An interface connection structure for efficient heat dissipation of power electronic devices and a preparation method thereof

By using metal-metal foam composites to regulate thermal conductivity and thermal expansion coefficients in high-performance power electronic devices, the problems of low thermal conductivity and mismatch of thermal expansion coefficients of existing thermal interface materials are solved, and efficient heat dissipation and high temperature stability are achieved , improves the reliability and life of the device.

CN115662966BActive Publication Date: 2024-11-01DALIAN UNIV OF TECH
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202211328767.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-27
Publication Date
2024-11-01
Estimated Expiration
2042-10-27

AI Technical Summary

Technical Problem

The existing thermal interface materials have low thermal conductivity, mismatched thermal expansion coefficient, high interconnection temperature, and limited service temperature in high-performance power electronic devices, resulting in insufficient heat dissipation performance, affecting the reliability and life of the device.

Method used

Using metal-metal foam composite materials as the interface connection structure, by regulating the ratio of porous foam metal and medium and high temperature lead-free solder, an interface connection structure with high thermal conductivity and low thermal expansion coefficient is designed to achieve low temperature connection and high temperature service, and reduce weight Melting temperature improves the matching degree of thermal conductivity and thermal expansion coefficient.

Benefits of technology

The matching degree of thermal conductivity and thermal expansion coefficient of the interface connecting structure is significantly improved, the residual thermal stress of the connecting structure is reduced, the high-temperature service stability of the power devices is enhanced, the thermal mismatch is reduced, and the heat dissipation efficiency and reliability are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115662966B_ABST
    Figure CN115662966B_ABST
Patent Text Reader

Abstract

The present invention provides an interface connection structure and preparation method for efficient heat dissipation of power electronic devices, including a first low-temperature solder layer and a second low-temperature solder layer, between which a metal-metal foam composite material is placed, and the metal-metal foam composite material has structural and performance designability, and the thermal conductivity and thermal expansion coefficient of the thermal interface connection structure can be adjusted according to the selected power device packaging material, so as to achieve a two-way synchronous improvement in heat dissipation efficiency and the matching degree of thermal expansion coefficients between various packaging materials. The first low-temperature solder layer is located between the upper substrate and the metal-metal foam composite material, and the second low-temperature solder layer is located between the metal-metal foam composite material and the lower substrate. During reflow soldering and subsequent service, the melting-reducing elements in the low-temperature solders on both sides and the medium- and high-temperature lead-free solders in the metal-metal foam composite material diffuse in both directions, so that the remelting temperature of the connection structure is higher than the melting point of the low-temperature solder layer, thereby achieving "low-temperature connection, high-temperature service".
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of high-performance and high-density microelectronic packaging, and in particular relates to an interface connection structure for efficient heat dissipation of power electronic devices and a preparation method thereof. Background Art

[0002] With the development of emerging fields such as new energy vehicles, fifth-generation mobile communication technology, photovoltaics, and radio frequency communications, the integration of devices has gradually increased. IGBT power devices and wide bandgap semiconductor devices with higher voltage ratings, higher switching frequencies, higher operating temperatures (greater than 500°C), and higher performance have entered a period of explosive growth and have broad application prospects. However, power devices generate heat when working at high power. As the heat continues to accumulate, the temperature of the chip will rise. In terms of the maximum junction temperature, the rated temperature of IGBT power devices is as high as 175°C, and the expected operating temperature of wide bandgap semiconductor devices can be as high as 300°C. Excessive temperature causes the output power of the device to be greatly attenuated, and the performance of the device cannot be fully utilized. Heat dissipation has become the main problem limiting the application of power devices. According to statistics, thermal fatigue failures caused by overheating account for 55% of IGBT device failures. [1-3] ( Fig.17 ), the heat dissipation performance directly affects the performance and life of power device products.

[0003] Take IGBT power devices as an example ( Fig.18 ), the heat generated by the chip needs to be dissipated through the heat sink. The thermal interface material (TIM) is located between the heater and the heat sink, playing an important bridging role in the heat transfer process.

[0004] However, existing thermal interface materials are difficult to meet the heat dissipation requirements of power devices, mainly in the following aspects:

[0005] Traditional heat dissipation materials mainly include thermal conductive silicone (0.4~4W / m·K), thermal conductive gel (2~5W / m·K), conductive pads (0.8~3W / m·K) and phase change materials (0.7~1.5W / m·K). [4-9] The thermal conductivity of these heat dissipation materials is low, which is several orders of magnitude lower than that of adjacent devices (e.g., Cu: 398 W / m·K) (Table 1). The heat transfer performance is poor and is far from meeting the heat dissipation requirements of high-performance chips.

[0006] Table 1 Thermal conductivity of various parts of power devices

[0007]

[0008]

[0009] The thermal conductivity of lead-free solder can reach 20-40W / m·K [10-12] , and the melted solder during the interconnection process can fill the small gap between the power device module and the heat sink connection interface, achieve good thermal contact, and reduce the interface thermal resistance. However, the solder requires the interconnection process temperature > melting point > service temperature. On the one hand, the melting point of the solder used as a thermal interface material must be lower than the melting point of the solder joint on the electronic device side to avoid remelting of the solder joint on the device side, which greatly limits the choice of thermal interface solder; on the other hand, the melting point of lead-free solder with higher thermal conductivity is generally above 200°C. The higher connection temperature will bring thermal stress to other devices on the substrate or the substrate itself, and even cause thermal damage, which will bring great hidden dangers to the stable service of subsequent electronic devices.

[0010] Power modules often use a stacked packaging structure, such as Fig.19 As shown in the figure, the thermal expansion coefficients of materials in different layers are different. The thermal expansion coefficients of the chip and substrate materials are both less than 8ppm / ℃, while the thermal expansion coefficient of lead-free solder TIM is between 15 and 30ppm / ℃. The difference in thermal expansion coefficients between the power module and the heat sink can easily cause thermal stress. The thermal interface material layer, which serves as a heat dissipation bridge, becomes a weak point, which will affect the reliability of the device during long-term thermal cycling or power cycling.

[0011] Therefore, thermal interface materials have become one of the bottlenecks in improving the heat dissipation performance of electronic products, and the development of new thermal interface connection materials and structures has become a top priority. When considering new thermal interface connection materials, lower connection temperature, thermal expansion coefficient matching, high thermal conductivity, high temperature resistance and good high temperature reliability should all be taken into account.

[0012] The literature on the application of porous foam metal in thermal interface materials in the prior art is as follows:

[0013] Porous foam metal materials have both porous structure and metallic properties, and have excellent properties such as low density, large specific surface area, high thermal conductivity, high specific strength and specific stiffness.

[0014] Chinese patent CN114479773A discloses a composite thermal interface material composed of foam metal and liquid metal, which mainly utilizes the inherent three-dimensional continuous structure of foam metal to solve the high-temperature melting and leakage problem of liquid metal in the thermal interface material; Chinese patents CN102504769A and CN103965839A mainly utilize the compressibility and flexibility of porous foam metal to prepare thermal interface materials with high elasticity and flexibility, while reducing material costs.

[0015] Chinese patent CN108511407A discloses a thermal interface material and a preparation method and an application method thereof. The thermal interface material having a sandwich structure is prepared by loading a low-melting-point metal and / or alloy on the upper and lower surfaces of a foam metal by electroplating, chemical plating, evaporation, sputtering, ion plating, etc., and is used to solve the heat dissipation problem of power devices. However, the above patent does not fully consider the thermal fatigue failure problem caused by the low effective thermal conductivity of the foam metal in the atmospheric environment and the large difference in thermal expansion coefficient between the thermal interface material and the adjacent packaging material.

[0016] In addition to the above technical solutions, the literature on thermal expansion coefficient mismatch in thermal interface materials is as follows:

[0017] The thermal transfer interface material and solder preform disclosed in China CN1894791B utilize thermal expansion coefficient modifying components in TIM to minimize the negative impact of thermal expansion coefficient mismatch. The beneficial effect mentioned in the article is "preferably, the thermal expansion coefficient mismatch between TIM and substrate is between about 5μm / m℃ and about 30μm / m℃. Even better, the thermal expansion coefficient mismatch between TIM and substrate is between about 5μm / m℃ and about 20μm / m℃. Even better, the thermal expansion coefficient mismatch between TIM and substrate is less than about 10μm / m℃". Accordingly, using the TIM designed by this patent, the thermal expansion coefficient mismatch between TIM and substrate is between 2 and 20ppm / ℃.

[0018] References

[0019] [1]Sheng K,Williams BW,Finney S JA review of IGBT models[J].IEEETransactions on Power Electronics.2000,15(6):1250-1266.

[0020] [2]Williams,Finney,Jon S,et al.Review of IGBT models[J].PowerElectronics IEEE Transactions on.2000,15(6):1250-1266.

[0021] [3]Smet V.Aging and failure modes of IGBT power modules undergoing power cycling in high temperature environments[D].2010.

[0022] [4]Wang B,Hu A,Tang Y.Junction temperature forecast and failureanalysis of IGBT based on electro-thermal model[J].Electric Machines&Control.2012,16(8):87-93.

[0023] [5]Luo X,Tang G F,Wen J L,et al.Over-current Failure Mechanism ofIGBT Within Voltage Source Converter Based High Voltage Direct Current[J].Zhongguo Dianji Gongcheng Xuebao / Proceedings of the Chinese Society ofElectrical Engineering.2009,29(33):1-7.

[0024] [6]Yamamoto T,Adachi A,Umezawa K,et al.Research on efficient water-cooled heatsink for wind power generation system[C].2010.

[0025] [7]Mcnamara A J,Joshi Y K,Zhang Z M.CHARACTERIZATION OFNANOSTRUCTURED THERMAL INTERFACE MATERIALS-A REVIEW[C].2011.

[0026] [8]Jadhav S G,Deppisch C.Coated thermal interface in integratedcircuit die[P].

[0027] [9]Hansson J,Zanden C,Ye L,et al.Review of current progress ofthermal interface materials for electronics thermal management applications[C].2016.

[0028]

[10] Jung D W,Kim J M,Yoon H W,et al.Solution-processable thermallyconductive polymer composite adhesives of benzyl-alcohol-modified boronnitride two-dimensional nanoplates[J].CHEMICAL ENGINEERING JOURNAL-LAUSANNE-.2019.

[0029]

[11] Thermal Conductivity of Polymers and Their Nanocomposites[J].Advanced Materials.2018,30(17).

[0030]

[12] Gordon,Rachel.Thermal interface materials:opportunities andchallenges for developers[J].Translational Materials Research.2015,2(2):20301.

[0031]

[13] Roy C K,Bhavnani S,Hamilton M C,et al.Investigation into theapplication of low melting temperature alloys as wet thermal interfacematerials[J].International Journal of Heat and Mass Transfer.2015,85:996-1002.

[0032]

[14] Dutta I,Raj R,Kumar P,et al.Liquid Phase Sintered Solders with Indium as Minority Phase for Next Generation Thermal Interface MaterialApplications[J].Journal of Electronic Materials.2009,38(12):2735-2745.

[0033]

[15] Vijay K.Solder-TIMs(Thermal Interface Materials) for superior thermal management in power electronics[C].2012. Summary of the invention

[0034] In order to meet the high heat dissipation requirements of high-performance power electronic devices and solve the problems of low thermal conductivity, mismatched thermal expansion coefficient, high interconnection temperature, and limited service temperature in the existing technical solutions, the present invention provides an interface connection structure and preparation method for efficient heat dissipation of power electronic devices. The metal-metal foam composite material used in this method has structural performance designability, and the thermal conductivity and thermal expansion coefficient of the thermal interface connection structure can be adjusted according to the selected power device packaging material, so as to achieve a two-way synchronous improvement in heat dissipation efficiency and the matching degree of thermal expansion coefficients between various packaging materials. The present invention can effectively improve the thermal conductivity of the connection structure and achieve "low temperature connection and high temperature service". The preparation process is relatively simple and the cost is low. It can not only be used as a thermal interface material between power electronic devices and heat sinks, but also as a high-temperature packaging chip interconnection material.

[0035] To achieve the above object, the present invention adopts the following technical solutions:

[0036] An interface connection structure for efficient heat dissipation of a power electronic device, the interface connection structure comprising a first low-temperature solder layer and a second low-temperature solder layer, a metal-metal foam composite material is placed between the first low-temperature solder layer and the second low-temperature solder layer; the first low-temperature solder layer is located between an upper substrate and the metal-metal foam composite material, and the second low-temperature solder layer is located between the metal-metal foam composite material and a lower substrate; the first low-temperature solder layer and the second low-temperature solder layer have a preset thickness, the metal-metal foam composite material is composed of porous foam metal and medium-high temperature lead-free solder, and has a preset thickness, thermal conductivity and thermal expansion coefficient, and the porous foam metal and medium-high temperature lead-free solder in the metal-metal foam composite material are regulated. The proportion of solder makes the thermal conductivity of the interface connection structure between 60 and 250 W / m·K, and the thermal expansion coefficient is adjustable between 12 and 25 ppm / °C. By selecting metal-metal foam composite materials with different physical and chemical properties and selecting the first low-temperature solder layer and the second low-temperature solder layer with different physical and chemical properties, the remelting temperature of the interface connection structure is adjusted to a preset value. During reflow soldering and subsequent service, the melting-reducing elements in the first low-temperature solder layer and the second low-temperature solder layer diffuse bidirectionally with the medium-high temperature lead-free solder in the metal-metal foam composite material, so that the remelting temperature of the connection structure is higher than the melting point of the low-temperature solder layer and lower than the melting point of the medium-high temperature lead-free solder of the metal-metal foam composite material, thereby achieving low-temperature connection and high-temperature service.

[0037] Furthermore, the metal matrix of the high melting point porous foam metal includes Cu, Ag, Al, and Mg.

[0038] Furthermore, the porosity of the high melting point and high thermal conductivity porous foam metal is 20% to 90%.

[0039] Furthermore, the pore size of the high melting point and high thermal conductivity porous foam metal is 20 to 200 μm.

[0040] Furthermore, the thickness of the metal-metal foam composite material is 20-500 μm.

[0041] Furthermore, the composition of the medium- and high-temperature lead-free solder is any one of pure Sn, Sn-Ag-Cu, Sn-Ag, Sn-Cu, Au-Sn, or an alloy formed by adding any one of Ni, Sb and Zn to the above components, having a melting point greater than 200°C and a thermal conductivity greater than 20 W / m·K.

[0042] Furthermore, the thickness of the first low-temperature solder layer is 5 to 50 μm, and the thickness of the second low-temperature solder layer is 5 to 50 μm.

[0043] Furthermore, the composition of the low-temperature solder is any one of Sn-Bi, Sn-In, Sn-Bi-In, Ag-In, or a low-temperature solder formed by adding any one of Cu, Ag, Ga, Sb to the above components, and the metal-metal foam composite material needs to be non-melting within the low-temperature solder brazing temperature range.

[0044] The connection structure of upper substrate / first low-temperature solder layer-metal-metal foam composite material-second low-temperature solder layer / lower substrate is subjected to reflow soldering at the soldering temperature of the first low-temperature solder layer and the second low-temperature solder layer to achieve metallurgical connection.

[0045] The metal-metal foam composite material in the connection structure described in the present invention does not melt within the low-temperature soldering temperature range. During the reflow soldering process, the first low-temperature solder layer and the second low-temperature solder layer melt at the same time, wherein the first low-temperature solder layer realizes a metallurgical connection between the upper substrate and the metal-metal foam composite material; and the second low-temperature solder layer realizes a metallurgical connection between the metal-metal foam composite material and the lower substrate.

[0046] The present invention also discloses a method for preparing the interface connection structure for efficient heat dissipation of the power electronic device, which specifically comprises the following steps:

[0047] Step 1: Prepare a metal-metal foam composite material. Clean the selected high melting point, high thermal conductivity porous foam metal in acetone or alcohol for 5 to 10 minutes, immerse it in liquid flux after vacuum drying, and then immerse it in molten medium and high temperature lead-free solder and take it out. After cooling, a metal-metal foam composite material is formed.

[0048] The time for the high melting point and high thermal conductivity porous foam metal to be immersed in the liquid flux is 3 to 5 minutes;

[0049] The porous foam metal is immersed in the molten medium-high temperature lead-free solder for 5 seconds to 1 minute;

[0050] Step 2: placing the metal-metal foam composite material prepared in step 1 between the first low-temperature solder layer and the second low-temperature solder layer, and forming an interconnected structure of upper substrate / first low-temperature solder layer / metal-metal foam composite material / second low-temperature solder layer / lower substrate in order from top to bottom;

[0051] The upper substrate is one of power electronic devices including a metal-oxide semiconductor field effect transistor discrete device, an insulated gate bipolar transistor power module, and a wide bandgap semiconductor device;

[0052] The lower substrate is one of aluminum, copper and copper alloy, which are heat sink materials for power electronic devices;

[0053] The first low-temperature solder layer and the second low-temperature solder layer may be the same or different low-temperature solders;

[0054] The first low-temperature solder layer and the second low-temperature solder layer can be low-temperature solder prefabricated sheets. When the prefabricated sheets are used, soldering flux needs to be coated on both sides of the prefabricated sheets.

[0055] The first low-temperature solder layer and the second low-temperature solder layer may be low-temperature solder paste. When solder paste is used, the low-temperature solder paste may be coated on the upper substrate and the lower substrate respectively by steel screen printing.

[0056] Step 3: Place the interconnected structure of upper substrate / first low-temperature solder layer / metal-metal foam composite material / second low-temperature solder layer / lower substrate in step 2 into a reflow soldering device and connect them in a protective atmosphere at the time and temperature required by the process.

[0057] The protective atmosphere is one of vacuum, argon, hydrogen and nitrogen;

[0058] The reflow soldering temperature is within a certain range above the highest melting points of the first and second low-temperature solder layers, and is 10 to 50° C. higher than the melting points of the low-temperature solders;

[0059] The reflow soldering time is 30s to 10min;

[0060] The obtained interface connection structure with high heat dissipation efficiency based on the metal-metal foam composite material can be used at a temperature greater than the melting point of the low-temperature solder layer and less than the melting point of the medium-high temperature lead-free solder in the metal-metal foam composite material.

[0061] Compared with the prior art, the present invention has the following advantages:

[0062] The interface connection structure for efficient heat dissipation of power electronic devices provided by the present invention has structural designability. During the reflow soldering process, the metal-metal foam metal composite material remains in a solid state, and the standoff height of the components can be effectively adjusted between 30 and 500 μm. Properly increasing the standoff height can reduce the shear stress generated by the temperature change of the connection structure during service, thereby improving the service reliability of the power device.

[0063] The metal-metal foam composite material in the interface connection structure for efficient heat dissipation of power electronic devices provided by the present invention has designable performance. By adjusting the ratio of porous foam metal and medium-high temperature lead-free solder in the metal-metal foam composite material, the thermal conductivity of the designed interface connection structure can be between 60 and 250 W / m·K (the thermal conductivity of traditional thermal interface materials is 0.4 to 5 W / m·K), and the thermal expansion coefficient is between 12 and 25 ppm / °C. The thermal conductivity and thermal expansion coefficient of the interface connection structure can be adjusted according to the selected power device packaging material to increase the matching degree of thermal expansion coefficients between the packaging materials, reduce thermal mismatch, reduce residual thermal stress of the connection structure, and improve the high-temperature service stability of the power device. At the same time, it solves the problems of low effective thermal conductivity and poor matching degree of thermal expansion coefficient of thermal interface materials in some solutions of the prior art. Taking the IGBT power module commonly used in new energy vehicles as an example, the equivalent thermal expansion coefficient of the IGBT power module is about 10ppm / ℃, and the thermal expansion coefficient of the Cu heat sink is 17ppm / ℃. When lead-free solder is used as TIM (thermal conductivity: 19~67W / m·K, thermal expansion coefficient: 15~30ppm / ℃), the mismatch between the thermal expansion coefficient of the IGBT module and the lead-free solder TIM is about 5~20ppm / ℃, and the mismatch between the thermal expansion coefficient of the lead-free solder TIM and the Cu heat sink is about 10ppm / ℃. The mismatch between them is about 0-13ppm / ℃; when the patented solution is adopted (thermal conductivity: 60-250W / m·K, thermal expansion coefficient: 12-25ppm / ℃), the thermal expansion coefficient mismatch between the IGBT module and the patented TIM is reduced to 2-15ppm / ℃, and the thermal expansion coefficient mismatch between the patented TIM and the Cu heat sink is about 0-8ppm / ℃. By adopting the patented solution, the effective thermal conductivity and the matching degree of thermal expansion coefficients between different materials are improved.

[0064] The present invention avoids the melting of the high-melting-point metal-metal foam composite material during the reflow soldering process, and uses the low-temperature solder layer to realize the interconnection between the upper substrate and the lower substrate at a relatively low soldering temperature; during the reflow soldering process, the melting-reducing elements in the low-temperature solders on both sides diffuse bidirectionally with the medium-high-temperature lead-free solder in the metal-metal foam composite material, so that the remelting temperature of the entire connection structure is higher than the low-temperature solder, that is, this interconnection structure can be used at a temperature greater than the melting point of the low-temperature solder layer and less than the melting point of the lead-free solder alloy in the metal-metal foam composite material, realizing "low-temperature connection, high-temperature service"; by adjusting the thickness of the low-temperature solder layer and the metal-metal foam composite layer, the remelting temperature of the interface connection structure can be set to a preset value. By adjusting the thickness of the low-temperature solder paste or the low-temperature solder prefabricated sheet and the metal-metal foam composite material, the remelting temperature of the interface connection structure is preset, which solves the problems of high connection temperature and limited service temperature in the prior art solution, and the process is simple and the cost is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0066] Figure 1 It is a schematic diagram of the preparation process of the metal-metal foam composite material of the present invention;

[0067] Figure 2 It is a schematic diagram of the interface connection structure in the present invention;

[0068] Figure 3 The microstructure diagram of the metal-metal foam composite material prepared in step 1 of Example 1 of the present invention;

[0069] Figure 4 This is a microstructure diagram of the Cu / Sn-58Bi / metal-metal foam composite material / Sn-58Bi / Al welding interface formed in Example 1 of the present invention;

[0070] Figure 5 The microstructure diagram of the metal-metal foam composite material prepared in step 1 of Example 2 of the present invention;

[0071] Figure 6 This is a microstructure diagram of the Cu / Sn-58Bi / metal-metal foam composite material / Sn-58Bi / Al welding interface formed in Example 2 of the present invention;

[0072] Figure 7 The microstructure diagram of the metal-metal foam composite material prepared in step 1 of Example 3 of the present invention;

[0073] Figure 8 This is a microstructure diagram of the Cu / Sn-58Bi / metal-metal foam composite material / Sn-58Bi / Al welding interface formed in Example 3 of the present invention;

[0074] Fig. 9 The microstructure diagram of the metal-metal foam composite material prepared in step 1 of Example 4 of the present invention;

[0075] Fig.10 This is a microstructure diagram of the Cu / Sn-58Bi / metal-metal foam composite material / Sn-58Bi / Al welding interface formed in Example 4 of the present invention;

[0076] Fig.11 The microstructure diagram of the metal-metal foam composite material prepared in step 1 of Example 5 of the present invention;

[0077] Fig.12 This is a microstructure diagram of the Cu / Sn-58Bi / metal-metal foam composite material / Sn-58Bi / Al welding interface formed in Example 5 of the present invention;

[0078] Fig.13 The microstructure diagram of the metal-metal foam composite material prepared in step 1 of Example 6 of the present invention;

[0079] Fig.14 This is a microstructure diagram of the Cu / Sn-58Bi / metal-metal foam composite material / Sn-58Bi / Al welding interface formed in Example 6 of the present invention;

[0080] Fig.15 This is a microstructure diagram of the Cu / Sn-57Bi-1Ag-metal-metal foam composite material / Sn-57Bi-1Ag / Al welding interface formed in Example 7 of the present invention;

[0081] Fig.16 This is a microstructure diagram of the IGBT module / Sn-52In-metal-metal foam composite material / Sn-52In / Al welding interface formed in Example 8 of the present invention.

[0082] Fig.17 This is the distribution diagram of the proportion of factors causing IGBT failure.

[0083] Fig.18 This is the heat dissipation path diagram of IGBT power devices.

[0084] Fig.19 This is the thermal expansion coefficient diagram of power device packaging materials. DETAILED DESCRIPTION

[0085] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0086] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only embodiments of a part of the present invention, not all embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0087] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0088] Unless otherwise specifically stated, the relative arrangement of the parts and steps described in these embodiments, the numerical expressions and numerical values ​​do not limit the scope of the present invention. At the same time, it should be clear that, for ease of description, the sizes of the various parts shown in the drawings are not drawn according to the actual proportional relationship. The technology, methods and equipment known to ordinary technicians in the relevant field may not be discussed in detail, but in appropriate cases, the technology, methods and equipment should be regarded as part of the authorization specification. In all examples shown and discussed here, any specific value should be interpreted as merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar numbers and letters represent similar items in the following drawings, so once an item is defined in one drawing, it does not need to be further discussed in subsequent drawings.

[0089] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. If not otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.

[0090] An interface connection structure for efficient heat dissipation of a power electronic device, the interface connection structure comprising a first low-temperature solder layer and a second low-temperature solder layer, a metal-metal foam composite material is placed between the first low-temperature solder layer and the second low-temperature solder layer; the first low-temperature solder layer is located between an upper substrate and the metal-metal foam composite material, and the second low-temperature solder layer is located between the metal-metal foam composite material and a lower substrate; the first low-temperature solder layer and the second low-temperature solder layer have a preset thickness, the metal-metal foam composite material is composed of porous foam metal and medium- and high-temperature lead-free solder, and has a preset thickness, thermal conductivity and thermal expansion coefficient, and the remelting temperature of the interface connection structure is adjusted to a preset value by selecting the metal-metal foam composite material and adjusting the thickness of the first low-temperature solder layer and the second low-temperature solder layer.

[0091] Furthermore, the metal matrix of the high melting point porous foam metal includes Cu, Ag, Al, and Mg.

[0092] Furthermore, the porosity of the high melting point and high thermal conductivity porous foam metal is 20% to 90%.

[0093] Furthermore, the pore size of the high melting point and high thermal conductivity porous foam metal is 20 to 200 μm.

[0094] Furthermore, the thickness of the metal-metal foam composite material is 20-500 μm.

[0095] Furthermore, the thickness of the first low-temperature solder layer is 5 to 50 μm, and the thickness of the second low-temperature solder layer is 5 to 50 μm; wherein the thickness of the first low-temperature solder layer and the second low-temperature solder layer may be the same or different.

[0096] The connection structure of upper substrate / first low-temperature solder layer-metal-metal foam composite material-second low-temperature solder layer / lower substrate is subjected to reflow soldering at the soldering temperature of the first low-temperature solder layer and the second low-temperature solder layer to achieve metallurgical connection.

[0097] The metal-metal foam composite material in the connection structure described in the present invention does not melt within the low-temperature soldering temperature range. During the reflow soldering process, the first low-temperature solder layer and the second low-temperature solder layer melt at the same time, wherein the first low-temperature solder layer realizes a metallurgical connection between the upper substrate and the metal-metal foam composite material; and the second low-temperature solder layer realizes a metallurgical connection between the metal-metal foam composite material and the lower substrate.

[0098] The present invention also discloses a method for preparing the interface connection structure for efficient heat dissipation of the power electronic device, which specifically comprises the following steps:

[0099] Step 1: Prepare metal-metal foam composite materials. Wash the selected high melting point and high thermal conductivity porous foam metal in acetone or alcohol for 5 to 10 minutes, immerse it in liquid flux after vacuum drying, and then immerse it in molten medium and high temperature lead-free solder and take it out. After cooling, a metal-metal foam composite material is formed. The process is as follows: Figure 1 shown.

[0100] The time for the high melting point and high thermal conductivity porous foam metal to be immersed in the liquid flux is 3 to 5 minutes;

[0101] The medium- and high-temperature lead-free solder is composed of any one of pure Sn, Sn-Ag-Cu, Sn-Ag, Sn-Cu, and Au-Sn, or an alloy formed by adding any one of Ni, Sb, and Zn to the above components, having a melting point greater than 200°C and a thermal conductivity greater than 20W / m·K;

[0102] The porous foam metal is immersed in the molten medium-high temperature lead-free solder for 5 seconds to 1 minute;

[0103] Step 2: Place the metal-metal foam composite material prepared in step 1 between the first low-temperature solder layer and the second low-temperature solder layer, and form an interconnected structure of upper substrate / first low-temperature solder layer-metal-metal foam composite material-second low-temperature solder layer / lower substrate in order from top to bottom, such as Figure 2 As shown;

[0104] The low-temperature solder is composed of any one of Sn-Bi, Sn-In, Sn-Bi-In, and Ag-In, or a low-temperature solder formed by adding any one of Cu, Ag, Ga, and Sb to the above components, and the metal-metal foam composite material is required to be insoluble in the low-temperature solder brazing temperature range;

[0105] The upper substrate may be one of power electronic devices including a metal-oxide semiconductor field effect transistor discrete device, an insulated gate bipolar transistor power module, and a wide bandgap semiconductor device;

[0106] The lower substrate is one of aluminum, copper and copper alloy, which are heat sink materials for power electronic devices;

[0107] The first low-temperature solder layer and the second low-temperature solder layer may be the same or different low-temperature solders;

[0108] The first low-temperature solder layer and the second low-temperature solder layer can be low-temperature solder prefabricated sheets. When the prefabricated sheets are used, soldering flux needs to be coated on both sides of the prefabricated sheets.

[0109] The first low-temperature solder layer and the second low-temperature solder layer may be low-temperature solder paste. When solder paste is used, the low-temperature solder paste may be coated on the upper substrate and the lower substrate respectively by steel screen printing.

[0110] Step 3: Place the interconnection structure of upper substrate / first low-temperature solder layer-metal-metal foam composite material-second low-temperature solder layer / lower substrate in step 2 into a reflow soldering device, and connect them in a protective atmosphere at the time and temperature required by the process.

[0111] The protective atmosphere is one of vacuum, argon, hydrogen and nitrogen;

[0112] The reflow soldering temperature is within a certain range above the highest melting points of the first and second low temperature solder layers, and is 10 to 50° C. higher than the melting points of the low temperature solders;

[0113] The reflow soldering time is 30s to 10min;

[0114] The obtained interface connection structure with high heat dissipation efficiency based on the metal-metal foam composite material can be used in service at a temperature greater than the melting point of the low-temperature solder layer and less than the melting point of the medium-high temperature lead-free solder in the metal-metal foam composite material.

[0115] Embodiment 1:

[0116] The interface connection structure and preparation method of a power electronic device with high efficiency heat dissipation of the present invention can be realized by the following steps:

[0117] Step 1: Prepare metal-metal foam composite materials. Select porous foam metal Cu with a thickness of 120 μm, a porosity of 76%, and a pore size of 60 μm and pure Sn (melting point: 232°C) to prepare metal-metal foam composite materials. Wash the selected porous foam metal Cu in acetone for 5 to 10 minutes, vacuum dry it, immerse it in liquid flux, and then immerse it in molten Sn for 10 seconds before taking it out. After cooling, a metal-metal foam composite material is formed. The microstructure is as follows Figure 3 As shown, the thermal conductivity of the prepared metal-metal foam composite material measured by a thermal conductivity detection instrument (Hot Disk TPS2500) is 68.6 W / m·K, and the thermal expansion coefficient at 150° C. is 20.6 ppm / ° C.

[0118] Step 2: Select 5 μm Sn-58Bi (melting point: 138°C) solder paste as the low-temperature solder layer, select pure Cu as the upper substrate, and pure Al (heat sink) as the lower substrate. From top to bottom, place the upper low-temperature solder layer Sn-58Bi, the metal-metal foam composite material prepared in step 1, and the lower low-temperature solder layer Sn-58Bi between the two substrates to form an interconnection structure.

[0119] Step 3: Place the interconnection structure in step 2 into a reflow soldering device and connect them under vacuum at a reflow soldering temperature of 180°C and a reflow soldering time of 5 minutes. The microstructure of the resulting interconnection structure is as follows: Figure 4 shown.

[0120] The remelting temperature of the interconnect structure was measured by differential scanning calorimetry (DSC). The remelting temperature was about 210°C, and the thermal conductivity of the Bi-containing metal-metal foam composite layer after welding was 57.6 W / m·K.

[0121] Embodiment 2:

[0122] The interface connection structure and preparation method of a power electronic device with high efficiency heat dissipation of the present invention can be realized by the following steps:

[0123] Step 1: Prepare metal-metal foam composite materials. Select porous foam metal Cu with a thickness of 115 μm, a porosity of 72%, and a pore size of 32 μm and pure Sn (melting point: 232°C) to prepare metal-metal foam composite materials. Wash the selected porous foam metal Cu in acetone for 5 to 10 minutes, vacuum dry it, immerse it in liquid flux, and then immerse it in molten Sn for 10 seconds before taking it out. After cooling, a metal-metal foam composite material is formed. The microstructure is as follows Figure 5 As shown, the thermal conductivity of the prepared metal-metal foam composite material measured by a thermal conductivity detection instrument (Hot Disk TPS2500) is 74.5 W / m·K, and the thermal expansion coefficient at 150° C. is 19.2 ppm / ° C.

[0124] Step 2: Select 5 μm Sn-58Bi (melting point: 138°C) solder paste as the low-temperature solder layer, select pure Cu as the upper substrate, and pure Al (heat sink) as the lower substrate. From top to bottom, place the upper low-temperature solder layer Sn-58Bi, the metal-metal foam composite material prepared in step 1, and the lower low-temperature solder layer Sn-58Bi between the two substrates to form an interconnection structure.

[0125] Step 3: Place the interconnection structure in step 2 into a reflow soldering device and connect them under vacuum at a reflow soldering temperature of 170°C and a reflow soldering time of 5 minutes. The microstructure of the resulting interconnection structure is as follows: Figure 6 shown.

[0126] The remelting temperature of the interconnect structure was measured and found to be about 213°C. The thermal conductivity of the Bi-containing metal-metal foam composite material layer after welding was 67.3 W / m·K.

[0127] Embodiment 3:

[0128] The interface connection structure and preparation method of a power electronic device with high efficiency heat dissipation of the present invention can be realized by the following steps:

[0129] Step 1: Prepare metal-metal foam composite materials. Select porous foam metal Cu with a thickness of 105 μm, a porosity of 65%, and a pore size of 30 μm and pure Sn (melting point: 232°C) to prepare metal-metal foam composite materials. Wash the selected porous foam metal Cu in acetone for 5 to 10 minutes, vacuum dry it, immerse it in liquid flux, and then immerse it in molten Sn for 10 seconds before taking it out. After cooling, a metal-metal foam composite material is formed. The microstructure is as follows Figure 7 As shown, the thermal conductivity of the prepared metal-metal foam composite material measured by a thermal conductivity detection instrument (Hot Disk TPS2500) is 87.6 W / m·K, and the thermal expansion coefficient at 150° C. is 17.7 ppm / ° C.

[0130] Step 2: Select 5 μm Sn-58Bi (melting point: 138°C) solder paste as the low-temperature solder layer, select pure Cu as the upper substrate, and pure Al (heat sink) as the lower substrate. From top to bottom, place the upper low-temperature solder layer Sn-58Bi, the metal-metal foam composite material prepared in step 1, and the lower low-temperature solder layer Sn-58Bi between the two substrates to form an interconnection structure.

[0131] Step 3: Place the interconnection structure in step 2 into a reflow soldering device and connect them under vacuum at a reflow soldering temperature of 180°C and a reflow soldering time of 5 minutes. The microstructure of the resulting interconnection structure is as follows: Figure 8 shown.

[0132] The remelting temperature of the interconnect structure was measured and found to be about 205°C. The thermal conductivity of the Bi-containing metal-metal foam composite material layer after welding was 80.6 W / m·K.

[0133] Embodiment 4:

[0134] The interface connection structure and preparation method of a power electronic device with high efficiency heat dissipation of the present invention can be realized by the following steps:

[0135] Step 1: Prepare metal-metal foam composite materials. Select porous foam metal Cu with a thickness of 130 μm, a porosity of 65%, and a pore size of 60 μm and pure Sn (melting point: 232°C) to prepare metal-metal foam composite materials. Wash the selected porous foam metal Cu in acetone for 5 to 10 minutes, vacuum dry it, immerse it in liquid flux, and then immerse it in molten Sn for 10 seconds before taking it out. After cooling, a metal-metal foam composite material is formed. The microstructure is as follows Fig. 9 As shown, the thermal conductivity of the prepared metal-metal foam composite material measured by a thermal conductivity detection instrument (Hot Disk TPS2500) is 86.9 W / m·K, and the thermal expansion coefficient at 150° C. is 18.5 ppm / ° C.

[0136] Step 2: Select a 10 μm Sn-58Bi (melting point: 138°C) preform as a low-temperature solder layer, select pure Cu as the upper substrate, and pure Al (heat sink) as the lower substrate. From top to bottom, place the upper low-temperature solder layer Sn-58Bi, the metal-metal foam composite material prepared in step 1, and the lower low-temperature solder layer Sn-58Bi between the two substrates to form an interconnected structure;

[0137] Step 3: Place the interconnection structure in step 2 into a reflow soldering device and connect them under vacuum at a reflow soldering temperature of 170°C and a reflow soldering time of 5 minutes. The microstructure of the resulting interconnection structure is as follows: Fig.10 shown.

[0138] The remelting temperature of the interconnect structure was measured and found to be about 184.2°C. The thermal conductivity of the Bi-containing metal-metal foam composite material layer after welding was 67.6 W / m·K.

[0139] Embodiment 5:

[0140] The interface connection structure and preparation method of a power electronic device with high efficiency heat dissipation of the present invention can be realized by the following steps:

[0141] Step 1: Prepare metal-metal foam composite materials. Select porous foam metal Cu with a thickness of 110 μm, a porosity of 60%, and a pore size of 22 μm and pure Sn (melting point: 232°C) to prepare metal-metal foam composite materials. Wash the selected porous foam metal Cu in acetone for 5 to 10 minutes, vacuum dry it, immerse it in liquid flux, and then immerse it in molten Sn for 10 seconds before taking it out. After cooling, a metal-metal foam composite material is formed. The microstructure is as follows Fig.11 As shown, the thermal conductivity of the prepared metal-metal foam composite material measured by a thermal conductivity detection instrument (Hot Disk TPS2500) is 98.4 W / m·K, and the thermal expansion coefficient at 150° C. is 17.6 ppm / ° C.

[0142] Step 2: Select 5 μm Sn-58Bi (melting point: 138°C) solder paste as the low-temperature solder layer, select pure Cu as the upper substrate, and pure Al (heat sink) as the lower substrate. From top to bottom, place the upper low-temperature solder layer Sn-58Bi, the metal-metal foam composite material prepared in step 1, and the lower low-temperature solder layer Sn-58Bi between the two substrates to form an interconnection structure.

[0143] Step 3: Place the interconnection structure in step 2 into a reflow soldering device and connect them under vacuum at a reflow soldering temperature of 170°C and a reflow soldering time of 5 minutes. The microstructure of the resulting interconnection structure is as follows: Fig.12 shown.

[0144] The remelting temperature of the interconnect structure was measured and found to be about 175°C. The thermal conductivity of the Bi-containing metal-metal foam composite material layer after welding was 89.5 W / m·K.

[0145] Embodiment 6:

[0146] The interface connection structure and preparation method of a power electronic device with high efficiency heat dissipation of the present invention can be realized by the following steps:

[0147] Step 1: Prepare metal-metal foam composite materials. Select porous metal foam Cu with a thickness of 130 μm, a porosity of 50%, and a pore size of 30 μm and pure Sn (melting point: 232°C) to prepare metal-metal foam composite materials. Wash the selected porous metal foam Cu in acetone for 5 to 10 minutes, vacuum dry it, immerse it in liquid flux, and then immerse it in molten Sn for 10 seconds before taking it out. After cooling, a metal-metal foam composite material is formed. The microstructure is as follows Fig.13 As shown, the thermal conductivity of the prepared metal-metal foam composite material measured by a thermal conductivity detection instrument (Hot Disk TPS2500) is 109.3 W / m·K, and the thermal expansion coefficient at 150° C. is 16.5 ppm / ° C.

[0148] Step 2: Select 10 μm Sn-58Bi (melting point: 138°C) solder paste as the low-temperature solder layer, select pure Cu as the upper substrate, and pure Al (heat sink) as the lower substrate. From top to bottom, place the upper low-temperature solder layer Sn-58Bi, the metal-metal foam composite material prepared in step 1, and the lower low-temperature solder layer Sn-58Bi between the two substrates to form an interconnection structure.

[0149] Step 3: Place the interconnection structure in step 2 into a reflow soldering device and connect them under vacuum at a reflow soldering temperature of 170°C and a reflow soldering time of 5 minutes. The microstructure of the resulting interconnection structure is as follows: Fig.14 shown.

[0150] The remelting temperature of the interconnect structure was measured and found to be about 197°C. The thermal conductivity of the Bi-containing metal-metal foam composite material layer after welding was 102.8 W / m·K.

[0151] Embodiment 7:

[0152] The interface connection structure and preparation method of a power electronic device with high efficiency heat dissipation of the present invention can be realized by the following steps:

[0153] Step 1: Prepare metal-metal foam composite materials. Select porous foam metal Cu with a thickness of 120 μm, a porosity of 65%, and a pore size of 60 μm and pure Sn (melting point: 232°C) to prepare metal-metal foam composite materials. Wash the selected porous foam metal Cu in acetone for 5 to 10 minutes, vacuum dry it, immerse it in liquid flux, and then immerse it in molten Sn for 10 seconds and then take it out. After cooling, a metal-metal foam composite material is formed. The microstructure is as follows Fig. 9 As shown, the thermal conductivity of the prepared metal-metal foam composite material was measured by a thermal conductivity detection instrument (Hot Disk TPS2500) to be 86.9 W / m·K, and the thermal expansion coefficient at 150°C was 18.5 ppm / °C ( Figure 7 ).

[0154] Step 2: Select a 10 μm Sn-57Bi-1Ag (melting point: 139°C) preform as a low-temperature solder layer, select pure Cu as the upper substrate, and pure Al (heat sink) as the lower substrate. From top to bottom, place the upper low-temperature solder layer Sn-57Bi-1Ag, the metal-metal foam composite material prepared in step 1, and the lower low-temperature solder layer Sn-57Bi-1Ag between the two substrates to form an interconnected structure;

[0155] Step 3: Place the interconnection structure in step 2 into a reflow soldering device and connect them under vacuum at a reflow soldering temperature of 160°C and a reflow soldering time of 6 minutes. The microstructure of the resulting interconnection structure is as follows: Fig.15 shown.

[0156] The remelting temperature of the interconnect structure was measured and found to be about 178°C. The thermal conductivity of the Bi-containing metal-metal foam composite material layer after welding was 92.8 W / m·K.

[0157] Embodiment 8:

[0158] The interface connection structure and preparation method of a power electronic device with high efficiency heat dissipation of the present invention can be realized by the following steps:

[0159] Step 1: Prepare metal-metal foam composite materials. Select porous foam metal Cu with a thickness of 200 μm, a porosity of 65%, and a pore size of 60 μm and pure Sn (melting point: 232°C) to prepare metal-metal foam composite materials. Wash the selected porous foam metal Cu in acetone for 5 to 10 minutes, vacuum dry it, immerse it in liquid flux, and then immerse it in molten Sn for 10 seconds before taking it out. After cooling, a metal-metal foam composite material is formed. The microstructure is as follows Fig. 9 As shown, the thermal conductivity of the prepared metal-metal foam composite material measured by a thermal conductivity detection instrument (Hot Disk TPS2500) is 86.9 W / m·K, and the thermal expansion coefficient at 150° C. is 18.5 ppm / ° C.

[0160] Step 2: Select a 15μm Sn-52In (melting point: 118°C) prefabricated sheet as the low-temperature solder layer, select an IGBT module commonly used in new energy vehicles as the upper substrate, the surface treatment layer of the surface to be welded is Sn-plated, and pure Al (heat sink) is used as the lower substrate. From top to bottom, place the upper low-temperature solder layer Sn-52In, the metal-metal foam composite material prepared in step 1, and the lower low-temperature solder layer Sn-52In between the substrates on both sides to form an interconnection structure;

[0161] Step 3: Place the interconnection structure in step 2 into a reflow soldering device and connect them under vacuum at a reflow soldering temperature of 150°C and a reflow soldering time of 6 minutes. The microstructure of the resulting interconnection structure is as follows: Fig.16 shown.

[0162] The remelting temperature of the interconnect structure was measured and found to be about 180°C. The thermal conductivity of the Bi-containing metal-metal foam composite material layer after welding was 80.8 W / m·K.

[0163] Embodiment 9:

[0164] The interface connection structure and preparation method of a power electronic device with high efficiency heat dissipation of the present invention can be realized by the following steps:

[0165] Step 1: Prepare a metal-metal foam composite material. Select a porous metal foam Cu and Sn-3.5Ag (melting point: 221°C) with a thickness of 200 μm, a porosity of 65%, and a pore size of 30 μm to prepare a metal-metal foam composite material. The selected porous metal foam Cu is cleaned in acetone for 5 to 10 minutes, vacuum dried and immersed in liquid solder flux, and then immersed in molten Sn-3.5Ag for 10 seconds before being taken out. After cooling, a metal-metal foam composite material is formed. The microstructure is similar to the metal-metal foam composite microstructure diagram in Example 8, and is not repeated here. The thermal conductivity of the prepared metal-metal foam composite material is measured by a thermal conductivity detection instrument (Hot Disk TPS2500) to be 93.2 W / m·K, and the thermal expansion coefficient at 150°C is 24 ppm / °C.

[0166] Step 2: Select a 10 μm Sn-58Bi (melting point: 138°C) preform as a low-temperature solder layer, select pure Cu as the upper substrate, and pure Al (heat sink) as the lower substrate. From top to bottom, place the upper low-temperature solder layer Sn-58Bi, the metal-metal foam composite material prepared in step 1, and the lower low-temperature solder layer Sn-58Bi between the two substrates to form an interconnected structure;

[0167] Step 3: Place the interconnection structure in step 2 into a reflow soldering device, and connect them under vacuum at a reflow soldering temperature of 170° C. and a reflow soldering time of 5 minutes.

[0168] The remelting temperature of the interconnect structure was measured and found to be about 192°C. The thermal conductivity of the Bi-containing metal-metal foam composite material layer after welding was 86.5 W / m·K.

[0169] Embodiment 10:

[0170] The interface connection structure and preparation method of a power electronic device with high efficiency heat dissipation of the present invention can be realized by the following steps:

[0171] Step 1: Prepare a metal-metal foam composite material. Select a porous metal foam Cu and Sn-3.0Ag-0.5Cu (melting point: 217°C) with a thickness of 300μm, a porosity of 90%, and a pore size of 100μm to prepare a metal-metal foam composite material. The selected porous metal foam Cu is cleaned in acetone for 5-10 minutes, vacuum dried and immersed in liquid solder flux, and then immersed in molten Sn-3.0Ag-0.5Cu for 15s and then taken out. After cooling, a metal-metal foam composite material is formed. The microstructure is similar to the metal-metal foam composite microstructure diagram in Example 8, and is not repeated here. The thermal conductivity of the prepared metal-metal foam composite material is measured by a thermal conductivity detection instrument (Hot Disk TPS2500) to be 79W / m·K, and the thermal expansion coefficient at 150°C is 20ppm / °C.

[0172] Step 2: Select 20 μm Sn-57Bi-1Ag (melting point: 139°C) solder paste as the low-temperature solder layer, select pure Cu as the upper substrate, and pure Cu (heat sink) as the lower substrate. From top to bottom, place the upper low-temperature solder layer Sn-57Bi-1Ag, the metal-metal foam composite material prepared in step 1, and the lower low-temperature solder layer Sn-57Bi-1Ag between the two substrates to form an interconnection structure;

[0173] Step 3: Place the interconnection structure in step 2 into a reflow soldering device, and connect them under vacuum at a reflow soldering temperature of 160° C. and a reflow soldering time of 5 minutes.

[0174] The remelting temperature of the interconnect structure was measured and found to be approximately 201°C. The thermal conductivity of the thermal interface structure after welding was 75 W / m·K.

[0175] Embodiment 11:

[0176] The interface connection structure and preparation method of a power electronic device with high efficiency heat dissipation of the present invention can be realized by the following steps:

[0177] Step 1: Prepare a metal-metal foam composite material. Select porous foam metal Ag and Sn (melting point: 232°C) with a thickness of 400 μm, a porosity of 30%, and a pore size of 120 μm to prepare a metal-metal foam composite material. The selected porous foam metal Ag is cleaned in acetone for 5 to 10 minutes, vacuum dried and immersed in liquid solder flux, and then immersed in molten Sn for 10 seconds before being taken out. After cooling, a metal-metal foam composite material is formed. The microstructure is similar to the metal-metal foam composite microstructure diagram in Example 8, and is not repeated here. The thermal conductivity of the prepared metal-metal foam composite material is measured by a thermal conductivity detection instrument (Hot Disk TPS2500) to be 221 W / m·K, and the thermal expansion coefficient at 150°C is 22 ppm / °C.

[0178] Step 2: Select 20 μm Sn-57Bi-1Ag (melting point: 139°C) solder paste as the low-temperature solder layer, select pure Cu as the upper substrate, and pure Cu (heat sink) as the lower substrate. From top to bottom, place the upper low-temperature solder layer Sn-57Bi-1Ag, the metal-metal foam composite material prepared in step 1, and the lower low-temperature solder layer Sn-57Bi-1Ag between the two substrates to form an interconnection structure;

[0179] Step 3: Place the interconnection structure in step 2 into a reflow soldering device, and connect them under vacuum at a reflow soldering temperature of 160° C. and a reflow soldering time of 6 minutes.

[0180] The remelting temperature of the interconnect structure was measured and found to be approximately 190°C. The thermal conductivity of the thermal interface structure after welding was 189 W / m·K.

[0181] Embodiment 12:

[0182] The interface connection structure and preparation method of a power electronic device with high efficiency heat dissipation of the present invention can be realized by the following steps:

[0183] Step 1: Prepare a metal-metal foam composite material. Select porous foam metal Ag and Sn (melting point: 232°C) with a thickness of 500 μm, a porosity of 80%, and a pore size of 200 μm to prepare a metal-metal foam composite material. The selected porous foam metal Ag is cleaned in acetone for 5 to 10 minutes, vacuum dried and immersed in liquid solder flux, and then immersed in molten Sn for 10 seconds before being taken out. After cooling, a metal-metal foam composite material is formed. The microstructure is similar to the metal-metal foam composite microstructure diagram in Example 8, and is not repeated here. The thermal conductivity of the prepared metal-metal foam composite material is measured by a thermal conductivity detection instrument (Hot Disk TPS2500) to be 162 W / m·K, and the thermal expansion coefficient at 150°C is 25 ppm / °C.

[0184] Step 2: Select 50 μm Sn-58Bi (melting point: 138°C) solder paste as the low-temperature solder layer, select pure Cu as the upper substrate, and pure Cu (heat sink) as the lower substrate. From top to bottom, place the upper low-temperature solder layer Sn-58Bi, the metal-metal foam composite material prepared in step 1, and the lower low-temperature solder layer Sn-58Bi between the two substrates to form an interconnection structure;

[0185] Step 3: Place the interconnection structure in step 2 into a reflow soldering device, and connect them under vacuum at a reflow soldering temperature of 160° C. and a reflow soldering time of 6 minutes.

[0186] The remelting temperature of the interconnect structure was measured and found to be about 200°C. The thermal conductivity of the thermal interface structure after welding was 131 W / m·K.

[0187] Therefore, the interface connection structures in the above-mentioned specific embodiments 1 to 12 all achieve "low temperature connection, high temperature service", and their thermal conductivity and thermal expansion coefficient can be adjusted. In actual application, the specific implementation method is determined based on the equivalent thermal expansion coefficient of the components to be connected, so as to achieve reasonable thermal expansion coefficient matching.

[0188] The above specific embodiments are further detailed descriptions of the present invention, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept and principle of the present invention, which should be regarded as belonging to the protection scope of the present invention.

Claims

1. An interface connection structure for efficient heat dissipation of power electronic devices, characterized in that: The interface connection structure comprises a first low-temperature solder layer and a second low-temperature solder layer, and a metal-metal foam composite material is placed between the first low-temperature solder layer and the second low-temperature solder layer; The first low-temperature solder layer is located between the upper substrate and the metal-metal foam composite material, and the second low-temperature solder layer is located between the metal-metal foam composite material and the lower substrate; the first low-temperature solder layer and the second low-temperature solder layer have a preset thickness, and the first low-temperature solder layer and the second low-temperature solder layer are both low-temperature solder preforms, and flux is coated on both sides of the preforms; or the first low-temperature solder layer and the second low-temperature solder layer are both low-temperature solder pastes, and the low-temperature solder pastes are respectively coated on the upper substrate and the lower substrate by steel screen printing; The metal-metal foam composite material is composed of porous foam metal and medium-high temperature lead-free solder and has a preset thickness, thermal conductivity and thermal expansion coefficient. The ratio of the porous foam metal and the medium-high temperature lead-free solder in the metal-metal foam composite material is regulated so that the thermal conductivity of the interface connection structure is between 60 and 250 W / m·K and the thermal expansion coefficient is adjustable between 12 and 25 ppm / ℃. The remelting temperature of the interface connection structure is adjusted to a preset value by selecting the metal-metal foam composite material with different physical and chemical properties and selecting the first low-temperature solder layer and the second low-temperature solder layer with different physical and chemical properties. During the reflow soldering and subsequent service process, the melting-reducing elements in the first low-temperature solder layer and the second low-temperature solder layer diffuse bidirectionally with the medium-high temperature lead-free solder in the metal-metal foam composite material, so that the remelting temperature of the connection structure is higher than the melting point of the low-temperature solder layer and lower than the melting point of the medium-high temperature lead-free solder in the metal-metal foam composite material, thereby realizing low-temperature connection and high-temperature service.

2. The interface connection structure for efficient heat dissipation of power electronic devices according to claim 1, characterized in that: Factors for selecting metal-metal foam composites with different physical and chemical properties include the porosity, pore size, thickness and material of porous foam metals with high melting point and high thermal conductivity. The composition of the medium- and high-temperature lead-free solder is any one of pure Sn, Sn-Ag-Cu, Sn-Ag, Sn-Cu, and Au-Sn, or an alloy with a melting point greater than 200°C and a thermal conductivity greater than 20 W / m·K formed by adding any one of Ni, Sb, and Zn to the above-mentioned components; the metal matrix of the porous foam metal includes Cu, Ag, Al, and Mg; the porosity of the high-melting-point and high-thermal-conductivity porous foam metal is 20% to 90%; the pore size of the high-melting-point and high-thermal-conductivity porous foam metal is 20 to 200 μm; and the thickness of the metal-metal foam composite material is 20 to 500 μm.

3. The interface connection structure for efficient heat dissipation of power electronic devices according to claim 1, characterized in that: Selecting the first low-temperature solder layer and the second low-temperature solder layer with different physical and chemical properties includes the thickness and material of the first low-temperature solder layer and the second low-temperature solder layer. The thickness of the first low-temperature solder layer is 5 ~ 50 μm, and the thickness of the second low-temperature solder layer is 5 ~ 50 μm; the composition of the low-temperature solder in the first low-temperature solder layer and the second low-temperature solder layer is any one of Sn-Bi, Sn-In, Sn-Bi-In, Ag-In, or a low-temperature solder formed by adding any one of Cu, Ag, Ga, Sb to the above components, and it is necessary to meet the requirement that the metal-metal foam composite material does not melt within the low-temperature solder brazing temperature range; the first low-temperature solder layer and the second low-temperature solder layer can be the same or different low-temperature solders.

4. A method for preparing an interface connection structure for efficient heat dissipation of a power electronic device according to any one of claims 1 to 3, characterized in that: The specific steps include: Step 1: Prepare a metal-metal foam composite material, wash the selected high melting point and high thermal conductivity porous foam metal in acetone or alcohol for 5 to 10 minutes, immerse it in liquid flux after vacuum drying, and then immerse it in molten medium-high temperature lead-free solder and take it out, and form a metal-metal foam composite material after cooling; Step 2: placing the metal-metal foam composite material prepared in step 1 between the first low-temperature solder layer and the second low-temperature solder layer, and forming an interconnected structure of upper substrate / first low-temperature solder layer / metal-metal foam composite material / second low-temperature solder layer / lower substrate in order from top to bottom; Step 3: Place the interconnected structure of upper substrate / first low-temperature solder layer / metal-metal foam composite material / second low-temperature solder layer / lower substrate in step 2 into a reflow soldering device and connect them in a protective atmosphere at the time and temperature required by the process.

5. The method for preparing an interface connection structure for efficient heat dissipation of a power electronic device according to claim 4, characterized in that: In step one, the time for immersing the high melting point and high thermal conductivity porous foam metal into the liquid flux is 3 to 5 minutes; in step one, the time for immersing the porous foam metal into the molten medium-high temperature lead-free solder is 5 seconds to 1 minute.

6. The method for preparing an interface connection structure for efficient heat dissipation of a power electronic device according to claim 4, characterized in that: In step 2, the upper substrate is one of power electronic devices including metal-oxide semiconductor field effect transistor discrete devices, insulated gate bipolar transistor power modules, and wide bandgap semiconductor devices; in step 2, the lower substrate is one of heat sink materials for power electronic devices, including aluminum, copper, and copper alloy.

7. The method for preparing an interface connection structure for efficient heat dissipation of a power electronic device according to claim 4, characterized in that: In step three, the reflow temperature is within a certain range above the highest melting points of the first low-temperature solder layer and the second low-temperature solder layer, and is 10 to 50° C. higher than the melting point of the low-temperature solder; and the reflow time is 30 s to 10 min.

8. The method for preparing an interface connection structure for efficient heat dissipation of a power electronic device according to claim 4, characterized in that: In step three, the obtained high-efficiency heat dissipation interface connection structure based on the metal-metal foam composite material can be used at a temperature greater than the melting point of the low-temperature solder layer and less than the melting point of the medium-high temperature lead-free solder in the metal-metal foam composite material.

Citation Information

Patent Citations

  • Elastic compound metal heat interface material and preparation method thereof

    CN102504769A

  • Preparation method for flexible heat-conducting pad

    CN103965839A

  • Thermal interface material and preparation method and application method thereof

    CN108511407A

  • Composite thermal interface material composed of foam metal and liquid metal

    CN114479773A

  • Heat-conducting interface material and solder prefabricated product

    CN1894791B