Lightweight building material and preparation method thereof
By forming silanol groups and aluminum hydroxide through hydrolysis polymerization and activated carbon doping within sepiolite fibers, combined with sodium methylsilicate sealing, the problems of lightweight wall panel materials and thermal insulation are solved, and the rigidity and moisture resistance of the materials are improved.
Patent Information
- Application Number
- CN202211333732.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-05
- Filing Date
- 2022-10-28
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-10-28
AI Technical Summary
Existing lightweight wall panel materials are not effective in reducing density and providing thermal insulation, and they are susceptible to moisture and deform after drying.
The silanol groups in sepiolite fibers form a hydrophobic polymer with the hydroxyl groups of aluminum hydroxide, combined with the doping structure of activated carbon in sepiolite fibers, and sodium methylsilicate is used as a surface sealing agent. Combined with the reaction under water vapor environment, a porous doping and rigid sealing are formed.
This has enabled the lightweighting of building materials, improved their rigidity and thermal insulation performance, and reduced water absorption.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of building materials, and in particular relates to a lightweight building material and a preparation method thereof. Background Art
[0002] At present, according to the needs of the development of new residential structural systems, the country promotes the use of light steel frame structural systems and their supporting prefabricated panels. On the basis of summarizing and promoting large bay load-bearing structures, new large bay load-bearing structural systems are being researched and developed. In particular, light steel structure insulation, energy-saving and lightweight earthquake-resistant wall panels are urgently needed by people and the needs of social progress and development. They will surely become the mainstream of new wall materials. There are many kinds of lightweight wall panels currently manufactured and used in the known technology, but the main material is cement mortar, which still cannot effectively reduce the bulk density, has no obvious insulation function, and is easily affected by moisture and deformed after drying. Summary of the invention
[0003] In view of the problems in the prior art, the present invention provides a lightweight building material, which solves the problem that the existing lightweight materials have poor effects. The silanol groups in the sepiolite fibers and the hydroxyl groups of aluminum hydroxide form a shrinkage polymerization, and the activated carbon doping structure in the sepiolite fibers is combined to achieve good porous doping, thereby making the building material lightweight.
[0004] In order to achieve the above technical objectives, the technical solution of the present invention is:
[0005] A lightweight building material comprises the following: sepiolite fiber, aluminum isopropylate, activated carbon, sodium methyl silicate, diatomaceous earth, distilled water, polyurethane and cement.
[0006] The mass ratio of the lightweight building materials is as follows:
[0007] 20-30 parts of sepiolite fiber, 10-20 parts of aluminum isopropylate, 3-6 parts of activated carbon, 2-4 parts of sodium methyl silicate, 20-30 parts of diatomaceous earth, 10-15 parts of distilled water, 2-4 parts of polyurethane resin, and 11-15 parts of cement.
[0008] A method for preparing a lightweight building material comprises the following steps:
[0009] Step 1, add sepiolite fiber to distilled water and stir evenly to form a fiber suspension, then add activated carbon and perform low-temperature ultrasound for 20-30 minutes to form a mixed suspension, the stirring speed for uniform stirring is 1000-2000r / min, the ultrasonic frequency of low-temperature ultrasound is 40-90kHz, and the temperature is 5-10°C;
[0010] Step 2, distilling the mixed suspension under reduced pressure to form fiber powder and distilled water, the pressure of the reduced pressure distillation is 70-80% of the atmospheric pressure, and the temperature is 90-100° C.;
[0011] Step 3, adding aluminum isopropyl ketone to ethanol and stirring evenly, then adding fiber powder, performing low-temperature ultrasound for 10-20 minutes, and drying to obtain fiber powder and ethanol, the stirring speed for uniform stirring is 500-1000r / min, the temperature of low-temperature ultrasound is 10-20°C, the ultrasonic frequency is 50-80kHz, and the drying temperature is 90-100°C;
[0012] Step 4, spraying sodium methyl silicate on the surface of the mixed powder and letting it stand for 1-2 hours, and then placing it in a water vapor environment for reaction for 2-3 hours after penetration to obtain prefabricated particles, the standing temperature is 40-60° C., and the pressure is 0.4-0.6 MPa; the water vapor in the water vapor environment comes from the distilled water in step 2, and the volume content of the water vapor in the water vapor environment is 8-10%, and the temperature is 100-110° C.;
[0013] Step 5, diatomaceous earth, polyurethane resin and prefabricated particles are mixed and stirred until they are completely dispersed, and then cement is added and rapidly stirred to obtain lightweight building materials by granulation. The mixing speed is 500-800 r / min, the rapid stirring speed is 1000-2000 r / min, and the granulation temperature is 180-250°C.
[0014] It can be seen from the above description that the present invention has the following advantages:
[0015] 1. The present invention solves the problem of poor effect of existing lightweight materials. It utilizes the silanol groups in sepiolite fibers and the hydroxyl groups of aluminum hydroxide to form a shrinkage polymerization, and cooperates with the doping structure of activated carbon in the sepiolite fibers to achieve good porous doping and lighten the building materials.
[0016] 2. The present invention utilizes sodium methyl silicate as a surface plugging agent to form a surface plugging during the standing process. In a water vapor environment, the silanol groups on the sodium methyl silicate and the hydroxyl groups in the sepiolite fibers form a polymerized plugging. The rigidity of the entire material is improved by utilizing the rigidity of the sodium methyl silicate. At the same time, the sepiolite fibers are softened under water vapor conditions and penetrate into the sodium methyl silicate, thereby achieving a rigid and strong plugging of the surface.
[0017] 3. The present invention utilizes aluminum isopropoxide to penetrate into the sepiolite fiber, forms permeable doping after drying, and forms an aluminum hydroxide structure under the action of distilled water, and in the subsequent granulation, a porous γ-alumina structure is formed in the sepiolite fiber. DETAILED DESCRIPTION
[0018] The present invention is described in detail with reference to the embodiments, but no limitation is imposed on the claims of the present invention.
[0019] Example 1
[0020] A lightweight building material
[0021] The mass ratio of the lightweight building materials is as follows:
[0022] 20g of sepiolite fiber, 10g of aluminum isopropylate, 3g of activated carbon, 2g of sodium methyl silicate, 20g of diatomaceous earth, 10g of distilled water, 2g of polyurethane resin, and 11g of cement.
[0023] A method for preparing a lightweight building material comprises the following steps:
[0024] Step 1, add sepiolite fiber to distilled water and stir evenly to form a fiber suspension, then add activated carbon and perform low-temperature ultrasound for 20 minutes to form a mixed suspension, the stirring speed for uniform stirring is 1000r / min, the ultrasonic frequency of low-temperature ultrasound is 40kHz, and the temperature is 5°C;
[0025] Step 2, distilling the mixed suspension under reduced pressure to form fiber powder and distilled water, the pressure of the reduced pressure distillation is 70% of the atmospheric pressure, and the temperature is 90° C.;
[0026] Step 3, adding aluminum isopropyl ketone to ethanol and stirring evenly, then adding fiber powder, low-temperature ultrasonic treatment for 10-20 minutes, drying to obtain fiber powder and ethanol, the stirring speed for uniform stirring is 500r / min, the temperature of low-temperature ultrasonic treatment is 10°C, the ultrasonic frequency is 50kHz, and the drying temperature is 90°C; the ethanol here is recovered for the next process treatment;
[0027] Step 4, spraying sodium methyl silicate on the surface of the mixed powder and letting it stand for 1 hour, and then placing it in a water vapor environment for reaction for 2 hours after penetration to obtain prefabricated particles, the standing temperature is 40° C., and the pressure is 0.4-0.6 MPa; the water vapor in the water vapor environment comes from the distilled water in step 2, and the water vapor volume content in the water vapor environment is 8%, and the temperature is 100° C.;
[0028] Step 5, diatomaceous earth, polyurethane resin and prefabricated particles are mixed and stirred until completely dispersed, and then cement is added and rapidly stirred to obtain lightweight building materials by granulation. The mixing and stirring speed is 800 r / min, the rapid stirring speed is 2000 r / min, and the granulation temperature is 250°C.
[0029] The product prepared in this embodiment has a compressive strength of 13.8 MPa, a thermal conductivity of 0.11 W / m·k, a water absorption rate of 27%, and a porosity of 11%.
[0030] Example 2
[0031] A lightweight building material
[0032] The mass ratio of the lightweight building materials is as follows:
[0033] 30g of sepiolite fiber, 20g of aluminum isopropylate, 3g of activated carbon, 2g of sodium methyl silicate, 30g of diatomaceous earth, 15g of distilled water, 4g of polyurethane resin, and 15g of cement.
[0034] A method for preparing a lightweight building material comprises the following steps:
[0035] Step 1, add sepiolite fiber to distilled water and stir evenly to form a fiber suspension, then add activated carbon and perform low-temperature ultrasound for 30 minutes to form a mixed suspension, the stirring speed for uniform stirring is 2000r / min, the ultrasonic frequency of low-temperature ultrasound is 90kHz, and the temperature is 10°C;
[0036] Step 2, distilling the mixed suspension under reduced pressure to form fiber powder and distilled water, the pressure of the reduced pressure distillation is 80% of the atmospheric pressure, and the temperature is 100° C.;
[0037] Step 3, adding aluminum isopropyl ketone to ethanol and stirring evenly, then adding fiber powder, low-temperature ultrasonic treatment for 20 minutes, drying to obtain fiber powder and ethanol, the stirring speed for uniform stirring is 1000 r / min, the temperature of low-temperature ultrasonic treatment is 20° C., the ultrasonic frequency is 80 kHz, and the drying temperature is 100° C.;
[0038] Step 4, spraying sodium methyl silicate on the surface of the mixed powder and letting it stand for 2 hours, and then placing it in a water vapor environment for reaction for 3 hours after penetration to obtain prefabricated particles, the standing temperature is 60° C., and the pressure is 0.6 MPa; the water vapor in the water vapor environment comes from the distilled water in step 2, and the volume content of the water vapor in the water vapor environment is 10%, and the temperature is 110° C.;
[0039] Step 5, diatomaceous earth, polyurethane resin and prefabricated particles are mixed and stirred until completely dispersed, and then cement is added and rapidly stirred to obtain lightweight building materials by granulation. The mixing and stirring speed is 800 r / min, the rapid stirring speed is 2000 r / min, and the granulation temperature is 250°C.
[0040] The product prepared in this embodiment has a compressive strength of 15.2 MPa, a thermal conductivity of 0.09 W / m·k, a water absorption rate of 22%, and a porosity of 13%.
[0041] Example 3
[0042] A lightweight building material
[0043] The mass ratio of the lightweight building materials is as follows:
[0044] 25g of sepiolite fiber, 15g of aluminum isopropylate, 5g of activated carbon, 3g of sodium methyl silicate, 25g of diatomaceous earth, 13g of distilled water, 3g of polyurethane resin, and 13g of cement.
[0045] A method for preparing a lightweight building material comprises the following steps:
[0046] Step 1, add sepiolite fiber to distilled water and stir evenly to form a fiber suspension, then add activated carbon and perform low-temperature ultrasound for 25 minutes to form a mixed suspension, the stirring speed for uniform stirring is 1500r / min, the ultrasonic frequency of low-temperature ultrasound is 70kHz, and the temperature is 8°C;
[0047] Step 2, distilling the mixed suspension under reduced pressure to form fiber powder and distilled water, the pressure of the reduced pressure distillation is 75% of the atmospheric pressure, and the temperature is 95° C.;
[0048] Step 3, adding aluminum isopropyl ketone to ethanol and stirring evenly, then adding fiber powder, low-temperature ultrasonic treatment for 15 minutes, drying to obtain fiber powder and ethanol, stirring evenly at a stirring speed of 800 r / min, low-temperature ultrasonic temperature of 15°C, ultrasonic frequency of 70kHz, and drying temperature of 95°C;
[0049] Step 4, spraying sodium methyl silicate on the surface of the mixed powder and letting it stand for 2 hours, and then placing it in a water vapor environment for reaction for 3 hours after penetration to obtain prefabricated particles, the standing temperature is 60° C., and the pressure is 0.5 MPa; the water vapor in the water vapor environment comes from the distilled water in step 2, and the water vapor volume content in the water vapor environment is 9%, and the temperature is 105° C.;
[0050] Step 5, diatomaceous earth, polyurethane resin and prefabricated particles are mixed and stirred until completely dispersed, and then cement is added and rapidly stirred to obtain lightweight building materials by granulation. The mixing and stirring speed is 700 r / min, the rapid stirring speed is 1500 r / min, and the granulation temperature is 220°C.
[0051] The product prepared in this embodiment has a compressive strength of 14.4 MPa, a thermal conductivity of 0.10 W / m·k, a water absorption rate of 23%, and a porosity of 12%.
[0052] In summary, the present invention has the following advantages:
[0053] 1. The present invention solves the problem of poor effect of existing lightweight materials. It utilizes the silanol groups in sepiolite fibers and the hydroxyl groups of aluminum hydroxide to form a shrinkage polymerization, and cooperates with the doping structure of activated carbon in the sepiolite fibers to achieve good porous doping and lighten the building materials.
[0054] 2. The present invention utilizes sodium methyl silicate as a surface plugging agent to form a surface plugging during the standing process. In a water vapor environment, the silanol groups on the sodium methyl silicate and the hydroxyl groups in the sepiolite fibers form a polymerized plugging. The rigidity of the entire material is improved by utilizing the rigidity of the sodium methyl silicate. At the same time, the sepiolite fibers are softened under water vapor conditions and penetrate into the sodium methyl silicate, thereby achieving a rigid and strong plugging of the surface.
[0055] 3. The present invention utilizes aluminum isopropoxide to penetrate into the sepiolite fiber, forms permeable doping after drying, and forms an aluminum hydroxide structure under the action of distilled water, and in the subsequent granulation, a porous γ-alumina structure is formed in the sepiolite fiber.
[0056] It is understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.
Claims
1. A lightweight building material comprising: sepiolite fiber, aluminum isopropoxide, activated carbon, sodium methyl silicate, diatomaceous earth, distilled water, polyurethane, and cement; The mass ratio of the lightweight building materials is as follows: 20-30 parts of sepiolite fiber, 10-20 parts of aluminum isopropoxide, 3-6 parts of activated carbon, 2-4 parts of sodium methyl silicate, 20-30 parts of diatomaceous earth, 10-15 parts of distilled water, 2-4 parts of polyurethane resin, and 11-15 parts of cement; The method for preparing the lightweight building material comprises the following steps: Step 1, add sepiolite fiber to distilled water and stir evenly to form a fiber suspension, then add activated carbon and perform low-temperature ultrasound for 20-30 minutes to form a mixed suspension, the stirring speed for uniform stirring is 1000-2000r / min, the ultrasonic frequency of low-temperature ultrasound is 40-90kHz, and the temperature is 5-10°C; Step 2, distilling the mixed suspension under reduced pressure to form fiber powder and distilled water, the pressure of the reduced pressure distillation is 70-80% of the atmospheric pressure, and the temperature is 90-100° C.; Step 3, adding aluminum isopropyl ketone to ethanol and stirring evenly, then adding fiber powder, performing low-temperature ultrasound for 10-20 minutes, and drying to obtain fiber powder and ethanol, the stirring speed for uniform stirring is 500-1000r / min, the temperature of low-temperature ultrasound is 10-20°C, the ultrasonic frequency is 50-80kHz, and the drying temperature is 90-100°C; Step 4, spraying sodium methyl silicate on the surface of the mixed powder and letting it stand for 1-2 hours, and then placing it in a water vapor environment for reaction for 2-3 hours after penetration to obtain prefabricated particles, the standing temperature is 40-60° C., and the pressure is 0.4-0.6 MPa; the water vapor in the water vapor environment comes from the distilled water in step 2, and the volume content of the water vapor in the water vapor environment is 8-10%, and the temperature is 100-110° C.; Step 5, diatomaceous earth, polyurethane resin and prefabricated particles are mixed and stirred until they are completely dispersed, and then cement is added and rapidly stirred to obtain lightweight building materials by granulation. The mixing speed is 500-800 r / min, the rapid stirring speed is 1000-2000 r / min, and the granulation temperature is 180-250°C.