A method for improving the calcination strength of magnesium pellets
By using calcium oxalate and humate as modifiers in the preparation of magnesia pellets, combined with high-pressure roller grinding technology, the problem of low roasting intensity of blast furnace pellets is solved, the effect of reducing roasting temperature and time is achieved, and significantly improved Improve pellet strength and reduce production costs.
Patent Information
- Application Number
- CN202211318937.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-10-26
AI Technical Summary
Domestic blast furnace pellets have a low ore ratio, and high-silica ores generate olivine that is difficult to reduce during the preparation and reduction process of oxidized pellets, resulting in low pellet roasting strength. Existing methods to improve strength require increasing roasting temperature and time, and increasing energy Consumption and cost.
Calcium oxalate and humate are used as modifiers, combined with high-pressure roller grinding technology, to improve the surface properties and mineralization ability of iron concentrate and magnesium-containing flux, promote solid-phase reaction, reduce roasting temperature and time, and improve magnesia balls. The roasting strength of the dough.
Under the same raw material conditions, the roasting temperature is reduced by 15 to 35°C, the time is shortened by 3 to 5 minutes, and the strength of the roasted pellets is increased to 2820N/piece. The operation is simple, the cost is low, and it meets the requirements of industrial production.
Abstract
Description
Technical Field
[0001] The invention relates to a method for improving the roasting strength of magnesium pellets and belongs to the field of steel metallurgy. Background Art
[0002] Pellets are ideal raw materials for blast furnaces because of their excellent metallurgical properties and good mechanical strength. At present, the proportion of pellets in foreign blast furnace ironmaking has exceeded 60%, even reaching 100%, but the proportion of domestic blast furnace pellets is generally less than 20%. Domestic high-quality iron ore resources are scarce, and high silicon content is a common situation of iron ore in my country. High-silicon ore is very easy to generate olivine that is difficult to reduce during the preparation and reduction of oxidized pellets, which seriously restricts its high-proportion application in blast furnaces. In order to enhance the metallurgical performance indicators of high-silicon ore, high-silicon magnesium pellets are usually prepared by adding magnesium-containing flux. Magnesium oxide will generate magnesia-iron spinel with iron minerals during roasting, which is beneficial to inhibit the reduction expansion of pellets and improve the reduction degree of pellets. However, magnesium-containing flux (magnesium oxide powder, magnesite, etc.) generates high-melting-point spinel during the preparation of oxidized pellets, which is not conducive to the consolidation of pellets. In addition, magnesium-containing carbonates have rich void structures themselves, and the pores generated by high-temperature decomposition significantly reduce the mechanical strength of the product pellets and increase the pellet pulverization rate. In order to ensure the strength of the pellets, the commonly used methods are to increase the roasting temperature, extend the roasting time, increase the proportion of bentonite, etc., but at the same time, this will significantly increase the energy consumption and process cost of the pellet production process.
[0003] Therefore, developing a method to improve the roasting strength of magnesium pellets is of great significance to optimizing the pellet preparation process and improving the quality of magnesium oxide pellets. Summary of the invention
[0004] In view of the current situation in the prior art that the suitable roasting temperature is high, the roasting time is long, and the strength of the roasted pellets is low when producing magnesium pellets, the purpose of the present invention is to provide a method for improving the roasting strength of magnesium pellets. The method is based on the use of a modifier containing active components such as calcium oxalate and humate combined with a high-pressure roller mill pretreatment technology, which can significantly improve the surface properties and mineralization capacity of iron concentrate and magnesium-containing flux, promote the dispersibility of magnesium-containing flux in iron concentrate, and improve the solid-phase reaction effect. Therefore, under the same raw material composition conditions, the roasting temperature can be reduced by 15 to 35°C, the roasting time can be shortened by 3 to 5 minutes, and the strength of the roasted pellets can be increased to 2820N / piece. In addition, the method is simple to operate, has low production cost, is environmentally friendly, and meets the requirements of industrial production.
[0005] In order to achieve the above technical purpose, the present invention provides a method for improving the roasting strength of magnesium pellets, which comprises mixing an iron concentrate raw material with a modifier and a magnesium-containing flux and then subjecting the mixture to a high-pressure roller mill treatment, mixing the material obtained by the high-pressure roller mill with a binder and water to form pellets, and sequentially drying, preheating and roasting the obtained pellets to obtain magnesium pellets; the modifier comprises calcium oxalate and humate.
[0006] The key to the technical solution of the present invention is that a special modifier (active ingredients are calcium oxalate and humate) is used in the process of pelletizing the refined iron ore raw material, and a high-pressure roller mill is used in combination. The combined effect of the two can effectively increase the solid-phase reaction rate during the pelletizing process, reduce the solid-phase reaction temperature, and increase the strength of the magnesium pellets. Calcium oxalate and humate are used as chemical modifiers. The synergistic effect of the two activates the surface activity of hematite and magnetite, promotes the contact between the iron ore particles and the magnesium-containing flux, and is beneficial to the solid-phase reaction during the roasting process. In particular, humate forms a bridge bond between the iron ore and the magnesium-containing flux particles, promotes the dispersion of the magnesium-containing flux in the iron ore, and is beneficial to reducing the element segregation during the roasting process. At the same time, humate and calcium oxalate can release a small amount of active gases such as H2 and CO during the preheating roasting process, which promotes the generation of appropriate defects on the surface of the iron mineral and reduces the activation energy of the solid-phase reaction. On the basis of the use of chemical modifiers, a high-pressure roller mill is further used to utilize high The mechanical force of the roller mill can, to a certain extent, crush and fracture the coarse-grained iron ore concentrate particles, increase the specific surface area of the pelletizing concentrate raw material, and greatly increase the contact area between the iron ore particles and the magnesium-containing flux by making the particle size of the iron ore concentrate and the magnesium-containing solvent finer, which is beneficial to the mineralization of the iron ore concentrate and the strength of the roasted pellets. At the same time, the mechanical energy of the high-pressure roller mill is used to promote the physical and chemical reaction between the calcium oxalate and humate modifiers and the surface of the iron ore particles, so that some calcium ions directly enter the voids and cracks on the surface of the iron ore concentrate, which can activate the lattice, promote the formation of micro-region liquid phase, and increase the solid-phase reaction rate in the subsequent roasting process. In summary, the combined effect of chemical modifiers and mechanical activation of the high-pressure roller mill provides favorable conditions for increasing the solid-phase reaction rate, reducing the reaction temperature, and increasing the strength of the roasted pellets during the roasting process.
[0007] As a preferred solution, the modifier is composed of calcium oxalate and humate in a mass percentage of 60% to 80% and 40% to 20%. Calcium oxalate and humate respectively activate the surface of iron ore particles and enhance dispersibility. Calcium oxalate can significantly activate iron ore particles during the roasting process, preferentially react in the solid phase to form a low-melting point liquid precursor, which is beneficial to reduce the activation energy of the solid phase reaction between iron minerals during the roasting process. Calcium oxalate alone has poor dispersibility and cannot be fully mixed with iron concentrate particles. Sodium humate is used to enhance the dispersing effect of calcium oxalate, but it is difficult to fully activate iron ore using humate alone.
[0008] As a preferred embodiment, the humate is sodium humate.
[0009] As a preferred solution, the mass of the modifier accounts for 0.1-0.3% of the dry mass of the iron ore concentrate. If the amount of the modifier is too low, an effective ion concentration cannot be formed on the surface of the iron ore concentrate. If the amount of the modifier is too high, the sodium humate is easy to agglomerate, which is not conducive to the smooth progress of the high-pressure roller milling process.
[0010] As a preferred solution, the iron ore concentrate raw material contains magnetite.
[0011] As a preferred solution, the iron ore concentrate raw material contains hematite; the mass of the hematite does not exceed 40% of the mass of the iron ore concentrate raw material. Both magnetite and hematite concentrate can be used to prepare magnesium pellets, but hematite mineralization is more difficult. If the proportion of hematite increases during the pellet production process, the roasting temperature needs to be further increased to ensure the strength of the finished pellets.
[0012] As a preferred solution, the particle size of the iron ore concentrate raw material satisfies that the mass percentage content of the -0.074 mm particle size is higher than 60%.
[0013] As a preferred solution, the water content of the iron ore concentrate is controlled at 6.2-7.9%. The iron ore concentrate must maintain a suitable water content, mainly because the physical and chemical effects of the modifier on the surface of the iron ore concentrate require sufficient water absorption, and the dispersion of the modifier also requires water. Therefore, the water content of the iron ore concentrate should not be too low, but excessive water will seriously affect the high-pressure roller mill process, because the high-pressure roller mill is sensitive to the surface water of the material, and too high water content will cause blockage and affect the roller mill effect.
[0014] As a preferred solution, the high pressure roller mill controls the mass percentage content of the material particle size at -0.074mm particle size to be higher than 90%. As a more preferred solution, the pressure of the high pressure roller mill is 50-150bar. High pressure roller mills are commonly used in the pretreatment process of iron ore concentrates, but it is not common to use high pressure roller mill mechanical activation to strengthen the activation effect of chemical modifiers on iron ore concentrates. Under the action of the mechanical force of the high pressure roller mill, not only can the coarse-grained iron ore concentrate particles be crushed and fractured, the specific surface area of the pelletizing concentrate raw material is increased, and the particle size of the iron ore concentrate raw material is finer, the contact area between the iron ore particles and the flux can be increased, which is beneficial to the mineralization of the iron ore concentrate and the strength of the roasted pellets. In particular, during the high pressure roller mill process, the physical and chemical reactions of calcium oxalate and humate modifiers on the surface of the iron ore particles can be strengthened, and some calcium and magnesium ions will directly enter the voids, cracks and other structures on the surface of the iron ore concentrate, which can activate the lattice, promote the formation of micro-region liquid phase, and increase the solid phase reaction rate in the subsequent roasting process.
[0015] The pelletizing process of the iron ore concentrate raw material of the present invention is a conventional pelletizing process in the prior art.
[0016] The binder used in the pelletizing process of the iron ore concentrate raw material of the present invention is common bentonite.
[0017] The amount of water added during the pelletizing process of the iron ore concentrate raw material of the present invention is a conventional amount.
[0018] The magnesium-containing flux in the pelletizing process of the iron ore concentrate raw material of the present invention is a common magnesium-containing flux such as magnesium oxide and magnesium carbonate.
[0019] Compared with the prior art, the technical solution of the present invention brings the following beneficial technical effects:
[0020] In the preparation process of the magnesium pellets of the present invention, a special chemical modifier is used, and the active ingredients are calcium oxalate and humate. The two act synergistically to activate the surface activity of hematite and magnetite, promote the contact between the iron ore particles and the magnesium-containing flux, and are beneficial to the solid phase reaction during the roasting process. In particular, the humate forms a bridge bond between the iron ore and the magnesium-containing flux particles, promotes the dispersion of the magnesium-containing flux in the iron ore, and is beneficial to reducing the element segregation during the roasting process. At the same time, humate and calcium oxalate can release a small amount of active gases such as H2 and CO during the preheating roasting process, which promotes the generation of appropriate defects on the surface of the iron mineral and reduces the activation energy of the solid phase reaction.
[0021] In the magnesium pellet preparation process of the present invention, a chemical modifier is used in combination with a high-pressure roller mill. The mechanical force of the high-pressure roller mill can not only increase the specific surface area of the pelletizing concentrate raw material, but also greatly increase the contact area between the iron ore particles and the flux by making the particle size of the iron concentrate and the magnesium-containing solvent finer, which is beneficial to the mineralization of the iron concentrate and to improving the strength of the roasted pellets. In addition, the mechanical energy of the high-pressure roller mill can be used to promote the physical and chemical reaction between the calcium oxalate and humate modifiers and the surface of the iron ore particles, so that part of the calcium and magnesium ions directly enter the voids, cracks and other structures on the surface of the iron concentrate, which can activate the lattice, promote the formation of the micro-region liquid phase, and increase the solid-phase reaction rate in the subsequent roasting process.
[0022] The amount of chemical modifier used in the preparation process of the magnesium pellets of the present invention is low, the cost is low, and the strength of the magnesium pellets can be significantly improved.
[0023] 4) The magnesium pellet preparation process of the present invention is simple to operate, low in cost, and has a low roasting temperature and a short time. The roasted pellets are of high quality, which is conducive to large-scale production. DETAILED DESCRIPTION
[0024] The following examples are intended to further illustrate the present invention, rather than to limit the scope of protection of the claims of the present invention.
[0025] Comparative Example 1
[0026] Conventional process, direct mixing, high roasting temperature and poor pellet strength.
[0027] Using a magnetite concentrate (particle size -0.074mm ratio of 63%) as raw material, firstly, the iron concentrate raw material and magnesium-containing flux (MgO powder 2%) and 1% bentonite are mixed and the moisture content of the pelletizing is controlled at 9.5% for pelletizing; finally, drying, preheating and roasting are performed to obtain the finished magnesium oxide pellets. The preheating temperature is 900℃, the time is 10min; the roasting temperature is 1300℃, the time is 13min, and the roasting ball strength is 2130N / piece.
[0028] Comparative Example 2
[0029] Compared with Example 1, the only difference is that no modifier is added (the ratio of calcium oxalate to sodium humate is 80%:20%).
[0030] The final calcined ball has a strength of 2230N / piece.
[0031] Comparative Example 3
[0032] Compared with Example 1, the only difference is that a modifier (sodium humate 100%) is added.
[0033] The final calcined ball has a strength of 2360N / piece.
[0034] Comparative Example 4
[0035] Compared with Example 1, the only difference is that a modifier (calcium oxalate 100%) is added.
[0036] The final calcined ball has a strength of 2330N / piece.
[0037] Comparative Example 5
[0038] Compared with Example 1, the only difference is that no high pressure roller milling is performed.
[0039] The final calcined ball has a strength of 2080N / piece.
[0040] Example 1
[0041] Using a magnetite concentrate (particle size -0.074mm ratio of 63%) as raw material, first dry the iron concentrate to 6.2% moisture, add 0.1% modifier (calcium oxalate and sodium humate ratio of 80%:20%) and magnesium flux (MgO powder 2%) and mix them thoroughly, then process the mixed material with high pressure roller mill, roller mill pressure of 50bar, the particle size of the material after roller milling is 90% -0.074mm ratio; then mix the iron concentrate after roller milling with 1% bentonite and control the ball moisture to 9.5% for ball making; finally dry, preheat and roast to obtain magnesium oxide pellets. Preheating temperature 900℃, time 10min; roasting temperature 1300℃, time 13min, roasting ball strength 2930N / piece.
[0042] Example 2
[0043] Using a magnetite concentrate (particle size -0.074mm ratio of 63%) as raw material, first dry the iron concentrate to 7.2% moisture, add 0.1% modifier (calcium oxalate and sodium humate ratio of 60%:40%) and magnesium flux (magnesite 2.5%) and mix them thoroughly, then process the mixed material by high pressure roller milling, roller milling pressure of 150bar, the particle size of the material after roller milling is 92% -0.074mm; then mix the iron concentrate after roller milling with 1% bentonite and control the ball moisture to 9.2% for ball making; finally dry, preheat and roast to obtain the finished magnesium oxide pellets. Preheating temperature 900℃, time 10min; roasting temperature 1250℃, time 12min, roasting ball strength 2850N / piece.
[0044] Example 3
[0045] A magnetite / hematite concentrate mixed ore (hematite accounts for 40%, particle size -0.074mm ratio is 75%) is used as raw material. First, the iron concentrate raw material is dried to 7.9% moisture, 0.3% modifier (calcium oxalate and sodium humate ratio 70%:30%) and magnesium-containing flux (MgO powder 2.5%) are added and fully mixed, and the mixed material is subjected to high-pressure roller milling, the roller milling pressure is 100bar, and the particle size of the material after roller milling is 96% -0.074mm; then the iron concentrate material after roller milling is mixed with 1% bentonite and the balling moisture is controlled to 9.3% for balling; finally, it is dried, preheated, and roasted to obtain the finished magnesium oxide pellets. The preheating temperature is 900℃, the time is 10min; the roasting temperature is 1270℃, the time is 11min, and the roasted ball strength is 2860N / piece.
[0046] Example 4
[0047] A magnetite / hematite concentrate mixed ore (hematite accounts for 20%, particle size -0.074mm ratio is 63%) is used as raw material. First, the iron concentrate raw material is dried to 7.9% moisture, 0.3% modifier (calcium oxalate and sodium humate ratio 70%:30%) and magnesium-containing flux (MgO powder 2.5%) are added and fully mixed, and the mixed material is subjected to high-pressure roller milling, the roller milling pressure is 100bar, and the particle size of the material after roller milling is 96% -0.074mm; then the iron concentrate material after roller milling is mixed with 1% bentonite and the balling moisture is controlled to 9.5% for balling; finally, it is dried, preheated, and roasted to obtain the finished magnesium oxide pellets. The preheating temperature is 900℃, the time is 10min; the roasting temperature is 1255℃, the time is 12min, and the roasted ball strength is 2820N / piece.
Claims
1. A method for improving the calcination strength of magnesium pellets, characterized in that: The iron ore concentrate raw material is mixed with a modifier and a magnesium-containing flux and then subjected to a high-pressure roller milling process. The material obtained by the high-pressure roller milling is mixed with a binder and water to form balls. The obtained balls are dried, preheated and roasted in sequence to obtain magnesium pellets; the modifier is composed of calcium oxalate and humate in a mass percentage of 60% to 80%: 40% to 20%.
2. A method for improving the calcination strength of magnesium pellets according to claim 1, characterized in that: The humate is sodium humate.
3. A method for improving the calcination strength of magnesium pellets according to claim 1 or 2, characterized in that: The mass of the modifier accounts for 0.1-0.3% of the dry mass of the iron ore concentrate raw material.
4. The method for improving the calcination strength of magnesium pellets according to claim 1, characterized in that: The iron ore concentrate raw material comprises magnetite.
5. A method for improving the calcination strength of magnesium pellets according to claim 1 or 4, characterized in that: The iron ore concentrate raw material contains hematite; the mass of the hematite does not exceed 40% of the mass of the iron ore concentrate raw material.
6. A method for improving the calcination strength of magnesium pellets according to claim 1 or 4, characterized in that: The particle size of the iron ore concentrate raw material satisfies that the mass percentage content of the -0.074 mm particle size is higher than 60%.
7. A method for improving the calcination strength of magnesium pellets according to claim 1 or 4, characterized in that: The moisture content of the iron ore concentrate is controlled at 6.2-7.9%.
8. The method for improving the calcination strength of magnesium pellets according to claim 1, characterized in that: The high pressure roller mill controls the material particle size to be higher than 90% by mass percentage at the -0.074 mm particle size level.
9. A method for improving the calcination strength of magnesium pellets according to claim 1 or 8, characterized in that: The high pressure roller grinding pressure is 50-150 bar.
Citation Information
Patent Citations
Cheap highly effective binder for pellet ore and preparation method thereof
CN101230416A
Method for preparing oxidated pellets from pure hematite concentrate
CN102417976A
Method for synchronously extracting boron and iron in paigeite
CN102899434A
Production method of fluxed composite carbon-containing pellets used in blast furnace
CN104975173A
Method for extracting valuable elements from jarosite slag
CN107267745A