A ceramic isolation agent and a preparation method thereof and a ceramic high-temperature refractory mica tape

By coating the mica tape paper surface with a ceramic isolating agent to form a ceramic layer, the problem of insufficient fire resistance of the mica tape at high temperatures is solved, the insulation and fire resistance properties at high temperatures are improved, and the cost is reduced, making it suitable for high temperature environments.

CN115662677BActive Publication Date: 2024-10-01PAMICA TECH CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211091177.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-07
Publication Date
2024-10-01
Estimated Expiration
2042-09-07

AI Technical Summary

Technical Problem

Mica tape has insufficient fire resistance and insulation properties at high temperatures and is easily broken down. Existing methods such as compounding PE film on the paper surface of mica tape cannot effectively solve its high-temperature insulation performance problem.

Method used

Ceramic release agent is used, which is composed of silicone adhesive, zirconia dispersion, fumed silica, glass powder, muscovite powder and calcined mica powder. It forms a ceramic layer through heating reaction and is coated on the mica tape paper. After surface drying, a ceramic high-temperature refractory mica tape is formed.

Benefits of technology

The ceramic layer is formed at a high temperature of 300-400℃, which improves the fire resistance and insulation performance of the mica tape, prevents breakdown, reduces costs, and provides moisture-proof performance, making it suitable for high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003837047100000011
    Figure BDA0003837047100000011
  • Figure BDA0003837047100000021
    Figure BDA0003837047100000021
  • Figure BDA0003837047100000031
    Figure BDA0003837047100000031
Patent Text Reader

Abstract

The present invention discloses a ceramic release agent and a preparation method thereof and a ceramic high-temperature fire-resistant mica tape. The release agent is prepared from a certain ratio of organic silicone resin, toluene, reinforcing agent, debugging agent, silane coupling agent, zirconium oxide dispersion, glass powder, muscovite powder, calcined mica powder and synthetic mica powder as raw materials. The preparation method of the mica tape is as follows: 1. Coating the ceramic release agent on the mica paper surface of the mica tape; 7.2. Drying and cooling the mica tape coated with the ceramic release agent layer to obtain the ceramic high-temperature fire-resistant mica tape. After high-temperature curing, the ceramic release agent has the properties of no silking, no tape break, no sticking, no anti-sticking and moisture-proof. The ceramic release agent is coated on the mica paper surface of the mica tape, which not only improves the voltage resistance, insulation performance and fire and high temperature resistance, but also makes the mica tape have excellent wrapping properties such as no silking, no anti-sticking, no tape break, no sticking and no wire sticking.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mica tapes, and in particular to a ceramic isolation agent and a preparation method thereof, and a ceramic high-temperature refractory mica tape. Background Art

[0002] With the rapid development of the mica tape industry, mica tape is now widely used as the insulation layer of wires and cables. Therefore, the use of mica tape in the wire and cable industry has increased rapidly, and higher requirements are placed on its fire resistance and insulation resistance. However, the breakdown performance of mica tape is not very good, mainly because impurities on the surface of mica paper are difficult to remove when making mica paper. After the mica tape is made and wrapped around the cable conductor, it is easy to be broken down when it is heated at 950℃ for 180 minutes and a voltage of 1000V is applied.

[0003] At present, the solution to the above problems of mica tape is to laminate a layer of PE film on the surface of mica tape, but it still cannot solve the problem of its insulation performance under high temperature. With the increasing demand for mica tape performance, it will be the top priority for mica tape industry companies to solve the insulation performance of mica tape under high temperature without increasing costs. Summary of the invention

[0004] Based on the above-mentioned prior art, the present invention provides a ceramic isolation agent and a preparation method thereof and a ceramic high-temperature refractory mica tape. The ceramic isolation agent has the properties of no threading, no tape breakage, no sticking, no anti-sticking and moisture-proof after high-temperature curing. The ceramic isolation agent is coated on the mica paper surface of the mica tape, which not only improves the voltage resistance, insulation performance and fire and high temperature resistance, but also makes the mica tape have excellent wrapping properties such as no threading, no anti-sticking, no tape breakage and no sticking.

[0005] The technical solution adopted to achieve the above-mentioned purpose of the present invention is:

[0006] A ceramic release agent, the release agent is composed of an organic silicon adhesive and water, the mass fraction of the organic silicon adhesive is 35-45%;

[0007] The organosilicon adhesive is prepared from the following raw materials in parts by weight:

[0008]

[0009]

[0010] Furthermore, the mass fraction of the zirconium oxide dispersion is 20%-30%.

[0011] Furthermore, the reinforcing agent is fumed silica.

[0012] Further, the adjusting agent is dibenzoyl peroxide.

[0013] Furthermore, the particle size of the glass powder is 1200 mesh, the particle size of the muscovite powder is 2000 mesh, the particle size of the calcined mica powder is 2000 mesh, and the particle size of the synthetic mica powder is 1200 mesh.

[0014] A method for preparing a ceramic release agent comprises the following steps:

[0015] 1. Mix the silicone resin, toluene, reinforcing agent, debugging agent, silane coupling agent, zirconium oxide dispersion, glass powder, muscovite powder, calcined mica powder and synthetic mica powder, mix them evenly, put them into a boiler for heating, stir and react at 50-70°C for 10-20 minutes, and after the reaction is completed, cool them to obtain a silicone adhesive;

[0016] 2. Evenly mix the organosilicon adhesive and water to obtain the ceramic release agent.

[0017] A ceramic high temperature refractory mica tape is prepared by the following method:

[0018] 1. Coat a layer of the ceramic release agent according to claim 1 on the mica paper surface of the mica tape;

[0019] 2. Dry and cool the mica tape coated with the ceramic release agent layer in step 6.1 to obtain the ceramic high-temperature refractory mica tape.

[0020] Furthermore, it is characterized in that: in step 2, the drying temperature is 90-170° C. and the drying time is 10-20 min.

[0021] Compared with the prior art, the beneficial effects and advantages of the present invention are:

[0022] 1. The release agent of the present invention is coated on the mica tape, and its efficacy mechanism at high temperature is: it forms a ceramic layer after decomposition under a high temperature flame of 300-400°C. Since the ceramic layer is formed at high temperature, it is transformed from low heat conduction to high thermal resistance, which effectively protects the mica from being broken down within 180 minutes at high temperature of 1000-1100°C. At the same time, the insulation resistance at high temperature is not less than 10MΩ, the insulation resistance of the bare mica tape is 13-15MΩ, and the insulation resistance of the overall cable combined with the cable structure is 75MΩ, and the insulation resistance at room temperature is above 500MΩ.

[0023] 2. The ceramic isolation agent of the present invention is characterized by adding some inorganic materials, which have moisture-proof and anti-sticking properties after curing, avoiding the need for drying the mica tape during use, reducing the use cost of the mica tape, and improving the use efficiency of the mica tape.

[0024] 3. The mica tape of the present invention has good fire resistance (it will not be broken down when it is heated at 950-1100°C for 180 minutes and when a voltage of 1KV is applied), high voltage resistance, no threading, no tape breakage, no sticking, and good moisture resistance, and can be placed in a humid environment for a long time without being corroded or deteriorated.

[0025] 4. The present invention solves the problem of raising the temperature of mica tape to 1100°C at high temperature. The ceramic isolation agent technology is used to melt the ceramic isolation agent and mica paper into a ceramic solid shell under a flame of 300-400°C to improve the fire resistance. This fills the problem that mica tape cannot be used for the outer layer of the cable. This will provide a new way of using ceramic high-temperature fire-resistant mica tape and expand the application scenarios. DETAILED DESCRIPTION

[0026] The present invention is described below in conjunction with specific embodiments, but is not intended to limit the scope of the present invention.

[0027] The raw materials used in the following examples are as follows:

[0028] 1. The manufacturer of silicone resin is Jiangyin Zhongxin Silicon Material Co., Ltd., and the brand is SH-021;

[0029] 2. The manufacturer of nano zirconium oxide is Hangzhou Hengna Materials Co., Ltd., and its mass fraction is NH-R30C;

[0030] 3. The manufacturer of fumed silica is Hubei Huifu Nanomaterials Co., Ltd.;

[0031] 4. The particle size of glass powder is 1200 mesh, the particle size of muscovite powder is 2000 mesh, the particle size of calcined mica powder is 2000 mesh, and the particle size of synthetic mica powder is 1200 mesh.

[0032] Example 1

[0033] A ceramic release agent, the release agent is composed of an organic silicon adhesive and water, the mass fraction of the organic silicon adhesive is 45%;

[0034] The organosilicon adhesive is prepared from the following raw materials in parts by weight:

[0035]

[0036] The zirconium oxide dispersion is prepared by dispersing nano zirconium dioxide in water, and the mass fraction thereof is 25%.

[0037] The preparation method of the above-mentioned ceramic isolation agent is as follows:

[0038] 1. Mix silicone resin, toluene, fumed silica, dibenzoyl peroxide, silane coupling agent, zirconium oxide dispersion, glass powder, muscovite powder, calcined mica powder and synthetic mica powder, mix well and heat in a boiler, stir and react at 60°C for 15 minutes, and after the reaction is completed, cool to obtain a silicone adhesive;

[0039] A ceramic high temperature refractory mica tape is prepared by the following method:

[0040] 1. Coat the mica paper surface of the original mica tape with the above-mentioned ceramic release agent;

[0041] 2. Place the mica tape coated with the ceramic release agent layer in step 1 into an oven for drying, control the oven temperature to 110° C., and control the drying time to 20 min;

[0042] 3. The dried mica tape is rolled up, and the rolled mica tape blank is cut into strips by a slitting machine and rolled up to obtain the ceramicized high-temperature refractory mica tape.

[0043] Example 2

[0044] A ceramic release agent, the release agent is composed of an organic silicon adhesive and water, the mass fraction of the organic silicon adhesive is 40%;

[0045] The organosilicon adhesive is prepared from the following raw materials in parts by weight:

[0046]

[0047] The zirconium oxide dispersion is prepared by dispersing nano zirconium dioxide in water, and the mass fraction thereof is 20%.

[0048] The preparation method of the above-mentioned ceramic isolation agent is as follows:

[0049] 1. Mix silicone resin, toluene, fumed silica, dibenzoyl peroxide, silane coupling agent, zirconium oxide dispersion, glass powder, muscovite powder, calcined mica powder and synthetic mica powder, mix well and heat in a boiler, stir and react at 65°C for 10 minutes, and after the reaction is completed, cool to obtain a silicone adhesive;

[0050] 2. Evenly mix the organosilicon adhesive and water to obtain the ceramic release agent.

[0051] A ceramic high temperature refractory mica tape is prepared by the following method:

[0052] 1. Coat the mica paper surface of the original mica tape with the above-mentioned ceramic release agent;

[0053] 2. Place the mica tape coated with the ceramic release agent layer in step 1 into an oven for drying, control the oven temperature to 130° C., and control the drying time to 15 min;

[0054] 3. The dried mica tape is rolled up, and the rolled mica tape blank is cut into strips by a slitting machine and rolled up to obtain the ceramicized high-temperature refractory mica tape.

[0055] Example 3

[0056] A ceramic release agent, the release agent is composed of an organic silicon adhesive and water, the mass fraction of the organic silicon adhesive is 40%;

[0057] The organosilicon adhesive is prepared from the following raw materials in parts by weight:

[0058]

[0059] The zirconium oxide dispersion is prepared by dispersing nano zirconium dioxide in water, and the mass fraction thereof is 30%.

[0060] The preparation method of the above-mentioned ceramic isolation agent is as follows:

[0061] 1. Mix silicone resin, toluene, fumed silica, dibenzoyl peroxide, silane coupling agent, zirconium oxide dispersion, glass powder, muscovite powder, calcined mica powder and synthetic mica powder, mix well and heat in a boiler, stir and react at 55°C for 20 minutes, and after the reaction is completed, cool to obtain a silicone adhesive;

[0062] 2. Evenly mix the organosilicon adhesive and water to obtain the ceramic release agent.

[0063] A ceramic high temperature refractory mica tape is prepared by the following method:

[0064] 1. Coat the mica paper surface of the original mica tape with the above-mentioned ceramic release agent;

[0065] 2. Place the mica tape coated with the ceramic release agent layer in step 1 into an oven for drying, control the oven temperature to 160° C., and control the drying time to 10 min;

[0066] 3. The dried mica tape is rolled up, and the rolled mica tape blank is cut into strips by a slitting machine and rolled up to obtain the ceramicized high-temperature refractory mica tape.

[0067] The ceramic high temperature refractory mica tapes prepared in Examples 1-3 were tested as follows:

[0068] 1. Thickness: Tested according to the method specified in the national standard GB / T5019.2-2009:

[0069] 2. Quantitative: Test according to the method specified in the national standard GB / T5019.2-2009;

[0070] 3. Tensile strength: Tested according to the method specified in the national standard GB / T5019.2-2009;

[0071] 4. Breakdown voltage: Tested according to the method specified in the national standard GB / T1408.1-2016;

[0072] 5. Volume resistivity (normal temperature): tested according to the method specified in the national standard GB / T31838.2-2019;

[0073] 6. Insulation resistance: actual parameters of customers

[0074] 7. Fire resistance: Tested in accordance with the method specified in the national standard GB / T19216.21-2003;

[0075] The test results are shown in the following table:

[0076] Performance indicators of mica tape

[0077]

[0078]

[0079] It can be seen from the above table that the mica tape of the present invention has moderate thickness and basis weight, and has good mechanical properties, voltage resistance, insulation properties and fire resistance.

Claims

1. A ceramic release agent, Features: The release agent is composed of an organic silicon adhesive and water, and the mass fraction of the organic silicon adhesive is 35-45%; The organosilicon adhesive is prepared from the following raw materials in parts by weight: 20-40 parts of silicone resin Toluene 25-35 parts Reinforcing agent 5-15 parts 0.5-1.5 parts of debugging agent Silane coupling agent 1.5-3 parts Zirconia dispersion 5-10 parts Glass powder 10-20 parts 5-15 parts of muscovite powder Calcined mica powder 15-25 parts 5-10 parts of synthetic mica powder; The reinforcing agent is fumed silica; The debugging agent is dibenzoyl peroxide.

2. The ceramic separator according to claim 1, Features: The mass fraction of the zirconium oxide dispersion is 20%-30%.

3. The ceramic separator according to claim 1, Features: The particle size of the glass powder is 1200 meshes, the particle size of the muscovite powder is 2000 meshes, the particle size of the calcined mica powder is 2000 meshes, and the particle size of the synthetic mica powder is 1200 meshes.

4. A method for preparing the ceramic separator according to claim 1, Features The steps include: 4.

1. Mix the silicone resin, toluene, reinforcing agent, debugging agent, silane coupling agent, zirconium oxide dispersion, glass powder, muscovite powder, calcined mica powder and synthetic mica powder, mix well and heat in a boiler, stir and react at 50-70°C for 10-20 minutes, and after the reaction is completed, cool to obtain a silicone adhesive; 4.

2. Evenly mix the organic silicon adhesive and water to obtain the ceramic release agent.

5. A ceramic high temperature refractory mica tape, characterized in that it is prepared by the following method: 5.

1. Coat a layer of the ceramic release agent according to claim 1 on the mica paper surface of the mica tape; 5.

2. Dry and cool the mica tape coated with the ceramic release agent layer in step 5.1 to obtain the ceramic high-temperature refractory mica tape.

6. The ceramic high temperature refractory mica tape according to claim 5, Features: In step 5.2, the drying temperature is 90-170° C. and the drying time is 10-20 min.