant fiber, and reduces the silver ions adsorbed on the surface of the plant fiber to nano silver particles in situ. During the entire preparation process, no organic reducing agent and surfactant are required. It is not only a green preparation method, but also the obtained product is a green product without adding toxic reagents. It can be directly used in a water purification device, and there is no need to purify the final purified composite material.
[0017] The water purification device of the present invention can completely separate oil droplets in water-in-oil emulsion, and the removal rate of dyes can be as high as 99.95%, and the removal rate of polystyrene microspheres can be as high as 99.89%. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] in:
[0020] Figure 1 This is a digital photo of the dried and peeled Caragana korshinskii branches obtained in Example 1.
[0021] Figure 2 This is a digital photo of the dried Caragana korshinskii powder obtained in Example 1.
[0022] Figure 3 This is a digital photo of the nanosilver particle loaded Caragana korshinskii fiber powder obtained in Example 1.
[0023] Figure 4 The scanning electron microscope photograph and transmission electron microscope photograph of the nano-silver particle loaded Caragana korshinskii fiber composite material obtained in Example 1 are shown.
[0024] Figure 5 This is the C, O and Ag element mapping observation of the nanosilver particle loaded Caragana korshinskii fiber composite material obtained in Example 1.
[0025] Figure 6 This is an energy dispersive x-ray spectrum (EDX) diagram of the nano-silver particle-loaded Caragana korshinskii fiber composite material obtained in Example 1.
[0026] Figure 7 The photos are of the water wettability test of the dried Caragana korshinskii powder and the Caragana korshinskii fiber composite material loaded with nano-silver particles obtained in Example 1, wherein a is the Caragana korshinskii powder, and b is the Caragana korshinskii powder composite material loaded with nano-silver particles.
[0027] Figure 8a Microscopic photographs of various oil-in-water emulsions.
[0028] Figure 8b for Figure 8a The microscopic photograph of the reclaimed water after the oil-in-water emulsion was filtered through the nanosilver particle-loaded Caragana korshinskii powder composite material obtained in Example 1.
[0029] Fig. 9 This is a digital photo of the process of separating the water-in-oil emulsion of the nano-silver particle-loaded Caragana korshinskii powder composite material obtained in Example 1.
[0030] Fig.10 These are digital photos of the nano-silver particle-loaded Caragana korshinskii powder composite material obtained in Example 1 before and after adsorption of 50 mg / L methylene blue solution.
[0031] Fig.11 This is a digital photo of the filtration separation process of the nano-silver particle-loaded Caragana korshinskii powder composite material obtained in Example 1 on a 10 mg / L polystyrene microsphere solution. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The invention discloses a nano-silver particle anchored plant fiber water purification composite material, comprising plant fiber powder and nano-silver particles loaded on the plant fiber powder, the fiber length of the plant fiber powder is 100-600 μm, and the particle size of the nano-silver particles is 3-5 nm.
[0034] The water purification composite material of the present invention uses plant fiber as a substrate. The fiber structure of the plant fiber has natural hydrophilicity, adsorption and degradability, and can be used for oil-water separation and adsorption of toxic organic compounds in sewage. The loaded nano silver particles (AgNPs) are currently the most promising environmental bactericide, which makes the plant fiber substrate have antibacterial properties and avoids the breeding of bacteria to pollute water quality.
[0035] The mutual adsorption between nanosilver particles and plant fibers, on the one hand, the plant fibers adsorb nanosilver particles and realize the regulation of the release rate of nanosilver particles, thereby protecting the nanosilver particles from being rapidly oxidized and losing their antibacterial functions; on the other hand, the plant fibers can also act as a protective agent to adjust the size of nanosilver particles, thereby improving the antibacterial activity of nanosilver particles.
[0036] In addition, the size of the nanosilver particles and plant fibers makes the plant fibers loaded with nanosilver particles more hydrophilic, which can significantly improve the oil-water separation efficiency of the plant fibers and the adsorption capacity for dyes and toxic organic compounds, achieving unexpected and significant sewage purification capabilities.
[0037] In a specific embodiment, the plant fiber powder is the powder of Caragana korshinskii after the dried peeled Caragana korshinskii branches are ground into powder. Studies have shown that the fiber of Caragana korshinskii contains a large amount of substances such as polysaccharides, polyphenols and flavonoids, and has good anti-oxidation functions. Moreover, its cellulose content is relatively high, and the comprehensive cellulose content reaches 72.71%. The rich cellulose structure makes Caragana korshinskii powder not only have good adsorption, can be used as a carrier of nano silver particles, but also has good natural hydrophilicity, can be used for oil-water separation and adsorption of toxic organic compounds in sewage. At present, Caragana korshinskii is a kind of deciduous shrub widely planted in the western region, which is characterized by strong vitality, extremely strong cold resistance, high temperature resistance, drought resistance, and resistance to barrenness, strong sprouting and regeneration ability, long life cycle, and an average annual growth of 67 cm in sandy loam with a water content of 4.08%, so it is an excellent shrub for windbreak and sand fixation, soil and water conservation, and ecological environment improvement. In recent years, the western and northern regions have continuously strengthened the scale of ecological restoration and greening, and the planting area of Caragana korshinskii has gradually expanded. In the Inner Mongolia Autonomous Region alone, the planting area of Caragana korshinskii has developed to more than 30 million mu, and the annual output of Caragana korshinskii biomass branches exceeds 10 million tons. However, at present, Caragana korshinskii biomass resources are usually directly incinerated or discarded after simple treatment, and a small part is used in low-value industries such as oil refining and free-range grazing feed. The low utilization rate of these plant wastes not only causes environmental pollution problems, but also is a waste of resources. Therefore, converting Caragana korshinskii directly into ecological and environmental materials without burning can not only expand new ways of processing and utilizing Caragana korshinskii resources, but also avoid environmental pollution caused by traditional utilization methods.
[0038] The present invention also discloses a method for preparing the nano-silver particle anchored plant fiber water purification composite material, which is characterized by comprising the following steps:
[0039] 1) Grind the dried plant fiber into plant fiber powder.
[0040] In the present invention, nanosilver particles are loaded on plant fiber powder. On the one hand, the utilization rate of biomass resources of plant fiber is improved. On the other hand, plant fiber contains antioxidant substances such as polysaccharides, polyphenols, flavonoids, etc. Under heating conditions, the above antioxidant substances can be activated, thereby reducing the silver ions adsorbed on the surface of the plant fiber powder to nanosilver particles (AgNPs) in situ. The reduction does not require any organic reducing agent and surfactant. It is not only a green preparation method, but also the obtained product is a green product without the addition of toxic reagents. It can be directly used in a water purification device, and there is no need to purify the final product.
[0041] In a preferred embodiment, the fiber length of the plant fiber powder is 100 μm to 600 μm, which has a large adsorption surface area and provides a larger surface energy, which not only facilitates the smooth progress of the reduction reaction, but also can obtain smaller nano-silver particles. The smaller the particle size of the nano-silver particles, the stronger its antibacterial ability. The particle size of the prepared nano-silver particles is 3nm to 5nm, which is smaller and has stronger antibacterial activity.
[0042] 2) dissolving silver salt to obtain a silver ion solution, and mixing the plant fiber powder and the silver ion solution to obtain a mixed solution.
[0043] The silver salt may be selected from at least one of silver nitrate, silver sulfate, silver chloride, silver acetate, and silver stearate.
[0044] In this step, the plant fiber powder is mixed to be fully dispersed in the silver ion solution, and the silver ions are uniformly adsorbed on the surface of the plant fiber powder.
[0045] The mixing method may include one or two or more of shaking, magnetic stirring, mechanical stirring, ultrasound and microwave assistance.
[0046] 3) The mixed solution is heated to reduce the silver ions adsorbed on the plant fiber powder to nano-silver particles, thereby obtaining a nano-silver particle-anchored plant fiber water purification composite material.
[0047] In this step, the antioxidant substances in the plant fiber are activated by heating to reduce the loaded silver ions. In a preferred embodiment, the heating temperature is 80°C to 120°C and the heating time is 2h to 8h, so that evenly distributed nano silver particles with smaller particle size can be obtained.
[0048] The preparation method of the present invention uses a heating method to activate the antioxidant substances in the plant fiber, and reduces the silver ions adsorbed on the surface of the plant fiber to nano silver particles in situ. During the entire preparation process, no organic reducing agent and surfactant are required. It is not only a green preparation method, but also the obtained product is a green product without adding toxic reagents. It can be directly used in a water purification device, and there is no need to purify the final purified composite material.
[0049] In a specific embodiment, the mass concentration of the silver salt in the silver ion solution is 0.1wt% to 5wt%, so that the generated nano-silver particles have an appropriate particle size range and sufficient loading amount. If the silver ion concentration is too high, it will not only waste raw materials, but also cause the nano-silver particles to agglomerate, which will reduce the activity of the nano-silver particles.
[0050] Preferably, the mass concentration of the silver salt in the silver ion solution is 1wt% to 5wt%. If the silver ion concentration is too low, the antibacterial effect is not obvious, and the wettability of the substrate plant fiber powder is not significantly improved.
[0051] In a specific embodiment, the mass of the silver salt in the mixed solution is 1% to 10% of the mass of the plant fiber powder.
[0052] The invention also discloses a water purification device, comprising a filter column and the nano silver particle anchored plant fiber water purification composite material filled in the filter column.
[0053] In a specific embodiment, the filling height of the nanosilver particle anchored plant fiber water purification composite material in the filter column is 2 cm to 5 cm.
[0054] Subsequent test data proved that the water purification device can completely separate the oil droplets in the water-in-oil emulsion, with a dye removal rate of up to 99.95% and a polystyrene microsphere removal rate of up to 99.89%.
[0055] The following are specific embodiments.
[0056] Example 1
[0057] 1) Peel the fresh Caragana korshinskii branches and dry them in an oven at 50°C to 90°C for 12h to 96h or air-dry them in a natural environment to prepare dried Caragana korshinskii branches, such as Figure 1 shown.
[0058] 2) Roller grinding, crushing, grinding, drying and sieving the dried Caragana korshinskii branches to obtain Caragana korshinskii dry powder, and sieving the Caragana korshinskii dry powder to obtain Caragana korshinskii dry powder with a fiber length of less than 600 μm, such as Figure 2 As shown;
[0059] 3) Dispersing 10 g of the obtained Caragana korshinskii dry powder into 0.1 L of a 1 wt % silver nitrate solution, placing the mixture in a tetrafluoroethylene reaction tank, stirring the mixture evenly by magnetic force, activating the mixture at 80° C. for 8 h, cooling the mixture naturally to room temperature, washing and drying the mixture, and obtaining Caragana korshinskii fibers loaded with nanosilver, such as Figure 3 As shown, the number is CK / Ag~1.
[0060] Example 2
[0061] 1) obtaining Caragana korshinskii dry powder by the same method as in Example 1, and sieving the Caragana korshinskii dry powder to obtain Caragana korshinskii dry powder having a fiber length of less than 250 μm;
[0062] 2) 100 g of the obtained Caragana korshinskii dry powder was dispersed into 0.15 L of a 2 wt% silver sulfate solution, placed in a tetrafluoroethylene reaction tank, and uniformly stirred by mechanical stirring. The mixture was activated at 120° C. for 2 h, naturally cooled to room temperature, washed and dried to obtain nanosilver-loaded Caragana korshinskii fibers, which were numbered CK / Ag~2.
[0063] Example 3
[0064] 1) obtaining Caragana korshinskii dry powder by the same method as in Example 1, and sieving the Caragana korshinskii dry powder to obtain Caragana korshinskii dry powder having a fiber length of less than 100 μm;
[0065] 2) 200 g of the obtained Caragana korshinskii dry powder was dispersed into 0.2 L of 3 wt % silver stearate solution, placed in a tetrafluoroethylene reaction tank, and uniformly stirred by mechanical stirring. The mixture was activated at 110° C. for 7 h, naturally cooled to room temperature, washed and dried to obtain nanosilver-loaded Caragana korshinskii fibers, which were numbered CK / Ag~3.
[0066] Example 4
[0067] 1) obtaining Caragana korshinskii dry powder by the same method as in Example 1, and sieving the Caragana korshinskii dry powder to obtain Caragana korshinskii dry powder having a fiber length of less than 600 μm;
[0068] 2) 60 g of the obtained Caragana korshinskii dry powder was dispersed in 0.15 L of 4 wt% silver nitrate solution, placed in a tetrafluoroethylene reaction tank, and uniformly stirred by mechanical stirring. The mixture was activated at 80° C. for 8 h, naturally cooled to room temperature, washed and dried to obtain nanosilver-loaded Caragana korshinskii fibers, which were numbered CK / Ag~4.
[0069] Example 5
[0070] 1) obtaining Caragana korshinskii dry powder by the same method as in Example 1, and sieving the Caragana korshinskii dry powder to obtain Caragana korshinskii dry powder having a fiber length of less than 150 μm;
[0071] 2) 500 g of the obtained Caragana korshinskii dry powder was dispersed in 0.1 L of a 5 wt% silver nitrate solution, placed in a tetrafluoroethylene reaction tank, and uniformly stirred by mechanical stirring. The mixture was activated at 80° C. for 8 h, naturally cooled to room temperature, washed and dried to obtain nanosilver-loaded Caragana korshinskii fibers, which were numbered CK / Ag~5.
[0072] Test Case
[0073] Macroscopic morphology observation
[0074] refer to Figure 1 to Figure 3 It can be seen that after being loaded with nanosilver particles, the color of the Caragana korshinskii fiber has changed significantly, from light yellow to reddish brown.
[0075] Microscopic morphology observation
[0076] The nano-silver loaded Caragana korshinskii composite material obtained in Example 1 was observed in microscopic form. Figure 4 As shown by Figure 4The scanning electron microscope and transmission electron microscope photos verified the in-situ formation of nanosilver particles on the surface of Caragana korshinskii fiber. It can be clearly observed that Caragana korshinskii fiber is a hollow tubular fiber with a smooth diameter of 10nm to 20nm. Among them, the transmission electron microscope provides visible evidence for the successful loading of nanosilver particles on the fiber surface, that is, nanosilver particles can be observed. The particle size of the nanosilver particles is 3nm to 5nm. The nanosilver-loaded Caragana korshinskii composite materials obtained in Examples 2 to 5 are similar in size to the nanosilver particles obtained in Example 1.
[0077] The element distribution (mapping) of the nano-silver particle loaded caragana fiber composite material obtained in Example 1 was observed, and the Figure 5 .Depend on Figure 5 It can be observed from the element mapping that the nano-silver particles are evenly distributed on the surface of the Caragana korshinskii fiber, well dispersed, and have no obvious agglomeration phenomenon. Therefore, the nano-silver particles obtained by the method of the present invention have a smaller particle size and better bactericidal activity.
[0078] Material composition analysis
[0079] Energy dispersive X-ray spectroscopy (EDX) was performed on the nano-silver particle loaded Caragana korshinskii fiber composite material obtained in Example 1 to obtain Figure 6 .Depend on Figure 6 Energy dispersive X-ray spectroscopy (EDX) revealed that the appearance of Ag characteristic peaks also confirmed the successful implantation of silver nanoparticles.
[0080] Water Wettability Test in Air
[0081] The water wettability of the Caragana korshinskii powder and the Caragana korshinskii fiber composite material obtained in Example 1 was tested in air. The results were obtained after microscopic observation. Figure 7 .Depend on Figure 7 It can be seen that the nanosilver particle-loaded Caragana fiber composite material exhibits stronger hydrophilicity than Caragana fiber powder. The loading of nanosilver particles enables Caragana powder to achieve a huge change in surface wettability, achieving unexpected results. The super-hydrophilic composite surface can wrap a large number of water molecules, forming a dense water-containing layer on the surface of Caragana fiber, achieving the purpose of oil-water separation.
[0082] The nanosilver-loaded Caragana korshinskii composite materials obtained in Examples 2 to 5 also achieved a huge change in surface wettability.
[0083] Oil-in-water emulsion separation test
[0084] The nanosilver particle loaded Caragana korshinskii fiber composite material obtained in Example 1 was subjected to a water-in-oil waste emulsion separation test to obtain Figure 8a and Figure 8b .in, Figure 8a The water-in-oil emulsions in the figure are microscope photos of gasoline / water emulsion, soybean oil / water emulsion, kerosene / water emulsion and carbon tetrachloride / water emulsion. Figure 8b This is a microscope photo of the filtrate after the emulsion is filtered through the nanosilver particle loaded Caragana korshinskii fiber composite material prepared in Example 1. Figure 8a and Figure 8b It can be seen that the oil droplets in the reclaimed water have been completely removed. The nanosilver-loaded Caragana korshinskii composite materials obtained in Examples 2 to 5 can also achieve the same effect as Example 1.
[0085] Fig. 9 This is a digital photo of the process of filtering the water-in-oil emulsion by the composite material of Caragana korshinskii powder loaded with nano-silver particles obtained in Example 1. The water-in-oil emulsion was prepared in the laboratory, the ratio of oil to deionized water in the water-in-oil emulsion was 1:9 (v:v), and the emulsifier was 1 mol / L dodecyltrimethylammonium bromide. Fig. 9 It can be seen that the nanosilver particle-loaded Caragana korshinskii fiber composite material obtained in Example 1 has a good separation effect on the oil-in-water waste emulsion, and the oil droplets in the oil-in-water emulsion are completely removed after separation, achieving the goal of water purification.
[0086] Test for removal of organic dyes from water
[0087] The nanosilver particle loaded Caragana korshinskii fiber composite material obtained in Example 1 was subjected to a dye removal test, and the results were as follows: Fig.10 . Fig.10 The digital photos of the solution before and after the adsorption of 50 mg / L methylene blue solution by the composite material of Caragana korshinskii powder loaded with nano-silver particles obtained in Example 1. Fig.10 It can be seen that the nano-silver particle-loaded Caragana fiber composite material exhibits efficient separation performance for methylene blue solution in water. Tested by an ultraviolet spectrophotometer, the removal rate is higher than 99.95%.
[0088] The removal rates of the nano-silver-loaded Caragana korshinskii composite materials obtained in Examples 2 to 5 for 50 mg / L methylene blue solution were 99.91%, 99.92%, 99.89% and 99.88% respectively.
[0089] Removal test of polystyrene microspheres in water
[0090] The nanosilver particle loaded Caragana korshinskii fiber composite material obtained in Example 1 was subjected to a polystyrene microsphere removal test, and the results were as follows: Fig.11 . Fig.11The digital photo is of the filtration separation process of 10 mg / L polystyrene microsphere solution by the nanosilver particle loaded Caragana korshinskii powder composite material obtained in Example 1. The nanosilver particle loaded Caragana korshinskii fiber composite material exhibits efficient separation performance for polystyrene microspheres in water, and the removal rate is higher than 99.89% as tested by fluorescence spectrophotometer.
[0091] The removal rates of the nano-silver loaded Caragana korshinskii composite materials obtained in Examples 2 to 5 for 10 mg / L polystyrene microsphere solution were 99.63%, 99.49%, 99.57% and 99.74%, respectively.
[0092] From the above experiments, we can see that the loaded nanosilver particles have greatly changed the wettability of the caragana fiber powder, making the composite material super hydrophilic, capable of efficiently separating oil-water mixtures and removing toxic organic compounds such as dyes and high molecular polymers from recycled water.
[0093] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A nano-silver particle anchored plant fiber water purification composite material, characterized in that: It comprises plant fiber powder and nano silver particles loaded on the plant fiber powder, wherein the fiber length of the plant fiber powder is 100 μm to 600 μm, the particle size of the nano silver particles is 3 nm to 5 nm, and the diameter of the plant fiber powder is 10 nm to 20 nm; The plant fiber powder is Caragana korshinskii powder obtained by grinding dried and peeled Caragana korshinskii branches into powder; The preparation method of the nano silver particle anchored plant fiber water purification composite material, The method comprises the following processes: grinding dried plant fibers into plant fiber powder; Dissolving silver salt to obtain a silver ion solution, and mixing the plant fiber powder and the silver ion solution to obtain a mixed solution; The mixed solution is heated to reduce the silver ions adsorbed on the plant fiber powder to nanosilver particles, thereby obtaining the nanosilver particle-anchored plant fiber water purification composite material; Wherein, the mass percentage concentration of the silver salt in the silver ion solution is 0.1wt% to 5wt%; The mass of the silver salt in the mixed solution is 1% to 10% of the mass of the plant fiber powder; The heating temperature is 80° C. to 120° C., and the heating time is 2 h to 8 h.
2. A method for preparing the nano-silver particle anchored plant fiber water purification composite material as claimed in claim 1, characterized in that: The process includes: grinding the dried plant fiber into plant fiber powder; Dissolving silver salt to obtain a silver ion solution, and mixing the plant fiber powder and the silver ion solution to obtain a mixed solution; The mixed solution is heated to reduce the silver ions adsorbed on the plant fiber powder to nano-silver particles, thereby obtaining the nano-silver particle-anchored plant fiber water purification composite material.
3. The preparation method according to claim 2, characterized in that: The heating temperature is 80° C. to 120° C., and the heating time is 2 h to 8 h.
4. The preparation method according to claim 2, characterized in that: The mass percentage concentration of the silver salt in the silver ion solution is 0.1 wt % to 5 wt %.
5. The preparation method according to claim 2, characterized in that: The mass of the silver salt in the mixed solution is 1% to 10% of the mass of the plant fiber powder.
6. The preparation method according to claim 2, characterized in that: The silver salt is selected from at least one of silver nitrate, silver sulfate, silver chloride, silver acetate and silver stearate.
7. The preparation method according to claim 2, characterized in that: The mixing method includes one or two or more of shaking, magnetic stirring, mechanical stirring, ultrasound and microwave assistance.
8. The preparation method according to claim 2, characterized in that: The fiber length of the plant fiber powder is 100 μm to 600 μm, and the particle size of the nano silver particles is 3 nm to 5 nm.
9. A water purification device, characterized in that: The invention comprises a filter column and the nanosilver particle anchored plant fiber water purification composite material as claimed in claim 1 or the nanosilver particle anchored plant fiber water purification composite material prepared by the preparation method as claimed in any one of claims 2 to 8 filled in the filter column.