A reactive low heat generating, flame retardant, antioxidant additive and its preparation method and application, vulcanized rubber

By developing Zn(II)-HFPB, a reactive additive containing phenolic hydroxyl, amino, aldehyde and other functional groups, the problem of single function of existing additives has been solved, and the flame retardant and anti-oxidative aging properties of rubber materials have been significantly improved. For heavy-duty rubber tracks, it achieves excellent thermal and oxidative aging resistance and fatigue resistance.

CN115651010BActive Publication Date: 2024-10-15ZHUZHOU TIMES NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211165434.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-23
Publication Date
2024-10-15
Estimated Expiration
2042-09-23

AI Technical Summary

Technical Problem

The existing low-temperature thermal additives have a single function and are difficult to effectively reduce the heat generation of rubber materials and improve the flame retardant and oxidative aging resistance, resulting in quality problems such as cracks and bulges in heavy-duty rubber tracks.

Method used

Develop a reactive low heat-generating, flame-retardant, and antioxidant additive Zn(II)-HFPB, which contains functional groups such as phenolic hydroxyl, amino, aldehyde, borate, and siloxy groups. It reacts with rubber and fillers through chemical reactions. , reduce the heat generation of rubber materials, and improve the flame retardant and anti-oxidative aging properties.

Benefits of technology

The additive Zn(II)-HFPB significantly improves the thermal oxidative aging resistance, compression resistance and fatigue resistance of rubber materials. It is suitable for use in track wheel rubber materials and achieves high universality and marketability through a simple preparation method. application value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115651010B_ABST
    Figure CN115651010B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of rubber additive synthesis, and specifically discloses a reactive low heat-generating, flame-retardant, and antioxidant auxiliary Zn(II)-HFPB and its preparation method and application. Zn(II)-HFPB contains five characteristic functional groups, namely phenolic hydroxyl, amino, aldehyde, borate, and siloxy groups, which can improve the anti-oxidation and aging performance of rubber materials, reduce the heat generation of rubber materials, and enable rubber materials to have certain flame retardant properties. Also disclosed are vulcanized rubber prepared from Zn(II)-HFPB and its preparation method, which has excellent heat-oxidation aging resistance, compression resistance, fatigue resistance, and smoke suppression effect, and is suitable for track wheel rubber materials. The preparation method of the present invention is simple and easy to operate, has high universality, can share organic synthesis instruments and equipment, has high equipment versatility, and has good market application value in the field of rubber industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of rubber additive synthesis, and in particular relates to a reactive low-heat-generating, flame-retardant, antioxidant additive, a preparation method thereof, and application thereof in rubber and vulcanized rubber. Background Art

[0002] In a broad sense, a low-noise thermal additive is an active small molecule containing special functional groups. It mainly connects rubber and carbon black through chemical bonding, thereby reducing the sliding of carbon black in rubber and improving the dynamic properties of the rubber. Most common low-noise thermal additives on the market are amine compounds with relatively simple functions. At present, domestic rubber tracks for 16t heavy-duty vehicles have quality problems such as cracks and bulges. In order to improve the durability of heavy-duty rubber tracks, we should start from reducing the heat generation of rubber materials, improving flame retardancy and anti-oxidation aging properties.

[0003] Therefore, developing a low-sound thermal additive that can reduce the heat generation of rubber materials and improve flame retardancy and anti-oxidation aging performance is of great significance to the technical field. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology, and provide a reactive low heat generating, flame retardant, antioxidant auxiliary agent and its preparation method and application, as well as a vulcanized rubber prepared from the auxiliary agent.

[0005] In order to solve the above technical problems, the technical solution proposed by the present invention is:

[0006] A reactive low heat generating, flame retardant, antioxidant additive, referred to as Zn(II)-HFPB, its structural formula is as follows:

[0007] (like Figure 1 ).

[0008] The additive Zn(II)-HFPB contains five characteristic functional groups, including phenolic hydroxyl, amino, aldehyde, borate, and siloxy. Among them, phenolic hydroxyl and secondary amino can capture free radicals and improve the anti-oxidation aging performance of rubber materials; primary amine can undergo amidation reaction with carboxyl-containing fillers, siloxy can undergo esterification reaction with hydroxyl-containing fillers, and aldehyde can undergo Prins condensation reaction with the double bond of rubber, so that fillers and rubber are bonded, which reduces sliding and heat generation of rubber materials; the combination of phenylboric acid and zinc can make rubber materials have certain flame retardant properties.

[0009] The preparation method of the above-mentioned reactive low heat generating, flame retardant and antioxidant auxiliary agent comprises the following steps:

[0010] (1) 3,5-diiodo-o-hydroxybenzaldehyde and 2-(bromomethyl)phenylboronic acid are reacted to obtain FPBA, and then FPBA is reacted with zinc oxide to obtain Zn(II)-FPBA; the reaction formula is as follows: Figure 2 As shown;

[0011] (2) The Zn(II)-FPBA and 2,2-bis(3-amino-4-hydroxyphenyl)propane are reacted to obtain Zn(II)-HPB; the reaction formula is as follows: Figure 3 As shown;

[0012] (3) The Zn(II)-HPB and 3-aminopropyltriethoxysilane are reacted to obtain Zn(II)-HFPB; the reaction formula is as follows: Figure 4 shown.

[0013] Preferably, in step (1), the specific preparation process of FPBA is as follows: 3,5-diiodo-o-hydroxybenzaldehyde, 2-(bromomethyl)phenylboronic acid and cesium carbonate are placed in a reaction container, reaction aid 1 is added, and the mixture is stirred at 30-60°C for reaction for 2-6h to obtain FPBA; then zinc oxide is added, the mixture is heated to 80-100°C, and the mixture is reacted for 5-8h, and then the mixture is filtered to remove the clear liquid, the solvent is concentrated, and the mixture is dried under vacuum to obtain Zn(II)-FPBA; the reaction aid 1 is any one of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), and dimethyl sulfoxide (DMSO); and the molar ratio of 3,5-diiodo-o-hydroxybenzaldehyde, 2-(bromomethyl)phenylboronic acid, cesium carbonate, reaction aid 1, and zinc oxide is 1.1-1.8:1.0:1.5-3.0:30-150:1.1-1.5.

[0014] Preferably, in step (2), the specific preparation process of Zn(II)-HPB is: Zn(II)-FPBA, 2,2-bis(3-amino-4-hydroxyphenyl)propane, carbonate, and iodine salt are placed in a reaction bottle, reaction aid 2 is added, and the reaction is carried out at 60-120° C. for 12-36 hours under a nitrogen atmosphere. After the reaction is completed, the temperature is cooled to room temperature to obtain Zn(II)-HPB; the carbonate is sodium carbonate or potassium carbonate; the iodine salt is potassium iodide or sodium iodide; the reaction aid 2 is any one of N,N-dimethylformyl, N,N-dimethylacetyl, dimethyl sulfoxide, and toluene; the molar ratio of Zn(II)-FPBA, 2,2-bis(3-amino-4-hydroxyphenyl)propane, carbonate, iodine salt, and reaction aid 2 is 1:0.9-1.1:2.0-6.0:0.1-1:30-200.

[0015] Preferably, in step (3), the specific preparation process of the Zn(II)-HFPB is: adding 3-aminopropyltriethoxysilane to the Zn(II)-HPB, reacting at 60-120° C. for 12-36 hours under a nitrogen atmosphere, filtering after the reaction, removing the lower layer solution, concentrating the solvent, and vacuum drying to obtain Zn(II)-HFPB; the molar ratio of the Zn(II)-HPB to 3-aminopropyltriethoxysilane is 1:1.0-1.2.

[0016] The above-mentioned reactive low heat generating, flame retardant and antioxidant auxiliary agent Zn(II)-HFPB is used in the preparation of vulcanized rubber.

[0017] The reaction mechanism model of Zn(II)-HFPB and rubber and filler is as follows Figure 5 shown.

[0018] Based on a general inventive concept, the present invention also provides a vulcanized rubber, wherein the raw materials of the rubber mainly include the following components in parts by mass: 30-70 parts of natural rubber, 70-30 parts of butadiene rubber, 3-10 parts of zinc oxide, 1-2 parts of stearic acid, 3-10 parts of antioxidant, 5-15 parts of plasticizer, 20-50 parts of carbon black, 10-30 parts of white carbon black, 3.0-5.0 parts of vulcanization accelerator, 0.3-0.5 parts of scorch retarder, 1-3 parts of sulfur, and 1-10 parts of the reactive low heat generating, flame retardant and antioxidant additive Zn(II)-HFPB.

[0019] The method for preparing the vulcanized rubber comprises the following steps:

[0020] Step S1: adding natural rubber and butadiene rubber into a rubber mixing device, heating and adding a chemical peptizer for plasticizing;

[0021] Step S2: adding zinc oxide, stearic acid, antioxidant, low freezing point plasticizer, carbon black, white carbon black, vulcanization accelerator, and scorch retarder, and performing low-temperature mixing;

[0022] Step S3: adding the Zn(II)-HFPB, mixing, obtaining a mixed rubber, and standing for a period of time;

[0023] Step S4: adding sulfur and accelerator, mixing, thinly passing or triangular bagging on an open mixing mill to obtain a second-stage mixed rubber, and leaving it for a period of time;

[0024] Step S5: performing vulcanization treatment to obtain vulcanized rubber.

[0025] Preferably, in step S1, the temperature of the plasticizing is 100°C-130°C, and the time is 5min-10min;

[0026] In step S2, the low-temperature mixing temperature is 80-120°C and the time is 3-5 minutes;

[0027] In step S3, the mixing temperature is 130°C-160°C, the mixing time is 3-10 minutes, and the mixing time is 3-6 hours;

[0028] In step S4, the mixing temperature is 70-90°C for 3-5 minutes; the thinning or triangular bagging is performed on an open mixing mill for 3-5 times or triangular bagging for 3-5 times; and the mixture is parked for 16-24 hours;

[0029] In step S5, the vulcanization treatment conditions are as follows: vulcanization temperature 150°C, vulcanization time 10min-30min, pressure 20MPa.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1. The additive Zn(II)-HFPB of the present invention contains five characteristic functional groups, namely, phenolic hydroxyl, amino, aldehyde, borate and siloxy groups. Among them, the phenolic hydroxyl and secondary amino groups can capture free radicals and improve the anti-oxidation aging performance of the rubber material; the primary amine group can undergo amidation reaction with the carboxyl-containing filler, the siloxy group can undergo esterification reaction with the hydroxyl-containing filler, the aldehyde group can undergo Prins condensation reaction with the double bond of the rubber, the filler and the rubber are bonded, the sliding is reduced, and the heat generation of the rubber material is reduced; the combination of phenylboric acid and zinc can realize that the rubber material has certain flame retardant properties.

[0032] 2. The vulcanized rubber of the present invention is prepared with the aid of Zn(II)-HFPB, has excellent resistance to thermal oxidative aging, compression resistance, fatigue resistance and smoke suppression effects, and is suitable for use in track wheel rubber materials.

[0033] 3. The preparation method of the present invention is simple and easy to operate, has high universality, can share organic synthesis instruments and equipment, has high equipment versatility, and has good market application value in the rubber industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0035] Figure 1 It is the structural formula of the reactive low heat generating, flame retardant and antioxidant additive Zn(II)-HFPB;

[0036] Figure 2It is the reaction formula for synthesizing Zn(II)-FPBA;

[0037] Figure 3 It is the reaction formula for synthesizing Zn(II)-HPB;

[0038] Figure 4 is the reaction formula for the synthesis of Zn(II)-HFPB;

[0039] Figure 5 It is the reaction mechanism model of Zn(II)-HFPB and rubber and filler;

[0040] Figure 6 is the Zn(II)-HFPB NMR spectrum;

[0041] Figure 7 It is the DMTA curve of 1# and 2# vulcanized rubber. DETAILED DESCRIPTION

[0042] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.

[0043] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0044] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0045] The present invention adopts a three-step method to synthesize Zn(II)-HFPB:

[0046] In the first step, 3,5-diiodo-o-hydroxybenzaldehyde reacts with 2-(bromomethyl)phenylboronic acid to obtain FPBA, and then FPBA reacts with zinc oxide to obtain Zn(II)-FPBA.

[0047] In the second step, Zn(II)-FPBA and 2,2-bis(3-amino-4-hydroxyphenyl)propane are reacted to obtain Zn(II)-HPB.

[0048] In the third step, Zn(II)-HPB and 3-aminopropyltriethoxysilane are reacted to obtain Zn(II)-HFPB.

[0049] The following is further described with reference to the embodiments.

[0050] Embodiment 1:

[0051] A reactive low-heat-generating, flame-retardant, antioxidant additive Zn(II)-HFPB of the present invention comprises the following steps:

[0052] (1) 3,5-diiodo-o-hydroxybenzaldehyde (0.15 mol, 56.1 g), 2-(bromomethyl)phenylboronic acid (0.1 mol, 21.4 g) and cesium carbonate (0.2 mol, 65.2 g) were placed in a reaction vessel, N,N-dimethylformamide (DMF) (5 mol, 365 g, 388 mL) was added, and the mixture was stirred at 45°C for 4 h; then zinc oxide (0.12 mol, 9.7 g) was added, the temperature was raised to 90°C, and the mixture was reacted for 6 h, then filtered, the clear liquid was taken, the solvent was concentrated, and vacuum dried to obtain Zn(II)-FPBA;

[0053] (2) Zn(II)-FPBA (0.1 mol, 57.0 g), 2,2-bis(3-amino-4-hydroxyphenyl)propane (0.1 mol, 25.8 g), sodium carbonate (or potassium carbonate) (0.3 mol, 41.4 g), and potassium iodide (0.02 mol, 3.3 g) were placed in a reaction bottle, and N,N-dimethylformyl (5 mol, 365 g, 388 mL) was added. The mixture was reacted at 90° C. for 24 h under a nitrogen atmosphere. After the reaction was completed, the mixture was cooled to room temperature to obtain Zn(II)-HPB;

[0054] (3) 3-Aminopropyltriethoxysilane (0.1 mol, 22.1 g) was added to Zn(II)-HPB (0.1 mol), and the reaction was continued at 90° C. for 24 h under a nitrogen atmosphere. After the reaction was completed, the lower layer of solution was filtered, the solvent was concentrated, and vacuum dried to obtain Zn(II)-HFPB.

[0055] The NMR spectrum of the above Zn(II)-HFPB is as follows: Figure 6 shown.

[0056] Embodiment 2:

[0057] A vulcanized rubber for a track wheel, the rubber formula is shown in Table 1.

[0058] The preparation method of the vulcanized rubber used for the crawler wheel is as follows:

[0059] S1: Add natural rubber and butadiene rubber into a general rubber mixing equipment, add chemical peptizer and mix for 5 minutes at a temperature of 130°C;

[0060] S2: Add zinc oxide, stearic acid, antioxidant (6PPD, RD, microcrystalline wax), plasticizer (coumarone), carbon black, white carbon black, and anti-scorch agent, and mix at 110°C for 5 minutes;

[0061] S3: adding Zn(II)-HFPB or Si69 prepared in Example 1, mixing for 5 min at a mixing temperature of 130° C. to obtain a mixed rubber, and standing for 4 h;

[0062] S4: Add sulfur and accelerator NOBS, mix for 5 minutes, mix at 90℃, pass through the mixer 5 times or make triangle bags 5 times, and then get the mixed rubber 1# and 2#;

[0063] S5: After the obtained mixed rubber was left to stand for 16 hours, vulcanized rubbers 1# and 2# were obtained according to the vulcanization conditions of vulcanization temperature of 150° C., vulcanization time of 15 min, and 20 MPa.

[0064] Table 1 Rubber formula (mass fraction)

[0065] raw materials Vulcanized rubber 1# Vulcanized rubber 2# Natural rubber 70 70 Butadiene rubber 30 30 Zinc Oxide 5 5 Stearic acid 2 2 6PPD 2 2 RD 2 2 Coumarone 5 5 Microcrystalline wax 2 2 Carbon Black 40 40 White Carbon Black 15 15 Zn(II)-HFPB \ 2 Si69 2 \ sulfur 2.5 2.5 Accelerator NOBS 0.4 0.4 Anti-scorch agent 0.3 0.3

[0066] The properties of vulcanizates 1# and 2# are shown in Table 2. In terms of conventional properties, the 300% tensile strength of the vulcanizate 2# filled with Zn(II)-HFPB is better than that of the vulcanizate 1#. In terms of thermal oxidative aging performance, the thermal oxidative aging resistance of the vulcanizate 2# filled with Zn(II)-HFPB is significantly better than that of the vulcanizate 1#, which is due to the consumption of free radicals by the phenol groups in Zn(II)-HFPB. The compression permanent deformation and resilience of the vulcanizate 2# are slightly better than those of the vulcanizate 1#. The compression temperature rise performance of the vulcanizate 2# is significantly better than that of the vulcanizate 1#, which may be because Zn(II)-HFPB connects the rubber and the filler, thereby reducing the sliding of the filler in the rubber and reducing the frictional heat generated by the filler in the rubber. Since Zn(II)-HFPB contains aluminum borate, it has a certain smoke suppression effect, making the maximum smoke density of the vulcanizate 2# 1 / 2 of the vulcanizate 1#.

[0067] Figure 7 The DMTA curves of vulcanized rubbers 1# and 2# show a glass transition region at -60℃-80℃, which corresponds to the glass transition temperature Tg of rubber. The Tg of 1# and 2# are basically the same. At 0℃-80℃, the tanδ of 2# is always lower than that of 1#. Small tanδ and compression temperature rise are conducive to reducing heat generation, thereby increasing the fatigue life of rubber products, which shows that 2# vulcanized rubber has better anti-fatigue performance than 1#.

[0068] Table 2 Rubber Properties

[0069]

Claims

1. A reactive low heat generating, flame retardant, antioxidant additive, characterized in that: It is abbreviated as Zn(II)-HFPB, and its structural formula is as follows: 。 2. A method for preparing the reactive low heat generating, flame retardant, antioxidant auxiliary agent as claimed in claim 1, characterized in that: The steps include: (1) 3,5-diiodo-o-hydroxybenzaldehyde and 2-(bromomethyl)phenylboronic acid are reacted to obtain FPBA, and then FPBA is reacted with zinc oxide to obtain Zn(II)-FPBA; (2) using the Zn(II)-FPBA and 2,2-bis(3-amino-4-hydroxyphenyl)propane to react to obtain Zn(II)-HPB; (3) reacting the Zn(II)-HPB with 3-aminopropyltriethoxysilane to obtain Zn(II)-HFPB; The structural formula of the FPBA is: ; The structural formula of the Zn(II)-FPBA is: ; The structural formula of the Zn(II)-HPB is: 。 3. The method for preparing the reactive low heat generating, flame retardant and antioxidant auxiliary agent according to claim 2, characterized in that: In step (1), the specific preparation process of FPBA is as follows: 3,5-diiodo-o-hydroxybenzaldehyde, 2-(bromomethyl)phenylboronic acid and cesium carbonate are placed in a reaction container, reaction aid 1 is added, and the reaction is stirred at 30-60° C. for 2-6 hours to obtain FPBA; then zinc oxide is added, the temperature is raised to 80-100° C., and the reaction is carried out for 5-8 hours, and then the supernatant is filtered, the solvent is concentrated, and vacuum drying is performed to obtain Zn(II)-FPBA; The reaction aid 1 is any one of N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.

4. The method for preparing the reactive low heat generating, flame retardant and antioxidant auxiliary agent according to claim 3, characterized in that: The molar ratio of the 3,5-diiodo-o-hydroxybenzaldehyde, 2-(bromomethyl)phenylboric acid, cesium carbonate, reaction aid 1 and zinc oxide is 1.1-1.8:1.0:1.5-3.0:30-150:1.1-1.

5.

5. The method for preparing the reactive low heat generating, flame retardant and antioxidant auxiliary agent according to claim 2, characterized in that: In step (2), the specific preparation process of Zn(II)-HPB is as follows: Zn(II)-FPBA, 2,2-bis(3-amino-4-hydroxyphenyl)propane, carbonate, and iodine salt are placed in a reaction bottle, reaction aid 2 is added, and the reaction is carried out at 60-120° C. for 12-36 hours under a nitrogen atmosphere. After the reaction is completed, the temperature is cooled to room temperature to obtain Zn(II)-HPB; The carbonate is sodium carbonate or potassium carbonate; the iodized salt is potassium iodide or sodium iodide; The reaction aid 2 is any one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and toluene; The molar ratio of the Zn(II)-FPBA, 2,2-bis(3-amino-4-hydroxyphenyl)propane, carbonate, iodine salt and reaction aid 2 is 1:0.9-1.1:2.0-6.0:0.1-1:30-200.

6. The method for preparing the reactive low heat generating, flame retardant and antioxidant auxiliary agent according to claim 2, characterized in that: In step (3), the specific preparation process of the Zn(II)-HFPB is as follows: 3-aminopropyltriethoxysilane is added to the Zn(II)-HPB, and the reaction is carried out at 60-120° C. for 12-36 hours under a nitrogen atmosphere. After the reaction is completed, the reaction is filtered, the lower layer of solution is taken, the solvent is concentrated, and vacuum drying is performed to obtain Zn(II)-HFPB; The molar ratio of the Zn(II)-HPB to 3-aminopropyltriethoxysilane is 1:1.0-1.

2.

7. Use of the auxiliary agent according to claim 1 or the reactive low heat generating, flame retardant and antioxidant auxiliary agent prepared by the preparation method according to any one of claims 2 to 6 in the preparation of vulcanized rubber.

8. A vulcanized rubber, characterized in that: The raw materials of the rubber include the following components in parts by mass: 30-70 parts of natural rubber, 70-30 parts of butadiene rubber, 3-10 parts of zinc oxide, 1-2 parts of stearic acid, 3-10 parts of antioxidant, 5-15 parts of plasticizer, 20-50 parts of carbon black, 10-30 parts of white carbon black, 3.0-5.0 parts of vulcanization accelerator, 0.3-0.5 parts of scorch retarder, 1-3 parts of sulfur, and 1-10 parts of the auxiliary agent according to claim 1 or the reactive low heat generating, flame retardant and antioxidant auxiliary agent Zn(II)-HFPB prepared by the preparation method according to any one of claims 2 to 6.

9. A method for preparing vulcanized rubber as claimed in claim 8, characterized in that: The steps include: Step S1: adding natural rubber and butadiene rubber into a rubber mixing device, heating and adding a chemical peptizer for plasticizing; Step S2: adding zinc oxide, stearic acid, antioxidant, plasticizer, carbon black, white carbon black, and anti-scorch agent, and mixing at low temperature; Step S3: adding the Zn(II)-HFPB, mixing to obtain a mixed rubber, and standing for 3-6 hours; Step S4: adding sulfur and vulcanization accelerator, mixing, thin-passing or triangle-packing on an open mixing mill to obtain a second-stage mixed rubber, and leaving it for 16-24 hours; Step S5: vulcanizing the obtained vulcanized rubber.

10. The method for preparing vulcanized rubber according to claim 9, characterized in that: In step S1, the temperature of the plasticizing is 100°C-130°C, and the time is 5min-10min; In step S2, the low-temperature mixing temperature is 80-120°C and the time is 3-5 minutes; In step S3, the mixing temperature is 130°C-160°C, the mixing time is 3-10 minutes, and the mixing time is 3-6 hours; In step S4, the mixing temperature is 70-90°C for 3-5 minutes; the thinning or triangular bagging is performed on an open mixing mill for 3-5 times or triangular bagging for 3-5 times; and the mixture is parked for 16-24 hours; In step S5, the vulcanization treatment conditions are as follows: vulcanization temperature 150°C, vulcanization time 10min-30min, pressure 20MPa.