Annealing process for preventing strip steel from bonding

By using cleaning agents and circulating fan heating technology with components such as sodium hydroxide, sodium carbonate, sodium dodecyl sulfate and N-(hydroxymethyl)nonanamide, the bonding problem during strip annealing is solved and the product is improved Surface quality and tensile strength reduce production costs.

CN119020790APending Publication Date: 2024-11-26河北海洪新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411072414.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The grease or other impurities attached to strip steel during production, processing and storage lead to bonding during the annealing process, affecting surface uniformity, increasing production difficulty, reducing product quality, and may lead to scrapping of finished products and increasing production costs.

Method used

High-pressure spray cleaning is carried out using sodium hydroxide, sodium carbonate, sodium dodecyl sulfate and N-(hydroxymethyl)nonanamide and other components. Combined with circulating fan heating and multi-stage cooling, the heating rate and cooling rate are controlled. , a uniform covering layer is formed to prevent bonding.

Benefits of technology

Effectively remove oil stains and impurities on the surface of strip steel, improve tensile strength, reduce the occurrence of bonding, and ensure product quality stability and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of strip steel heat treatment, and provides an annealing process for preventing strip steel bonding, which comprises the following steps: cleaning a strip steel raw material with a cleaning agent, annealing, cooling and rolling to obtain finished strip steel, the cleaning agent comprises sodium hydroxide, sodium carbonate, lauryl sodium sulfate and N-(hydroxymethyl) nonanamide. According to the technical scheme, the problem that the bonding phenomenon is serious in the prior art is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heat treatment of strip steel, and in particular to an annealing process for preventing strip steel from sticking. Background Art

[0002] During the production, processing and storage of steel strips, a certain amount of grease or other impurities often adhere to them. If these contaminants are not fully removed, they will become the source of adhesion during the annealing process. Improper temperature control during the annealing process will also cause abnormal changes in the metal surface, causing adhesion. Adhesion will cause the surface of the steel strip to be uneven, which is easy to cause scratches, deformation and other problems in the subsequent processing, increasing the difficulty of production. Adhesion on the surface of the steel strip will also affect its product quality, reduce the market competitiveness of the product, and even cause the finished product to be scrapped, increase production costs, and also cause damage to the rollers of the leveler. All of these have brought serious economic losses to the cold rolling mill. Therefore, optimizing an annealing process to prevent steel strip adhesion is an urgent problem to be solved. Summary of the invention

[0003] The invention proposes an annealing process for preventing strip steel from sticking, thereby solving the serious problem of sticking in the related art.

[0004] The technical solution of the present invention is as follows: The present invention proposes an annealing process for preventing strip steel from sticking, comprising the following steps: cleaning the strip steel raw material with a cleaning agent, annealing, cooling, and rolling to obtain a finished strip steel; the cleaning agent includes sodium hydroxide, sodium carbonate, sodium dodecyl sulfate and N-(hydroxymethyl) nonanamide.

[0005] As a further technical solution, the cleaning agent is a mixed solution of sodium hydroxide, sodium carbonate, sodium dodecyl sulfate, N-(hydroxymethyl) nonanamide and water.

[0006] As a further technical solution, the cleaning agent also includes 1-decyl-3-methylimidazolium hexafluorophosphate.

[0007] As a further technical solution, the mass ratio of the N-(hydroxymethyl)nonanamide and 1-decyl-3-methylimidazolium hexafluorophosphate is 2-4:1.

[0008] In the present invention, the decyl alkyl chain contained in 1-decyl-3-methylimidazolium hexafluorophosphate is a hydrophobic functional group, which can interact with grease and other hydrophobic impurities on the surface of the steel strip. During the phosphating process, this part can help to adsorb on the metal surface and play a certain protective and wetting role; the imidazole ring part makes it have good surface activity and solubility, so it helps to form a uniform covering layer, thereby improving the surface quality of the steel strip.

[0009] As a further technical solution, the cleaning is carried out by spraying, the temperature of the cleaning agent is 70-75°C, and the spraying pressure is 3.0-3.6 bar.

[0010] As a further technical solution, the annealing is to raise the temperature to 705° C. and keep the temperature for 10 to 12 hours.

[0011] As a further technical solution, a circulating fan is used to increase the temperature during the heating process, and the rotation speed of the circulating fan used during the heating process is 1800~2000r / min.

[0012] As a further technical solution, the heating rate is 30-40°C / h.

[0013] In the present invention, a moderate heating rate is used to heat the steel strip. If the heating rate is too fast or too slow, not only will the temperature of the steel strip rise unevenly, causing local overheating and affecting product quality, but it will also increase energy consumption and increase production costs. An appropriate heating rate helps to control temperature changes during the heat treatment process, ensure the quality stability and consistency of the product, and effectively improve the occurrence of steel strip bonding.

[0014] As a further technical solution, the heating rate is 35°C / h.

[0015] As a further technical solution, the cooling is performed in sequence by heating hood cooling, air cooling and water cooling, the temperature at which the heating hood cooling ends is 350°C, and the temperature at which the air cooling ends is 300°C.

[0016] As a further technical solution, the temperature at which the water cooling ends is 60°C.

[0017] As a further technical solution, the cooling rate of the heating hood is 15-25°C / h.

[0018] As a further technical solution, the cooling rate of the heating hood is 20°C / h.

[0019] In the present invention, appropriately extending the cooling time of the heating hood can further reduce the cooling speed of the high temperature section, reduce the temperature difference between hot and cold spots during the strip annealing process, and effectively control the occurrence of the sticking phenomenon. However, too long a cooling time will not only cause uneven temperature changes in the strip during the annealing process, affecting the quality stability of the product, causing a temperature difference between hot and cold spots, and even possibly affecting the performance of the product, but will also lead to an extension of the production cycle, thereby reducing production efficiency and affecting the overall production schedule and output. The present invention limits the cooling time of the heating hood, which can make the temperature of the strip change evenly during the annealing process, reduce the occurrence of the sticking phenomenon, and also help maintain the production schedule, improve production efficiency, and ensure that the production plan is completed on time.

[0020] The working principle and beneficial effects of the present invention are: According to the present invention, the hydroxymethyl functional group contained in N-(hydroxymethyl)nonanamide in the cleaning agent makes it hydrophilic, and can make the cleaning agent more easily dissolved in water and quickly mixed with impurities in the water, so as to better rinse the surface of the strip steel; in addition, the hydroxyl group also gives it surface activity, which helps to reduce the surface tension, so that the cleaning agent can more easily penetrate and cover the target surface; the nonane functional group makes N-(hydroxymethyl)nonanamide have a certain oil solubility and a removal effect on organic dirt such as grease and lubricants, and these hydrophobic parts can interact with oily dirt, which is conducive to removing it from the surface of the strip steel, thereby effectively preventing the occurrence of the strip steel bonding problem and improving the surface quality and tensile strength of the strip steel. DETAILED DESCRIPTION

[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Example 1 Weigh 60 parts of sodium hydroxide, 6 parts of sodium carbonate, 20 parts of sodium dodecyl sulfate, 5 parts of N-(hydroxymethyl) nonylamide and 100 parts of water, mix them evenly to make a cleaning agent, unwind the raw steel strip through the unwinder of the cleaning line and enter the cleaning section, spray the cleaning agent with high pressure (dilute with water to a mass fraction of 5%), the temperature of the cleaning agent is 70°C, the spraying pressure is 3.0 bar, and then rinse and dry, and the dried strip is wound on the coiler of the cleaning line; the cleaned strip is loaded into the furnace, and the air tightness test is carried out after the protective cover is pressed, and the annealing space is purged with nitrogen. After the gas joint has passed the air tightness test, the heating hood is ignited, and the protective gas (H2) is blown to raise the temperature to 705℃. During the heating process, the speed of the circulating fan is 1800r / min, and the heating rate is 20℃ / h. After keeping warm for 10 hours, it is cooled and first enters the heating hood cooling stage. The cooling rate is 15℃ / h. When the temperature drops to 350℃, air cooling is carried out. When the temperature is 300℃, water cooling is carried out. It is cooled to 60℃ and taken out of the furnace after nitrogen purging. The steel coils are packed in the final cooling station. After final cooling, the steel coils are transported to the front warehouse of the leveling unit.

[0023] Example 2 Weigh 60 parts of sodium hydroxide, 6 parts of sodium carbonate, 24 parts of sodium dodecyl sulfate, 6 parts of N-(hydroxymethyl) nonylamide, and 120 parts of water, mix them evenly to make a cleaning agent, unwind the raw steel strip through the unwinder of the cleaning line and enter the cleaning section, spray the cleaning agent with high pressure (diluted with water to a mass fraction of 5%), the temperature of the cleaning agent is 73°C, the spraying pressure is 3.3 bar, and then rinse and dry. The dried strip is wound on the coiler of the cleaning line; the cleaned strip is loaded into the furnace, the air tightness test is carried out after the protective cover is pressed, and the annealing space is purged with nitrogen After the gas joint has passed the air tightness test, the heating hood is ignited, and the protective gas (H2) is blown to raise the temperature to 705℃. During the heating process, the speed of the circulating fan is 1900r / min, and the heating rate is 20℃ / h. After keeping warm for 11 hours, it is cooled and first enters the heating hood cooling stage. The cooling rate is 20℃ / h. When the temperature drops to 350℃, air cooling is carried out. When the temperature is 300℃, water cooling is carried out. It is cooled to 70℃ and taken out of the furnace after nitrogen purging. The steel coils are packed in the final cooling station. After final cooling, the steel coils are transported to the front warehouse of the leveling unit.

[0024] Example 3 Weigh 60 parts of sodium hydroxide, 6 parts of sodium carbonate, 28 parts of sodium dodecyl sulfate, 7 parts of N-(hydroxymethyl) nonylamide and 140 parts of water, mix them evenly to make a cleaning agent, unwind the raw steel strip through the unwinder of the cleaning line and enter the cleaning section, spray the cleaning agent with high pressure (dilute with water to a mass fraction of 5%), the temperature of the cleaning agent is 75°C, the spraying pressure is 3.6 bar, and then rinse and dry. The dried strip is wound on the coiler of the cleaning line; the cleaned strip is loaded into the furnace, the air tightness test is carried out after the protective cover is pressed, and the annealing space is purged with nitrogen After the gas joint has passed the air tightness test, the heating hood is ignited, and the protective gas (H2) is blown to raise the temperature to 705℃. During the heating process, the speed of the circulating fan is 2000r / min, the heating rate is 20℃ / h, and it is cooled after 12 hours of insulation. First, it enters the heating hood cooling stage with a cooling rate of 25℃ / h. When the temperature drops to 350℃, it is air-cooled. When the temperature is 300℃, it is water-cooled. It is cooled to 80℃ and taken out of the furnace after nitrogen purging. The steel coils are packed in the final cooling station. After final cooling, the steel coils are transported to the front warehouse of the leveling unit.

[0025] Example 4 Compared with Example 2, the difference of Example 4 is that 6 parts of N-(hydroxymethyl)nonanamide are replaced by 3 parts of N-(hydroxymethyl)nonanamide and 3 parts of 1-decyl-3-methylimidazolium hexafluorophosphate.

[0026] Example 5 Compared with Example 2, the difference of Example 5 is that 6 parts of N-(hydroxymethyl)nonanamide are replaced by 4 parts of N-(hydroxymethyl)nonanamide and 2 parts of 1-decyl-3-methylimidazole hexafluorophosphate.

[0027] Example 6 Compared with Example 2, the difference of Example 6 is that 6 parts of N-(hydroxymethyl)nonanamide are replaced by 4.5 parts of N-(hydroxymethyl)nonanamide and 1.5 parts of 1-decyl-3-methylimidazole hexafluorophosphate.

[0028] Example 7 Compared with Example 2, the difference of Example 7 is that 6 parts of N-(hydroxymethyl)nonanamide are replaced by 4.8 parts of N-(hydroxymethyl)nonanamide and 1.2 parts of 1-decyl-3-methylimidazole hexafluorophosphate.

[0029] Example 8 Compared with Example 2, the difference of Example 8 is that 6 parts of N-(hydroxymethyl)nonanamide are replaced by 5 parts of N-(hydroxymethyl)nonanamide and 1 part of 1-decyl-3-methylimidazole hexafluorophosphate.

[0030] Example 9 Compared with Example 6, Example 9 is different in that the heating rate is changed to 30° C. / h.

[0031] Example 10 Compared with Example 6, Example 10 is different in that the heating rate is changed to 35° C. / h.

[0032] Embodiment 11 Compared with Example 6, Example 11 is different in that the heating rate is changed to 40° C. / h.

[0033] Comparative Example 1 Compared with Example 2, the difference in Comparative Example 1 is that N-(hydroxymethyl)nonanamide is replaced by an equal amount of 1-decyl-3-methylimidazole hexafluorophosphate.

[0034] Comparative Example 2 Compared with Example 2, Comparative Example 2 is different in that 1-decyl-3-methylimidazolium hexafluorophosphate and N-(hydroxymethyl)nonanamide are not added.

[0035] The strip steels obtained in Examples 1 to 11 and Comparative Examples 1 to 2 were tested according to the following method: 1. Oil cleaning rate: Take the experimental strip steel sample (10cm×10cm×2mm), weigh its mass W0, immerse the experimental strip steel sample in rolling oil, take it out after immersion for 1 minute, dry it naturally, weigh the mass W1 of the strip steel adhered with rolling oil, add pure water and 5% of the mass of pure water to the cleaning tank, stir and heat evenly, immerse the strip steel sample adhered with rolling oil into the cleaning tank for immersion degreasing, the immersion time is 1 minute, take the strip steel sample out of the washing tank, dry it naturally, weigh the mass W2 of the strip steel after cleaning, and calculate the oil cleaning rate according to the following formula: Oil cleaning rate (%) = [(W1-W0)-(W2-W0)] / (W1-W0) × 100%; 2. Tensile strength: Test the tensile strength of the sample according to the tensile strength test method specified in GB / T 3280-2015 "Stainless Steel Cold-rolled Steel Plate and Steel Strip".

[0036] The test results are shown in the following table: Table 1 Performance test results of the strip steel obtained in Examples 1 to 11 and Comparative Examples 1 to 2

[0037] Compared with Comparative Example 1, Examples 1 to 3 add N-(hydroxymethyl)nonanamide. As a result, the oil stain cleaning rate and tensile strength of Examples 1 to 3 are better than those of Comparative Example 1, indicating that the addition of N-(hydroxymethyl)nonanamide can effectively remove the oil stains on the surface of the strip and further improve the bonding problem of the strip.

[0038] Compared with Comparative Example 2 and Examples 1 to 3, Examples 4 to 8 simultaneously added N-(hydroxymethyl) nonanamide and 1-decyl-3-methylimidazole hexafluorophosphate. As a result, the oil cleaning rate and tensile strength of Examples 4 to 8 were better than those of Comparative Example 2 and Examples 1 to 3, indicating that N-(hydroxymethyl) nonanamide and 1-decyl-3-methylimidazole hexafluorophosphate played a synergistic role, which could further remove oil stains on the surface of the strip, reduce the occurrence of strip bonding, and enhance the strength of the strip.

[0039] Compared with Example 4, Examples 5 to 8 added N-(hydroxymethyl) nonanamide and 1-decyl-3-methylimidazolium hexafluorophosphate in different mass ratios. As a result, the oil cleaning rate and tensile strength of Examples 5 to 7 were better than those of Examples 4 and 8, indicating that when the mass ratio of N-(hydroxymethyl) nonanamide and 1-decyl-3-methylimidazolium hexafluorophosphate was 2 to 4:1, and the preferred mass ratio was 3:1, the cleaning agent had the best effect in removing oil stains, the least adhesion phenomenon, and the greatest strip strength.

[0040] Compared with Example 6, Examples 9 to 11 set different heating rates. As a result, Example 10 has the best oil cleaning rate and the greatest tensile strength, indicating that when the heating rate is 35°C / h, the occurrence of strip steel adhesion can be most effectively prevented.

[0041] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An annealing process for preventing strip steel from sticking, characterized in that: The following steps are involved: The steel strip raw material is cleaned by a cleaning agent, annealed, cooled and rolled to obtain a finished steel strip; the cleaning agent includes sodium hydroxide, sodium carbonate, sodium dodecyl sulfate and N-(hydroxymethyl) nonanamide.

2. The annealing process for preventing strip steel from sticking according to claim 1, characterized in that: The cleaning agent is a mixed solution of sodium hydroxide, sodium carbonate, sodium dodecyl sulfate, N-(hydroxymethyl) nonanamide and water.

3. The annealing process for preventing steel strip from sticking according to claim 1, characterized in that: The cleaning agent also includes 1-decyl-3-methylimidazolium hexafluorophosphate.

4. The annealing process for preventing steel strip from sticking according to claim 3, characterized in that: The mass ratio of the N-(hydroxymethyl)nonanamide to 1-decyl-3-methylimidazolium hexafluorophosphate is 2-4:

1.

5. The annealing process for preventing steel strip from sticking according to claim 1, characterized in that: The cleaning is performed by spraying, the temperature of the cleaning agent is 70-75° C., and the spraying pressure is 3.0-3.6 bar.

6. The annealing process for preventing steel strip from sticking according to claim 1, characterized in that: The annealing step is to raise the temperature to 705° C. and keep the temperature for 10 to 12 hours.

7. The annealing process for preventing steel strip from sticking according to claim 6, characterized in that: During the heating process, a circulating fan is used to heat the temperature, and the rotation speed of the circulating fan is 1800-2000r / min.

8. The annealing process for preventing steel strip from sticking according to claim 6, characterized in that: The heating rate is 30-40°C / h.

9. The annealing process for preventing steel strip from sticking according to claim 1, characterized in that: The cooling is performed in sequence by heating hood cooling, air cooling and water cooling. The temperature at which the heating hood cooling ends is 350° C., and the temperature at which the air cooling ends is 300° C.

10. An annealing process for preventing steel strip from sticking according to claim 9, characterized in that: The cooling rate of the heating mantle is 15-25°C / h.