Preparation method of nanostructure reinforced organic thermoelectric textile material

By forming nanostructures on organic thermoelectric fabric materials and using the nanophase energy filtering effect to increase the Seebeck coefficient and power factor, the problem of regulating the thermoelectric merit of organic thermoelectric fabric materials is solved, the thermoelectric performance is improved and the manufacturing process is simplified.

CN115637587BActive Publication Date: 2024-10-08TIANJIN POLYTECHNIC UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211101888.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-09
Publication Date
2024-10-08
Estimated Expiration
2042-09-09

AI Technical Summary

Technical Problem

It is difficult for existing organic thermoelectric fabric materials to achieve a balance between regulating the Seebeck coefficient, electrical conductivity and thermal conductivity, which limits the improvement of their thermoelectric figure of merit and affects thermoelectric performance.

Method used

By spraying the nanomaterial liquid onto the fiber material, a nanofiber-based product is formed, and the oxidant and dopant solution is added dropwise under low temperature conditions, left to stand and dry, to form a nanostructure-reinforced organic thermoelectric fabric material and introduce nanophase energy. Filtering effect, improving Seebeck coefficient and power factor.

Benefits of technology

The thermoelectric performance of organic thermoelectric fabric materials is significantly improved, the wearability is improved, the manufacturing process is simplified, and the cost and processing difficulty are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115637587B_ABST
    Figure CN115637587B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a nanostructure-enhanced organic thermoelectric textile material. The method comprises the following steps: spraying a nanomaterial liquid onto a fiber material or a fiber material product to obtain a nanofiber-based product, wherein the nanomaterial liquid is a mixture of a nanomaterial and a storage solvent, and the mass of the nanomaterial in the nanomaterial liquid sprayed per square centimeter of the fiber material or the fiber material product is 0.004-0.6 g; dripping an oxidant solution and a dopant solution onto the surface of the nanofiber-based product, allowing the solution to stand at 0-5°C for 5-20 min, then dripping a mixed solution, allowing the solution to stand at -26-0°C for 90-160 h, washing, and drying to obtain the nanostructure-enhanced organic thermoelectric textile material. The nanostructure-enhanced organic thermoelectric textile material of the invention introduces nanomaterials to form a nanophase energy filtering effect, thereby increasing the Seebeck coefficient and the power factor, and effectively improving the thermoelectric performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermoelectric fabrics, and in particular relates to a method for preparing a nanostructure reinforced organic thermoelectric fabric material. Background Art

[0002] With the discovery and continuous development of thermoelectric effect, quantum mechanics and semiconductor theory, thermoelectric materials have been gradually developed, from metal materials at the beginning to semiconductor thermoelectric materials, and then to soft and lightweight organic thermoelectric textile materials. Compared with the thermoelectric materials in the past, organic thermoelectric textile materials are environmentally friendly, have low manufacturing costs, are economically feasible and have broader application prospects. As a functional material for realizing temperature-to-electric conversion, organic thermoelectric textile materials need to continuously improve and break through their thermoelectric figure of merit in order to achieve excellent thermoelectric conversion efficiency and play an important practical significance for human society.

[0003] The conversion efficiency of organic thermoelectric textile materials is calculated by the thermoelectric figure of merit (ZT value). The thermoelectric figure of merit of organic thermoelectric textile materials is proportional to the Seebeck coefficient and electrical conductivity, and inversely proportional to thermal conductivity. Therefore, organic thermoelectric textile materials with good thermoelectric performance need to have a high Seebeck coefficient, high electrical conductivity and low thermal conductivity. By using nanostructures to regulate the balance between various properties, significant effects can be achieved. That is, by adding low-dimensional materials to organic thermoelectric matrix materials, the carrier concentration and mobility of thermoelectric materials are regulated to achieve the purpose of regulating the thermoelectric properties of organic thermoelectric textile materials. The prepared composite material has different dimensions, and an energy filtering effect will occur at the interface between the two phases, that is, high-energy carriers will pass through the phase boundary and grain boundary, while limiting the passage of low-energy carriers and phonons. Therefore, the Seebeck coefficient of the obtained composite material increases, and thus the power factor of the composite material is also increased. At present, there is a problem of interdependence among the various properties of the thermoelectric figure of merit of organic thermoelectric textile materials. It is difficult to achieve a balance among the Seebeck coefficient, electrical conductivity and thermal conductivity, which restricts the size of the thermoelectric figure of merit of organic thermoelectric textile materials and thus affects the thermoelectric performance of organic thermoelectric textile materials. Therefore, the regulation of the thermoelectric performance of organic thermoelectric textile materials still faces huge challenges. Summary of the invention

[0004] In view of the deficiencies in the prior art, an object of the present invention is to provide a method for preparing a nanostructure reinforced organic thermoelectric textile material.

[0005] Another object of the present invention is to provide a nanostructure reinforced organic thermoelectric textile material obtained by the above preparation method.

[0006] A method for preparing a nanostructure reinforced organic thermoelectric textile material comprises the following steps:

[0007] 1) spraying a nanomaterial liquid onto a fiber material or a fiber material product to obtain a nanofiber-based product, wherein the nanomaterial liquid is a mixture of a nanomaterial and a storage solvent, and the mass of the nanomaterial in the nanomaterial liquid sprayed per square centimeter of the fiber material or the fiber material product is 0.004 to 0.6 g;

[0008] In the step 1), the fiber material is natural fiber, chemical fiber or electrospun membrane.

[0009] In the above technical solution, the natural fiber is plant fiber or animal fiber, the plant fiber is made of cotton or linen, and the animal fiber is made of silk or wool;

[0010] The chemical fiber is a regenerated fiber, a synthetic fiber or an inorganic fiber, the regenerated fiber is a viscose fiber or an acetate fiber, the synthetic fiber is made of nylon, polyester, acrylic fiber, spandex, vinylon, chloroprene or polypropylene (PP), and the inorganic fiber is a basalt fiber, a carbon fiber or a glass fiber;

[0011] The material of the electrospun membrane is polyacrylonitrile (PAN), polyethylene terephthalate (PET), polyvinyl alcohol (PVA), polylactic acid (PLA) or polyetherimide (PEI).

[0012] In the step 1), the storage solvent is anhydrous ethanol or deionized water.

[0013] In the step 1), the concentration of the nanomaterial in the nanomaterial liquid is 0.01 to 0.04 g / mL.

[0014] In the step 1), the nanomaterial is an organic nanophase structure or a non-organic nanophase structure.

[0015] The method for preparing the organic nanophase structure is as follows: uniformly mixing a dispersant, a second solvent, a second oxidant and a reaction monomer, reacting at -10 to 70°C for 4 to 8 hours, centrifuging, and washing the solid obtained by centrifugation to obtain the organic nanophase structure, wherein the reaction monomer is a monomer capable of preparing a nanostructure, and the reaction monomer is one of 3,4-ethylenedioxythiophene (EDOT), pyrrole (Py), aniline (AN) and acetylene; the dispersant is used to induce the reaction monomer to form a nanostructure; the second solvent is deionized water or dilute hydrochloric acid; the ratio of the amount of the dispersant, the volume of the second solvent, the amount of the second oxidant and the volume of the reaction monomer is (30 to 65): (80 to 120): (8 to 22): (6 to 8), the unit of the volume is mL, and the unit of the amount of the substance is mmol.

[0016] In the above technical solution, the second oxidant is ferric chloride hexahydrate or ferric chloride.

[0017] In the above technical solution, the concentration of the dilute hydrochloric acid is 0.2-0.5 mol / L.

[0018] The method for preparing the non-organic nanophase structure is: uniformly mixing a reducing oxidant, a third solvent and an inorganic compound containing nanophase structural elements, reacting at 70-260° C. for 3-24 hours, centrifuging, and washing the solid obtained by centrifugation to obtain the non-organic nanophase structure, wherein the reducing oxidant is a reducing agent or an oxidizing agent, the reducing agent is L-ascorbic acid, ascorbic acid or hydrazine hydrate, the oxidizing agent is ferric chloride hexahydrate (FeCl3·6H2O) or ferric chloride (FeCl3), and the inorganic compound containing nanophase structural elements is tellurium dioxide (TeO2) or sodium tellurite (Na2TeO3).

[0019] In the above technical solution, the third solvent is deionized water or an organic solvent, and the organic solvent is ethylene glycol (EG) and / or diethylene glycol (DEG).

[0020] In the above technical solution, the cleaning is performed by alternating cleaning with water and alcohol, and the alcohol is anhydrous ethanol or methanol.

[0021] In the above technical solution, the ratio of the amount of the reducing oxidant, the volume of the third solvent and the amount of the inorganic compound containing the nanophase structure element is (2-6): (20-50): (0.6-2), the unit of the volume is mL, and the unit of the amount of the substance is mmol.

[0022] 2) dripping an oxidant solution and a dopant solution onto the surface of the nanofiber-based product, leaving it to stand at 0 to 5° C. for 5 to 20 minutes, then dripping a mixed solution, leaving it to stand at -26 to 0° C. for 90 to 160 hours, washing, and drying to obtain a nanostructure-enhanced organic thermoelectric textile material, wherein:

[0023] The oxidant solution is a mixture of a first oxidant and water, wherein the first oxidant is a mixture of one or more of sodium persulfate (Na2S2O8), ammonium persulfate ((NH4)2S2O8), potassium persulfate (K2S2O8), ferric p-toluenesulfonate ((C7H7O3S)3.Fe), ferric chloride (FeCl3) and potassium permanganate (KMnO4); the amount of the first oxidant in the oxidant solution dripped onto the surface of the nanofiber-based product per square centimeter is 0.001 to 0.005 mol;

[0024] The dopant solution is a mixture of a dopant and water, wherein the dopant is p-toluenesulfonic acid (TsOH), poly (4-styrenesulfonic acid) (PSS), sodium p-aminobenzenesulfonate (C6H6NaSO3) and camphorsulfonic acid (C 10 H 16 O4S) or a mixture of one or more thereof;

[0025] The mixed solution is a mixture of an organic thermoelectric reaction monomer and a first solvent;

[0026] The ratio of the amount of the first oxidant in the oxidant solution, the amount of the dopant in the dopant solution and the volume fraction of the organic thermoelectric reaction monomer in the mixed solution is (3-6): (3.1-6.2): ​​(0.2-0.25), the unit of the volume fraction is mL, and the unit of the amount of the substance is mmol.

[0027] In the step 2), the concentration of the first oxidant in the oxidant solution is 0.1-0.5 mol / L, the concentration of the dopant in the dopant solution is 0.1-0.5 mol / L, and the concentration of the organic thermoelectric reaction monomer in the mixed solution is 10-50 μL / mL.

[0028] In the step 2), the organic thermoelectric reaction monomer is 3,4-ethylenedioxythiophene (EDOT).

[0029] In the step 2), the first solvent is chloroform and / or dichloromethane.

[0030] In the step 2), the cleaning is performed by alternately washing with deionized water and ethanol, and the number of times of washing with deionized water and ethanol is at least 2 times.

[0031] In the step 2), the drying temperature is room temperature, and the drying time is at least 12 hours.

[0032] The nanostructure reinforced organic thermoelectric textile material obtained by the preparation method.

[0033] A method for preparing a PPy-coated nanostructure-enhanced organic thermoelectric textile material comprises the following steps:

[0034] The nanostructure enhanced organic thermoelectric textile material is placed on an ice surface, and the deposition step is repeated 3 to 5 times to obtain a PPy-coated nanostructure enhanced organic thermoelectric textile material, wherein the deposition step comprises: dripping 0.1 to 0.5 mol / L of FeCl3 aqueous solution and 0.1 to 0.5 mol / L of Py monomer aqueous solution on the nanostructure enhanced organic thermoelectric textile material, standing for at least 10 minutes, washing with deionized water, and drying, wherein the amount of FeCl3 in the FeCl3 aqueous solution added per square meter of the nanostructure enhanced organic thermoelectric textile material is 0.0005 to 0.0025 mol, and the amount of pyrrole in the Py monomer aqueous solution added per square meter of the nanostructure enhanced organic thermoelectric textile material is 0.0005 to 0.0025 mol.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] (1) The nanostructured organic thermoelectric textile material of the present invention introduces nanomaterials to form a nanophase energy filtering effect, thereby increasing the Seebeck coefficient and power factor, thereby greatly improving wearability and effectively improving thermoelectric performance.

[0037] (2) The preparation method of the nanostructure enhanced organic thermoelectric textile material of the present invention is simple and effective, and can regulate the thermoelectric properties of the nanostructure enhanced organic thermoelectric textile material, and also reduce the cost and processing difficulty of the manufacturing process to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 The reaction principle of the reaction monomers in the method for preparing the organic nanophase structure in Examples 1 to 5;

[0039] Figure 2 It is a structural schematic diagram of the filtration device;

[0040] Figure 3 (a-d) photos, (e) SEM and (e') SEM of nanofiber membrane;

[0041] Figure 4are photos and SEM, wherein (a) is a photo of the fiber material products in Comparative Example 1 and Examples 1 to 5 before being surface-modified with polydopamine (PDA), (b) is a photo of the fiber material products in Comparative Example 1 and Examples 1 to 5, (c) is a photo of the nanofiber-based products in Examples 1 to 5, (d) is a photo of the nanostructure-enhanced organic thermoelectric textile material in Examples 1 to 4, (e) is a photo of the PPy-coated nanostructure-enhanced organic thermoelectric textile material obtained in Example 5, (a') is a SEM of the fiber material products in Comparative Example 1 and Examples 1 to 5 before being surface-modified with polydopamine (PDA), (b') is a SEM of the fiber material products in Comparative Example 1 and Examples 1 to 5, and (c') is a photo of the nanostructure-enhanced organic thermoelectric textile material in Example 5. 1 to 5, (d') is the SEM of the nanostructure reinforced organic thermoelectric textile material in Examples 1 to 4, (e') is the SEM of the PPy coated nanostructure reinforced organic thermoelectric textile material obtained in Example 5, (a") is the SEM of the fiber material products in Comparative Example 1 and Examples 1 to 5 before surface modification with polydopamine (PDA), (b") is the SEM of the fiber material products in Comparative Example 1 and Examples 1 to 5, (c") is the SEM of the nanofiber-based product in Examples 1 to 5, (d") is the SEM of the nanostructure reinforced organic thermoelectric textile material in Examples 1 to 4, and (e") is the SEM of the PPy coated nanostructure reinforced organic thermoelectric textile material obtained in Example 5.

[0042] Figure 5 are photos and SEM, wherein a is a photo of the front side of the nanostructure enhanced organic thermoelectric textile material in Examples 1 to 4, a' is a photo of the back side of the nanostructure enhanced organic thermoelectric textile material in Examples 1 to 4, a", a'' are SEMs of the cross-section of the nanostructure enhanced organic thermoelectric textile material in Examples 1 to 4, b is a photo of the front side of the nanostructure enhanced organic thermoelectric textile material coated with PPy in Example 5, b' is a photo of the back side of the nanostructure enhanced organic thermoelectric textile material coated with PPy in Example 5, b", b'' are SEMs of the cross-section of the nanostructure enhanced organic thermoelectric textile material coated with PPy in Example 5, c, c' are SEMs of the nanostructure enhanced organic thermoelectric textile material coated with PPy in Example 5;

[0043] Figure 6 This is the SEM of the cross section of the PPy-coated nanostructure-reinforced organic thermoelectric textile material obtained in Example 5;

[0044] Figure 7FTIR spectra of the nanomaterial (PEDOT nw) in Example 1, the nanostructure enhanced organic thermoelectric textile material (PA-PEDOT nw-T) prepared in Example 2, and the PPy-coated nanostructure enhanced organic thermoelectric textile material (PA-PEDOT nw-Ty) prepared in Example 5;

[0045] Figure 8 (a) electrical conductivity, Seebeck coefficient and (b) power factor of the organic thermoelectric textile material prepared in Comparative Example 1 and the nanostructure-enhanced organic thermoelectric textile material prepared in Examples 1 to 4;

[0046] Fig. 9 (a) resistivity, (b) carrier concentration, (c) Hall coefficient and (d) carrier mobility of the organic thermoelectric textile material prepared in Comparative Example 1 and the nanostructure enhanced organic thermoelectric textile material prepared in Examples 1 to 4. DETAILED DESCRIPTION

[0047] The preparation method of the nanostructure reinforced organic thermoelectric textile material of the present invention is described in detail below with reference to the accompanying drawings.

[0048] Comparative Example 1

[0049] A method for preparing an organic thermoelectric textile material comprises the following steps:

[0050] 1) Spraying the storage solvent onto the fiber material product with a spray pot, wherein the fiber material product is a PA hydrophilic nonwoven fabric obtained by modifying a polypropylene nonwoven fabric (PP) with polydopamine (PDA) (PA hydrophilic nonwoven fabric is Sun, F.; Li, T.-T.; Zhang, X.; Shiu, B.-C.; Zhang, Y.; Ren, H.-T.; Peng, H.-K.; Lin, J.-H.; Lou, C.-W., Insitu growth polydopamine decorated polypropylen melt-blown membrane for highly efficient oil / water separation. Chemosphere 2020, 254., 2.2. Fabrication of PDA / APTES@PP composite membranes in 2. Material and methods). The storage solvent is anhydrous ethanol, and the storage solvent sprayed per square centimeter of the fiber material product is 0.00196 ml;

[0051] The method for preparing an organic nanophase structure is as follows: uniformly mix a dispersant, a second solvent, a second oxidant and a reaction monomer, react at 50° C. for 6 hours, centrifuge with deionized water and methanol for 3 times respectively to wash the solid obtained by centrifugation to obtain an organic nanophase structure, wherein the reaction monomer is 3,4-ethylenedioxythiophene (EDOT), the dispersant is purchased from Aladdin Chemical Reagent Co., Ltd. analytically pure sodium dodecylbenzene sulfonate (SDS), the dispersant is used to induce the reaction monomer to form a nanostructure, the second solvent is deionized water, and the second oxidant is ferric chloride hexahydrate; the ratio of the amount of the dispersant, the volume of the second solvent, the amount of the second oxidant and the volume of the reaction monomer is 65:100:8.1:7, the unit of the volume is mL, and the unit of the amount of the substance is mmol. (For details on the method of preparing organic nanophase structures, see Song, H.; Yao, Y.; Tang, C.; Zhang, L.; Lu, Y.; Sun, Q.; Huang, F.; Zuo, C., Tunable thermoelectric properties of free-standing PEDOT nanofiber film through adjusting its nanostructure. Synthetic Metals 2021, 275.)

[0052] 2) adding an oxidant solution and a dopant solution to the surface of the fiber material product obtained in step 1), allowing to stand at 0° C. for 5 min, then adding a mixed solution in a ventilated environment, sealing with a plastic wrap, allowing to stand at -13° C. for 120 h, washing with deionized water and ethanol alternately for 3 times each, and drying at room temperature for 12 h to obtain an organic thermoelectric textile material, wherein:

[0053] The oxidant solution is a mixture of a first oxidant and water, the concentration of the first oxidant in the oxidant solution is 0.3 mol / L, and the first oxidant is sodium persulfate (Na2S2O8); the amount of the first oxidant in the oxidant solution dripped per square centimeter of the surface of the fiber material product is 0.001 mol;

[0054] The dopant solution is a mixture of a dopant and water, the concentration of the dopant in the dopant solution is 0.31 mol / L, and the dopant is p-toluenesulfonic acid (TsOH);

[0055] The mixed solution is a mixture of an organic thermoelectric reaction monomer and a first solvent, the organic thermoelectric reaction monomer is 3,4-ethylenedioxythiophene (EDOT), the first solvent is chloroform, and the concentration of the organic thermoelectric reaction monomer in the mixed solution is 22.5 μL / mL.

[0056] The ratio of the amount of the first oxidant in the oxidant solution dripped onto the surface of each fiber material product, the amount of the dopant in the dopant solution and the volume fraction of the organic thermoelectric reaction monomer in the mixed solution is 3:3.1:0.225, the unit of volume fraction is mL, and the unit of amount of substance is mmol.

[0057] Example 1

[0058] A method for preparing a nanostructure reinforced organic thermoelectric textile material comprises the following steps:

[0059] 1) Spraying the nanomaterial liquid onto the fiber material product with a spray pot to obtain a nanofiber-based product, wherein the fiber material product is a PA hydrophilic nonwoven fabric obtained by modifying a polypropylene nonwoven fabric (PP) with polydopamine (PDA) (the PA hydrophilic nonwoven fabric is Sun, F.; Li, T.-T.; Zhang, X.; Shiu, B.-C.; Zhang, Y.; Ren, H.-T.; Peng, H.-K.; Lin, J.-H.; Lou, C.-W., In situ growth polydopamine decorated polypropylen melt-blown membrane for highly efficient oil / water separation. Chemosphere 2020, 254., 2.2. Fabrication of PDA / APTES@PP composite membranes in 2. Material and methods). The nanomaterial liquid is a mixture of nanomaterial and storage solvent, the storage solvent is anhydrous ethanol, the nanomaterial is an organic nanophase structure, the concentration of the nanomaterial in the nanomaterial liquid is 0.04g / mL, and the mass of the nanomaterial in the nanomaterial liquid sprayed per square centimeter of the fiber material product is 0.0049g;

[0060] The method for preparing an organic nanophase structure is as follows: uniformly mix a dispersant, a second solvent, a second oxidant and a reaction monomer, react at 50° C. for 6 hours, centrifuge with deionized water and methanol for 3 times respectively to wash the solid obtained by centrifugation to obtain an organic nanophase structure, wherein the reaction monomer is 3,4-ethylenedioxythiophene (EDOT), the dispersant is purchased from Aladdin Chemical Reagent Co., Ltd. analytically pure sodium dodecylbenzene sulfonate (SDS), the dispersant is used to induce the reaction monomer to form a nanostructure, the second solvent is deionized water, and the second oxidant is ferric chloride hexahydrate; the ratio of the amount of the dispersant, the volume of the second solvent, the amount of the second oxidant and the volume of the reaction monomer is 65:100:8.1:7, the unit of the volume is mL, and the unit of the amount of the substance is mmol. (For details on the method of preparing organic nanophase structures, see Song, H.; Yao, Y.; Tang, C.; Zhang, L.; Lu, Y.; Sun, Q.; Huang, F.; Zuo, C., Tunable thermoelectric properties of free-standing PEDOT nanofiber film through adjusting its nanostructure. Synthetic Metals 2021, 275.)

[0061] 2) adding an oxidant solution and a dopant solution to the surface of the nanofiber-based product, standing at 0°C for 5 minutes, then adding a mixed solution in a ventilated environment, sealing with a plastic wrap, standing at -13°C for 120 hours, washing with deionized water and ethanol alternately for 3 times each, and drying at room temperature for 12 hours to obtain a nanostructure-enhanced organic thermoelectric textile material, wherein:

[0062] The oxidant solution is a mixture of a first oxidant and water, the concentration of the first oxidant in the oxidant solution is 0.3 mol / L, and the first oxidant is sodium persulfate (Na2S2O8); the amount of the first oxidant in the oxidant solution dripped per square centimeter of the surface of the nanofiber-based product is 0.001 mol;

[0063] The dopant solution is a mixture of a dopant and water, the concentration of the dopant in the dopant solution is 0.31 mol / L, and the dopant is p-toluenesulfonic acid (TsOH);

[0064] The mixed solution is a mixture of an organic thermoelectric reaction monomer and a first solvent, the organic thermoelectric reaction monomer is 3,4-ethylenedioxythiophene (EDOT), the first solvent is chloroform, and the concentration of the organic thermoelectric reaction monomer in the mixed solution is 22.5 μL / mL.

[0065] The ratio of the amount of the first oxidant in the oxidant solution added to the surface of each nanofiber-based product, the amount of the dopant in the dopant solution and the volume fraction of the organic thermoelectric reaction monomer in the mixed solution is 3:3.1:0.225, the unit of volume fraction is mL, and the unit of amount of substance is mmol.

[0066] Example 2

[0067] A method for preparing a nanostructure reinforced organic thermoelectric textile material is basically the same as that of Example 1, except that in step 1), the mass of the nanomaterial in the nanomaterial liquid sprayed per square centimeter of the fiber material product is 0.0098 g.

[0068] Example 3

[0069] A method for preparing a nanostructure-enhanced organic thermoelectric textile material is basically the same as that in Example 1, except that in step 1), the mass of the nanomaterial in the nanomaterial liquid sprayed per square centimeter of the fiber material product is 0.0147 g.

[0070] Example 4

[0071] A method for preparing a nanostructured reinforced organic thermoelectric textile material is basically the same as that of Example 1, except that in step 1), the mass of the nanomaterial in the nanomaterial liquid sprayed per square centimeter of the fiber material product is 0.0196 g.

[0072] Example 5

[0073] A method for preparing a PPy-coated nanostructure-enhanced organic thermoelectric textile material comprises the following steps:

[0074] The nanostructure enhanced organic thermoelectric textile material obtained in Example 2 is placed on an ice surface, and the deposition step is repeated three times to obtain a PPy-coated nanostructure enhanced organic thermoelectric textile material, wherein the deposition step comprises: dripping 0.5M FeCl3 aqueous solution and 0.5M Py monomer aqueous solution on the nanostructure enhanced organic thermoelectric textile material, standing for 10 minutes, washing with deionized water three times to remove the residual oxidant FeCl3 aqueous solution and the PPy particles with loose surface on the nanostructure enhanced organic thermoelectric textile material, and drying at 60°C for 30 minutes, wherein the amount of FeCl3 in the FeCl3 aqueous solution added per square meter of the nanostructure enhanced organic thermoelectric textile material is 0.0025 mol, and the amount of pyrrole in the Py monomer aqueous solution added per square meter of the nanostructure enhanced organic thermoelectric textile material is 0.0025 mol; the Py monomer aqueous solution is a mixture of pyrrole and water.

[0075] The obtained PPy-coated nanostructure-enhanced organic thermoelectric textile material has an electrical conductivity of 1.62 S / cm, a Seebeck coefficient of 16.6 μV / K, and a power factor of 44.64 nW·K. -2 ·m -1 .

[0076] Example 6

[0077] A method for preparing a nanostructure reinforced organic thermoelectric textile material comprises the following steps:

[0078] 1) Spraying the nanomaterial liquid onto the fiber material product with a spray pot to obtain a nanofiber-based product, wherein the fiber material product is a PA hydrophilic nonwoven fabric obtained by modifying a polypropylene nonwoven fabric (PP) with polydopamine (PDA) (the PA hydrophilic nonwoven fabric is Sun, F.; Li, T.-T.; Zhang, X.; Shiu, B.-C.; Zhang, Y.; Ren, H.-T.; Peng, H.-K.; Lin, J.-H.; Lou, C.-W., In situ growth polydopamine decorated polypropylen melt-blown membrane for highly efficient oil / water separation. Chemosphere 2020, 254., 2.2. Fabrication of PDA / APTES@PP composite membranes in 2. Material and methods). The nanomaterial liquid is a mixture of nanomaterial and storage solvent, the storage solvent is anhydrous ethanol, the nanomaterial is an organic nanophase structure, the concentration of the nanomaterial in the nanomaterial liquid is 0.02g / mL, and the mass of the nanomaterial in the nanomaterial liquid sprayed per square centimeter of the fiber material product is 0.0046g;

[0079] The method for preparing an organic nanophase structure is as follows: uniformly mix a dispersant, a second solvent, a second oxidant and a reaction monomer, react at 0°C for 4 hours, centrifuge with deionized water and methanol for 3 times respectively to wash the solid obtained by centrifugation to obtain an organic nanophase structure, wherein the reaction monomer is pyrrole (Py), the dispersant is purchased from Aladdin Chemical Reagent Co., Ltd. analytically pure sodium dodecylbenzene sulfonate (SDS), the dispersant is used to induce the reaction monomer to form a nanostructure, the second solvent is dilute hydrochloric acid with a concentration of 0.5 mol / L, and the second oxidant is ferric chloride hexahydrate; the ratio of the amount of the dispersant, the volume of the second solvent, the amount of the second oxidant and the volume of the reaction monomer is 50:80:15:7.5, the unit of the volume is mL, and the unit of the amount of the substance is mmol.

[0080] 2) adding an oxidant solution and a dopant solution to the surface of the nanofiber-based product, standing at 0°C for 5 minutes, then adding a mixed solution in a ventilated environment, sealing with a plastic wrap, standing at -13°C for 120 hours, washing with deionized water and ethanol alternately for 3 times each, and drying at room temperature for 12 hours to obtain a nanostructure-enhanced organic thermoelectric textile material, wherein:

[0081] The oxidant solution is a mixture of a first oxidant and water, the concentration of the first oxidant in the oxidant solution is 0.3 mol / L, and the first oxidant is sodium persulfate (Na2S2O8); the amount of the first oxidant in the oxidant solution dripped per square centimeter of the surface of the nanofiber-based product is 0.001 mol;

[0082] The dopant solution is a mixture of a dopant and water, the concentration of the dopant in the dopant solution is 0.31 mol / L, and the dopant is p-toluenesulfonic acid (TsOH);

[0083] The mixed solution is a mixture of an organic thermoelectric reaction monomer and a first solvent, the organic thermoelectric reaction monomer is 3,4-ethylenedioxythiophene (EDOT), the first solvent is chloroform, and the concentration of the organic thermoelectric reaction monomer in the mixed solution is 22.5 μL / mL.

[0084] The ratio of the amount of the first oxidant in the oxidant solution added to the surface of each nanofiber-based product, the amount of the dopant in the dopant solution and the volume fraction of the organic thermoelectric reaction monomer in the mixed solution is 3:3.1:0.225, the unit of volume fraction is mL, and the unit of amount of substance is mmol.

[0085] The conductivity of the obtained nanostructure-enhanced organic thermoelectric textile material is 1.85S / cm, the Seebeck coefficient is 16.2μV / K, and the power factor is 48.55nW·K -2 ·m -1 .

[0086] Example 7

[0087] A method for preparing a nanostructure reinforced organic thermoelectric textile material comprises the following steps:

[0088] 1) using a spray pot to spray a nanomaterial liquid onto a fiber material to obtain a nanofiber-based product, wherein the fiber material is polypropylene (PP), the nanomaterial liquid is a mixture of a nanomaterial and a storage solvent, the storage solvent is anhydrous ethanol, the nanomaterial is a non-organic nanophase structure, the concentration of the nanomaterial in the nanomaterial liquid is 0.018 g / mL, and the mass of the nanomaterial in the nanomaterial liquid sprayed per square centimeter of the fiber material is 0.0088 g;

[0089] The method for preparing a non-organic nanophase structure is as follows: uniformly mix a reducing oxidant, a third solvent and an inorganic compound containing a nanophase structure element, react at 90°C for 20 hours, centrifuge, and wash the solid obtained by centrifugation to obtain a non-organic nanophase structure, wherein the reducing oxidant is a reducing agent, the reducing agent is ascorbic acid, the inorganic compound containing a nanophase structure element is sodium tellurite (Na2TeO3), the third solvent is deionized water, and washing is washing with water and alcohol alternately, the alcohol is anhydrous ethanol, and the ratio of the amount of the reducing oxidant, the volume of the third solvent and the amount of the inorganic compound containing the nanophase structure element is 6:50:0.625, the unit of the volume is mL, and the unit of the amount of the substance is mmol.

[0090] 2) adding an oxidant solution and a dopant solution to the surface of the nanofiber-based product, standing at 0°C for 5 minutes, then adding a mixed solution in a ventilated environment, sealing with a plastic wrap, standing at -13°C for 120 hours, washing with deionized water and ethanol alternately for 3 times each, and drying at room temperature for 12 hours to obtain a nanostructure-enhanced organic thermoelectric textile material, wherein:

[0091] The oxidant solution is a mixture of a first oxidant and water, the concentration of the first oxidant in the oxidant solution is 0.3 mol / L, and the first oxidant is sodium persulfate (Na2S2O8); the amount of the first oxidant in the oxidant solution dripped per square centimeter of the surface of the nanofiber-based product is 0.001 mol;

[0092] The dopant solution is a mixture of a dopant and water, the concentration of the dopant in the dopant solution is 0.31 mol / L, and the dopant is p-toluenesulfonic acid (TsOH);

[0093] The mixed solution is a mixture of an organic thermoelectric reaction monomer and a first solvent, the organic thermoelectric reaction monomer is 3,4-ethylenedioxythiophene (EDOT), the first solvent is chloroform, and the concentration of the organic thermoelectric reaction monomer in the mixed solution is 22.5 μL / mL.

[0094] The ratio of the amount of the first oxidant in the oxidant solution added to the surface of each nanofiber-based product, the amount of the dopant in the dopant solution and the volume fraction of the organic thermoelectric reaction monomer in the mixed solution is 3:3.1:0.225, the unit of volume fraction is mL, and the unit of amount of substance is mmol.

[0095] The conductivity of the obtained nanostructure-enhanced organic thermoelectric textile material is 20.2S / cm, the Seebeck coefficient is 22.4μV / K, and the power factor is 1013.55nW·K -2 ·m -1 .

[0096] Example 8

[0097] A method for preparing a nanostructure-enhanced organic thermoelectric textile material comprises the following steps:

[0098] 1) using a spray pot to spray a nanomaterial liquid onto a fiber material to obtain a nanofiber-based product, wherein the fiber material is polypropylene (PP), the nanomaterial liquid is a mixture of a nanomaterial and a storage solvent, the storage solvent is anhydrous ethanol, the nanomaterial is a non-organic nanophase structure, the concentration of the nanomaterial in the nanomaterial liquid is 0.04 g / mL, and the mass of the nanomaterial in the nanomaterial liquid sprayed per square centimeter of the fiber material is 0.055 g;

[0099] The method for preparing a non-organic nanophase structure is: uniformly mix a reducing oxidant, a third solvent and an inorganic compound containing a nanophase structure element, react at 160°C for 3 hours, centrifuge, and wash the solid obtained by centrifugation to obtain a non-organic nanophase structure, wherein the reducing oxidant is a reducing agent, the reducing agent is hydrazine hydrate, the inorganic compound containing a nanophase structure element is tellurium dioxide (TeO2), the third solvent is an organic solvent, the organic solvent is ethylene glycol (EG), washing is washing with water and alcohol alternately, the alcohol is anhydrous ethanol, the ratio of the amount of the reducing oxidant, the volume of the third solvent and the amount of the inorganic compound containing the nanophase structure element is 6:20:0.75, the unit of the volume is mL, and the unit of the amount of the substance is mmol.

[0100] 2) adding an oxidant solution and a dopant solution to the surface of the nanofiber-based product, standing at 0°C for 5 minutes, then adding a mixed solution in a ventilated environment, sealing with a plastic wrap, standing at -13°C for 120 hours, washing with deionized water and ethanol alternately for 3 times each, and drying at room temperature for 12 hours to obtain a nanostructure-enhanced organic thermoelectric textile material, wherein:

[0101] The oxidant solution is a mixture of a first oxidant and water, the concentration of the first oxidant in the oxidant solution is 0.3 mol / L, and the first oxidant is sodium persulfate (Na2S2O8); the amount of the first oxidant in the oxidant solution dripped per square centimeter of the surface of the nanofiber-based product is 0.001 mol;

[0102] The dopant solution is a mixture of a dopant and water, the concentration of the dopant in the dopant solution is 0.31 mol / L, and the dopant is p-toluenesulfonic acid (TsOH);

[0103] The mixed solution is a mixture of an organic thermoelectric reaction monomer and a first solvent, the organic thermoelectric reaction monomer is 3,4-ethylenedioxythiophene (EDOT), the first solvent is chloroform, and the concentration of the organic thermoelectric reaction monomer in the mixed solution is 22.5 μL / mL.

[0104] The ratio of the amount of the first oxidant in the oxidant solution added to the surface of each nanofiber-based product, the amount of the dopant in the dopant solution and the volume fraction of the organic thermoelectric reaction monomer in the mixed solution is 3:3.1:0.225, the unit of volume fraction is mL, and the unit of amount of substance is mmol.

[0105] The conductivity of the obtained nanostructure-enhanced organic thermoelectric textile material is 14.5S / cm, the Seebeck coefficient is 19.6μV / K, and the power factor is 5378.24nW·K -2 ·m -1 .

[0106] Depend on Figure 1 It can be seen that the reaction monomers in Examples 1 to 5 are oxidized, then activated, the polymerization reaction is triggered, and finally a polymer (PEDOT) is generated. In addition, the activation energy of the polymerization of the reaction monomers is low, and its reaction rate needs to be suppressed at low temperature to obtain a larger molecular weight.

[0107] Take an appropriate amount of the nanomaterial liquid in Example 1 and pour it into Figure 2 In the suction filtration device shown, a negative pressure environment is applied to the suction filtration device, so that the nanomaterial liquid is trapped on the filter membrane to form a nanofiber membrane. The suction filtration device is mainly used to verify that nanomaterials can improve the flexibility and conductivity of organic thermoelectric fabric materials.

[0108] Depend on Figure 3 It can be observed that in Example 1, the nanofiber membrane is obtained by intercepting the nanomaterial liquid through the suction filtration device, and the nanomaterial liquid can be made into a thin film through suction filtration, which verifies that the nanomaterial liquid can improve the flexibility and conductivity of the organic thermoelectric textile material. Figure 3 As shown in (a), it can be found that the nanofiber membrane is composed of a large number of nanomaterials. Among them, the nanomaterials overlap each other to form a mesh (see Figure 3 (e) and (e') of 3), and form a dense nanofilm under negative pressure. The formed nanofiber membrane can be peeled off from the polytetrafluoroethylene (PTFE) filter membrane to form a complete, independent pure nanomembrane (see Figure 3 (b)). The peeled nanofilm has a certain flexibility and can be restored to its original state after bending and folding (see Figure 3 (c)), but it is not resistant to stretching or small tearing and bursting. In addition, when the nanofilm is connected to a circuit with an LED light, the LED light in the circuit is lit ( Figure 3 (d)); and under small dynamic bending, the LED light can still maintain the same brightness. This shows that the nanofiber membrane also has good conductivity and certain electrical stability. At the same time, the conductivity of the nanofiber membrane was 533±5S·cm through the four-point probe test. -1Therefore, linear nanomaterials can greatly enhance the flexibility and conductivity of organic thermoelectric textile materials.

[0109] The fiber material products in Comparative Example 1 and Examples 1 to 6 have a white appearance before being surface modified with polydopamine (PDA), and their fiber surfaces are smooth without any attachments, such as Figure 4 The fiber material product has a brown appearance, and the fiber surface becomes rough, and there are obvious polydopamine particles attached (see Figure 4 (b), (b') and (b")). Afterwards, in Examples 1 to 5, the nanomaterial liquid was sprayed onto the surface of the fiber material product using a spray pot to obtain a nanofiber-based product. It can be found that the surface color of the nanofiber-based product was significantly deepened, and blue appeared locally, indicating that the nanomaterial was trapped on the surface of the fiber material product (see Figure 4 (c)). From the microscopic morphology of the nanofiber-based product, it can be observed that the nanomaterials are distributed between the fiber material products and can "weave a network" in the fiber gaps on the surface of the fiber material products (see Figure 4 (c')~(c")). In addition, the nanomaterials dispersed on the surface of the fiber material product can overlap between the fibers and form a connected nanofiber network, which is beneficial for the formation of a subsequent conductive network. Subsequently, low-temperature interfacial polymerization is performed on the nanofiber-based product to prepare a nanostructured reinforced organic thermoelectric textile material (see Figure 4 (d)). It can be found that after treatment, an obvious film is formed between the fibers of the nanostructured reinforced organic thermoelectric textile material ( Figure 4 d'、 Figure 4 d”)), and the film covers the fibers to form a complete conductive network. In addition, it can be observed that the film does not completely seal the gaps between the fibers, so the nanostructure enhanced organic thermoelectric textile material has a certain air permeability.

[0110] In addition, the actual picture of the PPy coated nanostructure reinforced organic thermoelectric fabric material obtained in Example 5 is shown in Figure 4 (e), it can be observed from the SEM image that the surface becomes rough (see Figure 4 e' and Figure 4 e”)) and showed obvious granular appearance, which means that polypyrrole has been deposited on the surface of the nanostructure enhanced organic thermoelectric textile material.

[0111] Depend on Figure 5The actual pictures and cross-sectional SEM pictures of the front and back surfaces of the nanostructure enhanced organic thermoelectric textile materials of Examples 1 to 4 can be observed, from which it can be clearly found that the front and back surfaces of the nanostructure enhanced organic thermoelectric textile materials have different appearances (a and a'). From its cross-sectional SEM picture, it can be observed that the nanostructure enhanced organic thermoelectric textile material still forms an obvious skin-core structure - the organic thermoelectric layer wraps the fiber (a" and a"'). In addition, it can be observed that the nanomaterial is wrapped by the organic thermoelectric material (PEDOT) to form a larger composite fiber. Figure 5 From the b and b', it can be seen that the nanostructure enhanced organic thermoelectric textile material obtained after polypyrrole coating in Example 5 has a black appearance. This is because the polypyrrole polymer is black, indicating that the polypyrrole has been deposited on the surface of the nanostructure enhanced organic thermoelectric textile material. Figure 5 In b” and b’”, it can be observed that polypyrrole is attached around the nanostructure enhanced organic thermoelectric textile material. The appearance of the nanostructure enhanced organic thermoelectric textile material fiber becomes rougher, and obvious polypyrrole particles are accumulated on its surface. In addition, the nanostructure enhanced organic thermoelectric textile material with deposited polypyrrole has a clearer skin-core structure morphology, such as Figure 5 As shown in c. The organic thermoelectric layer and the polypyrrole layer did not delaminate. Figure 5 c', indicating that the polydopamine layer can improve the surface properties of the nanostructure enhanced organic thermoelectric textile material, so that the polypyrrole layer can be coated on its surface without gaps.

[0112] Depend on Figure 6 On the left side, it can be observed that the cross section of the PPy-coated nanostructure-enhanced organic thermoelectric textile material obtained in Example 5 has a gradient structure. It can be seen that the upper surface layer is an organic thermoelectric film deposited with polypyrrole, the "wrinkled" structure is in the middle layer, and the lower surface layer is a relatively smooth skin-core structure. Figure 6 The right side shows the partial enlarged images of the upper surface layer, the middle layer, and the lower surface layer from top to bottom. This structure is similar to the microstructure of PEDOT deposited on hydrophilic fiber products, which means that the addition of nanomaterials will not hinder the formation of gradient structures.

[0113] Depend on Figure 7 It can be observed that in the infrared spectra of the nanostructure-enhanced organic thermoelectric textile materials of Comparative Example 1 and Example 2, in addition to the characteristic peaks of the fiber material products (2950, ​​2837, 1454, 1375 cm -1 etc.) and the characteristic peaks of polydopamine (3100~3400cm -1 (-NH and -OH stretching vibration), 1608cm -1 In addition to the C=C stretching vibration, there is also the stretching vibration peak of CS with PEDOT (683 cm -1), and the characteristic peaks of COC and CSC (1142 and 1054 cm -1 ), indicating that polydopamine and PEDOT were successfully deposited on the fiber material product. In Example 5, the infrared spectrum of the nanostructured reinforced organic thermoelectric textile material with deposited polypyrrole contained characteristic peaks similar to those of the nanostructured reinforced organic thermoelectric textile material, as well as characteristic peaks of polypyrrole (1540, 1166, 1035 cm -1 ), which means that polypyrrole is deposited on the nanostructure reinforced organic thermoelectric textile material.

[0114] The organic nanophase structure and organic thermoelectric material (PEDOT) formed in Examples 1 to 4 will affect the transport of carriers and phonons - limiting the migration of low-energy carriers and hindering the transport of phonons (see Fig. 9 ). Therefore, the thermal conductivity of nanostructure-enhanced organic thermoelectric textile materials will also be reduced, and the electrical conductivity will also decrease (see Figure 8 (a) and 9(a)). However, the introduction of nanomaterial liquid will increase the carrier concentration of nanostructure enhanced organic thermoelectric textile materials, see Fig. 9 As shown in (b), it also has a certain influence on the Hall coefficient ( Fig. 9 (c)); at the same time, due to the existence of energy filtering effect, the organic nanophase structure (PEDOT nanowires) and organic thermoelectric materials (PEDOT) will hinder the movement of low-energy carriers (see Fig. 9 (d)), the introduction of nanomaterials will increase the carrier concentration of nanostructure enhanced organic thermoelectric fabric materials; at the same time, due to the existence of energy filtering effect, the Seebeck coefficient of nanostructure enhanced organic thermoelectric fabric materials will be improved ( Figure 8 (a)), from 15.6μV / K to 20μV / K. In summary, the constructed microstructure can achieve the increase of the power factor of the nanostructure-enhanced organic thermoelectric textile material and the reduction of its thermal conductivity, thereby obtaining a higher thermoelectric figure of merit. Figure 8 It can be found in (b) that after adding organic thermoelectric material (PEDOT), the power factor of the nanostructure-enhanced organic thermoelectric material photothermoelectric fiber material product at room temperature is slightly improved (48nW·k -2 ·m -1 Increased to 51nW·k -2 ·m -1 ). Therefore, adding an appropriate amount of uniform nanomaterials is beneficial to improving the thermoelectric performance of nanostructure-enhanced organic thermoelectric materials.

[0115] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.

Claims

1. A method for preparing a nanostructure-enhanced organic thermoelectric textile material, characterized in that: The following steps are involved: 1) spraying a nanomaterial liquid onto a fiber material or a fiber material product to obtain a nanofiber-based product, wherein the nanomaterial liquid is a mixture of a nanomaterial and a storage solvent, and the mass of the nanomaterial in the nanomaterial liquid sprayed per square centimeter of the fiber material or the fiber material product is 0.004 to 0.6 g; The nano material is a non-organic nano phase structure. The method for preparing the non-organic nano phase structure is: uniformly mixing a reducing oxidant, a third solvent and an inorganic compound containing a nano phase structure element, reacting at 70-260° C. for 3-24 hours, centrifuging, and washing the solid obtained by centrifugation to obtain the non-organic nano phase structure, wherein the reducing oxidant is a reducing agent or an oxidizing agent, the reducing agent is ascorbic acid, hydrazine hydrate or sodium borohydride, the oxidizing agent is ferric chloride hexahydrate or ferric chloride, and the inorganic compound containing a nano phase structure element is tellurium dioxide or sodium tellurite; the ratio of the amount of the reducing oxidant, the volume of the third solvent and the amount of the inorganic compound containing the nano phase structure element is (2-6): (20-50): (0.6-2), the unit of the volume is mL, and the unit of the amount of the substance is mmol; 2) dripping an oxidant solution and a dopant solution onto the surface of the nanofiber-based product, standing at 0-5°C for 5-20 minutes, then dripping a mixed solution, standing at -26-0°C for 90-160 hours, washing, and drying to obtain a nanostructure-enhanced organic thermoelectric fabric material, wherein the oxidant solution is a mixture of a first oxidant and water, and the first oxidant is a mixture of one or more of sodium persulfate, ammonium persulfate, potassium persulfate, ferric p-toluenesulfonate, ferric chloride, and potassium permanganate; the amount of the first oxidant in the oxidant solution dripped per square centimeter of the surface of the nanofiber-based product is 0.001-0.005 mol; The dopant solution is a mixture of a dopant and water, and the dopant is a mixture of one or more of p-toluenesulfonic acid, poly(4-styrenesulfonic acid), sodium p-aminobenzenesulfonate and camphorsulfonic acid; The mixed solution is a mixture of an organic thermoelectric reaction monomer and a first solvent, and the organic thermoelectric reaction monomer is 3,4-ethylenedioxythiophene; The ratio of the amount of the first oxidant in the oxidant solution, the amount of the dopant in the dopant solution and the volume fraction of the organic thermoelectric reaction monomer in the mixed solution is (3-6): (3.1-6.2): ​​(0.2-0.25), the unit of the volume fraction is mL, and the unit of the amount of the substance is mmol.

2. The preparation method according to claim 1, characterized in that: In the step 1), the fiber material is natural fiber or chemical fiber; The natural fiber is plant fiber or animal fiber, the plant fiber is made of cotton or linen, and the animal fiber is made of silk or wool; The chemical fiber is a regenerated fiber, a synthetic fiber or an inorganic fiber, the regenerated fiber is a viscose fiber or an acetate fiber, the synthetic fiber is made of nylon, polyester, acrylic fiber, spandex, vinylon, chloroprene or polypropylene, and the inorganic fiber is a basalt fiber, a carbon fiber or a glass fiber.

3. The preparation method according to claim 1, characterized in that: In the step 1), the storage solvent is anhydrous ethanol or deionized water.

4. The preparation method according to claim 1, characterized in that: In the step 1), the concentration of the nanomaterial in the nanomaterial liquid is 0.01 to 0.04 g / mL.

5. The preparation method according to claim 4, characterized in that: The third solvent is deionized water or an organic solvent, and the organic solvent is ethylene glycol and / or diethylene glycol; in the step 1), the cleaning is washing with water and alcohol alternately, and the alcohol is anhydrous ethanol or methanol.

6. The preparation method according to claim 1, characterized in that: In the step 2), the concentration of the first oxidant in the oxidant solution is 0.1 to 0.5 mol / L.

7. The preparation method according to claim 1, characterized in that: The concentration of the dopant in the dopant solution is 0.1-0.5 mol / L.

8. The preparation method according to claim 1, characterized in that: The concentration of the organic thermoelectric reaction monomer in the mixed solution is 10 to 50 μL / mL.

9. The preparation method according to claim 1, characterized in that: In the step 2), the first solvent is chloroform and / or dichloromethane.

10. The preparation method according to claim 1, characterized in that: In the step 2), the cleaning is performed by alternately washing with deionized water and ethanol, and the number of times of washing with deionized water and ethanol is at least 2 times.

11. The preparation method according to claim 1, characterized in that: In the step 2), the drying temperature is room temperature, and the drying time is at least 12 hours.