A perovskite layer, its preparation method, preparation apparatus and application

By combining light treatment and plasma treatment, the problem of difficult control of nucleation and crystallization in the preparation of perovskite layers was solved, the preparation efficiency and production capacity were improved, the equipment cost was reduced, and the continuous automated production of perovskite layers was realized.

CN115568260BActive Publication Date: 2026-11-17WUXI UTMOST LIGHT TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211384084.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-07
Publication Date
2026-11-17
Estimated Expiration
2042-11-07

AI Technical Summary

Technical Problem

Existing methods for preparing perovskite layers suffer from problems such as difficulty in controlling nucleation and crystallization, large number of equipment and high cost, low utilization rate of precursor materials, and low production efficiency.

Method used

By combining light treatment and plasma treatment, the solvent in the perovskite wet film is evaporated, and the nucleation and crystallization growth of perovskite is achieved through the combined effect of light energy and ion energy, simplifying the preparation process of large-area perovskite layers.

Benefits of technology

It improves the preparation efficiency and production capacity of perovskite films, reduces equipment costs and process requirements, realizes continuous automated production, and is applicable to various perovskite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115568260B_ABST
    Figure CN115568260B_ABST
Patent Text Reader

Abstract

This invention provides a perovskite layer, its preparation method, preparation apparatus, and applications. The preparation method includes the following steps: coating an atomized perovskite solution onto a substrate to obtain a perovskite wet film; and performing photo-treatment and plasma treatment to nucleate and crystallize the perovskite wet film to obtain a perovskite layer. The preparation method of this invention simplifies the preparation process of a single-layer, large-area perovskite layer by combining photo-treatment and plasma treatment, improving the preparation efficiency and production capacity of perovskite films. Traditional heat treatment annealing takes more than ten minutes, while the method using simultaneous photo-treatment and plasma treatment takes only seconds, achieving the same or better film performance as traditional heat treatment, significantly reducing manufacturing time and equipment costs. Simultaneously, the preparation method also reduces the requirements for process conditions and production equipment in perovskite layer preparation and can meet the requirements for continuous automated production of perovskite layers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field and relates to a method for preparing a perovskite layer, and more particularly to a perovskite layer and its preparation method, preparation apparatus and application. Background Technology

[0002] Solar energy is an inexhaustible and clean energy source, available in every corner of the world without geographical limitations. Perovskite solar cells are a new type of solar cell. They have attracted worldwide attention due to their high visible light absorption, simple film-forming process, and rapid improvement in photoelectric conversion efficiency. Perovskite solar cells have experienced rapid development since 2009, with small-sized laboratory perovskite solar cells achieving an efficiency of 25.6%.

[0003] The first challenge for the industrialization of perovskite solar cells is how to prepare perovskite films on a large scale and uniformly. Currently, there are many methods for preparing perovskite films, broadly categorized into solution methods and vacuum methods. Solution methods involve dissolving the perovskite precursor material entirely in organic solvents such as N,N-dimethylformamide (DMF) or dimethyl sulfoxide (DMSO), and then preparing the film using methods such as spin coating, blade coating, or slot-die coating. Vacuum methods, on the other hand, involve directly preparing the perovskite precursor material onto a substrate under vacuum conditions using methods such as thermal evaporation, sputtering, near-space sublimation (CSS), vapor transport method (VTD), or near-space vapor transport method (CSVT), without any solvent involved in the entire process.

[0004] The post-processing of solution methods requires perovskite nucleation and crystallization through gas blowing, vacuum-assisted annealing, or anti-solvent heating. This makes it difficult to control perovskite nucleation and crystallization. Furthermore, solution methods require a large number of expensive pieces of equipment and are time-consuming. While vacuum methods can deposit perovskite films on substrates with different roughnesses or morphologies, vacuum evaporation methods suffer from difficulties in precisely controlling the proportions of components, low precursor material utilization, slow production cycle, high energy consumption, and high equipment costs.

[0005] CN112349844A discloses a perovskite material, its preparation method, a light-absorbing layer, and a perovskite solar cell. The preparation method includes: 1) spraying a B-site precursor onto a substrate to obtain a B-site precursor film; 2) spraying a precursor containing A-site and X-site substances onto the B-site precursor film to obtain a perovskite film; 3) subjecting the perovskite film to freeze-drying, followed by purging and annealing to obtain the perovskite material. However, this method for preparing the perovskite material requires a large number of expensive equipment units and makes it difficult to control the nucleation and crystallization of the perovskite.

[0006] CN109545975B discloses a method for preparing a textured, uniform perovskite film by in-situ freeze-sublimation crystallization with liquid film creep suppression, comprising the following steps: First, coating a perovskite precursor sol or solution onto a substrate with a pyramidal textured morphology to form a morphological perovskite liquid film; Second, freezing the perovskite liquid film; Third, degassing and sublimation treatment of the perovskite liquid film; Fourth, heat treatment of the perovskite film: annealing the degassed perovskite film at 70–150°C for 10–120 min to remove residual solvent and allow grains to fuse and grow, obtaining a fully covered, pyramidal-shaped textured, uniform perovskite film. However, this method for preparing a textured, uniform perovskite film by in-situ freeze-sublimation crystallization with liquid film creep suppression is complex, time-consuming, and costly, making it difficult to achieve large-scale application.

[0007] CN109155366A discloses a method for producing solid-state solar cells, the method comprising the following steps: providing a conductive support layer or current collector; applying a metal oxide layer on the conductive support layer; applying at least one sensitizer layer onto the metal oxide layer or onto a first optional layer covering the metal oxide layer, the first optional layer comprising a charge transport layer; applying a second optional layer onto the sensitizer layer, the second optional layer being selected from a charge transport layer, a protective layer, or a combination of both; and disposing a counter electrode or a metal electrode onto the sensitizer layer or the second optional layer. At least one sensitizer layer comprises an organic-inorganic perovskite or a metal halide perovskite, and is treated by applying a vacuum before annealing the sensitizer. (VASP refers to Vacuum Flash Evaporation Assisted Solution Process, and CP refers to Conventional Process). However, this method for producing solid-state solar cells is complex and requires sophisticated equipment.

[0008] Currently available methods for preparing perovskite layers all have certain drawbacks, including difficulty in controlling the nucleation and crystallization of perovskite, the need for a large number of expensive equipment, low utilization of precursor materials, and low production efficiency. Therefore, it is crucial to develop and design a novel method and apparatus for preparing perovskite layers. Summary of the Invention

[0009] To address the shortcomings of existing technologies, the present invention aims to provide a perovskite layer, its preparation method, preparation apparatus, and applications. This invention employs light treatment and plasma treatment, which, through the combined effect of light and ion energy, evaporates the solvent in the perovskite wet film, promoting perovskite nucleation and crystal growth, resulting in a black-phase perovskite film with superior performance. Simultaneously, the perovskite layer preparation method simplifies the process of preparing a single-layer, large-area perovskite layer by combining light treatment and plasma treatment. This transforms the difficult-to-control nucleation and crystallization process into an instant coating and treatment process, improving the preparation efficiency and production capacity of perovskite films. Traditional heat treatment annealing takes more than ten minutes, while this method... The method of simultaneously performing light and plasma treatment has a processing time in the order of seconds, but can achieve the same or better film performance as traditional heat treatment, greatly shortening manufacturing time and equipment costs. At the same time, the preparation method also reduces the requirements for process conditions and production equipment in the preparation of perovskite layers, and can also meet the requirements for continuous automated production of perovskite layers. The preparation method also reduces the difficulty of controlling perovskite nucleation and crystallization, and the quality of perovskite layers can be improved by adjusting the composition of the atomized perovskite solution, the coating process, the light treatment process, and the plasma treatment process. The preparation method is applicable to various perovskite materials and has a wide range of applications.

[0010] To achieve this objective, the present invention adopts the following technical solution:

[0011] In a first aspect, the present invention provides a method for preparing a perovskite layer, the method comprising the following steps:

[0012] A perovskite solution is coated onto a substrate to obtain a perovskite wet film; photo-treatment and plasma treatment are then performed to nucleate and crystallize the perovskite wet film, resulting in a perovskite layer.

[0013] This invention employs a combination of light and plasma treatment. The combined effect of light and ion energy evaporates the solvent in the perovskite wet film, promoting perovskite nucleation and crystal growth, resulting in a black-phase perovskite film with superior performance. Simultaneously, the perovskite layer preparation method simplifies the process of preparing a single-layer, large-area perovskite layer by combining light and plasma treatment. This transforms the difficult-to-control nucleation and crystallization process into an instant coating and treatment process, improving the efficiency and production capacity of perovskite film preparation. Traditional heat treatment annealing takes more than ten minutes, while the method using simultaneous light and plasma treatment takes only a short time. The process achieves film performance at the second level, yet yields results comparable to or better than traditional heat treatment, significantly reducing manufacturing time and equipment costs. Furthermore, the method lowers the requirements for process conditions and production equipment in perovskite layer preparation, and can meet the requirements for continuous automated production of perovskite layers. The method also reduces the difficulty of controlling perovskite nucleation and crystallization; the quality of the perovskite layer can be improved by adjusting the composition of the atomized perovskite solution, the coating process, the photo-treatment process, and the plasma treatment process. This method is applicable to various perovskite materials and has a wide range of applications.

[0014] As a preferred embodiment of the present invention, the coating includes ultrasonic spraying.

[0015] In this invention, ultrasonic spraying can greatly reduce the splashing of atomized perovskite solution during the coating process, thereby greatly reducing the waste of atomized perovskite solution and increasing the utilization efficiency of atomized perovskite solution.

[0016] Preferably, the power of the ultrasonic spraying is 5 to 10W, for example, it can be 5W, 6W, 7W, 8W, 9W or 10W, but it is not limited to the listed data. Other unlisted values ​​within this range are also applicable.

[0017] Preferably, the distance between the ultrasonic nozzle of the ultrasonic spraying and the substrate is 5 to 10 cm, for example, it can be 5 cm, 6 cm, 7 cm, 8 cm, 9 cm or 10 cm, but it is not limited to the listed data. Other unlisted values ​​within this range are also applicable.

[0018] As a preferred embodiment of the present invention, the light processing and plasma processing are performed simultaneously.

[0019] Preferably, the light processing includes infrared light processing and / or microwave light processing.

[0020] In this invention, infrared light treatment enables the perovskite wet film to absorb energy, the solvent to evaporate, and the perovskite to nucleate and crystallize; microwave light treatment enables the perovskite wet film to absorb energy, the solvent to evaporate, and the perovskite to nucleate and crystal grow.

[0021] Preferably, the power of the infrared light processing is 10 to 20W, for example, it can be 10W, 11W, 12W, 13W, 14W, 15W, 16W, 17W, 18W, 19W or 20W, but it is not limited to the listed data. Other unlisted values ​​within this range are also applicable.

[0022] Preferably, the distance between the infrared light processor and the substrate is 1 to 5 cm, for example, it can be 1 cm, 2 cm, 3 cm, 4 cm or 5 cm, but it is not limited to the listed data. Other unlisted values ​​within this range are also applicable.

[0023] Preferably, the working gas for the plasma treatment includes nitrogen and / or an inert gas.

[0024] The inert gas described in this invention includes any one or a combination of at least two of helium, neon, argon, krypton, xenon, or radon. Typical but non-limiting combinations include combinations of helium and neon, neon and argon, argon and krypton, xenon and radon, or helium, neon, and argon.

[0025] Preferably, the flow rate of the working gas for plasma treatment is 500 to 1500 sccm, for example, it can be 500 sccm, 600 sccm, 700 sccm, 800 sccm, 900 sccm, 1000 sccm, 1100 sccm, 1200 sccm, 1300 sccm, 1400 sccm or 1500 sccm, but it is not limited to the listed data, and other unlisted values ​​within this range are also applicable.

[0026] Preferably, the power of the plasma treatment is 100 to 200W, for example, it can be 100W, 110W, 120W, 130W, 140W, 150W, 160W, 170W, 180W, 190W or 200W, but it is not limited to the listed data. Other unlisted values ​​within this range are also applicable.

[0027] Preferably, the distance between the ion air knife and the substrate in the plasma treatment is 5 to 20 cm, for example, it can be 5 cm, 6 cm, 7 cm, 8 cm, 9 cm, 10 cm, 11 cm, 12 cm, 13 cm, 14 cm, 15 cm, 16 cm, 17 cm, 18 cm, 19 cm or 20 cm, but it is not limited to the listed data. Other unlisted values ​​within this range are also applicable.

[0028] In a second aspect, the present invention provides a perovskite layer preparation apparatus for the preparation method described in the first aspect, the perovskite layer preparation apparatus comprising a coating module and a nucleation and crystallization module arranged sequentially along the substrate moving direction;

[0029] The nucleation and crystallization module includes a light processing component and a plasma processing component.

[0030] The perovskite layer preparation device of the present invention can complete the nucleation and crystallization of perovskite wet film in one station or on one piece of equipment. It has low cost and small footprint, and can also achieve uninterrupted continuous production.

[0031] As a preferred embodiment of the present invention, the light processing component includes an infrared light processor and / or a microwave light processor.

[0032] The infrared light processor and / or microwave light processor of the present invention include a light source emitter, a light reflector, a power supply and a position adjustment component. The intensity of the light source emitted by the infrared light processor and / or microwave light processor and the position of the light source illuminating the substrate can be adjusted according to the actual situation.

[0033] Preferably, the light processing component is located above the substrate.

[0034] Preferably, the plasma treatment component includes an ion air knife.

[0035] The plasma treatment component of this invention also includes a gas source, pipelines, power supply, and upper and lower level adjustment mechanisms.

[0036] Preferably, the plasma processing component is located below the substrate.

[0037] As a preferred embodiment of the present invention, the coating module includes an ultrasonic spraying component.

[0038] In this invention, the ultrasonic spraying assembly is used to prepare a perovskite wet film on a substrate surface.

[0039] Preferably, the ultrasonic spraying assembly includes an ultrasonic sprayer and a spraying material tank connected to the ultrasonic sprayer, wherein the ultrasonic sprayer is located above the substrate.

[0040] Preferably, the ultrasonic sprayer includes at least two linearly arranged ultrasonic nozzles.

[0041] In this invention, the number of ultrasonic nozzles is determined according to the width of the substrate, and the spacing between the ultrasonic nozzles, the spraying angle, the distance between the nozzle and the substrate, and the speed at which the nozzle sprays the atomized perovskite solution are adjusted according to actual needs.

[0042] Preferably, the ultrasonic spraying assembly further includes a liquid collection tank located below the substrate, the liquid collection tank being used to collect perovskite solution or cleaning agent.

[0043] In this invention, the liquid collection tank is mainly used to collect perovskite solutions or cleaning agents generated in the substrate gap, the initial pre-spraying stage, the final stage of production, and the ultrasonic nozzle and pipeline cleaning stage.

[0044] As a preferred technical solution of the present invention, the perovskite layer preparation apparatus further includes a substrate transmission platform, wherein the substrate is placed on the substrate transmission platform;

[0045] The coating module and the nucleation and crystallization module are independently located on both sides of the substrate transmission platform.

[0046] In this invention, the substrate transmission platform is used to move the substrate during the preparation of the perovskite layer. The speed of substrate movement can be adjusted by the substrate transmission platform according to actual production needs.

[0047] As a preferred embodiment of the present invention, the perovskite layer preparation device further includes an exhaust fan, wherein the ultrasonic sprayer, liquid collection tank, nucleation and crystallization module and substrate transmission platform are all located inside the exhaust fan.

[0048] In this invention, the exhaust fan is used to discharge the solvent generated by the evaporation of the perovskite solution.

[0049] Preferably, along the substrate moving direction, the perovskite layer preparation apparatus further includes a feeding module located before the coating module.

[0050] In this invention, the feeding module is used to realize the feeding of the substrate, position correction and feeding speed control.

[0051] Preferably, the feeding module includes a feeding drive belt and a feeding driver for driving the feeding drive belt to move.

[0052] Preferably, along the substrate moving direction, the perovskite layer preparation apparatus further includes a discharge module located after the nucleation and crystallization module.

[0053] In this invention, the discharge module is used to realize the discharge, position correction and discharge speed control after the perovskite layer preparation is completed.

[0054] Preferably, the discharge module includes a discharge drive belt and a discharge driver for driving the discharge drive belt to move.

[0055] Preferably, the perovskite layer preparation apparatus further includes a drying chamber, in which the coating module, nucleation and crystallization module, substrate transmission platform, exhaust fan, feeding module and discharging module are all located, and the exhaust port of the exhaust fan extends out from inside the drying chamber.

[0056] In this invention, the drying room is used to provide a dry environment for the preparation of the perovskite layer, so as to avoid the adverse effects of moisture on the prepared perovskite layer.

[0057] Preferably, at least one filter is provided on the wall of the drying room.

[0058] Thirdly, by way of example, the perovskite layer preparation apparatus provided by the present invention includes:

[0059] The ultrasonic spraying assembly, plasma treatment assembly, infrared light processor, and / or microwave light processor are activated. After adjusting the process parameters, the feed driver drives the feed conveyor belt to move and feed the substrate onto the substrate conveyor platform. The substrate moves on the substrate conveyor platform, and the ultrasonic sprayer atomizes the perovskite liquid in the spraying material box and coats it onto the substrate to obtain a perovskite wet film. The substrate continues to move on the substrate conveyor platform, and the infrared light processor and / or microwave light processor perform light treatment on the substrate, while the plasma treatment assembly performs plasma treatment on the substrate. The light treatment and plasma treatment are performed simultaneously, and the perovskite wet film nucleates and crystallizes to obtain a perovskite layer. The discharge driver drives the discharge conveyor belt to move and send the substrate out of the substrate conveyor platform. After the perovskite layer on the substrate is prepared, it exits the perovskite layer preparation device and automatically enters the next process.

[0060] Fourthly, the present invention provides a perovskite layer, which is obtained by the preparation method described in the first aspect.

[0061] Fifthly, the present invention provides a perovskite solar cell, the perovskite solar cell comprising the perovskite layer described in the fourth aspect.

[0062] The substrate of the present invention includes a substrate and a first charge transport layer covering one side surface of the substrate. The perovskite solar cell includes a substrate, a perovskite layer, a second charge transport layer and an electrode layer stacked sequentially. The first charge transport layer of the substrate is adjacent to the perovskite layer.

[0063] Sixthly, the present invention provides a method for preparing perovskite solar cells, the method comprising the following steps:

[0064] (1) Deposit a first charge transport layer on the substrate;

[0065] (2) Deposit a perovskite layer on the first charge transport layer obtained in step (1);

[0066] (3) Deposit a second charge transport layer on the perovskite layer obtained in step (2);

[0067] (4) An electrode layer is deposited on the second charge transport layer obtained in step (3) to obtain a perovskite solar cell.

[0068] Preferably, the substrate in step (1) includes a conductive glass substrate and / or a textured substrate.

[0069] Preferably, the conductive glass substrate comprises indium tin oxide (ITO) conductive glass and / or fluorine-doped tin oxide (FTO) conductive glass.

[0070] Preferably, the textured substrate includes a crystalline silicon textured substrate for a perovskite-silicon tandem solar cell.

[0071] Preferably, the material of the first charge transport layer in step (1) includes any one or at least two combinations of CuSCN, CuI, CuO, Cu2O, NiO, V2O5, MoO3, Spiro-OMeTAD, P3HT, PTAA, PEDOT:PSS, TiO2, SnO2, ZTO, CdS, C60, ZMO, ZnO, or PCBM. Typical but non-limiting combinations include the combination of CuSCN and CuI, the combination of CuO and Cu2O, the combination of NiO and V2O5, the combination of MoO3 and Spiro-OMeTAD, the combination of P3HT and PTAA, the combination of PEDOT:PSS and TiO2, the combination of ZMO and ZnO, the combination of ZnO and PCBM, the combination of CuSCN, CuI, and CuO, or the combination of Cu2O, NiO, V2O5, and ZTO.

[0072] Preferably, the deposition method in step (1) includes any one or a combination of at least two of the following: evaporation, sputtering, chemical bath deposition, precursor solution spin coating, precursor solution scraping, or slot-die. Typical but non-limiting combinations include the combination of evaporation and sputtering, the combination of sputtering and chemical bath deposition, the combination of chemical bath deposition and precursor solution spin coating, the combination of precursor solution scraping and slot-die, or the combination of evaporation, sputtering, and chemical bath deposition.

[0073] Preferably, the thickness of the first charge transport layer in step (1) is in the range of 0.1 to 50 nm, for example, it can be 0.1 nm, 0.5 nm, 1 nm, 2 nm, 5 nm, 8 nm, 10 nm, 20 nm, 30 nm, 40 nm or 50 nm, but it is not limited to the listed data. Other unlisted values ​​within this range are also applicable.

[0074] Preferably, the material of the second charge transport layer in step (3) includes any one or at least two combinations of CuSCN, CuI, CuO, Cu2O, NiO, V2O5, MoO3, Spiro-OMeTAD, P3HT, PTAA, PEDOT:PSS, TiO2, SnO2, ZTO, CdS, C60, ZMO, ZnO, or PCBM. Typical but non-limiting combinations include the combination of CuSCN and CuI, the combination of CuO and Cu2O, the combination of NiO and V2O5, the combination of MoO3 and Spiro-OMeTAD, the combination of P3HT and PTAA, the combination of PEDOT:PSS and TiO2, the combination of ZMO and ZnO, the combination of ZnO and PCBM, the combination of CuSCN, CuI, and CuO, or the combination of Cu2O, NiO, V2O5, and ZTO.

[0075] Preferably, the deposition method in step (3) includes any one or a combination of at least two of the following: evaporation, sputtering, chemical bath deposition, precursor solution spin coating, precursor solution scraping, or slot-die. Typical but non-limiting combinations include the combination of evaporation and sputtering, the combination of sputtering and chemical bath deposition, the combination of chemical bath deposition and precursor solution spin coating, the combination of precursor solution scraping and slot-die, or the combination of evaporation, sputtering, and chemical bath deposition.

[0076] Preferably, the thickness of the second charge transport layer in step (3) is in the range of 5 to 50 nm, for example, it can be 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm or 50 nm, but it is not limited to the listed data. Other unlisted values ​​within this range are also applicable.

[0077] Preferably, the electrode layer in step (4) includes any one or a combination of at least two of the following: a metal electrode layer, a transparent conductive oxide electrode layer, or a metal nanowire electrode layer. Typical but non-limiting combinations include a combination of a metal electrode layer and a transparent conductive oxide electrode layer, a combination of a transparent conductive oxide electrode layer and a metal nanowire electrode layer, or a combination of a metal electrode layer, a transparent conductive oxide electrode layer, and a metal nanowire electrode layer.

[0078] Preferably, the material of the metal electrode layer includes any one or at least two combinations of Ag, Cu, Au, Al, Mo or Cr. Typical but non-limiting combinations include Ag and Cu, Cu and Au, Au and Al, Mo and Cr, Ag, Cu and Au, or Ag, Cu, Al and Mo.

[0079] Preferably, the thickness of the metal electrode layer is 40 to 100 nm, for example, it can be 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm, but it is not limited to the listed data. Other unlisted values ​​within this range are also applicable.

[0080] Preferably, the deposition method of the metal electrode layer includes evaporation and / or magnetron sputtering.

[0081] Preferably, the material of the transparent conductive oxide electrode layer includes any one or a combination of at least two of ITO, aluminum-doped zinc oxide (AZO), tungsten-doped indium oxide (IWO), or zinc-doped indium oxide (IZO). Typical but non-limiting combinations include combinations of ITO and AZO, combinations of AZO and IWO, combinations of IWO and IZO, or combinations of ITO, IWO, and IZO.

[0082] Preferably, the thickness of the transparent conductive oxide electrode layer is 50 to 100 nm, for example, it can be 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm or 100 nm, but it is not limited to the listed data. Other unlisted values ​​within this range are also applicable.

[0083] Preferably, the deposition method of the transparent conductive oxide electrode layer includes evaporation and / or magnetron sputtering.

[0084] Compared with the prior art, the present invention has the following beneficial effects:

[0085] (1) In this invention, light treatment and plasma treatment are used, which can evaporate the solvent in the perovskite wet film through the combined effect of light energy and ion energy, so that the perovskite nucleates and crystallizes and grows, resulting in a black phase perovskite film with better performance.

[0086] (2) The perovskite layer preparation method in this invention simplifies the preparation process of a single-layer large-area perovskite layer by combining light treatment and plasma treatment. It transforms the difficult-to-control nucleation and crystallization into an instant coating and treatment to form a film layer, thereby improving the preparation efficiency and production capacity of perovskite film layers. Traditional heat treatment annealing takes more than ten minutes, while the method of simultaneous light treatment and plasma treatment takes only seconds, but can achieve the same or better film layer performance as traditional heat treatment, greatly shortening the manufacturing time and equipment cost.

[0087] (3) The method for preparing the perovskite layer in this invention also reduces the requirements for process conditions and production equipment for preparing the perovskite layer, and can also meet the requirements for continuous automated production of the perovskite layer.

[0088] (4) The perovskite layer preparation method provided by the present invention reduces the difficulty of controlling perovskite nucleation and crystallization. By adjusting the composition of the atomized perovskite solution, perovskite layers with different compositions and structures can be obtained. The preparation method has a wide range of applications. Different coating processes can be selected according to different substrates to obtain the optimal perovskite layer, thereby enhancing the performance of perovskite solar cells. The solvent evaporation rate and the perovskite nucleation and crystallization growth rate in the perovskite wet film can be controlled by adjusting the light wave range of the light treatment and the parameters of the plasma treatment, thereby obtaining a high-quality perovskite layer.

[0089] (5) The method for preparing the perovskite layer provided by the present invention can be applied to various perovskite materials, and the application scope of the preparation method is relatively wide. Attached Figure Description

[0090] Figure 1 This is a schematic diagram of the perovskite layer preparation device in Embodiment 1 of the present invention.

[0091] Figure 2 This is a schematic diagram of the perovskite solar cell structure in Embodiment 1 of the present invention.

[0092] Figure 3 This is a SEM image of the perovskite layer surface in Example 1 of the present invention.

[0093] Figure 4 This is a SEM image of the cross-section of the perovskite layer in Example 1 of the present invention.

[0094] Figure 5 This is a SEM image of the perovskite layer surface in Comparative Example 3 of the present invention.

[0095] Figure 6 This is a SEM image of the cross-section of the perovskite layer in Comparative Example 3 of the present invention.

[0096] Among them, 1-light processing component; 2-plasma processing component; 3-ultrasonic sprayer; 4-spraying material box; 5-liquid collection tank; 6-substrate transmission platform; 7-exhaust fan; 8-feed transmission belt; 9-feed driver; 10-discharge transmission belt; 11-drying room; 12-exhaust vent; 13-filter; 14-substrate; 15-first charge transport layer; 16-perovskite layer; 17-second charge transport layer; 18-electrode layer. Detailed Implementation

[0097] It should be understood that in the description of this invention, the terms "center," "longitudinal," "lateral," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. These terms are used only for the convenience of describing the invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the invention. Furthermore, the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined with "first," "second," etc., may explicitly or implicitly include one or more of that feature. In the description of this invention, unless otherwise stated, "a plurality of" means two or more.

[0098] It should be noted that, in the description of this invention, unless otherwise explicitly specified and limited, the terms "set," "connected," and "linked" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0099] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0100] In one specific embodiment, the present invention provides a method for preparing a perovskite layer, the method comprising the following steps:

[0101] A perovskite solution is coated onto a substrate to obtain a perovskite wet film; photo-treatment and plasma treatment are then performed to nucleate and crystallize the perovskite wet film, resulting in a perovskite layer.

[0102] The perovskite layer preparation method provided by this invention simplifies the preparation process of a single-layer, large-area perovskite layer by combining light treatment and plasma treatment. This transforms the difficult-to-control nucleation and crystallization process into an instant coating, treatment, and film formation, improving the preparation efficiency and production capacity of perovskite films, reducing the requirements for process conditions and production equipment, and meeting the requirements for continuous automated production of perovskite layers. The preparation method reduces the difficulty of controlling perovskite nucleation and crystallization, and the quality of the perovskite layer can be improved by adjusting the composition of the atomized perovskite solution, the coating process, the light treatment process, and the plasma treatment process. The preparation method is applicable to various perovskite materials and has a wide range of applications.

[0103] Furthermore, the coating includes ultrasonic spraying.

[0104] In this invention, ultrasonic spraying can greatly reduce the splashing of atomized perovskite solution during the coating process, thereby greatly reducing the waste of atomized perovskite solution and increasing the utilization efficiency of atomized perovskite solution.

[0105] Furthermore, the light treatment and plasma treatment are performed simultaneously.

[0106] In this invention, light treatment and plasma treatment are performed simultaneously. The combined effect of light energy and ion energy can cause the solvent in the perovskite wet film to evaporate, allowing the perovskite to nucleate and crystallize, resulting in a black phase perovskite film with superior performance. At the same time, since the time for perovskite film curing and crystallization achieved by light treatment and plasma treatment is shorter than that of traditional heat treatment annealing, which takes more than ten minutes, the processing time of the method using light treatment and plasma treatment is in the second range, but the same or better film performance can be achieved as traditional heat treatment, greatly reducing manufacturing time and equipment costs.

[0107] Furthermore, the light processing includes infrared light processing and / or microwave light processing.

[0108] In this invention, infrared light treatment enables the perovskite wet film to absorb energy, the solvent to evaporate, and the perovskite to nucleate and crystallize; microwave light treatment enables the perovskite wet film to absorb energy, the solvent to evaporate, and the perovskite to nucleate and crystal grow.

[0109] In another specific implementation, such as Figure 1 As shown, the present invention provides a perovskite layer preparation apparatus for the above preparation method, the perovskite layer preparation apparatus comprising a coating module and a nucleation and crystallization module arranged sequentially along the substrate moving direction;

[0110] The nucleation and crystallization module includes a light processing component 1 and a plasma processing component 2.

[0111] The perovskite layer preparation device of the present invention can complete the nucleation and crystallization of perovskite wet film in one station or on one piece of equipment. It has low cost and small footprint, and can also achieve uninterrupted continuous production.

[0112] Furthermore, the light processing component 1 includes an infrared light processor and / or a microwave light processor.

[0113] The infrared light processor and / or microwave light processor of the present invention include a light source emitter, a light reflector, a power supply and a position adjustment component. The intensity of the light source emitted by the infrared light processor and / or microwave light processor and the position of the light source illuminating the substrate can be adjusted according to the actual situation.

[0114] Furthermore, the light processing component 1 is located above the substrate.

[0115] Furthermore, the plasma treatment component 2 includes an ion air knife.

[0116] The ion treatment component 2 of the present invention also includes a gas source, pipelines, power supply and upper and lower adjustment mechanism.

[0117] Furthermore, the plasma processing component 2 is located below the substrate.

[0118] Furthermore, the coating module includes an ultrasonic spraying assembly.

[0119] In this invention, the ultrasonic spraying assembly is used to prepare a perovskite wet film on a substrate surface.

[0120] Furthermore, the ultrasonic spraying assembly includes an ultrasonic sprayer 3 and a spraying material box 4 connected to the ultrasonic sprayer 3, wherein the ultrasonic sprayer 3 is located above the substrate.

[0121] Furthermore, the ultrasonic sprayer 3 includes at least two linearly arranged ultrasonic nozzles.

[0122] In this invention, the number of ultrasonic nozzles is determined according to the width of the substrate, and the spacing between the ultrasonic nozzles, the spraying angle, the distance between the nozzle and the substrate, and the speed at which the nozzle sprays the atomized perovskite solution are adjusted according to actual needs.

[0123] Furthermore, the ultrasonic spraying assembly also includes a liquid collection tank 5 located below the substrate, the liquid collection tank 5 being used to collect perovskite solution or cleaning agent.

[0124] In this invention, the liquid collection tank 5 is mainly used to collect perovskite solution or cleaning agent generated in the substrate gap, the initial pre-spraying stage, the final stage of production, and the ultrasonic nozzle and pipeline cleaning stage.

[0125] Furthermore, the perovskite layer preparation apparatus also includes a substrate transmission platform 6, on which the substrate is placed;

[0126] The coating module and the nucleation and crystallization module are independently disposed on both sides of the substrate transmission platform 6.

[0127] In this invention, the substrate transmission platform 6 is used to move the substrate during the preparation of the perovskite layer. The speed of substrate movement can be adjusted by the substrate transmission platform 6 according to actual production needs.

[0128] Furthermore, the perovskite layer preparation device also includes an exhaust fan 7, and the ultrasonic sprayer 3, liquid collection tank 5, nucleation and crystallization module and substrate transmission platform 6 are all located inside the exhaust fan 7.

[0129] In this invention, the exhaust fan 7 is used to discharge the solvent generated by the evaporation of the perovskite solution.

[0130] Furthermore, along the substrate moving direction, the perovskite layer preparation apparatus also includes a feeding module located before the coating module.

[0131] In this invention, the feeding module is used to realize the feeding of the substrate, position correction and feeding speed control.

[0132] Furthermore, the feeding module includes a feeding drive belt 8 and a feeding driver 9 for driving the feeding drive belt 8 to move.

[0133] Furthermore, along the substrate moving direction, the perovskite layer preparation apparatus also includes a discharge module located after the nucleation and crystallization module.

[0134] In this invention, the discharge module is used to realize the discharge, position correction and discharge speed control after the perovskite layer preparation is completed.

[0135] Furthermore, the discharge module includes a discharge drive belt 10 and a discharge driver for driving the discharge drive belt 10 to move.

[0136] Furthermore, the perovskite layer preparation device also includes a drying chamber 11, in which the coating module, nucleation and crystallization module, substrate transmission platform 6, exhaust fan 7, feeding module and discharging module are all located. The exhaust port 12 of the exhaust fan 7 extends out from the drying chamber 11.

[0137] In this invention, the drying room 11 is used to provide a dry environment for the preparation of the perovskite layer, so as to avoid the adverse effects of moisture on the prepared perovskite layer.

[0138] Furthermore, at least one filter 13 is provided on the wall of the drying room 11.

[0139] In another specific embodiment, exemplarily, the working method of the perovskite layer preparation apparatus provided by the present invention includes:

[0140] The ultrasonic spraying assembly, plasma treatment assembly 2, and infrared light processor and / or microwave light processor are activated. After adjusting the process parameters, the feed driver 9 drives the feed conveyor belt 8 to move and feed the substrate onto the substrate transmission platform 6. The substrate moves on the substrate transmission platform 6, and the ultrasonic sprayer 3 atomizes the perovskite liquid in the spraying material box 4 and coats it onto the substrate to obtain a perovskite wet film. The substrate continues to move on the substrate transmission platform 6, and the infrared light processor and / or microwave light processor perform light treatment on the substrate, while the plasma treatment assembly 2 performs plasma treatment on the substrate. The light treatment and plasma treatment are performed simultaneously, and the perovskite wet film nucleates and crystallizes to obtain a perovskite layer. The discharge driver drives the discharge conveyor belt 10 to move and send the substrate out of the substrate transmission platform 6. After the perovskite layer on the substrate is prepared, it exits the perovskite layer preparation device and automatically enters the next process.

[0141] In another specific embodiment, the present invention provides a perovskite layer obtained by the above-described method for preparing a perovskite layer.

[0142] In another specific embodiment, the present invention provides a perovskite solar cell, the perovskite solar cell comprising the perovskite layer described above.

[0143] like Figure 2 As shown, the substrate of the present invention includes a substrate 14 and a first charge transport layer 15 covering one side surface of the substrate 14. The perovskite solar cell includes a substrate, a perovskite layer 16, a second charge transport layer 17 and an electrode layer 18 stacked sequentially. The first charge transport layer 15 of the substrate is adjacent to the perovskite layer 16.

[0144] In another specific embodiment, the present invention provides a method for preparing perovskite solar cells, the method comprising the following steps:

[0145] (1) Deposit a first charge transport layer 15 on a conductive glass substrate 14 or a textured substrate 14;

[0146] (2) Deposit a perovskite layer 16 on the first charge transport layer 15 obtained in step (1);

[0147] (3) Deposit a second charge transport layer 17 on the perovskite layer 16 obtained in step (2);

[0148] (4) An electrode layer 18 is deposited on the second charge transport layer 17 obtained in step (3) to obtain a perovskite solar cell.

[0149] Preferably, the substrate 14 in step (1) includes a conductive glass substrate and / or a textured substrate.

[0150] Furthermore, the conductive glass substrate includes ITO conductive glass and / or FTO conductive glass.

[0151] Furthermore, the textured substrate includes a crystalline silicon textured substrate for perovskite-silicon tandem solar cells.

[0152] Further, in step (1), the material of the first charge transport layer 15 includes any one or a combination of at least two of CuSCN, CuI, CuO, Cu2O, NiO, V2O5, MoO3, Spiro-OMeTAD, P3HT, PTAA, PEDOT:PSS, TiO2, SnO2, ZTO, CdS, C60, ZMO, ZnO or PCBM.

[0153] Further, the deposition method described in step (1) includes any one or a combination of at least two of the following: evaporation, sputtering, chemical bath deposition, spin coating with precursor solution, blade coating with precursor solution, or slot-die method.

[0154] Further, in step (1), the thickness of the first charge transport layer 15 ranges from 0.1 to 50 nm.

[0155] Further, in step (3), the material of the second charge transport layer 17 includes any one or a combination of at least two of CuSCN, CuI, CuO, Cu2O, NiO, V2O5, MoO3, Spiro-OMeTAD, P3HT, PTAA, PEDOT:PSS, TiO2, SnO2, ZTO, CdS, C60, ZMO, ZnO or PCBM.

[0156] Further, the deposition method described in step (3) includes any one or a combination of at least two of the following: evaporation, sputtering, chemical bath deposition, spin coating with precursor solution, blade coating with precursor solution, or slot-die method.

[0157] Furthermore, in step (3), the thickness of the second charge transport layer 17 ranges from 5 to 50 nm.

[0158] Further, the electrode layer 18 in step (4) includes any one or a combination of at least two of the following: a metal electrode layer, a transparent conductive oxide electrode layer, or a metal nanowire electrode layer.

[0159] Furthermore, the material of the metal electrode layer includes any one or a combination of at least two of Ag, Cu, Au, Al, Mo, or Cr.

[0160] Furthermore, the thickness of the metal electrode layer is 40–100 nm.

[0161] Furthermore, the deposition method of the metal electrode layer includes evaporation and / or magnetron sputtering.

[0162] Furthermore, the material of the transparent conductive oxide electrode layer includes any one or a combination of at least two of ITO, AZO, IWO, or IZO-doped material.

[0163] Furthermore, the thickness of the transparent conductive oxide electrode layer is 50–100 nm.

[0164] Preferably, the deposition method of the transparent conductive oxide electrode layer includes evaporation and / or magnetron sputtering.

[0165] Example 1

[0166] This embodiment provides a method for fabricating a perovskite solar cell, the method comprising:

[0167] (1) A NiO thin film with a thickness of 20 nm was prepared on FTO conductive glass by sputtering to obtain a substrate;

[0168] (2) Turn on the ultrasonic sprayer, ion air knife and infrared light processor. Adjust the power of the ultrasonic sprayer to 8W, the distance between the ultrasonic nozzle and the substrate to 8cm, the power of the infrared light processor to 15W, the distance between the infrared light processor and the substrate to 3cm, the flow rate of the working gas N2 of the ion air knife to 1000sccm, the power of the ion air knife to 150W, and the distance between the ion air knife and the substrate to 10cm.

[0169] The feed driver moves the feed conveyor belt and feeds the substrate onto the substrate conveyor platform; the substrate moves on the substrate conveyor platform, and the ultrasonic sprayer sprays 1.2 mol / L FA from the raw material tank. 0.85 Cs 0.15 After the PbI3 solution is atomized, it is coated onto the substrate to obtain a perovskite wet film. The substrate continues to move on the substrate transmission platform. The infrared light processor performs infrared light treatment on the substrate, and the ion air knife performs plasma treatment on the substrate. The infrared light treatment and plasma treatment are performed simultaneously. After the perovskite wet film nucleates and crystallizes, a perovskite layer is obtained. The discharge driver drives the discharge transmission belt to move and send the substrate out of the substrate transmission platform. The perovskite layer on the substrate is then prepared.

[0170] (3) A CuSCN layer with a thickness of 25 nm is deposited on the perovskite layer obtained in step (2) by sputtering.

[0171] (4) An Ag electrode layer with a thickness of 60 nm is deposited on the CuSCN layer obtained in step (3) by evaporation to obtain a perovskite solar cell.

[0172] In step (2) of this embodiment, the time for the substrate to pass through the infrared light processor and the ion air knife is 3 seconds.

[0173] The surface and cross-sectional morphology of the perovskite layer prepared in step (2) were tested using a scanning electron microscope, and the results were as follows: Figure 3 and Figure 4 The scanning electron microscope image shown is from Figure 3 and Figure 4 It can be seen that the perovskite film obtained by infrared light treatment and plasma treatment has a large grain size, and the grains are densely packed with a smooth surface.

[0174] Example 2

[0175] This embodiment provides a method for fabricating a perovskite solar cell, the method comprising:

[0176] (1) A CuSCN thin film with a thickness of 0.1 nm was prepared on ITO conductive glass by evaporation to obtain a substrate;

[0177] (2) Turn on the ultrasonic sprayer, ion air knife and microwave light processor. Adjust the power of the ultrasonic sprayer to 5W, the distance between the ultrasonic nozzle and the substrate to 10cm, the power of the microwave light processor to 20W, the distance between the microwave light processor and the substrate to 1cm, the flow rate of the working gas N2 of the ion air knife to 500sccm, the power of the ion air knife to 200W, and the distance between the ion air knife and the substrate to 5cm.

[0178] The feed driver moves the feed conveyor belt and feeds the substrate onto the substrate conveyor platform. As the substrate moves on the platform, an ultrasonic sprayer atomizes a 0.8 mol / L CsPbI3 solution from the coating material tank and coats it onto the substrate, forming a perovskite wet film. The substrate continues to move on the platform, where a microwave optical processor performs microwave optical treatment, and an ion air knife performs plasma treatment. These processes occur simultaneously, and the perovskite wet film nucleates and crystallizes to form a perovskite layer. Finally, the discharge driver moves the discharge conveyor belt and sends the substrate off the substrate conveyor platform, completing the preparation of the perovskite layer on the substrate.

[0179] (3) A MoO3 layer with a thickness of 50 nm is deposited on the perovskite layer obtained in step (2) by sputtering.

[0180] (4) A Cu electrode layer with a thickness of 40 nm is deposited on the MoO3 layer obtained in step (3) by magnetron sputtering to obtain a perovskite solar cell.

[0181] In step (2) of this embodiment, the time for the substrate to pass through the infrared light processor and the ion air knife is 2 seconds.

[0182] Example 3

[0183] This embodiment provides a method for fabricating a perovskite solar cell, the method comprising:

[0184] (1) A ZMO thin film with a thickness of 50 nm was prepared on FTO conductive glass by chemical bath deposition to obtain a substrate;

[0185] (2) Turn on the ultrasonic sprayer, ion air knife and infrared light processor. Adjust the power of the ultrasonic sprayer to 10W, the distance between the ultrasonic nozzle and the substrate to 5cm, the power of the infrared light processor to 10W, the distance between the infrared light processor and the substrate to 5cm, the flow rate of the working gas N2 of the ion air knife to 1500sccm, the power of the ion air knife to 100W, and the distance between the ion air knife and the substrate to 20cm.

[0186] The feed driver moves the feed conveyor belt and feeds the substrate onto the substrate conveyor platform. As the substrate moves on the platform, an ultrasonic sprayer atomizes a 1.6 mol / L CsPbI3 solution from the coating material tank and coats it onto the substrate, forming a perovskite wet film. The substrate continues to move on the platform, where an infrared light processor performs infrared light treatment, and an ion air knife performs plasma treatment. The infrared light treatment and plasma treatment are performed simultaneously, and the perovskite wet film nucleates and crystallizes to form a perovskite layer. Finally, the discharge driver moves the discharge conveyor belt and sends the substrate off the substrate conveyor platform, completing the preparation of the perovskite layer on the substrate.

[0187] (3) A SnO2 layer with a thickness of 5 nm is deposited on the perovskite layer obtained in step (2) by evaporation;

[0188] (4) An AZO electrode layer with a thickness of 50 nm is deposited on the SnO2 layer obtained in step (3) by magnetron sputtering to obtain a perovskite solar cell.

[0189] In step (2) of this embodiment, the time for the substrate to pass through the infrared light processor and the ion air knife is 4 seconds.

[0190] Example 4

[0191] This embodiment provides a method for preparing a perovskite solar cell. Except for adjusting the power of the ultrasonic sprayer to 2W, the rest is the same as in Embodiment 1.

[0192] In step (2) of this embodiment, the time for the substrate to pass through the infrared light processor and the ion air knife is 3 seconds.

[0193] Example 5

[0194] This embodiment provides a method for preparing a perovskite solar cell. Except for adjusting the power of the ultrasonic sprayer to 15W, the rest is the same as in Embodiment 1.

[0195] In step (2) of this embodiment, the time for the substrate to pass through the infrared light processor and the ion air knife is 3 seconds.

[0196] Example 6

[0197] This embodiment provides a method for fabricating a perovskite solar cell. Except for adjusting the distance between the ultrasonic nozzle and the substrate to 2 cm, the rest is the same as in Embodiment 1.

[0198] In step (2) of this embodiment, the time for the substrate to pass through the infrared light processor and the ion air knife is 2 seconds.

[0199] Example 7

[0200] This embodiment provides a method for fabricating a perovskite solar cell. Except for adjusting the distance between the ultrasonic nozzle and the substrate to 15 cm, the rest is the same as in Embodiment 1.

[0201] In step (2) of this embodiment, the time for the substrate to pass through the infrared light processor and the ion air knife is 4 seconds.

[0202] Example 8

[0203] This embodiment provides a method for fabricating a perovskite solar cell. Except for adjusting the power of the infrared light processor to 5W, the rest is the same as in Embodiment 1.

[0204] In step (2) of this embodiment, the time for the substrate to pass through the infrared light processor and the ion air knife is 5 seconds.

[0205] Example 9

[0206] This embodiment provides a method for fabricating a perovskite solar cell. Except for adjusting the power of the infrared light processor to 25W, the rest is the same as in Embodiment 1.

[0207] In step (2) of this embodiment, the time for the substrate to pass through the infrared light processor and the ion air knife is 2 seconds.

[0208] Example 10

[0209] This embodiment provides a method for fabricating a perovskite solar cell. Except for adjusting the distance between the infrared light processor and the substrate to 0.5 cm, the rest is the same as in Embodiment 1.

[0210] In step (2) of this embodiment, the time for the substrate to pass through the infrared light processor and the ion air knife is 2 seconds.

[0211] Example 11

[0212] This embodiment provides a method for fabricating a perovskite solar cell. Except for adjusting the distance between the infrared light processor and the substrate to 8 cm, the rest is the same as in Embodiment 1.

[0213] In step (2) of this embodiment, the time for the substrate to pass through the infrared light processor and the ion air knife is 5 seconds.

[0214] Example 12

[0215] This embodiment provides a method for preparing a perovskite solar cell. Except for adjusting the flow rate of the working gas N2 of the ion air knife to 300 sccm, the rest is the same as in Example 1.

[0216] In step (2) of this embodiment, the time for the substrate to pass through the infrared light processor and the ion air knife is 5 seconds.

[0217] Example 13

[0218] This embodiment provides a method for preparing a perovskite solar cell. Except for adjusting the flow rate of the working gas N2 of the ion air knife to 2000 sccm, the rest is the same as in Example 1.

[0219] In step (2) of this embodiment, the time for the substrate to pass through the infrared light processor and the ion air knife is 2 seconds.

[0220] Example 14

[0221] This embodiment provides a method for fabricating a perovskite solar cell. Except for adjusting the power of the ion air knife to 50W, the rest is the same as in Embodiment 1.

[0222] In step (2) of this embodiment, the time for the substrate to pass through the infrared light processor and the ion air knife is 4 seconds.

[0223] Example 15

[0224] This embodiment provides a method for preparing a perovskite solar cell. Except for adjusting the power of the ion air knife to 250W, the rest is the same as in Embodiment 1.

[0225] In step (2) of this embodiment, the time for the substrate to pass through the infrared light processor and the ion air knife is 2 seconds.

[0226] Example 16

[0227] This embodiment provides a method for fabricating a perovskite solar cell. Except for adjusting the distance between the ion air knife and the substrate to 3 cm, the rest is the same as in Embodiment 1.

[0228] In step (2) of this embodiment, the time for the substrate to pass through the infrared light processor and the ion air knife is 2 seconds.

[0229] Example 17

[0230] This embodiment provides a method for fabricating a perovskite solar cell. Except for adjusting the distance between the ion air knife and the substrate to 25 cm, the rest is the same as in Embodiment 1.

[0231] In step (2) of this embodiment, the time for the substrate to pass through the infrared light processor and the ion air knife is 5 seconds.

[0232] Comparative Example 1

[0233] This comparative example provides a method for fabricating a perovskite solar cell, the method comprising:

[0234] (1) A NiO thin film with a thickness of 20 nm was prepared on FTO conductive glass by sputtering to obtain a substrate;

[0235] (2) Turn on the ultrasonic sprayer and infrared light processor, adjust the power of the ultrasonic sprayer to 8W, the distance between the ultrasonic nozzle and the substrate to 7cm, the power of the infrared light processor to 15W, the distance between the infrared light processor and the substrate to 3cm, and the transmission speed of the substrate transmission platform to the substrate to 8m / min.

[0236] The feed driver moves the feed conveyor belt and feeds the substrate onto the substrate conveyor platform; the substrate moves on the substrate conveyor platform, and the ultrasonic sprayer sprays 1.2 mol / L FA from the raw material tank. 0.85 Cs 0.15 After the PbI3 solution is atomized, it is coated on the substrate to obtain a perovskite wet film. The substrate continues to move on the substrate transmission platform, and the infrared light processor performs infrared light treatment on the substrate. After the perovskite wet film nucleates and crystallizes, a perovskite layer is obtained. The discharge driver drives the discharge transmission belt to move and send the substrate out of the substrate transmission platform. The perovskite layer on the substrate is then prepared.

[0237] (3) A CuSCN layer with a thickness of 25 nm is deposited on the perovskite layer obtained in step (2) by sputtering.

[0238] (4) An Ag electrode layer with a thickness of 60 nm is deposited on the CuSCN layer obtained in step (3) by evaporation to obtain a perovskite solar cell.

[0239] In step (2) of this embodiment, the substrate passes through the infrared light processor for 8 seconds.

[0240] Comparative Example 2

[0241] This comparative example provides a method for fabricating a perovskite solar cell, the method comprising:

[0242] (1) A NiO thin film with a thickness of 20 nm was prepared on FTO conductive glass by sputtering to obtain a substrate;

[0243] (2) Turn on the ultrasonic sprayer and ion air knife, adjust the power of the ultrasonic sprayer to 8W, the distance between the ultrasonic nozzle and the substrate to 7cm, the flow rate of the working gas N2 of the ion air knife to 1000sccm, the power of the ion air knife to 150W, the distance between the ion air knife and the substrate to 10cm, and the transmission speed of the substrate transmission platform to the substrate to 8m / min.

[0244] The feed driver moves the feed conveyor belt and feeds the substrate onto the substrate conveyor platform; the substrate moves on the substrate conveyor platform, and the ultrasonic sprayer sprays 1.2 mol / L FA from the raw material tank. 0.85 Cs 0.15 After the PbI3 solution is atomized, it is coated on the substrate to obtain a perovskite wet film. The substrate continues to move on the substrate transmission platform, and the substrate is subjected to plasma treatment by an ion air knife. After the perovskite wet film nucleates and crystallizes, a perovskite layer is obtained. The discharge driver drives the discharge transmission belt to move and send the substrate out of the substrate transmission platform. The perovskite layer on the substrate is then prepared.

[0245] (3) A CuSCN layer with a thickness of 25 nm is deposited on the perovskite layer obtained in step (2) by sputtering.

[0246] (4) An Ag electrode layer with a thickness of 60 nm is deposited on the CuSCN layer obtained in step (3) by evaporation to obtain a perovskite solar cell.

[0247] In step (2) of this embodiment, the substrate passes through the ion air knife for 9 seconds.

[0248] Comparative Example 3

[0249] This comparative example provides a method for fabricating a perovskite solar cell, the method comprising:

[0250] (1) A NiO thin film with a thickness of 20 nm was prepared on FTO conductive glass by sputtering to obtain a substrate;

[0251] (2) The ultrasonic sprayer sprays 1.2 mol / L FA from the coating material tank. 0.85 Cs 0.15 After the PbI3 solution is atomized, it is coated on the substrate to obtain a perovskite wet film. Then, it is placed in a cavity and quickly evacuated to a vacuum level of less than 20 Pa to pre-cur the wet film. Then, it is transferred to an annealing furnace for annealing at 150°C for 15 min to finally obtain a black phase perovskite thin film.

[0252] (3) A CuSCN layer with a thickness of 25 nm is deposited on the perovskite layer obtained in step (2) by sputtering.

[0253] (4) An Ag electrode layer with a thickness of 60 nm is deposited on the CuSCN layer obtained in step (3) by evaporation to obtain a perovskite solar cell.

[0254] In this embodiment, the curing and crystallization of the perovskite wet film to obtain the perovskite thin film requires at least 15 minutes.

[0255] The surface and cross-sectional morphology of the perovskite layer prepared in step (2) were tested using a scanning electron microscope, and the results were as follows: Figure 5 and Figure 6 The scanning electron microscope image shown.

[0256] The perovskite solar cells prepared in Examples 1-19 and Comparative Examples 1-3 were subjected to IV testing. The test results are shown in Table 1. The test method was as follows: under standard test conditions, the irradiance of the light source was made to reach 1000 W / m². 2 The device temperature needs to be stable at 25±1℃.

[0257] Table 1

[0258]

[0259]

[0260] From Table 1 and Figures 3-6 We can obtain:

[0261] (1) The perovskite solar cells prepared in Examples 1-3 have larger perovskite grains and higher film quality. In this invention, light treatment and plasma treatment are used, which can evaporate the solvent in the wet perovskite film through the combined effect of light energy and ion energy, so as to promote the nucleation and growth of perovskite crystals, resulting in a black phase perovskite film with better performance. At the same time, the perovskite layer preparation method simplifies the preparation process of a single-layer large-area perovskite layer by combining light treatment and plasma treatment, transforming the difficult-to-control nucleation and crystallization into a film layer that is coated, treated and formed immediately, thereby improving the preparation efficiency and production capacity of perovskite film layers. Traditional heat treatment annealing takes more than ten minutes, while the light treatment method can achieve the same results. The method of simultaneous heat treatment and plasma treatment has a processing time in the seconds range, but can achieve film performance that is the same as or better than that of traditional heat treatment, greatly reducing manufacturing time and equipment costs. Simultaneously, the preparation method reduces the requirements for process conditions and production equipment in perovskite layer preparation, and can also meet the requirements for continuous automated production of perovskite layers. The preparation method also reduces the difficulty of controlling perovskite nucleation and crystallization; the quality of the perovskite layer can be improved by adjusting the composition of the atomized perovskite solution, the coating process, the phototreatment process, and the plasma treatment process. The preparation method is applicable to various perovskite materials and has a wide range of applications.

[0262] (2) By comparing Example 1 with Examples 4 and 5, it can be seen that the power of ultrasonic spraying in this invention will affect the quality of the perovskite layer, thereby affecting the performance of the prepared perovskite solar cell. When the power of ultrasonic spraying is too low, the performance of the perovskite film will deteriorate. This is because the perovskite composition is unbalanced and the organic components are excessive. When the power of ultrasonic spraying is too high, the performance of the perovskite film will deteriorate. This is because the perovskite composition is unbalanced and the lead iodide is excessive.

[0263] (3) By comparing Example 1 with Examples 6 and 7, it can be seen that the distance between the ultrasonic nozzle and the substrate in ultrasonic spraying in this invention will affect the quality of the perovskite layer, thereby affecting the performance of the prepared perovskite solar cell. When the distance between the ultrasonic nozzle and the substrate in ultrasonic spraying is too small, the performance of the perovskite film will deteriorate. This is because the perovskite composition is unbalanced and the organic component is excessive. When the distance between the ultrasonic nozzle and the substrate in ultrasonic spraying is too large, the performance of the perovskite film will deteriorate. This is because the perovskite composition is unbalanced and the lead iodide is excessive.

[0264] (4) By comparing Example 1 with Examples 8 and 9, it can be seen that the power of infrared light treatment in this invention will affect the quality of the perovskite layer, thereby affecting the performance of the prepared perovskite solar cell. When the power of infrared light treatment is too low, the performance of the perovskite film will deteriorate. This is because the perovskite composition is unbalanced and the organic components are excessive. When the power of infrared light treatment is too high, the performance of the perovskite film will deteriorate. This is because the perovskite composition is unbalanced and the lead iodide is excessive.

[0265] (5) By comparing Example 1 with Examples 10 and 11, it can be seen that the distance between the infrared light processor and the substrate in the infrared light treatment of the present invention will affect the quality of the perovskite layer, thereby affecting the performance of the prepared perovskite solar cell. When the distance between the infrared light processor and the substrate is too small, the performance of the perovskite film will deteriorate. This is due to the imbalance of perovskite composition and the excess of lead iodide.

[0266] When the distance between the infrared light processor and the substrate is too large, the performance of the perovskite film will deteriorate. This is due to the imbalance of perovskite composition and the excess of organic components.

[0267] (6) By comparing Example 1 with Examples 12 and 13, it can be seen that the flow rate of the working gas in the plasma treatment of the present invention will affect the quality of the perovskite layer, thereby affecting the performance of the prepared perovskite solar cell. When the flow rate of the working gas in the plasma treatment is too low, the performance of the perovskite film will deteriorate. This is because the perovskite composition is unbalanced and the organic components are excessive. When the flow rate of the working gas in the plasma treatment is too high, the performance of the perovskite film will deteriorate. This is because the perovskite composition is unbalanced and the lead iodide is excessive.

[0268] (7) By comparing Example 1 with Examples 14 and 15, it can be seen that the power of plasma treatment in this invention will affect the quality of the perovskite layer, thereby affecting the performance of the prepared perovskite solar cell. When the power of plasma treatment is too low, the performance of the perovskite film will deteriorate. This is because the perovskite composition is unbalanced and the organic components are excessive. When the power of plasma treatment is too high, the performance of the perovskite film will deteriorate. This is because the perovskite composition is unbalanced and the lead iodide is excessive.

[0269] (8) By comparing Example 1 with Examples 16 and 17, it can be seen that the distance between the ion air knife and the substrate in the plasma treatment of the present invention will affect the quality of the perovskite layer, thereby affecting the performance of the prepared perovskite solar cell. When the distance between the ion air knife and the substrate in the plasma treatment is too small, the performance of the perovskite film will deteriorate. This is because the perovskite composition is unbalanced and lead iodide is excessive. When the distance between the ion air knife and the substrate in the plasma treatment is too large, the performance of the perovskite film will deteriorate. This is because the perovskite composition is unbalanced and organic components are excessive.

[0270] (9) By comparing Example 1 and Comparative Example 1, it can be seen that the plasma treatment in the present invention can evaporate the solvent in the perovskite wet film, accelerate the solidification and crystallization speed of the perovskite film layer, and improve the production efficiency. However, the plasma treatment alone will affect the quality of the perovskite layer, thereby affecting the performance of the prepared perovskite solar cell.

[0271] (10) By comparing Example 1 and Comparative Example 2, it can be seen that the light treatment in this invention will affect the quality of the perovskite layer, thereby affecting the performance of the prepared perovskite solar cell. The light treatment in this invention can make the solvent in the perovskite wet film evaporate, accelerate the solidification and crystallization speed of the perovskite film layer, and improve the production efficiency. However, the light treatment alone will affect the quality of the perovskite layer, thereby affecting the performance of the prepared perovskite solar cell.

[0272] (11) By comparing Example 1 and Comparative Example 3, it can be seen that the curing and crystallization speed of the perovskite film in this invention is much higher than that of traditional heat treatment, which greatly improves the preparation efficiency of the perovskite film. Moreover, the requirements for process conditions and production equipment when preparing the perovskite film in this application are low, and it can also meet the requirements for continuous automated production of perovskite film, which is conducive to large-scale and low-cost promotion and use. At the same time, the performance of the perovskite solar cell prepared in this invention can reach or even surpass that of the perovskite solar cell prepared by traditional heat treatment, indicating that the perovskite layer preparation method in this invention is a feasible and efficient method.

[0273] In summary, this invention employs both light and plasma treatment, which, through the combined effect of light and ion energy, causes the solvent in the perovskite wet film to evaporate, promoting perovskite nucleation and crystal growth, resulting in a black phase perovskite film with superior performance. The perovskite layer preparation method in this invention simplifies the preparation process of a single-layer, large-area perovskite layer by combining light and plasma treatment. This transforms the difficult-to-control nucleation and crystallization process into an instant coating and treatment process, improving the preparation efficiency and production capacity of perovskite films. Traditional heat treatment annealing takes more than ten minutes, while the method using simultaneous light and plasma treatment takes only seconds, achieving the same or better film performance as traditional heat treatment, significantly reducing manufacturing time and equipment costs. Furthermore, this preparation method reduces the preparation time of perovskite films. The requirements for process conditions and production equipment for the perovskite layer can also meet the requirements for continuous automated production of the perovskite layer; the preparation method reduces the difficulty of controlling perovskite nucleation and crystallization, and perovskite layers with different compositions and structures can be obtained by adjusting the composition of the atomized perovskite solution, making the preparation method widely applicable; different coating processes can be selected according to different substrates to obtain the optimal perovskite layer, thereby enhancing the performance of perovskite solar cells; the rate of solvent evaporation and the rate of perovskite nucleation and crystallization growth in the perovskite wet film can be controlled by adjusting the light wave range of the light treatment and the parameters of the plasma treatment, thereby obtaining a high-quality perovskite layer; the preparation method is applicable to various perovskite materials, making it widely applicable.

[0274] The above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.

Claims

1. A method for preparing a perovskite layer, characterized in that, The preparation method includes the following steps: A perovskite solution is coated onto a substrate to obtain a perovskite wet film; photo-treatment and plasma treatment are performed to nucleate and crystallize the perovskite wet film to obtain a perovskite layer. The light treatment and plasma treatment are performed simultaneously. The light processing includes infrared light processing and / or microwave light processing; The power of the infrared light processing is 10~20W; The power of the plasma treatment is 100~200W.

2. The preparation method according to claim 1, characterized in that, The coating includes ultrasonic spraying.

3. The preparation method according to claim 2, characterized in that, The ultrasonic spraying power is 5~10W.

4. The preparation method according to claim 2, characterized in that, The distance between the ultrasonic nozzle and the substrate in the ultrasonic spraying process is 5-10 cm.

5. The preparation method according to claim 1, characterized in that, The distance between the infrared light processor and the substrate is 1~5cm.

6. The preparation method according to claim 1, characterized in that, The working gas for the plasma treatment includes nitrogen and / or an inert gas.

7. The preparation method according to claim 1, characterized in that, The flow rate of the working gas for plasma treatment is 500~1500 sccm.

8. The preparation method according to claim 1, characterized in that, The distance between the ion air knife used in the plasma treatment and the substrate is 5~20cm.

9. The preparation method according to claim 1, characterized in that, The preparation method is carried out using a perovskite layer preparation device; The perovskite layer preparation device includes a coating module and a nucleation and crystallization module arranged sequentially along the substrate moving direction; The nucleation and crystallization module includes a light processing component and a plasma processing component.

10. The preparation method according to claim 9, characterized in that, The light processing component includes an infrared light processor and / or a microwave light processor.

11. The preparation method according to claim 9, characterized in that, The light processing component is located above the substrate.

12. The preparation method according to claim 9, characterized in that, The plasma processing component includes an ion air knife.

13. The preparation method according to claim 9, characterized in that, The plasma processing component is located below the substrate.

14. The preparation method according to claim 9, characterized in that, The coating module includes an ultrasonic spraying assembly.

15. The preparation method according to claim 14, characterized in that, The ultrasonic spraying assembly includes an ultrasonic sprayer and a spraying material tank connected to the ultrasonic sprayer, wherein the ultrasonic sprayer is located above the substrate.

16. The preparation method according to claim 15, characterized in that, The ultrasonic sprayer includes at least two linearly arranged ultrasonic nozzles.

17. The preparation method according to claim 16, characterized in that, The ultrasonic spraying assembly also includes a liquid collection tank located below the substrate, which is used to collect perovskite solution or cleaning agent.

18. The preparation method according to claim 17, characterized in that, The perovskite layer preparation apparatus further includes a substrate transmission platform, on which the substrate is placed; The coating module and the nucleation and crystallization module are independently located on both sides of the substrate transmission platform.

19. The preparation method according to claim 18, characterized in that, The perovskite layer preparation device also includes an exhaust fan, and the ultrasonic sprayer, liquid collection tank, nucleation and crystallization module and substrate transmission platform are all located inside the exhaust fan.

20. The preparation method according to claim 19, characterized in that, Along the substrate moving direction, the perovskite layer preparation apparatus also includes a feeding module located before the coating module.

21. The preparation method according to claim 20, characterized in that, The feeding module includes a feeding drive belt and a feeding driver that drives the feeding drive belt to move.

22. The preparation method according to claim 20, characterized in that, Along the substrate moving direction, the perovskite layer preparation apparatus also includes a discharge module located after the nucleation and crystallization module.

23. The preparation method according to claim 22, characterized in that, The discharge module includes a discharge drive belt and a discharge driver that drives the discharge drive belt to move.

24. The preparation method according to claim 22, characterized in that, The perovskite layer preparation apparatus also includes a drying chamber, in which the coating module, nucleation and crystallization module, substrate transmission platform, exhaust fan, feeding module and discharging module are all located, and the exhaust port of the exhaust fan extends out from inside the drying chamber.

25. The preparation method according to claim 24, characterized in that, At least one filter is installed on the walls of the drying room.

Citation Information

Patent Citations

  • High efficiency large area perovskite solar cells and process for producing the same

    CN109155366A

  • A liquid film creep suppression in-situ freeze sublimation crystallization preparation method for uniformly textured perovskite films

    CN109545975B

  • Perovskite material, preparation method thereof, light absorption layer and perovskite cell

    CN112349844A

  • Device and method for preparing large-area perovskite thin film

    CN111710783A

  • Method for forming perovskite layers using atmospheric pressure plasma

    US20180204709A1