An aramid separator for lithium batteries and its preparation method and apparatus
By preparing oriented ultrafine aramid fiber bundles using a fabrication device and combining them with biaxial stretching and heat setting, the safety and electrolyte wettability issues of existing lithium-ion battery separators during high-power charging and discharging are solved. This achieves an improvement in the mechanical strength and electrochemical performance of high-performance aramid separators, making them suitable for various batteries and electronic devices.
Patent Information
- Application Number
- CN202211232621.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-10
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-10-10
Smart Images

Figure CN115652528B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of new materials, and specifically relates to an aramid separator for lithium batteries, its preparation method and application. Background Technology
[0002] In recent years, with the rapid development of electronic and electrical devices such as mobile phones, laptops, and new energy vehicles, lithium-ion batteries have emerged as a green and high-energy power source among various energy storage options. The separator is an indispensable component of lithium batteries, positioned between the positive and negative electrodes. It primarily serves two functions in lithium-ion and lithium-ion batteries: firstly, it separates the positive and negative electrodes, preventing direct contact between them and potential internal short circuits; secondly, it can provide a buffer for lithium... + Provides a transmission channel, enabling Li + The separator can migrate freely between electrodes, ensuring normal battery cycling. While the presence of the battery separator effectively reduces the risk of short circuits, it also increases its internal resistance. The separator itself does not participate in electrochemical reactions, but its structure and performance directly affect the overall performance of the lithium battery.
[0003] The performance of the separator has a significant impact on battery performance, providing a migration channel for lithium ions while isolating the positive and negative electrodes. As a power component in most electronic products, lithium batteries must possess good cycle life and safety performance, and a high-quality separator can effectively ensure enhanced electrochemical performance and safety characteristics. Existing technologies mostly use polyethylene and polypropylene separators, such as Chinese patents 201010578194.5 and 201310303894.7. However, lithium-ion batteries made from polyolefins are increasingly failing to meet practical needs, limiting their application and development. In particular, during high-power charging and discharging, the separator shrinks due to localized overheating, leading to short circuits and other safety issues. Furthermore, polyolefin separators have relatively low wettability to the electrolyte, which also hinders the efficient directional movement of lithium ions within the separator, limiting the electrochemical performance of lithium-ion batteries. To improve the temperature resistance of polyolefin materials, developers have coated the surface of the separator substrate with materials such as ceramic separators, PVDF-coated composite separators, and silicon nitride composite membranes, as shown in Chinese patents 202210440112.3, 201310015994.X, and 201410284617.0. By coating with high-temperature resistant coatings, the thermal stability of the separator can be improved to a certain extent. However, this prolongs the separator preparation process and complicates the process. Therefore, there is an urgent need to develop high-performance battery separator materials and their key manufacturing technologies.
[0004] Aramid, as a high-temperature resistant specialty polymer material, is widely used in industry. It possesses extremely high thermal stability (up to 400℃), excellent self-extinguishing properties, and good wettability to electrolytes, making it a promising candidate material for high-performance membranes. Currently, meta-aramid materials for membranes are mainly prepared via electrospinning, as illustrated in Chinese patents 201910686373.1, 201811529222.7, and 201810835751.3. However, electrospinning itself has limitations, such as low efficiency, high cost, and relatively low membrane strength, making it unsuitable for large-scale applications. Therefore, there is an urgent need to develop a technology for preparing aramid membranes that is suitable for large-scale production. Summary of the Invention
[0005] The primary objective of this invention is to overcome the shortcomings and deficiencies of the prior art and provide a method for preparing an aramid separator for lithium batteries.
[0006] Another object of the present invention is to provide an aramid separator for lithium batteries prepared by the method described above.
[0007] Another object of the present invention is to provide an apparatus for preparing an aramid separator for lithium batteries by the method described above.
[0008] The objective of this invention is achieved through the following technical solution:
[0009] An apparatus for preparing fine fibers includes a liquid inlet unit, a collector, and a booster. The collector is a motor-driven collecting plate. The liquid inlet unit includes a liquid inlet plate and a liquid inlet delivery pipe. The liquid inlet plate includes a liquid distribution plate with a plurality of liquid inlet holes and a first mesh surface covering the liquid distribution plate. The liquid inlet delivery pipe is connected to the liquid distribution plate. A docking plate covered with a second mesh surface is disposed opposite the first mesh surface of the liquid inlet plate. The booster drives the liquid inlet plate and / or the docking plate to move, causing the first mesh surface and the second mesh surface to reciprocate between close contact and a distance of more than 5 cm. After contact and separation, the two mesh surfaces generate fiber pulling. Each time the distance between the two mesh surfaces reaches or approaches its maximum, the collecting plate passes through the space between the two mesh surfaces to collect the fine fibers.
[0010] Preferably, the first and second mesh surfaces are mesh blankets or mesh grids; the liquid inlet plate and the docking plate are horizontally arranged.
[0011] Preferably, the collector consists of two or more collecting plates that rotate around the motor spindle, and the collecting plates can rotate at a certain angle; the docking plate is located below the liquid inlet plate, and the booster drives the docking plate to move up and down.
[0012] A method for preparing an aramid separator for lithium batteries includes the following steps:
[0013] (1) Preparation of aramid polymer solution;
[0014] (2) Preparation of ultrafine aramid fiber bundles: The aramid polymer dispersion obtained by diluting the aramid polymer solution in step (1) is introduced into the liquid inlet unit of the above device. The booster is turned on so that the first mesh surface and the second mesh surface are in close contact and then separated, generating countless fine filaments between the two mesh surfaces. The collector collects the aramid filaments through the gap between the two mesh surfaces. When the collector leaves, the two mesh surfaces are in close contact again under the drive of the booster and then separated and drawn. The collector collects the aramid filaments through the gap between the two mesh surfaces again. This cycle is repeated to collect oriented ultrafine aramid fiber bundles.
[0015] (3) A aramid separator for lithium batteries is prepared by biaxial stretching and heat setting of ultrafine aramid fiber bundles.
[0016] The liquid inlet plate in step (2) is square and made of stainless steel, chrome-plated alloy, or plastic for the surface layer; the dimensions of the liquid inlet plate and the docking plate can also be adjusted according to actual production. The dimensions of the collection plate can be adjusted according to the distance between the liquid inlet plate and the docking plate.
[0017] Preferably, the concentration of the aramid polymer dispersion in step (2) is 5-30% by mass; the maximum distance between the first and second mesh surfaces is 5-100 cm; the liquid feeding speed is 0.1-50 mL / min; and the collecting plate rotates a certain angle in the same direction after each time it leaves the gap between the two mesh surfaces.
[0018] Preferably, in step (1), the preparation of the aramid polymer solution is as follows: a neutral aramid polymer solution is prepared by polymerizing m-phenylenediamine and isophthaloyl chloride in an organic solvent under low temperature and protective atmosphere conditions; the molar ratio of m-phenylenediamine to isophthaloyl chloride is 100:(85-120); and isophthaloyl chloride is added in 2-5 batches.
[0019] Preferably, the concentration of the aramid polymer dispersion in step (2) is 10-25% by mass, more preferably 15-22%.
[0020] Preferably, the maximum distance between the first and second mesh surfaces is 15-50 cm, the angle of rotation of the collecting plate is 30-90 degrees each time, the liquid feeding speed is 10-40 mL / min, and the aramid polymer dispersion is also subjected to vacuum defoaming pretreatment.
[0021] The liquid inlet temperature in step (2) is 20-130°C, preferably 50-130°C.
[0022] The water used for washing in step (3) is deionized water or ultrapure water.
[0023] Preferably, the ultrafine aramid fiber bundles in step (3) are pretreated as follows before stretching: the ultrafine aramid fiber bundles collected in step (2) are successively replaced and washed with extract and water.
[0024] The extraction solution in step (3) is a solution with a curing effect (a single solvent, an aqueous solution of a solvent, an alcoholic solution of a solvent, or other solutions with a curing effect); preferably an aqueous solution or alcoholic solution of one or more of dimethylacetamide, dimethylformamide, dimethyl sulfoxide, ethylene glycol, glycerol, and acetone; more preferably, an aqueous solution or an alcoholic solution of N,N-dimethylacetamide or a mixed solution of N,N-dimethylacetamide with ethylene glycol and water; the extraction process is accompanied by ultrasonic treatment.
[0025] Preferably, the bidirectional stretching in step (3) specifically involves a transverse stretching of 1.1-3.0 times and a longitudinal stretching of 1.1-3.0 times; the heat setting temperature is 260-330℃, and the time is 1-60 min; the ultrasonic treatment conditions are a power of 200-1500W, a temperature of 30±10℃, and a time of 1-30 min; and the water washing conditions are a temperature of 30-90℃ and a time of 1-60 min.
[0026] Preferably, in step (1) the preparation of aramid polymer: under low temperature and nitrogen protection atmosphere, the cosolvent and m-phenylenediamine are dissolved in N,N-dimethylacetamide, and then isophthaloyl chloride is added to obtain a reaction solution; as the reaction proceeds, the temperature of the reaction solution gradually increases, and after heat preservation treatment, an alkaline agent is added for neutralization to prepare a neutral aramid polymer solution.
[0027] Preferably, the co-solvent is one or more of lithium bromide, lithium chloride, calcium chloride, and calcium bromide; the heat preservation treatment is performed at 40-80°C for 0.5-12 hours; and the alkaline agent is one or more of calcium oxide, calcium hydroxide, lithium hydroxide, magnesium hydroxide, sodium hydroxide, and organic amines.
[0028] An aramid separator for lithium batteries is prepared by the above method.
[0029] The aramid-coated membrane can be used in the preparation of lithium batteries, lithium-sulfur batteries, electrical insulation materials, adsorption and filtration materials, and flexible electronic device substrates.
[0030] The method and apparatus for preparing aramid membranes described above are also applicable to membrane formation from other raw materials, such as para-aramid, polyacrylonitrile, viscose, spandex and other synthetic fiber polymers.
[0031] The present invention has the following advantages and effects compared with the prior art:
[0032] (1) This invention obtains multilayered aramid separators of different thicknesses by changing the spatial position of the receiving plate and the number of times it passes through the receiving plate in the molding device. These separators exhibit excellent liquid absorption rate, porosity, temperature resistance, mechanical properties, and electrochemical properties, significantly improving the safe application of lithium batteries. The prepared aramid separator has a unique microporous structure and a larger specific surface area, which can significantly improve the interfacial bonding strength of the fibers within the aramid membrane, effectively enhancing the mechanical strength and electrochemical performance of the aramid separator. This can prevent short circuits caused by punctures or lithium dendrites, thus improving the safety performance of lithium batteries. In addition, the excellent electrolyte adsorption and retention capabilities of the lithium battery separator can effectively reduce the interfacial resistance of the lithium battery, optimize the electrical performance of the lithium battery, and extend the service life of the lithium battery.
[0033] (2) By changing the distance between the upper and lower plates and the liquid flow rate, this invention can easily obtain aramid membranes of different diameters, and effectively control the porosity of the aramid membrane. The amide groups in the meta-aramid macromolecules are interconnected by meta-phenyl groups. Their covalent bonds do not have a conjugation effect, and their internal rotation energy is relatively lower than that of para-aromatic polyamide fibers. The macromolecular chains exhibit a flexible structure and can withstand a certain amount of external force. When the polymer molecules are stretched, the chemical bond length increases and the bond angle increases, which promotes the straightening and alignment of the aramid polymer molecular chains, thereby achieving controllable and adjustable diameter of aramid single fibers, and thus regulating the microporous structure of the aramid membrane.
[0034] (3) The aramid membrane prepared by the present invention has a smaller diameter and a larger specific surface area, which can significantly improve the interfacial bonding strength of the fibers in the aramid membrane, effectively enhance the mechanical strength and dielectric properties of the aramid membrane, and can be widely used in the field of high-end battery membrane new materials.
[0035] (4) The preparation of aramid membrane and its preparation technology of the present invention is not only simple and convenient to operate, but also has higher production efficiency than the current conventional preparation methods. It is suitable for continuous industrial production and has wide applications in new energy batteries, filtration and separation, functional textiles, flexible circuit boards and other fields.
[0036] (5) After longitudinal and transverse stretching, residual stress is eliminated, and the molecular chains or crystals are arranged in an orderly manner along the planar direction. The orientation structure of the macromolecules is fixed under tension or relaxation. Under tension, the fiber interface is also tightly bonded, overcoming the technical difficulties of brittle and easily broken membranes produced by conventional methods. The mechanical strength and pore structure are further improved. This technical solution further expands the industrialization process and application scope of aramid membranes.
[0037] (6) The efficient preparation technology of aramid membrane of the present invention can also increase its functionalization and performance by adding functional units (such as functional nanoparticles, conductive polymers, thermally conductive fillers, etc.) to aramid polymers. This is of great significance for the diversified application of aramid membranes in various fields such as battery membranes, reinforcing materials, textile materials, electrically insulating nanopaper, flexible electronic devices, and adsorption filter media. Attached Figure Description
[0038] Figure 1 This is a flowchart illustrating the preparation process of the aramid separator of this invention.
[0039] Figure 2 This is a schematic diagram of an aramid diaphragm forming device.
[0040] Figure 3 This is a surface electron microscope image of the aramid membrane prepared in Example 4.
[0041] Figure 4 This is a surface electron microscope image of the aramid membrane prepared in Example 4, showing the diameter distribution of the aramid fine fibers.
[0042] Figure 5 This is a surface electron microscope image of the aramid membrane prepared in Example 5.
[0043] Figure 6 This is a surface electron microscope image of the aramid membrane prepared in Example 5, showing the diameter distribution of the aramid fine fibers. Detailed Implementation
[0044] The present invention will be further described in detail below with reference to embodiments, but the embodiments of the present invention are not limited thereto. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in this technical field. Test methods in the following embodiments that do not specify specific experimental conditions are generally performed under conventional experimental conditions. Unless otherwise specified, the reagents and raw materials used in the present invention are all commercially available.
[0045] The starting materials used in the preparation method of this invention can be purchased from the market or prepared according to existing technical methods.
[0046] like Figure 2 As shown, the apparatus for preparing the aramid diaphragm according to this embodiment includes: first-fourth collecting plates 1-4, upper liquid inlet plate 5, lower plate 6, booster 7, liquid inlet conveying pipe 8, upper liquid inlet plate distribution plate 9, upper liquid inlet plate mesh 10, lower plate mesh 11, lower plate bottom plate 12, motor 13, rotary shifter 14, and feed manifold 15.
[0047] Example 1
[0048] An aramid separator for lithium batteries and its preparation method, comprising the following steps:
[0049] (1) Preparation of aramid polymer: Under nitrogen protection at 15°C, an appropriate amount of co-solvent lithium bromide and m-phenylenediamine were dissolved in N,N-dimethylacetamide, wherein the molar ratio of m-phenylenediamine to isophthaloyl chloride was 100:85; then isophthaloyl chloride was added in one batch to obtain a reaction solution; as the reaction proceeded, the reaction solution was kept at 50°C for 12 h, and after the heat treatment, calcium oxide was added for neutralization to prepare a neutral aramid polymer solution.
[0050] (2) Preparation of aramid membrane: The neutral aramid polymer solution obtained in step (1) is diluted to an appropriate concentration of aramid polymer dispersion and then defoamed under vacuum. The solution is then transported to the liquid inlet delivery pipe 8. Figure 2 On the upper inlet plate 5 of the molding equipment, the booster 7 is turned on, and the lower plate 6 is lifted so that it comes into close contact with the upper inlet plate 5 and then separates. Due to the rough surface of the mesh of the upper and lower plates, countless fine filaments are generated in the two plates under the action of surface tension. At this time, the first collecting plate 1 passes through the gap between the two plates and collects the aramid filaments on the surface of the first collecting plate 1. After the first collecting plate 1 leaves the two plates, the first collecting plate 1 automatically rotates 90 degrees clockwise (maintaining this position until the plate passes through and leaves the gap between the two plates again). The circulating booster 7 continues to work, lifting the lower plate 6, which comes into close contact with the upper inlet plate 5 and then separates. At this time, the second collecting plate just passes through the gap between the two plates and collects the aramid filaments on the surface of the second collecting plate 2. After the second collecting plate 2 leaves the two plates, the second collecting plate 2 automatically rotates 90 degrees clockwise (maintaining this position until the plate passes through and leaves the gap between the two plates again). This process is repeated so that the aramid filaments form a warp and weft interwoven membrane on the collecting plate. After a certain period of collection, oriented ultrafine aramid fiber bundles are obtained. The upper liquid inlet plate in step (2) is a square with a side length of 30mm, and the surface material is stainless steel; the dimensions of the upper liquid inlet plate and the lower plate can also be adjusted according to actual production. The material of the collecting plate is stainless steel.
[0051] The concentration of the aramid polymer dispersion is 5% by mass; the size of the collecting plate is adjusted according to the distance between the upper and lower plates; the distance between the upper and lower plates can be adjusted to 5cm; the inlet rate is 10mL / min under the condition of an inlet temperature of 20℃.
[0052] (3) Stretching and shaping of aramid membrane: The aramid membrane obtained on the collection plate is replaced and washed in the extraction solution and washing solution. Finally, it is stretched longitudinally and transversely on a biaxial stretching machine and then heat-shaped in a high-temperature oven to finally prepare a high-performance aramid membrane.
[0053] The extraction solution was a mixed solution with a mass ratio of dimethylacetamide: glycerol: water = 40:30:20. The extraction process was accompanied by ultrasonic treatment at a power of 200W, a temperature of 30℃, and a time of 1 min. The washing water was deionized water at a temperature of 30℃ for 1 min. The biaxial stretching was specifically a transverse stretching of 1.1 times and a longitudinal stretching of 1.1 times. The heat setting temperature was 260℃ for 60 min.
[0054] Example 2
[0055] An aramid separator for lithium batteries and its preparation method, comprising the following steps:
[0056] (1) Preparation of aramid polymer: Under nitrogen protection at 10°C, an appropriate amount of cosolvent lithium chloride and m-phenylenediamine were dissolved in N,N-dimethylacetamide, wherein the molar ratio of m-phenylenediamine to isophthaloyl chloride was 100:115; then isophthaloyl chloride was added in two portions to obtain a reaction solution; as the reaction proceeded, the reaction solution was kept at 60°C for 8 hours, and after the heat treatment, calcium hydroxide was added for neutralization to prepare a neutral aramid polymer solution.
[0057] (2) Preparation of aramid membrane: Refer to Example 1. The concentration of the aramid polymer dispersion is 13% by mass; the size of the collecting plate is adjusted according to the distance between the upper and lower plates; the distance between the upper and lower plates can be adjusted to 20cm; the inlet temperature is 60℃ and the inlet rate is 20mL / min.
[0058] (3) Stretching and shaping of aramid membrane: The aramid membrane obtained on the collection plate is replaced and washed in the extraction solution and washing solution. Finally, it is stretched longitudinally and transversely on a biaxial stretching machine and then heat-shaped in a high-temperature oven to finally prepare a high-performance aramid membrane.
[0059] The extraction solution was a mixed solution with a mass ratio of dimethylacetamide: glycerol: water = 40:25:25. The extraction process was accompanied by ultrasonic treatment at a power of 500W, a temperature of 50℃, and a time of 10min. The washing water was deionized water at a temperature of 55℃ for 10min. The biaxial stretching was specifically a transverse stretching of 1.5 times and a longitudinal stretching of 1.5 times. The heat setting temperature was 280℃ for 30min.
[0060] Example 3
[0061] An aramid separator for lithium batteries and its preparation method, comprising the following steps:
[0062] (1) Preparation of aramid polymer: Lithium chloride and m-phenylenediamine were dissolved in N,N-dimethylacetamide under nitrogen protection at 5°C, with a molar ratio of m-phenylenediamine to isophthaloyl chloride of 100:104; then isophthaloyl chloride was added in three portions to obtain a reaction solution; as the reaction proceeded, the reaction solution was kept at 80°C for 4 hours, and after the heat treatment, calcium oxide was added for neutralization to prepare a neutral aramid polymer solution.
[0063] (2) Preparation of aramid membrane: Refer to Example 1.
[0064] The concentration of the aramid polymer dispersion is 20% by mass; the size of the collecting plate is adjusted according to the distance between the upper and lower plates; the distance between the upper and lower plates can be adjusted to 50cm; the inlet rate is 50mL / min under the condition of an inlet temperature of 130℃.
[0065] (3) Stretching and shaping of aramid membrane: The aramid membrane obtained on the collection plate is replaced and washed in the extraction solution and washing solution. Finally, it is stretched longitudinally and transversely on a biaxial stretching machine and then heat-shaped in a high-temperature oven to finally prepare a high-performance aramid membrane.
[0066] The extraction solution was a mixed solution with a mass ratio of dimethylacetamide: glycerol: water = 35:35:30. The extraction process was accompanied by ultrasonic treatment at a power of 800W, a temperature of 60℃, and a time of 30min. The washing water was deionized water at a temperature of 65℃ for 30min. The biaxial stretching was specifically a transverse stretching of 2.0 times and a longitudinal stretching of 2.0 times. The heat setting temperature was 300℃ for 10min.
[0067] Example 4
[0068] An aramid separator for lithium batteries and its preparation method, comprising the following steps:
[0069] (1) Preparation of aramid polymer: Lithium chloride and m-phenylenediamine were dissolved in N,N-dimethylacetamide under nitrogen protection at 8°C, with a molar ratio of m-phenylenediamine to isophthaloyl chloride of 100:120; then isophthaloyl chloride was added in 5 portions to obtain a reaction solution; as the reaction proceeded, the reaction solution was kept at 70°C for 8 hours, and after the heat treatment, calcium hydroxide was added for neutralization to prepare a neutral aramid polymer solution.
[0070] (2) Preparation of aramid membrane: Refer to Example 1.
[0071] The concentration of the aramid polymer dispersion is 28% by mass; the size of the collecting plate is adjusted according to the distance between the upper and lower plates; the distance between the upper and lower plates can be adjusted to 40cm; the inlet rate is 40mL / min under the condition of an inlet temperature of 110℃.
[0072] (3) Stretching and shaping of aramid membrane: The aramid membrane obtained on the collection plate is replaced and washed in the extraction solution and washing solution. Finally, it is stretched longitudinally and transversely on a biaxial stretching machine and then heat-shaped in a high-temperature oven to finally prepare a high-performance aramid membrane.
[0073] The extraction solution is a mixed solution with a mass ratio of dimethylacetamide: glycerol: water = 40:30:20. The extraction process is accompanied by ultrasonic treatment at a power of 1500W, a temperature of 90℃, and a time of 10 min. The washing water is deionized water at a temperature of 90℃ for 1 min. The washing water is either deionized water or ultrapure water. The biaxial stretching specifically involves a transverse stretching of 2.3 times and a longitudinal stretching of 2.3 times. The heat setting temperature is 330℃ for 1 min.
[0074] Example 5
[0075] An aramid separator for lithium batteries and its preparation method, comprising the following steps:
[0076] (1) Preparation of aramid polymer: Lithium chloride and m-phenylenediamine were dissolved in N,N-dimethylacetamide under nitrogen protection at 7°C, with a molar ratio of m-phenylenediamine to isophthaloyl chloride of 100:102; then isophthaloyl chloride was added in two portions to obtain a reaction solution; as the reaction proceeded, the reaction solution was kept at 60°C for 5 hours, and after the heat treatment, calcium oxide was added for neutralization to prepare a neutral aramid polymer solution.
[0077] (2) Preparation of aramid membrane: Refer to Example 1.
[0078] The concentration of the aramid polymer dispersion is 22% by mass; the size of the collecting plate is adjusted according to the distance between the upper and lower plates; the distance between the upper and lower plates can be adjusted to 40cm; the inlet rate is 35mL / min under the condition of an inlet temperature of 90℃.
[0079] (3) Stretching and shaping of aramid membrane: The aramid membrane obtained on the collection plate is replaced and washed in the extraction solution and washing solution. Finally, it is stretched longitudinally and transversely on a biaxial stretching machine and then heat-shaped in a high-temperature oven to finally prepare a high-performance aramid membrane.
[0080] The extraction solution was a mixed solution with a mass ratio of dimethylacetamide: glycerol: water = 30:30:35. The extraction process was accompanied by ultrasonic treatment at a power of 1200W, a temperature of 60℃, and a time of 20min. The washing water was deionized water at a temperature of 60℃ for 10min. The biaxial stretching was specifically a transverse stretching of 3.0 times and a longitudinal stretching of 3.0 times. The heat setting temperature was 310℃ for 2min.
[0081] Compare with Example 1
[0082] The aramid polymer dispersion obtained in step (2) of Example 3 was used to prepare a film by electrospinning, and then various indicators were tested. The results are listed in Table 1.
[0083] Compare with Example 2
[0084] In step (3) of Example 3, the longitudinal stretch ratio was 2.5, and the other membrane-making processes remained unchanged. Finally, the membrane products were tested for various indicators, and the results are listed in Table 1.
[0085] Compare with Example 3
[0086] In Example 3, the collection plate in step (2) was replaced with nylon material, while the rest of the membrane manufacturing process remained unchanged. Finally, the membrane product was tested for various indicators, and the results are listed in Table 1.
[0087] The performance testing reference standards for the aramid separator involved in the embodiments of the present invention are as follows, and the test results are listed in Table 1.
[0088] Test methods: Thickness is specified according to GB / T 20628.2-2006; tensile strength and elongation at break are tested according to GB / T29627.2-2013 using the strip specimen method; moisture content is determined according to GB / T29627.2-2013; for heat shrinkage rate, the diaphragm is treated at 250℃ for 24 hours, and the percentage change in area after shrinkage is recorded by photographing and recording the results. The formula is: (A0-A) / A0×100, where A... o This refers to the initial area of the diaphragm, where A is the final area of the diaphragm after heat treatment. The liquid absorption rate is determined as follows: a circular diaphragm with a diameter of 18 mm is immersed in lithium hexafluorophosphide electrolyte for 4 hours, and the mass after immersion is measured. Liquid absorption rate = [(M1-M0) / M0]×100; where M0 and M1 are the masses of the diaphragm before and after immersion in the electrolyte, in grams; puncture resistance is determined according to ASTM F1306-90; porosity is tested using the n-butanol absorption method: a circular diaphragm with a diameter of 18 mm is immersed in n-butanol solution for 4 hours, and the mass after immersion is measured. The porosity is calculated using the formula: porosity = [(M1-M0) / ρV]×100, where M0 and M1 are the masses of the diaphragm before and after immersion in n-butanol, in grams; ρ is the density of n-butanol, 0.81 g / cm³. 3 V represents the volume of the diaphragm, in cm³. 3Ion conductivity was calculated by measuring the bulk impedance of the simulated battery. Ion conductivity = L / (R×A), where L is the thickness of the separator; A is the effective contact area of the separator; and R is the bulk resistance of the separator (Ω). Battery assembly: In an argon-filled glove box, button batteries were assembled in the following order: positive electrode shell / stainless steel sheet / separator / stainless steel sheet / negative electrode shell. After sealing, the batteries were left to stand for 12 hours before testing. Battery cycle performance was tested by constant current charging and discharging at a current density of 0.5C for 100 cycles, with a voltage range of 3.0V to 4.2V. The capacity retention rate (%) was calculated by dividing the capacity after 100 cycles by the capacity of the first test.
[0089] Table 1. Detection data of the high-performance aramid membranes prepared in the examples.
[0090]
[0091] As shown in Table 1, the high-performance aramid separator described in this invention outperforms lithium battery separators prepared by electrospinning in all aspects. The aramid separator prepared by this invention exhibits excellent puncture resistance, effectively preventing short circuits caused by separator punctures. Furthermore, improving the puncture resistance of the separator helps reduce the deformation of the separator pores, thus promoting the lithium... + Uniform flow. (By) Figure 4 and 6 It is known that the aramid fibers used in this invention have an average diameter of less than 1 μm, which can effectively increase the bonding effect between the aramid fibers during the forming process; the dense microporous structure formed by the interlacing gaps of the aramid fibers facilitates Li + The smooth flow of the membrane ensures its safe use. This invention enables the aramid membrane to achieve a balance between thickness, porosity, and mechanical properties, thus guaranteeing the safe use of high-performance batteries. In summary, this invention produces a thin, lightweight, and high-strength aramid membrane, synergistically achieving a balance between porosity, thickness, and mechanical properties, ensuring the safe use of high-performance batteries.
[0092] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. A method for preparing an aramid separator for lithium batteries, characterized in that, Includes the following steps: (1) Preparation of aramid polymer solution: a neutral aramid polymer solution is prepared by polymerization reaction of m-phenylenediamine and isophthaloyl chloride in an organic solvent at low temperature and under a protective atmosphere; the molar ratio of m-phenylenediamine to isophthaloyl chloride is 100:(85-120); isophthaloyl chloride is added in 2-5 batches; (2) Preparation of ultrafine aramid fiber bundles: The aramid polymer dispersion obtained by diluting the aramid polymer solution in step (1) is introduced into the liquid inlet unit of the device for preparing fine fibers. The booster is turned on so that the first and second mesh surfaces are in close contact and then separated, generating countless fine filaments between the two mesh surfaces. The collector collects the aramid filaments through the gap between the two mesh surfaces. When the collector leaves, the two mesh surfaces are in close contact again under the drive of the booster and then separated and drawn. The collector collects the aramid filaments through the gap between the two mesh surfaces again. This cycle is repeated to collect oriented ultrafine aramid fiber bundles. (3) A aramid separator for lithium batteries is prepared by biaxial stretching and heat setting of ultrafine aramid fiber bundles; The apparatus for preparing fine fibers includes a liquid inlet unit, a collector, and a booster. The collector is a motor-driven collecting plate. The liquid inlet unit includes a liquid inlet plate and a liquid inlet delivery pipe. The liquid inlet plate includes a liquid distribution plate with several liquid inlet holes and a first mesh surface covering the liquid distribution plate. The liquid inlet delivery pipe is connected to the liquid distribution plate. A docking plate covered with a second mesh surface is provided opposite the first mesh surface of the liquid inlet plate. The booster drives the liquid inlet plate and / or the docking plate to move, so that the first mesh surface and the second mesh surface reciprocate between close contact and a distance of more than 5 cm. After contact and separation, the two mesh surfaces generate filaments. The collecting plate passes through the space between the two mesh surfaces to collect the fine fibers. The concentration of the aramid polymer dispersion in step (2) is 5-30% by mass; the maximum distance between the first and second mesh surfaces is 5-100 cm; the liquid feeding speed is 0.1-50 mL / min; the temperature of the aramid polymer dispersion entering the liquid feeding unit is 20-130℃; and the collecting plate rotates a certain angle in the same direction after each time it leaves the gap between the two mesh surfaces. Before stretching, the ultrafine aramid fiber bundles in step (3) are pretreated as follows: the ultrafine aramid fiber bundles collected in step (2) are successively replaced and washed with water in an extractant and water; the extractant is an aqueous solution or alcoholic solution of one or more of dimethylacetamide, dimethylformamide, dimethyl sulfoxide, ethylene glycol, glycerol, and acetone; the extraction process is accompanied by ultrasonic treatment.
2. The preparation method according to claim 1, characterized in that, The first and second mesh surfaces are mesh blankets or mesh grids; the liquid inlet plate and the docking plate are horizontally arranged.
3. The preparation method according to claim 2, characterized in that, The collector consists of two or more collecting plates that rotate around the motor spindle, and each collecting plate can rotate at a certain angle; the docking plate is located below the liquid inlet plate, and the booster drives the docking plate to move up and down.
4. The preparation method according to claim 1, characterized in that, The concentration of the aramid polymer dispersion in step (2) is 10-25% by mass, the maximum distance between the first and second mesh surfaces is 15-50 cm, the angle of rotation of the collecting plate is 30-90 degrees each time, the liquid feeding speed is 10-40 mL / min, and the aramid polymer dispersion is also subjected to vacuum defoaming pretreatment.
5. The preparation method according to claim 1, 2, 3, or 4, characterized in that, Step (3) specifically involves biaxial stretching of 1.1-3.0 times in the transverse direction and 1.1-3.0 times in the longitudinal direction; the heat setting temperature is 260-330℃, and the time is 1-60 min; the extraction solution is N,N-dimethylacetamide or a mixed solution of N,N-dimethylacetamide, ethylene glycol, and water; the ultrasonic treatment conditions are 200-1500W power, 30±10℃ temperature, and 1-30 min time; the water washing conditions are 30-90℃ temperature and 1-60 min time.
6. The preparation method according to claim 5, characterized in that, Step (1) Preparation of aramid polymer: Under low temperature and nitrogen protection atmosphere, the cosolvent and m-phenylenediamine are dissolved in N,N-dimethylacetamide, and then isophthaloyl chloride is added to obtain a reaction solution; as the reaction proceeds, the temperature of the reaction solution gradually increases. After heat preservation treatment, an alkaline agent is added for neutralization to prepare a neutral aramid polymer solution. The co-solvent is one or more of lithium bromide, lithium chloride, calcium chloride, and calcium bromide; the heat preservation treatment is performed at 40-80°C for 0.5-12 hours; the alkaline agent is one or more of calcium oxide, calcium hydroxide, lithium hydroxide, magnesium hydroxide, sodium hydroxide, and organic amine.
7. The aramid separator for lithium batteries prepared by the method according to any one of claims 1-6.
Citation Information
Patent Citations
Multilayer polyolefin battery diaphragm and preparation method thereof
CN102544416A
High-density polyethylene resin composition for microporous membrane and preparation method of high-density polyethylene resin composition
CN103342842A
Silicon nitride composite separator and preparation method thereof
CN103928647A
Ceramic diaphragm and preparation method thereof
CN105206779A
A preparation method of aramid lithium battery composite separator
CN109004155A