Method for producing light-transmitting conductive sheet

By forming a light-transmitting conductive layer on the base material sheet by multiple sputterings, and using an indium-tin composite oxide of indium oxide and tin oxide to form the inner and outer layers, the problem of high resistivity of the existing transparent conductive film is solved, and the A light-transmitting conductive layer with low resistivity is produced, and the resistivity is further optimized through a crystallization process.

CN115667573BActive Publication Date: 2024-10-25NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180038168.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-05-25
Filing Date
2021-03-18
Publication Date
2024-10-25
Estimated Expiration
2041-03-18

AI Technical Summary

Technical Problem

The resistivity of existing transparent conductive films cannot meet the requirements for low resistivity.

Method used

A light-transmitting conductive layer is formed in the thickness direction of the base material sheet by multiple sputterings where electric power is applied to multiple targets respectively. The inner layer and the outer layer are formed using an indium-tin composite oxide of indium oxide and tin oxide, and are controlled The power density and sputtering gas ratio are adjusted to form an outer layer that is denser than the inner layer, thereby reducing the resistivity of the light-transmissive conductive layer.

Benefits of technology

The manufacturing of a light-transmitting conductive layer with low resistivity is achieved, meeting the requirement of low resistivity, and the resistivity is further optimized through the crystallization process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115667573B_ABST
    Figure CN115667573B_ABST
Patent Text Reader

Abstract

In a method for manufacturing a light-transmitting conductive sheet (1), a light-transmitting conductive layer (3) is formed on a substrate sheet (2) by multiple sputtering by applying power to a plurality of targets (51), (52), (53), and (54). The method comprises the following steps: a first step of applying power to a first target (51) formed of an indium-tin composite oxide having a tin oxide content exceeding 8% by mass to form an inner layer (6) on the substrate sheet (2); and a second step of applying power to a second target (52) formed of an indium-tin composite oxide, a third target (53) formed of an indium-tin composite oxide, and a fourth target (54) formed of an indium-tin composite oxide to form an outer layer (22) on the inner layer (6). The ratio (P1 / P) of the power density P1 of the first target (51) to the total power density P of the second target (52), the third target (53), and the fourth target (54) is 0.20 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a light-transmitting conductive sheet. Background Art

[0002] Conventionally, there is known a transparent conductive film including a transparent conductive film formed of ITO on the surface of a base film.

[0003] For example, a method has been proposed in which a lower layer and an upper layer are sequentially stacked on the upper surface of a base film by sputtering twice (see, for example, Patent Document 1 below).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 8-174746 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] However, a transparent conductive film is required to have a low resistivity. However, the transparent conductive film described in Patent Document 1 has a disadvantage in that it cannot meet the above requirement.

[0009] The present invention provides a method for producing a light-transmitting conductive sheet having a light-transmitting conductive layer with low resistivity.

[0010] Solutions for solving problems

[0011] The present invention (1) includes a method for manufacturing a translucent conductive sheet, the manufacturing method comprising the steps of forming a translucent conductive layer on one side of a substrate sheet in the thickness direction by multiple sputterings in which power is applied to multiple targets respectively, the aforementioned step of forming the translucent conductive layer comprises the following steps: a first step of applying power to a first target to form an inner layer on one side of the aforementioned thickness direction of the aforementioned substrate sheet, the aforementioned first target is included in the aforementioned multiple targets, contains indium oxide and tin oxide, and is formed of an indium-tin composite oxide having a tin oxide content exceeding 8% by mass; and a second step of applying power to a target other than the aforementioned first target to form an outer layer on one side of the aforementioned thickness direction of the aforementioned inner layer, the ratio (P1 / P) of the power density P1 of the aforementioned first target to the total power density P of the aforementioned multiple targets is less than 0.20.

[0012] In the method for manufacturing a light-transmitting conductive sheet, since the ratio of the power density P1 of the first target to the total power density P of the plurality of targets (P1 / P) is 0.20 or less, an outer layer denser than an inner layer can be formed, thereby reducing the resistivity of the light-transmitting conductive layer. As a result, a light-transmitting conductive sheet having a light-transmitting conductive layer with a low resistivity can be manufactured.

[0013] In addition, in this method of producing a light-transmitting conductive sheet, since the inner layer is formed by applying power to the first target formed of an indium-tin composite oxide having a tin oxide content exceeding 8 mass %, the resistivity of the light-transmitting conductive layer can be sufficiently reduced.

[0014] The present invention (2) includes a method for manufacturing a light-transmitting conductive sheet as described in (1), wherein the first step is performed by sputtering in an atmosphere of a sputtering gas containing a reactive gas, and the second step is performed by sputtering in an atmosphere of a sputtering gas containing a reactive gas, and the ratio (R1 / R2) of the proportion R1 of the reactive gas in the sputtering gas in the first step to the proportion R2 of the reactive gas in the sputtering gas in the second step is less than 1.

[0015] The present invention (3) includes the method for producing a light-transmitting conductive sheet according to (1) or (2), further comprising a third step of crystallizing the light-transmitting conductive layer after the second step.

[0016] Effects of the Invention

[0017] According to the production method of the present invention, a light-transmitting conductive sheet including a light-transmitting conductive layer having a low resistivity can be produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a schematic diagram of a sputtering apparatus used in one embodiment of the method for producing a light-transmitting conductive sheet of the present invention.

[0019] Figure 2 is to use Figure 1 A cross-sectional view of a light-transmitting conductive sheet manufactured by a sputtering device.

[0020] Figure 3 yes Figure 1 A schematic diagram of a modified example of the sputtering device shown.

[0021] Figure 4 is to use Figure 3 A cross-sectional view of a light-transmitting conductive sheet manufactured by a sputtering device.

[0022] Figure 5 This is a processed image of the TEM photograph of Example 1.

[0023] Figure 6 This is an image-processed image of the TEM photograph of Comparative Example 1. DETAILED DESCRIPTION

[0024] (One embodiment of a method for producing a light-transmitting conductive sheet of the present invention)

[0025] Reference Figure 1-2One embodiment of the method for producing the light-transmitting conductive sheet of the present invention will be described.

[0026] The method for manufacturing the light-transmitting conductive sheet 1 includes a step of forming a light-transmitting conductive layer 3 on one side in the thickness direction of the base sheet 2 by sputtering by applying power to each of the plurality of targets 51, 52, 53, and 54. It should be noted that, in this embodiment, the plurality of targets 51, 52, 53, and 54 include a first target 51, a second target 52, a third target 53, and a fourth target 54.

[0027] (Sputtering device)

[0028] First, the sputtering device 30 used in the sputtering will be described. Figure 1 As shown, the sputtering device 30 includes a conveying unit 35, a sputtering unit 36, and a winding unit 37 in this order.

[0029] The transport unit 35 includes transport rollers 38 .

[0030] The sputtering unit 36 ​​includes a film forming roller 40, a first film forming chamber 41, and a plurality of film forming chambers 42, 43, and 44. In this embodiment, the plurality of film forming chambers 42, 43, and 44 are a second film forming chamber 42, a third film forming chamber 43, and a fourth film forming chamber 44.

[0031] The film-forming roller 40 includes a cooling device (not shown) configured to cool the film-forming roller 40 .

[0032] The first film forming chamber 41 accommodates the first target 51, the first gas supply machine 61, and the discharge port of the first pump 91. The first target 51, the first gas supply machine 61, and the discharge port of the first pump 91 are arranged at intervals relative to the film forming roller 40. In the first film forming chamber 41, a magnet (not shown) is arranged on the side of the first target 51 opposite to the film forming roller 40. The magnetic field strength of the magnet is adjusted so that the horizontal magnetic field strength on the first target 51 is, for example, 10 mT or more and 200 mT or less.

[0033] The material of the first target 51 is ITO (Indium-Tin Composite Oxide). ITO contains indium oxide and tin oxide.

[0034] The content of tin oxide in ITO exceeds 8% by mass. On the other hand, when the content of tin oxide is 8% by mass or less, the resistivity of the light-transmitting conductive layer 3 cannot be sufficiently reduced.

[0035] The content of tin oxide in ITO is preferably 8.5% by mass or more, more preferably 9% by mass or more, and further preferably 9.5% by mass or more, and is, for example, 30% by mass or less, preferably 25% by mass or less, more preferably 20% by mass or less, and further preferably 15% by mass or less. If the content of tin oxide is below the upper limit, the resistivity can be stably reduced.

[0036] The content of indium oxide in ITO is the remainder of the content of tin oxide.

[0037] It should be noted that ITO can be doped with a trace amount (for example, 5 mass % or less) of at least one selected from the group consisting of Zn, Ga, Sb, Ti, Si, Zr, Mg, Al, Au, Ag, Cu, Pd and W as needed.

[0038] The material of the first target 51 includes a sintered body of a conductive oxide. By placing the first target 51 in the sputtering device 30 and applying a predetermined electric power density P1 to the first target 51, the constituent material of the first target 51 can be sputtered.

[0039] The first gas supply machine 61 is configured to supply a sputtering gas to the first film forming chamber 41. Examples of the sputtering gas include inert gases such as nitrogen, argon, krypton, and xenon, and mixed gases such as inert gases and reactive gases such as oxygen, preferably mixed gases. If the sputtering gas is a mixed gas, the first gas supply machine 61 includes a first inert gas supply machine 71 and a first reactive gas supply machine 72, which supply the inert gas and the reactive gas to the first film forming chamber 41, respectively.

[0040] The second film forming chamber 42 is arranged adjacent to the first film forming chamber 41 in the circumferential direction of the film forming roller 40. The second film forming chamber 42 accommodates a second target 52 as an example of a target, a second gas supply machine 62, and a discharge port of a second pump 92. The second target 52, the second gas supply machine 62, and the discharge port of the second pump 92 are arranged at intervals relative to the film forming roller 40. In the second film forming chamber 42, a magnet (not shown) is arranged on the side of the second target 52 opposite to the film forming roller 40. The magnetic field strength of the magnet is adjusted so that the horizontal magnetic field strength on the second target 52 is, for example, 10 mT or more and 200 mT or less.

[0041] The material of the second target 52 is ITO. There is no particular limitation on the content of tin oxide in ITO. The content of tin oxide in ITO is, for example, 1% by mass or more, preferably 5% by mass or more, and more preferably more than 8% by mass. In addition, it is, for example, 30% by mass or less, preferably 25% by mass or less, more preferably 20% by mass or less, and more preferably 15% by mass or less. Preferably, the content of tin oxide in the material of the second target 52 is the same as the content of tin oxide in the material of the first target 51.

[0042] The material of the second target 52 includes a sintered body of a conductive oxide. By placing the second target 52 in the sputtering device 30 and applying a predetermined electric power density P2 to the second target 52, the constituent material of the second target 52 can be sputtered.

[0043] The second gas supply machine 62 is configured to supply a sputtering gas to the second film forming chamber 42. As the sputtering gas, for example, the above-mentioned inert gas and the above-mentioned mixed gas can be listed, and preferably the mixed gas is listed. If the sputtering gas is a mixed gas, the second gas supply machine 62 includes a second inert gas supply machine 73 and a second reactive gas supply machine 74, and the inert gas and the reactive gas are supplied to the second film forming chamber 42 respectively.

[0044] The third film forming chamber 43 is adjacent to the second film forming chamber 42 in the circumferential direction of the film forming roller 40, and is arranged on the side of the second film forming chamber 42 opposite to the first film forming chamber 41. The third film forming chamber 43 accommodates a third target 53 as an example of a target, a third gas supply machine 63, and a discharge port of a third pump 93. The third target 53, the third gas supply machine 63, and the discharge port of the third pump 93 are arranged at intervals relative to the film forming roller 40. In the third film forming chamber 43, a magnet (not shown) is arranged on the side of the third target 53 opposite to the film forming roller 40. The magnetic field strength of the magnet is adjusted so that the horizontal magnetic field strength is, for example, 10 mT or more and 200 mT or less.

[0045] The material of the third target 53 is ITO. There is no particular limitation on the content of tin oxide in ITO. The content of tin oxide in ITO is, for example, 1% by mass or more, preferably 5% by mass or more, and more preferably more than 8% by mass. In addition, it is, for example, 30% by mass or less, preferably 25% by mass or less, more preferably 20% by mass or less, and more preferably 15% by mass or less. Preferably, the content of tin oxide in the material of the third target 53 is the same as the content of tin oxide in the material of the first target 51.

[0046] The material of the third target 53 includes a sintered body of a conductive oxide. By placing the third target 53 in the sputtering device 30 and applying a predetermined electric power density P3 to the third target 53, the constituent material of the third target 53 can be sputtered.

[0047] The third gas supply machine 63 is configured to supply a sputtering gas to the third film forming chamber 43. As the sputtering gas, for example, the above-mentioned inert gas and the above-mentioned mixed gas can be listed, and preferably the mixed gas is listed. If the sputtering gas is a mixed gas, the third gas supply machine 63 includes a third inert gas supply machine 75 and a third reactive gas supply machine 76, and the inert gas and the reactive gas are supplied to the third film forming chamber 43 from them respectively.

[0048] The fourth film forming chamber 44 is adjacent to the third film forming chamber 43 in the circumferential direction of the film forming roller 40, and is arranged on the side of the third film forming chamber 43 opposite to the second film forming chamber 42. Thus, in the sputtering unit 36, the first film forming chamber 41, the second film forming chamber 42, the third film forming chamber 43, and the fourth film forming chamber 44 are arranged in sequence in the circumferential direction. The fourth film forming chamber 44 accommodates a fourth target 54 as an example of a target, a fourth gas supply machine 64, and a discharge port of a fourth pump 94. The fourth target 54, the fourth gas supply machine 64, and the discharge port of the fourth pump 94 are arranged at intervals relative to the film forming roller 40. In the fourth film forming chamber 44, a magnet (not shown) is arranged on the side of the fourth target 54 opposite to the film forming roller 40. The magnetic field strength of the magnet is adjusted in such a way that the horizontal magnetic field strength is, for example, greater than 10 mT and less than 200 mT.

[0049] The material of the fourth target 54 is ITO. There is no particular limitation on the content of tin oxide in ITO. The content of tin oxide in ITO is, for example, 1% by mass or more, preferably 5% by mass or more, and more preferably more than 8% by mass. In addition, it is, for example, 30% by mass or less, preferably 25% by mass or less, more preferably 20% by mass or less, and more preferably 15% by mass or less. Preferably, the content of tin oxide in the material of the fourth target 54 is the same as the content of tin oxide in the material of the first target 51.

[0050] The material of the fourth target 54 includes a sintered body of a conductive oxide. By placing the fourth target 54 in the sputtering device 30 and applying a predetermined power density P4 to the fourth target 54, the constituent material of the fourth target 54 can be sputtered.

[0051] The fourth gas supply machine 64 is configured to supply a sputtering gas to the fourth film forming chamber 44. As the sputtering gas, for example, the above-mentioned inert gas and the above-mentioned mixed gas can be listed, and preferably the mixed gas is listed. If the sputtering gas is a mixed gas, the fourth gas supply machine 64 includes a fourth inert gas supply machine 77 and a fourth reactive gas supply machine 78, and the inert gas and the reactive gas are respectively supplied from them to the fourth film forming chamber 44.

[0052] The winding section 37 includes a winding roller 39 .

[0053] (Step of forming a light-transmitting conductive layer on a substrate sheet)

[0054] Next, a step of forming the light-transmitting conductive layer 3 on the base sheet 2 using the sputtering device 30 will be described in detail.

[0055] In this step, first, the base sheet 2 is prepared.

[0056] The base sheet 2 has a thickness and extends in a plane direction perpendicular to the thickness direction. Specifically, the base sheet 2 has a film shape extending in the plane direction. The base sheet 2 has flexibility.

[0057] The base sheet 2 includes at least a base layer 4. Specifically, the base sheet 2 includes a base layer 4 and a hard coating layer 5 in this order on one side in the thickness direction. In this embodiment, the number of base sheets 2 included in the light-transmitting conductive sheet 1 is one.

[0058] The substrate layer 4 has a film shape extending in the surface direction. The substrate layer 4 forms the other side of the substrate sheet 2 in the thickness direction. The material of the substrate layer 4 is not particularly limited, and examples thereof include polymers, glass, and the like. Polymers are preferably cited. As polymers, olefin resins such as polyethylene, polypropylene, and cycloolefin polymers (COP), polyester resins such as polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate, (meth) acrylic resins such as polyacrylates and / or polymethacrylates (acrylic resins and / or methacrylic resins), resins such as polycarbonate resins, polyether sulfone resins, polyarylate resins, melamine resins, polyamide resins, polyimide resins, cellulose resins, and polystyrene resins are preferably cited, and PET is more preferably cited. The thickness of the base material layer 4 is, for example, 1 μm or more, preferably 10 μm or more, more preferably 30 μm or more, and, for example, 300 μm or less, preferably 100 μm or less, more preferably 75 μm or less.

[0059] The hard coating layer 5 is a scratch protection layer for making the light-transmitting conductive layer 3 less susceptible to scratches. The hard coating layer 5 forms one side of the substrate sheet 2 in the thickness direction. The hard coating layer 5 is in contact with the entire surface of the substrate layer 4 in the thickness direction. As a material for the hard coating layer 5, a cured product of a hard coating composition (acrylic resin, urethane resin, etc.) described in Japanese Patent Publication No. 2016-179686 can be cited. The thickness of the hard coating layer 5 is, for example, 0.1 μm or more, preferably 0.5 μm or more, and, for example, 10 μm or less, preferably 5 μm or less.

[0060] (Physical properties of substrate)

[0061] The thickness of the base sheet 2 is, for example, 1 μm or more, preferably 10 μm or more, more preferably 15 μm or more, further preferably 30 μm or more, and, for example, 310 μm or less, preferably 210 μm or less, more preferably 110 μm or less, further preferably 80 μm or less.

[0062] The total light transmittance (JIS K 7375-2008) of the base sheet 2 is, for example, 60% or more, preferably 80% or more, more preferably 85% or more, and, for example, 100% or less.

[0063] (Installation of substrate sheet on sputtering device)

[0064] Next, the base sheet 2 is mounted on the sputtering device 30 . Specifically, the base sheet 2 is placed on the transport roll 38 , the film forming roll 40 , and the winding roll 39 .

[0065] Next, while driving the first pump 91, the sputtering gas is supplied from the first gas supply machine 61 to the first film forming chamber 41. If the sputtering gas is a mixed gas, the ratio R1 of the reactive gas to the inert gas in the mixed gas is, for example, 0.001 or more, preferably 0.005 or more, and for example, 0.2 or less, preferably 0.1 or less, on a volume basis. The pressure of the first film forming chamber 41 is, for example, 0.01 Pa or more and 1 Pa or less.

[0066] While driving the second pump 92, the sputtering gas is supplied from the second gas supply machine 62 to the second film forming chamber 42. If the sputtering gas is a mixed gas, the ratio R2 of the reactive gas to the inert gas in the mixed gas is, for example, 0.001 or more, preferably 0.005 or more, and for example, 0.2 or less, preferably 0.1 or less, on a volume basis. The ratio of the ratio R1 of the reactive gas in the mixed gas in the first film forming chamber 41 to the ratio R2 of the reactive gas in the mixed gas in the second film forming chamber 42 (the ratio R1 to the ratio R2) (R1 / R2) is, for example, 3.0 or less, preferably 2 or less, more preferably 1 or less, more preferably 0.9 or less, further preferably 0.8 or less, particularly preferably 0.7 or less, and for example, 0.01 or more, preferably 0.1 or more, and more preferably 0.5 or more. If R1 / R2 is greater than the above lower limit, the resistivity of the light-transmitting conductive layer 3 can be further reduced. The pressure of the second film forming chamber 42 is, for example, 0.01 Pa or more and 1 Pa or less.

[0067] While driving the third pump 93, the sputtering gas is supplied from the third gas supply device 63 to the third film forming chamber 43. If the sputtering gas is a mixed gas, the ratio R3 of the reactive gas in the mixed gas is the same as the ratio R2 of the reactive gas in the second film forming chamber 42. The pressure of the third film forming chamber 43 is, for example, 0.01 Pa or more and 1 Pa or less.

[0068] While the fourth pump 94 is driven, the sputtering gas is supplied from the fourth gas supply device 64 to the fourth film forming chamber 44. If the sputtering gas is a mixed gas, the ratio R4 of the reactive gas in the mixed gas is the same as the ratio R2 of the reactive gas in the second film forming chamber 42. The pressure of the fourth film forming chamber 44 is, for example, 0.01 Pa or more and 1 Pa or less.

[0069] The cooling device is driven to cool (the surface of) the deposition roller 40. The temperature (surface temperature) of the deposition roller 40 is, for example, 20°C or less, preferably 10.0°C or less, preferably 0.0°C or less, and, for example, -50°C or more, preferably -25°C or more.

[0070] (Applying power to each target and starting sputtering in each film forming chamber)

[0071] Power is applied to the first target 51, the second target 52, the third target 53, and the fourth target 54. Specifically, power is applied to the first target 51 at a power density P1, power is applied to the second target 52 at a power density P2, power is applied to the third target 53 at a power density P3, and power is applied to the fourth target 54 at a power density P4.

[0072] It should be noted that the power source applied to the first target 51, the second target 52, the third target 53, and the fourth target 54 is not particularly limited, and examples thereof include DC and RF. The power source is preferably DC.

[0073] The ratio (P1 / P) of the power density P1 of the first target 51 to the total power density P (=P1+P2+P3+P4) of the power density P1 of the first target 51, the power density P2 of the second target 52, the power density P3 of the third target 53, and the power density P4 of the fourth target 54 is 0.20 or less. On the other hand, if the ratio (P1 / P) of the power density P1 of the first target 51 to the total power density P exceeds 0.20, the resistivity of the light-transmitting conductive layer 3 cannot be reduced. The ratio (P1 / P) of the power density P1 of the first target 51 to the total power density P is preferably 0.18 or less, more preferably 0.15 or less, further preferably 0.10 or less, and particularly preferably 0.05 or less.

[0074] In addition, the ratio (P1 / P) of the power density P1 of the first target 51 to the total power density P is, for example, 0.001 or more, preferably 0.01 or more. If the ratio (P1 / P) of the power density P1 of the first target 51 to the total power density P is greater than the above lower limit, sputtering in the first film forming chamber 41 can be reliably performed.

[0075] The power density P3 of the third target 53 is similar to the power density P2 of the second target 52, and the power density P4 of the fourth target 54 is similar to the power density P3 of the third target 53. It is preferable that the power density P2, the power density P3, and the power density P4 are the same.

[0076] The power density P1 is, for example, 0.1 W / cm 2 Above, for example, 10 W / cm 2 The power density P2, the power density P3, and the power density P4 are each, for example, 0.1 W / cm2 Above, for example, 15W / cm 2 the following.

[0077] Next, the conveying roller 38, the film forming roller 40, and the winding roller 39 are driven to deliver the base sheet 2 from the conveying roller 38. The base sheet 2 sequentially moves through the first film forming chamber 41, the second film forming chamber 42, the third film forming chamber 43, and the fourth film forming chamber 44 while contacting the surface of the film forming roller 40. At this time, the base sheet 2 is cooled by contacting the surface of the film forming roller 40.

[0078] In the vicinity of the first target 51, the sputtering gas is ionized by applying power at a power density P1 to the first target 51. Then, the ionized gas collides with the first target 51, knocking out the ITO of the first target 51 to form particles, which adhere (deposit) to the substrate sheet 2 to form the inner layer 6 (first step).

[0079] Next, near the second target 52, power is applied to the second target 52 at a power density P2 to ionize the sputtering gas to generate ionized gas. Next, the ionized gas collides with the second target 52, knocking out the ITO of the second target 52 to form particles, which adhere (deposit) to the inner layer 6 to form the first layer 7.

[0080] Next, near the third target 53, power is applied to the third target 53 at a power density P3 to ionize the sputtering gas to generate ionized gas. Next, the ionized gas collides with the third target 53, knocking out the ITO of the third target 53 to form particles, which adhere (deposit) to the first layer 7 to form the second layer 8.

[0081] Next, near the fourth target 54, power is applied to the fourth target 54 at a power density P4 to ionize the sputtering gas and generate ionized gas. Next, the ionized gas collides with the fourth target 54, knocking out the ITO of the fourth target 54 to form particles, which are attached (deposited) to the second layer 8 to form the third layer 9 (second step).

[0082] The second step forms the outer layer 22 composed of the first layer 7, the second layer 8 and the third layer 9. That is, the outer layer 22 includes the first layer 7, the second layer 8 and the third layer 9 in this order on one side in the thickness direction, which are in contact with the inner layer 6, and the adjacent layers are in contact with each other.

[0083] The ratio of the power density P1 of the first target 51 to the total power density P (P1 / P) is 0.20 or less, that is, the total power density P is extremely high relative to the power density P1 of the first target 51. Therefore, the film quality of the inner layer 6 is different from that of the outer layer 22, and therefore, the boundary between the inner layer 6 and the first layer 7 can sometimes be clearly observed by, for example, TEM.

[0084] The thickness of the inner layer 6 is, for example, 1 nm or more, preferably 2 nm or more, and, for example, 30 nm or less, preferably 20 nm or less. The ratio of the thickness of the inner layer 6 to the thickness of the light-transmitting conductive layer 3 is, for example, 0.005 or more, preferably 0.01 or more, and, for example, 0.2 or less, preferably 0.1 or less.

[0085] The total thickness of the outer layer 22 composed of the first layer 7, the second layer 8 and the third layer 9 is, for example, 10 nm or more, preferably 30 nm or more, more preferably 50 nm or more, and, for example, 480 nm or less, preferably 250 nm or less, more preferably 200 nm or less, and further preferably 145 nm or less. The ratio of the thickness of the outer layer 22 to the thickness of the translucent conductive layer 3 is the remainder of the ratio of the thickness of the inner layer 6 to the thickness of the translucent conductive layer 3.

[0086] It should be noted that the boundary between the first layer 7 and the second layer 8 cannot be clearly observed. The boundary between the second layer 8 and the third layer 9 cannot be clearly observed.

[0087] The inner layer 6 and the outer layer 22 form the light-transmitting conductive layer 3. The inner layer 6 is formed on the other surface in the thickness direction of the light-transmitting conductive layer 3. The outer layer 22 is in contact with the entire surface of the inner layer 6 in the thickness direction.

[0088] The thickness of the light-transmitting conductive layer 3 is, for example, greater than 15 nm, preferably greater than 30 nm, more preferably greater than 40 nm, further preferably greater than 50 nm, further preferably greater than 80 nm, and particularly preferably greater than 100 nm. In addition, it is, for example, less than 500 nm, preferably less than 300 nm, more preferably less than 300 nm, further preferably less than 200 nm, and further preferably less than 150 nm.

[0089] The light-transmitting conductive layer 3 immediately after film formation is, for example, amorphous.

[0090] Thus, a light-transmitting conductive sheet 1 including the base sheet 2 and the light-transmitting conductive layer 3 in this order in the thickness direction is obtained. Since the light-transmitting conductive layer 3 is amorphous, the light-transmitting conductive sheet 1 can be obtained as an amorphous light-transmitting conductive sheet 10 .

[0091] Then, the light-transmitting conductive layer 3 is crystallized as necessary (third step).

[0092] In order to crystallize the light-transmitting conductive layer 3, for example, the amorphous light-transmitting conductive sheet 10 is heated. The heating temperature is, for example, 80°C or more, preferably 110°C or more, more preferably 140°C or more, and further preferably 160°C or more. In addition, for example, it is 250°C or less, preferably less than 200°C, and more preferably 180°C or less. In addition, the heating time is, for example, 1 minute or more, preferably 5 minutes or more, more preferably 1 hour or more, and further preferably 1.5 hours or more. In addition, for example, it is 5 hours or less, and preferably 3 hours or less. Alternatively, the amorphous light-transmitting conductive sheet 10 may be placed at room temperature for a long time. For example, the amorphous light-transmitting conductive sheet 10 is placed in an atmosphere of 20°C or more and 40°C or less for, for example, 500 hours or more, preferably 1500 hours or more, and for example, 3000 hours or less.

[0093] (Physical properties of light-transmitting conductive layer)

[0094] The total light transmittance (JIS K7375-2008) of the light-transmitting conductive layer 3 (specifically, the crystalline light-transmitting conductive layer 3 ) is, for example, 60% or more, preferably 80% or more, more preferably 85% or more, and for example, 100% or less.

[0095] The surface resistance of the light-transmitting conductive layer 3 (specifically, the crystallized light-transmitting conductive layer 3) is, for example, 200Ω / □ or less, preferably 100Ω / □ or less, more preferably 50Ω / □ or less, further preferably 20Ω / □ or less, and, for example, exceeds 0Ω / □. The surface resistance is measured by a four-terminal method in accordance with JIS K7194.

[0096] The resistivity of the light-transmitting conductive layer 3 (specifically, the crystalline light-transmitting conductive layer 3) is, for example, 4.0×10 -4 Ωcm or less, preferably 2.5×10 -4 Ωcm or less, more preferably 2.3×10 -4 Ωcm or less, more preferably 2.2×10 -4 Ωcm or less, more preferably 2.1×10 -4 Ωcm or less, and for example, more than 0 Ωcm, and further 0.1×10 -4 Ωcm or more, and further 0.5×10 -4 Ωcm or more, and further 1.0×10 -4 Ωcm or more. Resistivity is obtained by multiplying the surface resistance by the thickness.

[0097] (Physical properties of light-transmitting conductive sheet)

[0098] The thickness of the light-transmitting conductive sheet 1 is, for example, 1 μm or more, preferably 10 μm or more, more preferably 20 μm or more, further preferably 40 μm or more, and, for example, 310 μm or less, preferably 210 μm or less, more preferably 120 μm or less, further preferably 90 μm or less.

[0099] The total light transmittance (JIS K 7375-2008) of the light-transmitting conductive sheet 1 is, for example, 60% or more, preferably 80% or more, more preferably 85% or more, and for example, 100% or less.

[0100] (Application of light-transmitting conductive sheet)

[0101] The light-transmitting conductive sheet 1 (a light-transmitting conductive sheet having a crystallized light-transmitting conductive layer 3) can be used for various articles. As articles, for example, it can be used for touch sensors, electromagnetic wave shields, dimming elements (voltage-driven dimming elements such as PDLC, PNLC, SPD, and current-driven dimming elements such as electrochromic (EC)), photoelectric conversion elements (electrodes of solar cell elements represented by organic thin-film solar cells and dye-sensitized solar cells, etc.), heat ray control components (such as near-infrared reflection and / or absorption components, such as far-infrared reflection and / or absorption components), antenna components (light-transmitting antennas), heater components (light-transmitting heaters), image display devices, lighting, etc.

[0102] The article includes the light-transmitting conductive film 10 and components corresponding to each article.

[0103] Such an article is obtained by fixing the light-transmitting conductive film 10 and members corresponding to each article.

[0104] Specifically, for example, the light-transmitting conductive layer 3 (including the light-transmitting conductive layer 3 having a pattern shape) in the light-transmitting conductive film 10 and a member corresponding to each article are fixed via a fixing functional layer.

[0105] Examples of the anchoring function layer include an adhesive layer and a pressure-sensitive adhesive layer.

[0106] As the fixing function layer, as long as it has transparency, it can be used without special material restrictions. The fixing function layer is preferably formed by a resin. As the resin, for example, acrylic resin, silicone resin, polyester resin, polyurethane resin, polyamide resin, polyvinyl ether resin, vinyl acetate / vinyl chloride copolymer, modified polyolefin resin, epoxy resin, fluororesin, natural rubber and synthetic rubber can be listed. In particular, from the perspective of excellent optical transparency and showing appropriate adhesive properties such as wettability, aggregation and adhesion, and excellent weather resistance and heat resistance, as the resin, acrylic resin is preferably selected.

[0107] In the resin forming the fixing function layer, in order to suppress the corrosion and migration of the light-transmitting conductive layer 3, a known anticorrosive agent and an anti-migration agent (for example, the material disclosed in Japanese Patent Laid-Open No. 2015-022397) may be added. In addition, in the fixing function layer (the resin forming the fixing function layer), in order to suppress the degradation of the article when it is used outdoors, a known ultraviolet absorber may be added. Examples of the ultraviolet absorber include benzophenone compounds, benzotriazole compounds, salicylic acid compounds, oxalic acid anilide compounds, cyanoacrylate compounds, and triazine compounds.

[0108] In addition, the resin layer 11 in the light-transmitting conductive film 10 and the components corresponding to the articles may be fixed via the fixing functional layer. In this case, the light-transmitting conductive layer 3 (including the light-transmitting conductive layer 3 having a pattern shape) is exposed in the light-transmitting conductive film 10. Therefore, a cover layer may be arranged on one side of the light-transmitting conductive layer 3 in the thickness direction.

[0109] The cover layer is a layer that covers the light-transmitting conductive layer 3 , and can improve the reliability of the light-transmitting conductive layer 3 and suppress functional degradation due to damage.

[0110] The material of the covering layer is preferably a dielectric. The covering layer is formed of a mixture of a resin and an inorganic material. As the resin, the resins exemplified in the fixing function layer can be cited. As the inorganic material, the materials exemplified in the materials of the intermediate layer described later can be cited.

[0111] Furthermore, in the mixture of the resin and the inorganic material, from the same viewpoint as that of the above-mentioned anchoring functional layer, a corrosion inhibitor, an anti-migration agent, and an ultraviolet absorber may be added.

[0112] The above-mentioned articles have excellent reliability because they include the above-mentioned light-transmitting conductive film 10. Specifically, touch sensors, dimming elements, photoelectric conversion elements, heat ray control components, antennas, electromagnetic wave shielding components, image display devices, heater components, and lighting have excellent reliability because they include the above-mentioned light-transmitting conductive film 10.

[0113] (Effects of one embodiment)

[0114] Then, in the method for manufacturing the light-transmitting conductive sheet 1, since the ratio of the power density P1 of the first target 51 to the total power density P (P1 / P) is 0.20 or less, the inner layer 6 with high crystallinity can be formed, thereby reducing the resistivity of the light-transmitting conductive layer 3. As a result, the light-transmitting conductive sheet 1 having the light-transmitting conductive layer 3 with low resistivity can be manufactured.

[0115] In the method for producing the light-transmitting conductive sheet 1 , since the inner layer 6 is formed by applying power to the first target 51 composed of an indium-tin composite oxide having a tin oxide content exceeding 8 mass %, the resistivity of the light-transmitting conductive layer 3 can be sufficiently reduced.

[0116] In addition, since the ratio R1 of the proportion of reactive gas in the sputtering gas in the first film forming chamber 41 to the proportion R2 of reactive gas in the sputtering gas in the second film forming chamber 42 (R1 / R2) is less than 1, the crystallinity of the inner layer 6 can be improved. As a result, a translucent conductive sheet 1 having a translucent conductive layer 3 with lower resistivity can be manufactured.

[0117] Furthermore, since the method for producing the light-transmitting conductive sheet 1 includes the third step of crystallizing the light-transmitting conductive layer 3 , it is possible to produce the light-transmitting conductive sheet 1 including the light-transmitting conductive layer 3 having a lower resistivity.

[0118] (Variation Example)

[0119] In the variant, the same components and processes as those in one embodiment are marked with the same reference numerals, and detailed description thereof is omitted. In addition, unless otherwise specified, the variant can exert the same effects as those in one embodiment. Furthermore, one embodiment and its variant can be appropriately combined.

[0120] The inert gas constituting the sputtering gas may be a single inert gas or a mixed inert gas obtained by mixing a plurality of inert gases. Specifically, for example, the inert gas may be only argon gas, or a mixed inert gas obtained by mixing argon gas, krypton gas, and xenon gas in any proportion.

[0121] Furthermore, the types of inert gases supplied to the film forming chambers may be different. For example, the inert gas of the first gas supply device 61 may be argon gas, and the inert gas of the second gas supply device 62 may be krypton gas.

[0122] The number of the multiple targets may be 2, 3, or 5 or more. If the number of the multiple targets is 2, the total power density P is P1+P2. Figure 3 As shown in FIG. 1 , the sputtering device 30 includes only a first film forming chamber 41 and a second film forming chamber 42. Figure 3 The light-transmitting conductive layer 3 formed by the sputtering device 30 shown in FIG. Figure 4 As shown, the inner layer 6 and the outer layer 22 are sequentially arranged on one side along the thickness direction.

[0123] The substrate sheet 2 may also have other functional layers. Figure 2 As shown by the dotted line, an anti-adhesion layer 25 may be provided on the other surface of the base material layer 4 in the thickness direction.

[0124] If the number of the multiple targets is 3, the total power density P is P1+P2+P3.

[0125] If the number of the multiple targets is 5, the total power density P is P1+P2+P3+P4+P5.

[0126] As one embodiment, a manufacturing method is disclosed in which (the surface of) the deposition roller 40 is cooled. On the other hand, in a modified example, the temperature of the deposition roller 40 is increased. The temperature of the deposition roller 40 is, for example, higher than 20° C. and lower than 180° C.

[0127] Example

[0128] Hereinafter, the present invention will be described in more detail with reference to the following embodiments and comparative examples. It should be noted that the specific numerical values ​​such as the blending ratio (containing ratio), physical property values, and parameters used in the following descriptions can be replaced by the upper limit values ​​(values ​​defined in the form of "below", "less than") or lower limits (values ​​defined in the form of "above", "exceeding") corresponding to the blending ratio (containing ratio), physical property values, and parameters described in the above-mentioned "Specific Implementation Methods" and corresponding to them. In addition, in the case of not particularly mentioned in the following descriptions, "parts" and "%" are mass references.

[0129] Example 1

[0130] On one side in the thickness direction of the substrate layer 4 formed of a long PET film (manufactured by Toray Industries, Ltd., with a thickness of 50 μm), a UV-curable hard coating composition containing an acrylic resin was applied and cured by irradiation with ultraviolet light to form a 2 μm-thick hard coating layer 5. Thus, a substrate sheet 2 having a substrate layer 4 and a hard coating layer 5 was prepared.

[0131] Next, the substrate sheet 2 is mounted on the sputtering device 30. The temperature of the film forming roller 40 is set to -8°C. The first pump 91, the second pump 92, the third pump 93, and the fourth pump 94 are driven. In the sputtering device 30, the materials of the first target 51, the second target 52, the third target 53, and the fourth target 54 are all sintered bodies of indium oxide and tin oxide. The concentration of tin oxide in the sintered body is 10% by mass.

[0132] Argon gas is supplied from the first inert gas supply machine 71 to the first film forming chamber 41, and oxygen gas is supplied from the first reactive gas supply machine 72 to the first film forming chamber 41. The gas pressure of the first film forming chamber 41 is 0.4 Pa. The ratio R1 (volume basis) of oxygen gas to argon gas in the mixed gas (argon gas and oxygen gas) in the first film forming chamber 41 is 0.010. The first target 51 is charged with an electric power density P1 (0.7 W / cm 2) to sputter the first target 51. The horizontal magnetic field intensity on the first target 51 is 90 mT. The power applied to the first target 51 uses DC.

[0133] Argon gas is supplied from the second inert gas supply machine 73 to the second film forming chamber 42, and oxygen gas is supplied from the second reactive gas supply machine 74 to the second film forming chamber 42. The gas pressure of the second film forming chamber 42 is 0.4 Pa. The ratio R2 (volume basis) of oxygen gas to argon gas in the mixed gas (argon gas and oxygen gas) in the second film forming chamber 42 is 0.017. The second target 52 is charged with an electric power density P2 (5.0 W / cm 2 ) to apply power to the second target 52 for sputtering. The horizontal magnetic field intensity on the second target 52 is 90 mT. The power applied to the second target 52 uses DC.

[0134] Argon gas is supplied from the third inert gas supply device 75 to the third film forming chamber 43, and oxygen gas is supplied from the third reactive gas supply device 76 to the third film forming chamber 43. The gas pressure of the third film forming chamber 43 is 0.4 Pa. The ratio R3 (volume basis) of oxygen to argon in the mixed gas (argon and oxygen) in the third film forming chamber 43 is 0.017. The third target 53 is charged with an electric power density P3 (5.0 W / cm 2 ) to apply power to the third target 53 for sputtering. The horizontal magnetic field intensity on the third target 53 is 90 mT. The power applied to the third target 53 uses DC.

[0135] Argon gas is supplied from the fourth inert gas supply device 77 to the fourth film forming chamber 44, and oxygen gas is supplied from the fourth reactive gas supply device 78 to the fourth film forming chamber 44. The gas pressure of the fourth film forming chamber 44 is 0.4 Pa. The ratio R4 (volume basis) of oxygen to argon in the mixed gas (argon and oxygen) in the fourth film forming chamber 44 is 0.017. The fourth target 54 is charged with an electric power density P4 (5.0 W / cm 2 ) to apply power to the fourth target 54 for sputtering. The horizontal magnetic field strength on the fourth target 54 is 90 mT. The power applied to the fourth target 54 uses DC.

[0136] The ratio of the power density P1 of the first target 51 to the total electrode density P of the power density P1 of the first target 51, the power density P2 of the second target 52, the power density P3 of the third target 53 and the power density P4 of the fourth target 54 (P1 / P=P1 / (P1+P2+P3+P4)) is 0.04.

[0137] Thus, the inner layer 6 and the outer layer 22 are sequentially formed on one side in the thickness direction of the base sheet 2. The inner layer 6 and the outer layer 22 form an amorphous light-transmitting conductive layer 3. Thus, a light-transmitting conductive sheet 1 (amorphous light-transmitting conductive sheet 10) having the base sheet 2 and the light-transmitting conductive layer 3 sequentially on one side in the thickness direction is manufactured.

[0138] Examples 2 to 6, Comparative Example 1, Comparative Example 2

[0139] The concentration of tin oxide of the first target 51, the power density of each target (P1, P2, P3, P4), the proportion of oxygen in the mixed gas R1~R4, the total thickness of the inner layer 6 and the outer layer 22, etc. are changed according to Table 1. Otherwise, the same procedure as in Example 1 is followed to manufacture a translucent conductive sheet 1 (amorphous translucent conductive sheet 10).

[0140] (evaluate)

[0141] The light-transmitting conductive sheet 1 of each example and each comparative example was heated in a hot air oven at 165° C. for 2 hours to crystallize the light-transmitting conductive layer 3. The light-transmitting conductive layer 3 was evaluated for the following items. The results are shown in Table 1.

[0142] (Surface resistance)

[0143] The surface resistance of the light-transmitting conductive layer 3 was measured by a four-probe method in accordance with JIS K7194 (1994).

[0144] (Resistivity)

[0145] The resistivity is obtained by multiplying the surface resistance of the light-transmitting conductive layer 3 by the thickness of the light-transmitting conductive layer 3 .

[0146] (Identification and thickness of inner layer, etc.)

[0147] The light-transmitting conductive sheet 1 was processed by the FIB microsampling method to expose a cross section, and then FE-TEM observation of the cross section was performed.

[0148] FIB equipment: FB2200 manufactured by Hitachi, Ltd. Accelerating voltage: 10 kV

[0149] FE-TEM device: JEM-2800 manufactured by JEOL Ltd. Accelerating voltage: 200 kV

[0150] The TEM photograph of Example 1 is shown in Figure 5 The TEM image of Comparative Example 1 is shown in Figure 6 .

[0151] [Table 1]

[0152]

[0153] It should be noted that the above invention is given as an exemplary embodiment of the present invention, but this is merely a simple illustration and should not be interpreted as limiting. Modifications of the present invention that are clear to those skilled in the art are included in the scope of protection of the claims.

[0154] Industrial Applicability

[0155] The light-transmitting conductive sheet is used for, for example, a touch sensor, a light-adjusting element, a photoelectric conversion element, a heat ray control member, an antenna, an electromagnetic wave shielding member, an image display device, a heater member, and lighting.

[0156] Description of Reference Numerals

[0157] 1 Translucent conductive sheet

[0158] 2. Substrate sheet

[0159] 3 Translucent conductive layer

[0160] 6 Inner layer

[0161] 22 Outer layer

[0162] 30 Sputtering device

[0163] 51 First Target

[0164] P1 Electric power density of the first target

[0165] P Total power density

[0166] R1 Oxygen ratio in the mixed gas (first step)

[0167] R2 The proportion of oxygen in the mixed gas (second step)

Claims

1. A method for producing a light-transmitting conductive sheet, It is characterized in that The manufacturing method comprises the steps of forming a light-transmitting conductive layer on one surface in the thickness direction of a substrate sheet by performing multiple sputtering operations in which power is applied to each of multiple targets. The step of forming the light-transmitting conductive layer comprises the following steps: In a first step, electric power is applied to a first target to form an inner layer on one side of the substrate sheet in the thickness direction, wherein the first target is included in the plurality of targets and contains indium oxide and tin oxide, and is formed of an indium-tin composite oxide having a tin oxide content exceeding 8% by mass; and In a second step, electric power is applied to targets other than the first target to form an outer layer on one surface in the thickness direction of the inner layer. A ratio of the power density P1 of the first target to the total power density P of the plurality of targets, that is, P1 / P, is 0.10 or less.

2. The method for producing a light-transmitting conductive sheet according to claim 1, It is characterized in that The first step is to perform sputtering in an atmosphere of a sputtering gas containing a reactive gas. The second step is to perform sputtering in an atmosphere of a sputtering gas containing a reactive gas. A ratio R1 / R2 of a ratio R1 of the reactive gas in the sputtering gas in the first step to a ratio R2 of the reactive gas in the sputtering gas in the second step is 1 or less.

3. The method for producing a light-transmitting conductive sheet according to claim 1 or 2, It is characterized in that After the second step, a third step of crystallizing the light-transmitting conductive layer is further provided.

4. A method for producing a light-transmitting conductive sheet, It is characterized in that The manufacturing method comprises the steps of forming a light-transmitting conductive layer on one surface in the thickness direction of a substrate sheet by performing multiple sputtering operations in which power is applied to each of multiple targets. The step of forming the light-transmitting conductive layer comprises the following steps: In a first step, electric power is applied to a first target to form an inner layer on one side of the substrate sheet in the thickness direction, wherein the first target is included in the plurality of targets and contains indium oxide and tin oxide, and is formed of an indium-tin composite oxide having a tin oxide content exceeding 8% by mass; and In a second step, electric power is applied to targets other than the first target to form an outer layer on one surface in the thickness direction of the inner layer. The first step is to perform sputtering in an atmosphere of a sputtering gas containing an inert gas and a reactive gas. In the first step, the ratio of the reactive gas to the inert gas is 0.1 or less on a volume basis. A ratio of the electric power density P1 of the first target to the total electric power density P of the plurality of targets, that is, P1 / P, is 0.20 or less.

5. The method for producing a light-transmitting conductive sheet according to claim 4, It is characterized in that The second step is to perform sputtering in an atmosphere of a sputtering gas containing an inert gas and a reactive gas. In the first step, a ratio of the reactive gas to the inert gas is 0.1 or less on a volume basis.

6. The method for producing a light-transmitting conductive sheet according to claim 4 or claim 5, It is characterized in that The second step is to perform sputtering in an atmosphere of a sputtering gas containing a reactive gas. A ratio R1 / R2 of a ratio R1 of the reactive gas in the sputtering gas in the first step to a ratio R2 of the reactive gas in the sputtering gas in the second step is 1 or less.

7. The method for producing a light-transmitting conductive sheet according to claim 4 or claim 5, It is characterized in that After the second step, a third step of crystallizing the light-transmitting conductive layer is further provided.