A reagent for selectively capturing quartz in a weakly alkaline environment and an application method thereof
By using metal cation activators and anion and cation composite collectors in silicate minerals, the problems of poor quartz flotation selectivity and low recovery rate are solved, efficient quartz separation and recovery is achieved, and costs and the environment are reduced. Influence.
Patent Information
- Application Number
- CN202211028831.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-26
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-08-26
AI Technical Summary
In a weakly alkaline environment, the flotation selectivity of quartz in silicate minerals is poor and the recovery rate is not high. It is difficult to achieve high purity and efficient quartz separation with existing technology.
Using an agent containing a metal cation activator and an anion and cation composite collector, by adding the activator and composite collector to the slurry, the pH value is adjusted between 7-12, and the flotation process is carried out, including rough separation, Selecting and sweeping to improve the recovery rate and quality of quartz.
It achieves efficient capture and separation of quartz in a weakly alkaline environment, reduces the dosage of chemicals, reduces costs, improves the purity and recovery rate of quartz, has a green cleaning effect, and is suitable for industrial applications.
Smart Images

Figure CN115582207B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mineral flotation, and in particular relates to an agent for selectively capturing quartz in a weakly alkaline environment and an application method thereof. Background Art
[0002] Quartz is one of the most widely distributed minerals on the earth's surface. It has fascinating properties and has triggered active exploration activities in traditional industries (such as glassware and ceramics). In particular, high-purity quartz has excellent physical and chemical properties and is widely used in high-tech fields (such as photovoltaics and semiconductor microelectronics). It is a new type of strategic non-metallic mineral resource. However, quartz usually coexists with feldspar silicate minerals, or as a gangue mineral with a variety of other useful minerals. Therefore, it is of great significance to actively explore methods to effectively separate quartz from other minerals.
[0003] Flotation is an indispensable method for obtaining high-quality quartz, because most paragenetic minerals can be separated from quartz by appropriate reagents. There are generally two common methods for quartz flotation: one is the cationic flotation method such as fatty amines, quaternary ammonium salts, ether amines, etc.; the other is the flotation method using metal ions as activators and anionic collectors, such as sodium oleate, sodium alkyl sulfonate, sodium alkyl sulfate, etc. 2+ , Cu 2+ , Pb 2+ Mg 2+ , Fe 3+ wait.
[0004] In recent years, anion-cation composite collectors have attracted the attention of many researchers due to their great application potential in mineral flotation, enhanced oil recovery, nanomaterials and other related fields. Compared with single ion collectors, anion-cation composite collectors have different charges and show the greatest synergistic effect between their surfactant molecules. And a large number of studies have shown that anion-cation composite collectors have strong collection ability and selectivity in the flotation of feldspar, spokes, schist, coal, fluorite, calcite and muscovite. Although studies have reported that metal ion-activated quartz and anion-cation composite collectors have a vital positive effect on the flotation process, the flotation performance of composite collectors in metal ion-activated quartz systems is still rarely explored. At the same time, the process of using metal ion activation and composite collectors to obtain extremely high purity and extremely high recovery rate has rarely been reported so far.
[0005] Therefore, the present invention proposes a reagent and a flotation method for selectively capturing quartz in a weakly alkaline environment to treat silicate minerals. Summary of the invention
[0006] In order to solve the problems of poor flotation selectivity and low flotation recovery rate of quartz in silicate minerals, the present invention aims to provide a reagent and an application method for selectively collecting quartz in a weakly alkaline environment.
[0007] The present invention proposes a flotation method which is highly efficient, feasible and can be used for industrial production, can reduce the dosage of the used reagents, and can realize the efficient collection and separation of quartz in silicate ores in a weakly alkaline environment, thereby achieving the effects of reducing costs and being green and clean.
[0008] At the same time, the present invention can further improve the purity of the product.
[0009] To achieve the above purpose, this application provides the following technologies:
[0010] The present invention discloses a reagent for selectively collecting quartz in a weakly alkaline environment, wherein the reagent comprises an activator and a composite collector; the activator is a salt containing metal cations, and the composite collector comprises a collector component A and a collector component B; the activator and the composite collector are added to the ore pulp in proportion to perform flotation.
[0011] In roughing, the amount of activator added is 100-250g / t; the amount of composite collector added is 140-240g / t;
[0012] in,
[0013] The collector component A is an amine, which is composed of at least one amine in Formula 1, Formula 2, and Formula 3;
[0014] R1-NH2 Formula 1
[0015] R2-NH2 Formula 2
[0016] R3O-CH2-CH2-CH2-NH2 Formula 3
[0017] The collector component B is composed of a substance having at least one structure of Formula 4, Formula 5, and Formula 6;
[0018] CH3(CH2)7CH=CH(CH2)7C00Na Formula 4,
[0019] CH3(CH2) 11 O-SO3Na Formula 5,
[0020] C6H5-CO-NH-OH Formula 6;
[0021] The R1 is C8~C 15 Alkyl, R2 is C 16 ~C 20 The alkyl group of R3 is a hydrocarbon group or an aromatic hydrocarbon group (the aromatic hydrocarbon group is C6H5-);
[0022] As a preferred embodiment of the present invention, a reagent for selectively capturing quartz in a weakly alkaline environment, wherein R1 is C 10 ~C 13 Alkyl, R2 is C 17 ~C 19 The alkyl group of R3 is a long-chain hydrocarbon group or an aromatic hydrocarbon group. The carbon chain length of the long-chain hydrocarbon group is C8 to C 14 .
[0023] The metal cation is selected from at least one of calcium ion, magnesium ion and iron ion, preferably calcium ion.
[0024] As a further preference, the R1 is C 11 ~C 12 Alkyl, R2 is C 18 The alkyl group of R2 is a long-chain hydrocarbon group or an aromatic hydrocarbon group; and the longest carbon chain of the long-chain hydrocarbon group contains C10-12.
[0025] Preferably, the present invention provides a reagent for selectively collecting quartz in a weakly alkaline environment, wherein the collector component A is an amine compound, and the structural formula can be various, and Formula 1 is used more frequently;
[0026] The collector component B is a compound having a structural formula of Formula 4,
[0027] and / or the collector component B is a compound having a structural formula of Formula 5,
[0028] And / or the collector component B is a compound with the structural formula 6.
[0029] During the research, it was found that the composite collector composed of collector component A of formula 1 and collector component B of formula 4 has a better synergistic effect, which is beneficial to further improve the flotation separation effect of quartz and feldspar in silicate minerals.
[0030] Preferably, in the present invention, a reagent for selectively collecting quartz in a weakly alkaline environment, the mass ratio of the collector component A to the collector component B in the composite collector is 2-20:45; preferably 3-20:45, more preferably 3-15:45, and even more preferably 3-9:45. Of course, the ratio of 1-2:10 is also particularly suitable for the mass ratio of A to B in the composite collector of the present invention.
[0031] In the composite collector system of the present invention, the collector component A is a cationic collector, and the collector component B is an anionic collector. The present application has found that the two components form an anionic and cationic composite collector in an appropriate ratio, which can effectively improve the flotation separation effect of quartz and feldspar in silicate minerals, reduce the amount of collector used in the flotation process, achieve the purpose of sorting in a weakly alkaline environment, and improve the recovery rate and grade of quartz.
[0032] The activator is preferably calcium chloride or a mixed metal salt containing calcium chloride.
[0033] The invention discloses an application of a reagent for selectively capturing quartz in a weakly alkaline environment, comprising the following steps:
[0034] Step (1): grinding the silicate mineral containing quartz and gangue, and obtaining a slurry after slurry adjustment;
[0035] Step (2): adding a salt containing metal cations to the slurry and adjusting the pH of the slurry to above 7;
[0036] Step (3): adding a composite collector to the ore pulp for flotation, wherein the flotation process includes roughing, cleaning and scavenging in sequence;
[0037] Step (4): Obtain the final concentrate and tailings.
[0038] The metal cation-containing salt is preferably calcium chloride or a mixed metal salt containing calcium chloride.
[0039] As a preferred embodiment, the present invention uses an agent for selectively collecting quartz in a weakly alkaline environment, and the technical route adopted is: grinding - adding an activator - adjusting pH - adding a collector - 1 roughing 1 fine 1 sweeping, and the intermediate ore is sequentially returned to the roughing flotation closed-circuit process.
[0040] As a preferred embodiment; the application of a reagent for selectively capturing quartz in a weakly alkaline environment of the present invention,
[0041] During roughing, the amount of activator added is 100-250 g / t, preferably 130-220 g / t, more preferably 150-200 g / t; the amount of composite collector added is 140-240 g / t, preferably 160-220 g / t, more preferably 190-200 g / t;
[0042] During the selection, the amount of the activator added is 60-130 g / t, preferably 70-120 g / t, and more preferably 80-110 g / t; the amount of the composite collector added is 70-130 g / t, preferably 90-110 g / t, and more preferably 95-105 g / t;
[0043] During the sweeping, the amount of the activator added is 10-80 g / t, preferably 30-60 g / t, and more preferably 40-50 g / t; the amount of the composite collector added is 30-70 g / t, preferably 40-60 g / t, and more preferably 45-55 g / t.
[0044] The activator is provided by calcium chloride.
[0045] In industrial applications, sodium hydroxide and hydrochloric acid are used to control the pH value of the slurry.
[0046] After optimization, the pH of the slurry in step (2) is adjusted to between 7 and 12.
[0047] After further optimization, the pH of the slurry in step (2) is adjusted to 8-10.
[0048] After further optimization, the pH of the slurry in step (2) is adjusted to 8.5-9.5.
[0049] In the present invention, under the coordination of pH, an appropriate amount of activator and an appropriate amount of composite collector, the slurry temperature is maintained at room temperature, which can further improve the separation effect and increase the grade of quartz and the flotation recovery rate.
[0050] In the present invention, both crushing and grinding processes can be achieved using existing equipment and methods.
[0051] Preferably, the particle size of the particles after grinding is concentrated at about 100 μm, and the particle size accumulated to 100 μm accounts for 50-60%.
[0052] Compared with the prior art, the present invention has the following beneficial effects:
[0053] 1. The composite collector of the present invention comprises a collector component A and a collector component B in appropriate amounts and in a special ratio, and through the synergistic effect of the two, the flotation separation effect of quartz and feldspar in silicate minerals is effectively improved;
[0054] 2. The present application provides the specific structural formulas of collector component A and collector component B, and proposes that collector component A is a cationic collector and collector component B is an anionic collector. The recovery rate and grade of quartz can be further improved by the component ratio;
[0055] 3. The flotation method of the present application can reduce the dosage of the reagents used, and realize the efficient capture and separation of quartz in silicate ores in a weakly alkaline environment, thereby achieving the effect of reducing costs and green cleaning, and reducing damage to the ecological environment, and has high economic potential.
[0056] 4. The raw materials of the composite collector of the present application are easily available and easy to prepare, and the flotation method is simple and easy to operate, providing technical support for large-scale industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 The present invention is a flow chart of the flotation method for silicate minerals. DETAILED DESCRIPTION
[0058] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0059] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0060] The technical route adopted in the embodiment is: grinding - adding activator - adjusting pH - adding collector - 1 roughing 1 fine 1 scavenging, and the medium ore is sequentially returned to the roughing flotation closed-circuit process.
[0061] The recovery rate measured in the embodiment = the mass of quartz in the concentrate / the mass of quartz in the raw material * 100%.
[0062] Example series 1
[0063] In order to make a clearer comparison, this implementation case uses purchased pure quartz, which is crushed and soaked in 3% hydrochloric acid for 10 hours to remove surface impurities and then repeatedly rinsed with deionized water to obtain a quartz powder sample;
[0064] Taking quartz with a purity of 99.67% as the research object, the flotation performance of the composite collector under different pH values was investigated by changing the pH value of the slurry in the flotation experiment.
[0065] Table 1 Analysis of the main oxide components (wt%) in the selected pure quartz
[0066]
[0067] Collector component A (using the structure of formula 1); the specific group of R1 is a C12 alkyl group;
[0068] Collector component B (using the structure of formula 4);
[0069] The dosage ratio of collector component A: collector component B is 1:10.
[0070] The specific experimental operation process is as follows: use a zirconia jaw crusher and a pot-type ceramic ball mill to crush it to less than 0.25mm, the particle size is enriched at about 100μm, and the particle size accumulates to 100μm, accounting for 50% to 60%; each experiment uses an XFG-50 micro-flotation machine to perform flotation experiments at a speed of 1900rpm. First, 2g of quartz sample is taken as the research object, the research object is weighed together with 35mL of deionized water, and placed in a 40mL flotation tank and stirred for 1mi n; then add calcium chloride at a standard of 180g / t, then add pH adjuster and stir for 1min to adjust pH to the specified value (3, 4, 5, 6, 7, 8, 9, 10, 11, 12); then add composite collector at a standard of 200g / t and stir for 3min; insert a bubbling plate for roughing, manually scrape off the upper mineralized foam for 3min during roughing, and the coarse concentrate is scraped into the coarse concentrate basin with the foam, and the tailings remain in the flotation tank; then the coarse concentrate is mixed with 35m 1. Weigh the tailings obtained after roughing with 35ml deionized water, put them into a 40ml flotation cell and stir for 1min, add calcium chloride at a standard of 90g / t, add pH adjuster and stir for 1min, adjust pH to the corresponding value during roughing, then add composite collector at a standard of 100g / t and stir for 2min; insert a bubbling plate for concentration, manually scrape the foam for 2min during concentration, the concentrate is scraped into the concentrate basin with the foam, and the tailings remain in the flotation tank; weigh the tailings obtained after roughing with 35ml deionized water, put them into a 40ml flotation cell and stir for 1min, add calcium chloride at a standard of 45g / t, add pH adjuster and stir for 1min, adjust pH to the corresponding value during roughing, then add composite collector at a standard of 50g / t and stir for 1.5min; manually scrape the foam for 2min, the obtained middlings are sequentially returned to the roughing, and the final tailings remain in the flotation tank; finally, filter, dry and weigh the foam product and residue, calculate the recovery rate, and summarize to prepare Table 2.
[0071] Table 2 Recovery of quartz under different pH conditions in implementation series 1
[0072]
[0073] It can be seen from Table 2 that when the composite collector is added to the solution containing calcium chloride, the recovery rate of quartz increases significantly with the increase of pH value. When the pH is 9, the recovery rate exceeds 80%, and when the pH is 10, the recovery rate exceeds 90%. Therefore, the composite collector provided by the present application can obtain a quartz recovery rate of about 80% in a weakly alkaline environment by controlling the ratio of collector component A and collector component B, which meets the production requirements of today's green mines, and reduces the difficulty and operating cost of subsequent wastewater treatment, reduces the damage to the ecological environment, and has high economic potential and application prospects.
[0074] Example series 2
[0075] This implementation case uses a silicate mineral from Hunan as the raw ore and adopts Figure 1 The flotation method shown was used for the experiments.
[0076] Table 3 Analysis of the main chemical components of the selected raw ore
[0077]
[0078] The specific experimental operation process is as follows: take 500g of the original ore, crush it with a ball mill to less than 0.25mm, the particle size is enriched at about 100μm, and the particle size accumulates to 100μm, accounting for 50-60%; pour it into a 1.5L flotation tank together with an appropriate amount of water and weigh it, add calcium chloride according to the standard of 180g / t, and then add a pH adjuster to control the pH of the slurry to 9, and stir for 1min; then add a composite collector (amount see Table 4), stir for 3min; start automatic scraping, scrape the foam for 5min; perform roughing, the coarse concentrate is scraped into the coarse concentrate basin with the foam, and the tailings remain in the flotation tank; then put the coarse concentrate and an appropriate amount of deionized water into a 1.5L flotation tank and weigh it, add calcium chloride according to the standard of 90g / t, and then add After the pH adjuster controls the pH of the pulp to 9, stir for 1 minute; then add the composite collector at a standard of 100g / t and stir for 2 minutes; automatically scrape the foam for 3 minutes to carry out concentration, the concentrate is scraped into the concentrate basin along with the foam, and the tailings remain in the flotation tank; weigh the tailings obtained after roughing together with an appropriate amount of deionized water, put into a 1.5L flotation tank and weigh, add calcium chloride at a standard of 45g / t, and then add the pH adjuster to control the pH of the pulp to 9, stir for 1 minute; then add the composite collector at a standard of 50g / t and stir for 1.5 minutes; automatically scrape the foam for 2 minutes, and the obtained middlings are returned to the roughing in sequence, and finally the tailings remain in the flotation tank; finally, filter, dry and weigh the foam product and the residue, and calculate the recovery rate.
[0079] Collector component A (using the structure of formula 1); the specific group of R1 is a C12 alkyl group;
[0080] Collector component B (using the structure of formula 4);
[0081] The dosage ratio of collector component A: collector component B is 1:10.
[0082] The amount of composite collector added was changed to conduct multiple experiments, and the recovery rate of quartz was calculated and summarized in Table 4. Roughing: The amount of activator calcium chloride added was 180 g / t, and the amount of composite collector used was shown in Table 4;
[0083] Table 4 Recovery rate of quartz under different composite collector dosages
[0084]
[0085] In Table 4, when the dosage of the composite collector is 200 g / t, the SiO2 content in the obtained quartz concentrate reaches 98.50%.
[0086] It can be seen from Table 3 that as the dosage of the composite collector increases from 20 g / t to 230 g / t during roughing, the recovery rate of quartz shows a trend of first increasing and then decreasing. In particular, when the dosage is 150-200 g / t, the recovery rate of quartz reaches a peak value of more than 80%. Compared with the prior art, it not only improves the recovery rate of quartz, but also reduces the dosage of collector, which meets the requirements of industrial application and has economic potential.
[0087] Example series 3
[0088] This implementation case uses a silicate mineral from Hunan as the raw ore (the specific composition of the raw ore is the same as in Example 2), and adopts Figure 1 The flotation method shown was used for the experiments.
[0089] The specific experimental operation process is as follows: take 500g of the original ore, crush it with a ball mill to less than 0.25mm, the particle size is enriched at about 100μm, and the particle size accumulates to 100μm, accounting for 50-60%; pour it into a 1.5L flotation tank together with an appropriate amount of water and weigh it, add calcium chloride (the amount of calcium chloride is shown in Table 5), and then add a pH adjuster to control the pH of the slurry to 10, and stir for 1min; add a composite collector at a standard of 200g / t and stir for 3min; start automatic scraping and scraping for 5min; rough selection, the coarse concentrate is scraped into the coarse concentrate basin with the foam, and the tailings remain in the flotation tank; then put the coarse concentrate and an appropriate amount of deionized water into a 1.5L flotation tank and weigh it, add calcium chloride at a standard of 90g / t, and then add After adding pH adjuster to control the pH of the pulp to 10, stir for 1 minute; then add composite collector at a standard of 100g / t and stir for 2 minutes; automatically scrape and froth for 3 minutes, select, the concentrate is scraped into the concentrate basin along with the foam, and the tailings remain in the flotation tank; weigh the tailings obtained after roughing together with an appropriate amount of deionized water, put into a 1.5L flotation tank and weigh, add calcium chloride at a standard of 45g / t, and then add pH adjuster to control the pH of the pulp to 10, stir for 1 minute; then add composite collector at a standard of 50g / t and stir for 1.5 minutes; automatically scrape and froth for 2 minutes, the obtained middlings are returned to the roughing in sequence, and the final tailings remain in the flotation tank; finally, filter, dry and weigh the foam product and residue, and calculate the recovery rate.
[0090] Collector component A (using the structure of formula 1); the specific group of R1 is a C12 alkyl group;
[0091] Collector component B (using the structure of formula 4);
[0092] The dosage ratio of collector component A: collector component B is 1:10.
[0093] Multiple experiments were conducted by varying the amount of calcium chloride used, and the recovery rates of quartz were calculated and summarized in Table 5.
[0094] Table 5 Recovery of quartz under different calcium chloride dosages:
[0095]
[0096] It can be seen from Table 5 that as the amount of calcium chloride increased from 0 to 150 g / t during roughing, the quartz recovery rate increased from 2.34% to 90%. When the amount of calcium chloride was further increased to 250 g / t, the quartz recovery rate did not change significantly. When it was increased to 300 g / t, the amount of calcium chloride was too much, resulting in Ca 2+ The concentration is too high and the recovery rate is reduced;
[0097] Under alkaline conditions, calcium hydroxide can be produced, inhibiting the flotation of quartz.
[0098] That is, during roughing, when the calcium chloride dosage is 150g / t, the quartz surface is ideally activated, which can improve the sorting effect and increase the flotation recovery rate of quartz.
[0099] Example series 4
[0100] This series of examples uses a silicate mineral from Anhui as the raw ore, and uses Figure 1 The flotation method shown was tested.
[0101] Table 6 Analysis of the main chemical components of the selected raw ore
[0102]
[0103] The specific experimental operation process is as follows: take 500g of the original ore, crush it with a ball mill to less than 0.25mm, the particle size is enriched at about 100μm, and the particle size accumulates to 100μm, accounting for 50-60%; pour it into a 1.5L flotation tank together with an appropriate amount of water and weigh it, add calcium chloride at a standard of 180g / t, and then add a pH adjuster to control the pH of the slurry to 9, and stir for 1min; then add a composite collector (amount see Table 7), stir for 3min; start automatic scraping, scrape the foam for 5min; the coarse concentrate is scraped into the coarse concentrate basin with the foam, and the tailings remain in the flotation tank; then put the coarse concentrate and an appropriate amount of deionized water into a 1.5L flotation tank and weigh it, add calcium chloride at a standard of 90g / t, and then add After the pH adjuster controls the pH of the pulp to 9, stir for 1 minute; then add the composite collector at a standard of 100g / t and stir for 2 minutes; automatically scrape the foam for 3 minutes, the concentrate is scraped into the concentrate basin along with the foam, and the tailings remain in the flotation tank; weigh the tailings obtained after roughing together with an appropriate amount of deionized water, put into a 1.5L flotation tank and weigh, add calcium chloride at a standard of 45g / t, and then add the pH adjuster to control the pH of the pulp to 9, stir for 1 minute; then add the composite collector at a standard of 50g / t and stir for 1.5 minutes; automatically scrape the foam for 2 minutes, the obtained middlings are returned to the roughing in sequence, and finally the tailings remain in the flotation tank; finally, filter, dry and weigh the foam product and the residue, and calculate the recovery rate.
[0104] Collector component A (using the structure of formula 1); the specific group of R1 is a C12 alkyl group;
[0105] Collector component B (using the structure of formula 4);
[0106] Roughing: The amount of calcium chloride added as activator is 180 g / t, and the amount of composite collector is shown in Table 7;
[0107] The dosage of collector component A was changed from 0 to 50 g / t; the dosage of collector component B was kept constant at 150 g / t. After conducting multiple groups of experiments, the calculated quartz recoveries were summarized to obtain Table 7.
[0108] Table 7 Recovery rate of quartz at different dosages of collector component A
[0109]
[0110]
[0111] It can be seen from Table 7 that as the dosage of collector component A increases from 0 to 50 g / t, the recovery rate of quartz generally shows a trend of first increasing and then decreasing. In particular, when the concentration is 8 g / t, the recovery rate of quartz reaches more than 80%. When the concentration is further increased, the recovery rate increases less, and the recovery rate decreases when it increases to 50 g / t.
[0112] As recorded in Table 7: the dosage of collector component A is 10 g / t, the recovery rate of quartz is 82.25%, and the SiO2 content in the product reaches 97.01 wt%.
[0113] That is, it shows that under the weakly alkaline condition of calcium chloride and collector component B, collector component A shows a good activation effect on the flotation of quartz, and the two have a synergistic effect, which further shows that the composite collector described in the present invention can be used to selectively collect quartz, improve the sorting effect, and increase the flotation recovery rate and grade of quartz.
[0114] In summary of the above embodiments, the composite collector and flotation method proposed in the present application can selectively capture quartz in a weakly alkaline environment, thereby improving the grade and recovery rate of quartz.
[0115] The above description is only an embodiment of the present invention, and does not limit the scope of patent protection of the present invention. For ordinary technicians in this field, the present invention can be modified, changed and replaced in various ways without departing from the spirit and principle of the present invention. Any improvement or equivalent replacement made by using the contents of the present invention specification and drawings, directly or indirectly applied in other related technical fields, should be included in the scope of patent protection of the present invention.
Claims
1. A reagent for selectively capturing quartz in a weakly alkaline environment, characterized in that: The reagent includes an activator and a composite collector; the activator is a salt containing metal cations, and the composite collector includes a collector component A and a collector component B; the activator and the composite collector are added to the ore pulp in proportion to perform flotation, and the metal cation is selected from at least one of calcium ions, magnesium ions, and iron ions; The mass ratio of collector component A to collector component B in the composite collector is 2-20:45; In roughing, the amount of activator added is 100-250g / t; the amount of composite collector added is 140-240g / t; in, The collector component A is an amine, which is composed of at least one amine in Formula 1, Formula 2, and Formula 3; R1-NH2 formula 1, R2-NH2 formula 2, R3O-CH2-CH2-CH2-NH2 formula 3, The collector component B is composed of a substance having at least one structure of Formula 4, Formula 5, and Formula 6; CH3(CH2)7CH=CH(CH2)7C00Na Formula 4, CH3(CH2) 11 O-SO3Na 5, C6H5-CO-NH-OH Formula 6; The R1 is C8~C 15 Alkyl, R2 is C 16 ~C 20 The alkyl group of R3 is a hydrocarbon group or an aromatic hydrocarbon group.
2. The reagent for selectively capturing quartz in a weakly alkaline environment according to claim 1, characterized in that: The R1 is C 10 ~C 13 Alkyl, R2 is C 17 ~C 19 The alkyl group of R3 is a long-chain hydrocarbon group or an aromatic hydrocarbon group; the carbon chain length of the long-chain hydrocarbon group is C8 to C 14 .
3. The reagent for selectively capturing quartz in a weakly alkaline environment according to claim 1, characterized in that: The R1 is C 11 ~C 12 Alkyl, R2 is C 18 The alkyl group of R3 is a long-chain hydrocarbon group or an aromatic hydrocarbon group; and the longest carbon chain in the long-chain hydrocarbon group contains C10-12; and the metal cation is a calcium ion.
4. The reagent for selectively capturing quartz in a weakly alkaline environment according to claim 1, characterized in that: The mass ratio of collector component A to collector component B in the composite collector is 3-20:
45.
5. An application of a reagent for selectively capturing quartz in a weakly alkaline environment as claimed in any one of claims 1 to 4, characterized in that; The following steps are involved: Step (1): grinding the silicate mineral containing quartz and gangue, and obtaining a slurry after slurry adjustment; Step (2): adding a salt containing metal cations to the slurry and adjusting the pH of the slurry to above 7; Step (3): adding a composite collector to the ore pulp for flotation, wherein the flotation process includes roughing, cleaning and scavenging in sequence; during roughing, the amount of activator added is 100-250 g / t; the amount of composite collector added is 140-240 g / t; Step (4): Obtain the final concentrate and tailings.
6. The use of a reagent for selectively capturing quartz in a weakly alkaline environment according to claim 5, characterized in that: The technical route adopted is: grinding - adding activator - adjusting pH - adding collector - 1 roughing 1 fine 1 sweeping, and the intermediate ore is returned to the roughing flotation closed-circuit process in sequence.
7. The use of a reagent for selectively capturing quartz in a weakly alkaline environment according to claim 5, characterized in that: In roughing, the amount of activator added is 100-250g / t; the amount of composite collector added is 140-240g / t; During the selection, the amount of activator added is 60-130g / t; the amount of composite collector added is 70-130g / t; During scavenging, the amount of activator added is 10-80g / t; The addition amount of the composite collector is 30-70g / t.
8. The use of a reagent for selectively capturing quartz in a weakly alkaline environment according to claim 5, characterized in that: In step (2), the pH of the slurry is adjusted to between 7 and 12.
9. The use of a reagent for selectively capturing quartz in a weakly alkaline environment according to claim 5, characterized in that: In step (2), the pH of the slurry is adjusted to 8-10.
10. The use of a reagent for selectively capturing quartz in a weakly alkaline environment according to claim 5, characterized in that: The particle size after grinding is concentrated at 100µm, and the particle size accumulated to 100µm accounts for 50-60%.
Citation Information
Patent Citations
Beneficiation method for rubidium-containing feldspar quarry
CN105597926A
Anionic combined collector for fluoride-free flotation separation of quartz and feldspar as well as preparation method and application of anionic combined collector
CN107899753A