Airbag fabric

By using polyamide yarns with high formic acid relative viscosity and halogen:copper molar ratio in airbag fabrics, both thermal puncture and air permeability are solved, and a thinner and safer airbag fabric design is achieved.

CN115667620BActive Publication Date: 2024-12-03INVISTA TEXTILES (U K) LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180036839.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-11-06
Filing Date
2021-05-20
Publication Date
2024-12-03
Estimated Expiration
2041-05-20

AI Technical Summary

Technical Problem

The existing airbag fabrics are easily pierced by hot particles and hot gas at high temperatures, causing damage to the passengers. With the tendency of reducing the weight and size of the airbag module, it is difficult to take into account both air permeability and pinhole failure resistance.

Method used

Using spinned synthetic polyamide yarns, the yarns are cooked before, during or after weaving, so that they exhibit high relative viscosity of formic acid and halogen:copper molar ratio, and control sodium content, forming high Welding resistance woven fabric.

Benefits of technology

It improves the pinhole failure resistance and melt-through resistance of the airbag fabric, ensures that air permeability is not damaged under a thinner structure, and enhances vehicle safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115667620B_ABST
    Figure CN115667620B_ABST
Patent Text Reader

Abstract

A woven fabric comprises spun synthetic polyamide yarns woven in warp and weft directions, wherein the polyamide yarns in the woven fabric exhibit a formic acid relative viscosity of at least 60, a halogen:copper molar ratio of at least 2.0, and a sodium content of no more than 25 ppm, and wherein the woven fabric exhibits a melt-through resistance of at least 2.10 seconds at 450° C. The present invention also provides an airbag made of the woven fabric and a method of manufacturing the woven fabric.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to finished woven fabrics comprising spun synthetic polyamide yarns suitable for use as improved airbag fabrics and a method of making the same. Background Art

[0002] Inflatable airbags are key components of vehicle safety systems and are installed in almost every vehicle produced worldwide. Typically, inflatable airbags are made of woven fabrics of nylon yarn or polyester yarn. In order to meet the requirements for effective inflation, the airbag fabric must meet certain tensile strength requirements and have the ability to prevent air from passing through, and therefore it is desirable that the airbag has extremely low air permeability. As used herein, "airbag" refers to an inflatable passive safety restraint for automobiles and many other forms of transportation including flight applications. In recent years, the number of airbags and the areas covered by these airbags in various types of vehicle cabins have increased. The multi-airbag configuration when used includes airbags for the front seating area, airbags for side impact protection, airbags for rear seat purposes, airbags for inflatable curtains used in the canopy lining area, and airbags or pedestrian airbags used in inflatable seat belts. There is a constant trend towards smaller and lighter vehicles in automobiles, which means that there is less space available for mandatory safety components such as airbags. Automotive manufacturers are targeting improvements to crash impact safety systems in general and air bag modules in particular in terms of safety, environmental footprint, and cost.

[0003] Reduction in the weight of an airbag module per unit area of ​​deployable airbags generally results in a reduction in overall weight without compromising safety. This has become increasingly important as the number of airbags per vehicle has increased dramatically to provide occupant protection at multiple angles. Airbag modules are therefore required to be more efficient in size and weight.

[0004] Reductions in the size of airbag inflators also result in overall weight reduction and greater cost savings. To ensure equal effectiveness, smaller inflators run hotter than their historical counterparts.

[0005] The trend in the air bag module industry is toward thinner, lighter fabrics for use with smaller, hotter inflators. However, this more aggressive design has resulted in incidents where hot particles and / or hot gases from air bag deployment exhaust have pierced the air bag fabric, which can injure vehicle occupants and lead to recalls of millions of modules. As the number of air bags per vehicle and their relative proximity to occupants increases, protection from hot particle piercing and hot gas release, collectively referred to herein as fabric pinhole failures, becomes increasingly important in efforts to improve vehicle safety.

[0006] The object of the present invention is to provide an airbag fabric which has a greater resistance to pinhole failures in order to maintain the benefits in terms of reduced weight and improved cost effectiveness of the airbag module. Thus, a particular object of the present invention is to provide an airbag fabric which has a greater resistance to pinhole failures and which is also relatively thinner and lighter than conventional airbag fabrics, in particular without compromising air permeability or compromising it to an unacceptable level. Summary of the invention

[0007] According to a first aspect of the present invention, there is provided a woven fabric comprising spun synthetic polyamide yarn, wherein the fabric is made of polyamide yarn woven in warp and weft directions, wherein the polyamide yarn in the woven fabric exhibits a formic acid relative viscosity of at least 60, a halogen:copper molar ratio of at least 2.0 and a sodium content of not more than 25 ppm (preferably not more than 20 ppm, preferably not more than 15 ppm, preferably not more than 10 ppm), and wherein the woven fabric exhibits a melt-through resistance of at least 2.10 seconds at 450°C.

[0008] The inventors have discovered that characterization of a fabric's melt-through resistance can predict the likelihood of pinhole failure in a full airbag module deployment test.

[0009] The inventors have surprisingly found that the formic acid relative viscosity of the scoured yarn (also referred to herein as "relative viscosity") is a key influence on the melt-through resistance of the finished fabric, and yarns exhibiting higher relative viscosity exhibit higher melt-through resistance. Thus, such yarns can prevent hot particles from piercing the airbag during deployment under new and more efficient airbag module designs.

[0010] Furthermore, the inventors have surprisingly discovered that even though neither the relative viscosity nor the concentration of copper halogen has a measurable effect on the melting point of the fiber or fabric at the levels described herein, an effective concentration of copper halogen in the polymer of the fabric satisfactorily maintains the effect provided by the high relative viscosity. Furthermore, the inventors have discovered that, surprisingly, the molar ratio of halogen to copper in the finished fabric is satisfactorily maintained above an effective level to maintain the effect that the increased relative viscosity of the polymer has on melt-through resistance.

[0011] According to a second aspect of the present invention, there is provided an article, preferably an airbag, made from the woven fabric of the first aspect.

[0012] According to a third aspect of the present invention, there is provided a method for manufacturing a woven fabric of the first aspect, comprising the steps of weaving a spun synthetic polyamide yarn and scouring the yarn before, during or after weaving, so that the polyamide yarn in the woven fabric exhibits a formic acid relative viscosity of at least 60, a halogen:copper molar ratio of at least 2.0 and a sodium content of not more than 25 ppm (preferably not more than 20 ppm, preferably not more than 15 ppm, preferably not more than 10 ppm).

[0013] According to a fourth aspect of the present invention, there is provided use of the woven fabric according to the first aspect of the present invention for improving the pinhole failure resistance of an airbag made of the woven fabric. DETAILED DESCRIPTION

[0014] The woven fabric of the present invention is composed of high tenacity spun synthetic polyamide yarn. The yarn is made of fibers in the form of continuous filaments. Such filaments are formed by extruding a molten polymer through a spinneret at high temperature and pressure and then side-blown in air, coated with a spin finish lubricant, stretched between pairs of guide rollers, slightly deformed to provide sufficient entanglement to form a coherent yarn, and then wound on a cardboard tube as a bobbin.

[0015] The spinning oil on the filaments facilitates the treatment of the yarn during the production process of the yarn and is subsequently removed to provide a finished woven fabric. The removal of spinning oils such as lubricants or oils and antistatic substances, dust, contaminants, etc. from the yarn is typically implemented by a scouring treatment as conventionally used in the art, such as by rinsing or impregnating with conventional agents such as water (optionally with a predetermined pH level), surfactants, detergents, alkalis, chelating agents, emulsifiers, etc. Such scouring treatments are typically implemented during weaving and / or after weaving. In particular, the substances can be removed during the weaving process (such as a water jet weaving process) used to manufacture woven fabrics. In this regard, it will be appreciated by those skilled in the art that the term "remove" or "removal" does not necessarily imply complete removal of the substances described, but complete or substantially complete removal is included in the term.

[0016] It will be appreciated that the polyamide yarn in the woven fabric of the present invention is a scoured yarn. As used herein, the term "scoured yarn" refers to a yarn from which spinning oil or other lubricant or oil has been removed. The relative viscosity of the yarn is defined herein as the relative viscosity after the spinning oil has been removed from the yarn. The removal of the spinning oil can be implemented before weaving, during weaving, or after weaving (preferably during weaving or after weaving). Thus, the removal of the spinning oil (or "scouring") can be implemented by a conventional scouring process of the yarn before weaving or during weaving and preferably during weaving (such as in a water jet weaving process). Alternatively, the removal of the spinning oil can be implemented after the yarn has been woven into a fabric.

[0017] The relative viscosity of the yarn refers to the relative viscosity of the scour-finished yarn in the finished woven fabric, and is preferably the same as the relative viscosity of the yarn supplied to the weaving process.

[0018] In the woven fabric of the present invention, at least most (and preferably all) of the yarns used in the warp direction of the fabric are preferably formed by synthetic fibers made from a single polyamide component. Similarly, at least most (and preferably all) of the yarns used in the weft direction of the fabric are preferably formed by synthetic fibers made from a single polyamide component. In a preferred but non-limiting embodiment, at least most (and preferably all) of the yarns used in the warp and weft directions of the fabric are formed by synthetic fibers formed from a single polyamide component. Preferably, a single polyamide is used in each of the warp and weft directions and preferably, the same polyamide is used in the warp and weft directions.

[0019] Suitable polyamide fibers are preferably selected from polyamide fibers formed from nylon 6,6, nylon 6, nylon 6,12, nylon 7, nylon 12, nylon 4,6 or copolymers or mixtures thereof. In a preferred but non-limiting embodiment, the polyamide is nylon 6,6.

[0020] The relative viscosity of the yarn is preferably at least 70, preferably at least 78, preferably at least 85, preferably at least 90, and typically not more than 150, typically not more than 110, typically not more than 100. Preferably, the relative viscosity is in the range of from 60 to 110, preferably in the range of from 70 to 110, preferably in the range of from 85 to 100. The inventors have observed that there is no clear relationship between melt-through resistance and the melting point of the polyamide in the base yarn or fabric. Thus, the positive correlation between melt-through resistance and relative viscosity observed by the inventors surprisingly gives that, over the relevant relative viscosity range, the melting point of a polyamide yarn with a high relative viscosity (RV) is difficult to effectively distinguish from the melting point of a corresponding polyamide yarn with a low relative viscosity.

[0021] Polyamide yarns exhibiting such relative viscosity values ​​can be prepared by conventional means in the art. For example, as known in the art, the relative viscosity can be increased by increasing the degree of polymerization (i.e., molecular weight) of the polyamide. For example, the molecular weight and relative viscosity can be increased by a solid-state polymerization step (typically carried out at an elevated temperature (e.g., about 180° C.) under dry nitrogen).

[0022] In the woven fabric of the present invention, at least a majority (and preferably all) of the yarns in the warp direction are yarns having a tenacity of from 6.8 to 10.1 g / den. Similarly, at least a majority (and preferably all) of the yarns in the weft direction are yarns having a tenacity of from 6.8 to 10.1 g / den. In a preferred but non-limiting embodiment, at least a majority (and preferably all) of the yarns in the warp and weft directions are yarns having a tenacity of from 6.8 to 10.1 g / den.

[0023] The yarn used in the present invention preferably has a linear mass density within the range of from about 100 to about 2000 decitex, preferably from about 150 to about 1000 decitex, preferably from about 150 to about 940 decitex, preferably from about 150 to about 750 decitex.

[0024] The mass density per unit length of the fibers constituting the yarn is preferably in the range of from about 1 to about 25 DPF (decitex perfilament), or in the range of from about 2 to about 12 DPF.

[0025] The woven fabric of the present invention is preferably made of yarns having an end count / dm of from 90 to 300, preferably from 160 to 240. Preferably, the woven fabric presents a symmetrical construction. Thus, the end count / dm of the warp yarns is preferably the same as the end count / dm of the weft yarns.

[0026] The yarn used in the present invention may also include various additives used in the production and processing of the fiber. Suitable additives include, but are not limited to, heat stabilizers, antioxidants, light stabilizers, smoothing agents, antistatic agents, plasticizers, thickeners, pigments, flame retardants, fillers, adhesives, color fixatives, softeners, or combinations thereof.

[0027] Copper compounds have been conventionally added to polyamide yarns, typically before or during fiber spinning (and preferably added to the polyamide before spinning) to improve long-term oxidative degradation of airbag fabrics over long periods of storage. The effectiveness of these additives has conventionally been measured by the retention of fabric strength (tenacity) over long storage intervals at elevated temperatures. Suitable copper compounds include copper halides (preferably copper bromide and / or copper iodide), copper acetate, copper phosphate, copper salicylate, copper stearate and copper benzoate, and copper compounds with 1,4-xylenediamine, mercaptobenzimidazole or benzimidazole. The copper compound may be in oxidation state I or II. The inventors have surprisingly observed that the presence of copper in the polyamide is positively correlated with an improvement in the resistance to melt-through, despite the fact that the melting point of the polyamide remains unchanged. Even more surprisingly, the inventors have observed that the presence of copper together with a higher relative viscosity of the polyamide provides a further improvement in the resistance to melt-through. The copper compound is preferably present in the range of 10-500 ppm, preferably in the range of 50-150 ppm, preferably in the range of 60-120 ppm (calculated as elemental copper), based on the weight of the polyamide yarn in the finished fabric. Copper bromide and / or copper iodide are particularly preferred.

[0028] The inventors have determined that the effectiveness of copper in improving the melt-through resistance of woven fabrics is related to the molar ratio of halogen:copper in the yarn. Preferably, the molar ratio of halogen:copper in the yarn of the woven fabric of the present invention (i.e., the molar ratio of halogen:copper in the finished fabric) is at least 2.0:1, preferably at least 3.0:1, preferably at least 4.0:1, preferably at least 6.0:1. The inventors have found that such a halogen-copper molar ratio unexpectedly improves the melt-through resistance. Preferably, the molar ratio of halogen:copper in the finished fabric does not exceed 25.0:1, preferably does not exceed 20.0:1. Thus, preferably, the halogen:copper ratio is in the range of 2.0:1 to 25.0:1, preferably in the range of 3.0:1 to 25.0:1, preferably in the range of 4.0:1 to 25.0:1, preferably in the range of 6.0:1 to 25.0:1.

[0029] The inventors have also determined that the concentration of halogens (particularly bromine and / or iodine) in yarns is not maintained after fabric formation due to loss into water in the scouring and rinsing steps before or after weaving and into any water in the weaving process (such as water jet weaving). Exposure of the fiber or finished fabric to water removes the halogens, with the rate of loss depending on many factors, including the volume of water, temperature, pH, and identity of the base used in the scouring process. Such treatment of yarns and fabrics typically employs a scouring agent such as potassium hydroxide or sodium hydroxide. Typically, about 15-50% of the halogen content of the yarn is lost during such treatment of yarns and fabrics (for this purpose, they are collectively referred to herein as the "scouring process"), with 80% or more lost in harsh scouring processes.

[0030] Preferably, the molar ratio of halogen:copper is maintained in the present invention by controlling the harshness of the scouring process to minimize halogen loss and ensure a sufficiently high molar ratio in the finished fabric. Scouring treatments to remove spinning finishes can be achieved by various means and are well known in the art, and can therefore be adjusted accordingly by those skilled in the art, such as by controlling one or more of the volume of water, temperature, pH, residence time, and the identity and / or concentration of the alkali used in the process. Scouring treatments are also sometimes employed to finalize the configuration or size of the final fabric; for example, mild scouring treatments employed for that purpose are typically performed by rinsing in water at an elevated temperature.

[0031] Preferably, the temperature in the scouring step is below 95°C, preferably below 75°C.

[0032] Preferably, the final pH of the scouring bath is at least 10, preferably at least 11.

[0033] Preferably, the residence time in the scouring bath does not exceed 5 minutes / m 2 Fabric, preferably not more than 3 minutes / m 2 Fabric, preferably not more than 2 minutes / m 2 fabric.

[0034] Preferably, the concentration of sodium ions in the scouring bath or fluid is below 35 ppm, preferably below 10 ppm.

[0035] In one embodiment, the scouring bath contains potassium hydroxide rather than sodium hydroxide because the base controls the pH.

[0036] The severity of the scouring process is suitably determined by measuring the residual sodium content in the finished fabric, a lower residual sodium content corresponding to a less severe scouring process. The residual sodium content does not exceed 25 ppm, preferably does not exceed 20 ppm, preferably does not exceed 15 ppm, preferably does not exceed 10 ppm (calculated as elemental sodium) based on the total weight of the finished woven fabric (i.e. after weaving and scouring).

[0037] Alternatively or additionally, the molar ratio of halogen:copper in the yarn of the woven fabric can be controlled by controlling the halogen loading in the base fiber or yarn to ensure a molar ratio of halogen:copper of at least 2.0:1 (preferably at least 4.0:1, preferably at least 6.0:1) in the finished woven fabric. The halogen loading in the base yarn is defined herein as the halogen loading in the fiber or yarn before any spinning oil is removed from the yarn. Thus, in this embodiment, the halogen loading in the base yarn is preferably a molar ratio of halogen:copper in the base yarn of at least 4.0:1, preferably at least 8.0:1, preferably at least 10.0:1, preferably at least 12.0:1. It will be appreciated that the appropriate halogen loading in the base yarn is preferably determined using knowledge of the subsequent scouring process. However, for mild scouring processes (i.e., no more than 50% of the halogen content is lost in a mild scouring process), a halogen:copper molar ratio of at least 4.0:1, preferably at least 8.0:1 or at least 10.0:1 or at least 12.0:1 in the raw yarn will be sufficient to achieve the objectives of the present invention. For yarns and fabrics that will undergo more severe scouring processes in which 80% or more of the halogen content is lost, the halogen content in the raw yarn may be increased accordingly, such as to at least 15.0:1 or at least 20.0:1, even though the manufacturing cost will be increased. However, depending on the scouring conditions, even high levels of halogen undergo almost quantitative removal, and a loss of melt-through resistance occurs as a result.

[0038] In order to control the halogen loading in the raw yarn, a halide salt (other than copper halide), other than a copper compound, such as a potassium halide (preferably potassium bromide or potassium iodide) may be added to the yarn. Preferably, the halide salt is added to the polyamide before spinning. It will be appreciated that in the present invention, the halide salt is not a sodium salt.

[0039] In yet other embodiments, the sodium concentration in the final fabric is minimized to the desired levels described herein by controlling the sodium content of the water used in the weaving and / or scouring process steps, such as by a treatment system for the supply water. Thus, in order to minimize the unintentional introduction of sodium ions into the fabric during water jet weaving, the sodium content of the weaving water may be controlled, such as by a membrane reverse osmosis system capable of rejecting at least 90% of the sodium ions in the supply water. Alternatively or additionally, in order to minimize the unintentional introduction of sodium ions into the fabric due to the scouring process, the sodium content of the water used in the scouring process may be controlled, such as by a membrane reverse osmosis system capable of rejecting at least 90% of the sodium ions in the supply water. The water in the weaving step or the scouring step may be recycled. Spinning finishes are typically rich in oils and fats, and in order to avoid degrading the performance of the water treatment system by clogging the reverse osmosis system, it is preferred to use an ultrafiltration membrane system to filter out any fats or oils before removing the sodium.

[0040] The woven fabric of the present invention can be formed by warp yarns and weft yarns using weaving techniques known in the art. Suitable weaving techniques include, but are not limited to, plain weave, twill weave, satin weave, modified weaves of these types, one piece woven OPW weaving or multi-axial weaving. Suitable looms that can be used for weaving include water jet looms, air jet looms or rapier looms, and preferably the looms are water jet looms. These looms can also be used with jacquards to create OPW structures. The fabric can be finished according to any method known in the art, including drying on the loom, scouring, can be dried and heat-set. Preferably, the woven fabric of the present invention is a water jet woven fabric dried on the loom, or dried by an independent process. In water jet weaving, the spinning oil is dissolved in water and the scraping of the yarns relative to each other and the healds and reeds of the loom remove the spinning oil from the yarn.

[0041] The woven fabric of the present invention preferably exhibits a weight of from 50 to 500 g / m 2 , preferably not more than 300g / m 2 , preferably not more than 260g / m 2 , preferably not more than 225g / m 2 , and preferably at least about 80 g / m 2 , preferably at least about 100 g / m 2 , preferably at least about 150 g / m 2 , and typically at least 170 g / m 2 In a preferred embodiment, the woven fabric of the present invention exhibits a total fabric weight of from 150 to 260 g / m 2 , preferably from 170 to 225 g / m 2 Total fabric weight.

[0042] The woven fabric of the present invention preferably exhibits a strength of not more than 750 kg / m 3 , preferably not more than 725kg / m 3 , typically not exceeding 700kg / m 3 The fabric density.

[0043] The total thickness of the woven fabric of the present invention is preferably not more than 0.40 mm.

[0044] The woven fabric of the present invention preferably has a melt-through resistance at 450° C. of at least 2.10 seconds, preferably at least 2.20 seconds, preferably at least 2.30 seconds, preferably at least 2.40 seconds, preferably at least 2.50 seconds, preferably at least 2.60 seconds, as measured as described herein. The inventors have observed that melt-through resistance increases with increasing fabric weight.

[0045] The woven fabrics of the present invention preferably exhibit a relative humidity of not more than 6.0 1 / dm2 when the fabric is unaged. 2 / min, preferably not more than 5.0l / dm 2 / min, preferably not more than 4.0 l / dm 2 / min, preferably not more than 3.0 l / dm 2 / min, preferably not more than 2.0l / dm 2 / minute static air permeability (SAP).

[0046] The woven fabric of the present invention preferably exhibits a dynamic air permeability (DAP) of not more than 700 mm / s, preferably not more than 600 mm / s, preferably not more than 500 mm / s, preferably not more than 400 mm / s, preferably not more than 300 mm / s, preferably not more than 200 mm / s when the fabric is not aged.

[0047] Preferably, the fabric has a tear strength of at least 120 N, preferably at least 150 N, preferably at least 170 N in both the warp and weft directions when the fabric is not aged.

[0048] The woven fabric of the present invention is preferably uncoated. It is known in the art that there are coated woven fabrics, which include a layer or coating applied to the surface of the woven fabric for the purpose of reducing air permeability. Such prior art woven fabrics containing additional layers or coatings are referred to herein as "coated woven fabrics" and are in the form of any coating, web, net, laminate or film that may have been used to impart a reduction in air permeability or an increase in thermal resistance. Examples of such coatings include chloroprene rubber, silicone-based coatings, polydimethylenesiloxane, polyurethanes, and rubber components. Examples of such nets, nets, and films include polyurethanes, polyacrylates, polyamides, polyesters, polyolefins, polyolefin elastomers, and mixtures and copolymers thereof. It will be appreciated that the preferred uncoated woven fabrics of the present invention are not "coated woven fabrics" as defined herein. In one embodiment, the woven fabric of the present invention is further treated by applying a layer or coating to the surface of the woven fabric to further increase the fabric's resistance to pinhole creation by excessively hot gases and / or hot particles during high energy (heat) inflation.

[0049] In a second aspect, the present invention also provides an article made from the woven fabric described herein, wherein the article is selected from airbags, canvas, inflatable slides, temporary shelters, tents, pipes, covers and printed media, and in particular wherein the article is an airbag. The term "airbag", as used herein, includes airbag cushions. Airbag cushions are typically formed from multiple panels of fabric and can be inflated quickly. The fabric of the present invention can be used in airbags that are sewn from multiple pieces of fabric or from one-time woven (OPW) fabrics. One-time woven (OPW) fabrics can be made by any method known to those skilled in the art.

[0050] According to a third aspect of the present invention, there is provided a method of making a woven fabric as described herein, comprising the steps of weaving a spun synthetic polyamide yarn and scouring the yarn before, during or after weaving, whereby the polyamide yarn exhibits in the woven fabric a formic acid relative viscosity of at least 60, a halogen:copper molar ratio of at least 2.0 and a sodium content of not more than 25 ppm.

[0051] As described above, the method of making a woven fabric preferably includes controlling the severity of the scouring treatment. Alternatively or additionally, the method of making a woven fabric includes controlling the halogen loading in the raw yarn from which the woven fabric is made to ensure a halogen: copper molar ratio of at least 2.0:1 (preferably at least 4.0:1, preferably at least 6.0:1) in the finished woven, preferably wherein the halogen loading in the raw yarn is a halogen: copper molar ratio in the raw yarn of at least 4.0:1, preferably at least 8.0:1, preferably at least 10.0:1, preferably at least 12.0:1. Alternatively or additionally, the method includes controlling the sodium concentration in the woven fabric by controlling the sodium content in the feed water used in the weaving and / or scouring treatment steps, such as by a membrane reverse osmosis 2 system capable of rejecting at least 90% of the sodium ions in the feed water.

[0052] According to a fourth aspect of the present invention, there is provided the use of a woven fabric according to the first aspect of the present invention to improve the pinhole failure resistance of an airbag made from said woven fabric, in particular with respect to the level of melt-through resistance described herein.

[0053] It will be appreciated that preferences and elements described in relation to the first aspect herein are equally applicable to the second, third and fourth aspects.

[0054] The following test methods were used to characterize the woven fabrics disclosed herein.

[0055] (i) Formic acid relative viscosity

[0056] Relative viscosity (RV) measurements were performed on fabrics according to ASTM D789-19 using a 90% formic acid solution. For each replicate of this analysis, a 20 gram fabric sample was required. Prior to the RV measurement, each sample was treated to remove any residual fiber lubricant oil, also known as a spinning oil. To remove the lubricant, each piece of fabric was soaked in enough methylene chloride to completely cover the sample. The sample was allowed to soak in a covered extraction funnel for 20 minutes while stirring. The process was then repeated. Once the second methylene chloride rinse was completed, the fabric was soaked in enough 1:1 methanol:methylene chloride to completely cover the sample. The sample was allowed to soak in a covered extraction funnel for 20 minutes while stirring. The process was repeated two more times. Once all five soaking steps were completed, the residual solvent was blown off the fabric sample using clean pressurized air. The fabric was then allowed to air dry thoroughly in an exhaust hood. Once dry, ASTM D789-19 was used to measure the relative viscosity of the fabric sample.

[0057] (ii) Melt-through resistance

[0058] In order to measure the resistance to melt penetration of woven fabrics, a "hot rod" test was used. Each fabric piece was 75 mm wide (warp) and 100 cm long (weft). Three fabric pieces (one for each test temperature) were required for each fabric sample. Before testing, the fabric pieces were conditioned for at least 24 hours before testing in a controlled atmosphere (20 ± 2 ° C and 65 ± 4% relative humidity). The test used a 12L14 carbon steel cylindrical rod, which was 50 mm long, 11 mm in diameter and each end was rounded at its edge with a 2 mm radius to give a flat end of 7 mm in diameter, weighing 36.5 g, with a specific heat capacity of 502.4 J / (kg ° K). The rod was heated in a muffle furnace for at least one hour to a controlled temperature to ensure temperature stabilization before testing. The hot rod was transferred to a conveyor tube and contacted with a fabric piece placed horizontally below the conveyor tube. Three fabric pieces were tested at 450 ° C, 550 ° C and 650 ° C. First, the test site must be at least 20 cm away from the selvedge of the fabric. The optical sensor in the transmission tube and the piezoelectric sensor attached to the catch tray located on the underside of the fabric allow accurate measurement of the time required for the rod to penetrate the fabric once contact is made. The time recorded in this test is the total time (seconds) between the rod blocking the light beam and hitting the catch tray, where the total time is equal to the residence time of the rod on the fabric plus 0.19 seconds (0.19 is the time for the rod to freely fall between the light beam and the catch tray in the absence of fabric). The time required for the rod to melt through the fabric (i.e. the residence time of the rod on the fabric) is then calculated and this time period is defined as the resistance to melt through. Longer melt through times indicate increased thermal resistance. Each test was repeated 10 times at each temperature to characterize the time required to melt through the fabric sample in seconds.

[0059] (iii) Elemental analysis

[0060] Elemental analysis was performed using neutron activation analysis.

[0061] (iv) Fabric Count

[0062] The yarn count of the fabric was evaluated using ISO-7211-2.

[0063] (v) Fabric thickness

[0064] The thickness test is performed on fabric samples that have been conditioned to standard laboratory conditions of 20±2°C and 65±4% relative humidity for at least 24 hours. Multiple samples are cut from the fabric in such a way that no two samples have any common warp or weft yarns. The samples are not cut within 20 cm of the selvedge or at any wrinkled, obviously damaged or dirty fabric area. The samples are suitably cut by using a cutting die using hydraulic pressure. An electronic micrometer with a test range of 0-25 mm and an accuracy of 0.001 mm (with a 6.5 mm diameter jaw) is used to measure the thickness of five samples and record the results. The reported results (in mm) are the arithmetic average of the results of five independent samples.

[0065] (vi) Fabric weight

[0066] Fabric weight is measured according to ISO 3801 (1977) with EASC modifications and according to EASC Operating Guide 99040180 (Sections 3.05 and 4.01) for testing of covered fabrics. The weight test is performed on samples of fabric that have been conditioned to standard laboratory conditions of 20±2°C and 65±4% relative humidity for at least 24 hours. Five square samples of size 10×10 cm (each oriented at 45° to the warp direction) are cut from the sample diagonally across the fabric in such a way that no two samples have any common warp or weft yarns. The samples are not cut within 10 cm of the selvedge or in any wrinkled fabric area, visibly damaged fabric area or dirty fabric area. The samples are cut out by using a 10×10 cm cutting die using hydraulic pressure. Once cut, the five samples are weighed on a three decimal place balance in grams and the results are recorded. Each result is multiplied by 100 to give the weight in g / m 2 The fabric weight reported is the arithmetic average of the five results.

[0067] (vii) Static Air Permeability (SAP)

[0068] Static air permeability SAP is measured according to ISO 9237 (1995), but with the following modifications:

[0069] (a) Test area is 100cm 2 .

[0070] (b) The test pressure (partial vacuum) is 500Pa.

[0071] (c) Each individual test value is corrected for edge leakage.

[0072] (d) Static air permeability testing is conducted at six points across and along the fabric by testing six separate areas of the warp and weft threadlines within the fabric.

[0073] (e) Reported static air permeability (in l / dm 2 / minute) is the arithmetic mean of six measurements.

[0074] (viii) Dynamic Air Permeability (DAP)

[0075] Dynamic air permeability is defined as the average velocity (mm / s) of air or gas within the selected test pressure range of 30-70 kPa (converted to a pressure of 100 kPa (14.2 psi)) and a temperature of 20°C. Dynamic air permeability is measured according to test standard ASTM D 6476-12, but with the following modifications:

[0076] (a) The limits of the measuring pressure range (as set on the test instrument) are 30-70 kPa;

[0077] (b) The initial pressure (as set on the test instrument) is adjusted to achieve a peak pressure of 100 ± 5 kPa.

[0078] (c) Test head volume is 400 cm 3 , unless the specified starting pressure cannot be achieved using that head, in which case an interchangeable volume of 100, 200, 800 or 1600 cm2 shall be used as appropriate for the fabric under test. 3 Test head.

[0079] (d) Dynamic air permeability testing is conducted at six points across and along the fabric using six separate areas of the warp and weft yarns in the fabric for testing.

[0080] (e) The reported dynamic air permeability (in mm / s) is the arithmetic mean of six measurements.

[0081] (ix) Tearing strength

[0082] The tearing force (also called tear strength) of a fabric expressed in Newtons (N) is determined according to standard ISO 13937-2 (2000), but with the modifications listed below:

[0083] (a) Fabric specimen size is 150 mm x 200 mm (with a 100 mm slit extending from the midpoint of the narrow end to the center.

[0084] (b) Tear tests are performed on 5 warp specimens and 5 weft specimens cut diagonally across each test fabric and avoiding any area within 200 mm of the selvedge of the fabric.

[0085] (c) Warp tear results are obtained from test specimens that tear across the warp (i.e., the warp threads are torn), while weft tear results are obtained from test specimens that tear across the weft (i.e., the weft threads are torn).

[0086] (d) According to ISO 13937-2 Annex D / D.2, the feet of each specimen were folded in half to be fixed on Instron clamp grips.

[0087] (e) The test results are evaluated in accordance with ISO 13937-2, Section 10.2 “Calculation using electronic equipment”.

[0088] (f) Warp Tear Force is reported as the arithmetic mean of the tear force results of five warp specimens, and Weft Tear Force is reported as the arithmetic mean of the tear force results of five weft specimens, both in Newtons (N).

[0089] (x) Calculation of fabric density

[0090] Fabric density is expressed by g / m 2 ) Divide the fabric weight by the fabric thickness measurement (mm) to convert to kg / m 3 units to calculate.

[0091] The present invention is further illustrated by the following examples. It will be appreciated that these examples are for illustrative purposes only and are not intended to limit the present invention to that illustrated. Modifications of detail may be made thereto without departing from the scope of the present invention.

[0092] Example

[0093] Example 1

[0094] A series of woven fabrics were made from a 209×209 warp count / dm construction using nylon 6,6 yarns with different relative viscosities. In each fabric, the warp yarns were identical to the weft yarns. The melt penetration resistance of each fabric was tested at 450°C, 550°C, and 650°C. Figure 1 As shown in Figure 2, the results show that the melt-through resistance is unexpectedly found to increase with the relative viscosity (RV). Figure 1 It is seen that increasing the relative viscosity from about 70 to about 85 satisfactorily increases the melt-through resistance by 0.2 seconds, a significant improvement on the time scale of airbag deployment. The most satisfactory melt-through resistance performance is achieved at an RV of at least 78, preferably at least 85.

[0095] Example 2

[0096] Another series of woven fabrics were made from a 209×209 warp count / dm construction using nylon 6,6 yarns each with a different halogen:Cu molar ratio. In each fabric, the warp yarns were identical to the weft yarns, and the yarns in the finished fabrics exhibited a relative viscosity of 66 and a residual sodium content of less than 10 ppm. The melt-through resistance of each fabric was tested at 450°C, 550°C, and 650°C. Figure 2 As shown, the results demonstrate that the melt-through resistance for fabrics having a relatively high halogen:Cu molar ratio is better than that for fabrics having a relatively low halogen:Cu molar ratio.

[0097] Further investigation of the meltthrough resistance at 450°C of a range of other fabric samples (all having a 209×209 warp count / dm construction) confirmed that effect, as Figure 3 The most satisfactory melt-through resistance performance is obtained at a molar ratio of halogen:Cu of at least 4.0:1, preferably at least 6.0:1. Thus, for 60 ppm of Cu, the fabric should preferably maintain at least 302 ppm of bromine or at least 480 ppm of iodine for effective melt-through resistance.

[0098] Example 3

[0099] Another series of woven fabrics were made from nylon 6,6 yarn, similar to the above but using different scouring conditions to evaluate the effects of (i) residence time in the scouring process, (ii) pH of the scouring bath, and (iii) temperature of the scouring bath on the molar ratio of halogen:Cu.

[0100] The inventors observed that the molar ratio of halogen:Cu is inversely correlated with the fabric residence time during the scouring process, such as Figure 4 The inventors also observed that the molar ratio of halogen:Cu in the scouring fabric is related to the pH of the scouring bath, as shown in Figure 5 The inventors also observed that the halogen loss observed due to exposure to alkaline scouring was not mitigated by neutralizing the pH of the scouring bath components with a weak acid. Surprisingly, it was found that the weak acid exacerbated the halogen removal from the yarn or fabric in such a neutralized bath component (1each). The inventors also observed that the molar ratio of halogen:Cu in the fabric was also inversely related to the scouring bath temperature, as shown in FIG. Figure 6 shown.

[0101] Example 4

[0102] Another series of woven fabrics were prepared, similar to the above, to investigate the residual sodium content. The inventors observed that fabrics with the same construction (209×209 ends / dm) and relative viscosity (66) but with different residual sodium contents had different melt-through resistance, such as Figure 7 As shown. Thus, fabrics with low residual sodium content have high resistance to melt-through. Analysis of woven nylon 6,6 fabrics of the same construction but with a different range of relative viscosities (65 to 86) gives the same correlation.

[0103] Example 5

[0104] The inventors also observed that fabrics with high relative viscosity (RV) were found to be more sensitive to the effects of residual sodium, i.e. different levels of sodium had a greater effect on melt-through resistance at higher relative viscosities. High RV (at least 75) fabrics and low RV (less than 75) fabrics of the same construction (209×209 ends / dm) were scoured with various concentrations of sodium under various aggressive commercial scouring conditions. The results are presented in Figure 8 , Figure 8 Further evidence is provided that fabrics with higher levels of residual sodium exhibit poorer meltthrough resistance, and this effect is demonstrated to be more pronounced for high RV fabrics.

[0105] Example 6

[0106] Another series of experiments were conducted to investigate the correlation of residual sodium levels with melt-through resistance. Sodium was added to greige woven fabrics by immersion in a NaOH bath or a NaCl bath for a short time and at a low temperature compared to the industrially effective scouring process. No effect on melt-through resistance was observed, demonstrating that the presence of sodium on the fabric does not itself cause a reduction in melt-through resistance. Rather, the residual sodium content is an indication of the severity of the scouring process, and it is exposure to sodium under harsh conditions that results in poor melt-through resistance.

[0107] The inventors have also found that rinsing the harshly scoured fabric in deionized water at various temperatures and soaking times results in low sodium content of the fabric but does not restore the melt-through resistance, which confirms that the residual sodium content in the finished fabric is indicative of, but does not cause, a reduction in melt-through resistance and is indicative of the relative severity of the scouring process. Thus, the selection of scouring conditions to maximize the melt-through resistance of a given polyamide woven fabric is important.

Claims

1. A woven fabric comprising spun synthetic polyamide yarns woven in warp and weft directions, wherein: The polyamide yarns in the woven fabric exhibit a formic acid relative viscosity of at least 70, a halogen:copper molar ratio of at least 2.0, and a sodium content of no more than 25 ppm, and wherein the woven fabric exhibits a melt-through resistance of at least 2.10 seconds at 450°C.

2. The woven fabric according to claim 1, wherein: The relative viscosity is at least 78.

3. The woven fabric according to claim 1, wherein: The relative viscosity is at least 85.

4. The woven fabric according to claim 1, wherein: The relative viscosity is at least 90.

5. The woven fabric according to claim 1, wherein: The polyamide yarn includes copper bromide or copper iodide.

6. The woven fabric according to claim 1, wherein: The molar ratio of halogen:copper in the polyamide yarns of the woven fabric is at least 4.0:

1.

7. The woven fabric according to claim 1, wherein: The molar ratio of halogen:copper in the polyamide yarns of the woven fabric is at least 6.0:

1.

8. The woven fabric according to claim 1, wherein: The polyamide yarn exhibits a copper content, calculated as elemental copper, of 60 to 120 ppm, relative to the total weight of the polyamide yarn in the woven fabric.

9. The woven fabric according to claim 1, wherein: The polyamide yarn exhibits a sodium content of not more than 20 ppm.

10. The woven fabric according to claim 1, wherein: The polyamide yarn exhibits a sodium content of not more than 15 ppm.

11. The woven fabric according to claim 1, wherein: The polyamide yarn exhibits a sodium content of not more than 10 ppm.

12. The woven fabric according to claim 1, wherein: The polyamide yarns from which the woven fabric is made exhibit a molar ratio of halogen:copper of at least 4.0:

1.

13. The woven fabric according to claim 1, wherein: The polyamide yarns from which the woven fabric is made exhibit a molar ratio of halogen:copper of at least 8.0:

1.

14. The woven fabric according to claim 1, wherein: The polyamide yarns from which the woven fabric is made exhibit a molar ratio of halogen:copper of at least 10.0:

1.

15. The woven fabric according to claim 1, wherein: The polyamide yarns from which the woven fabric is made exhibit a molar ratio of halogen:copper of at least 12.0:

1.

16. The woven fabric according to claim 1, wherein: The polyamide yarns from which the woven fabric is made also include a halide salt other than copper halide or sodium halide.

17. The woven fabric according to claim 1, wherein: The polyamide yarns making up the woven fabric also include potassium bromide or potassium iodide.

18. The woven fabric according to claim 1, wherein: The yarns in the warp and weft directions are yarns having a tenacity of from 6.8 to 10.1 g / den.

19. The woven fabric of claim 1, exhibiting a melt-through resistance at 450°C of at least 2.20 seconds.

20. The woven fabric of claim 1, exhibiting a meltthrough resistance at 450°C of at least 2.30 seconds.

21. The woven fabric of claim 1, exhibiting a melt-through resistance at 450°C of at least 2.40 seconds.

22. The woven fabric of claim 1, exhibiting a melt-through resistance at 450°C of at least 2.50 seconds.

23. The woven fabric according to claim 1, having a weight of from 50 to 500 g / m 2 Total fabric weight.

24. The woven fabric according to claim 1, having a weight of not more than 300 g / m 2 Total fabric weight.

25. The woven fabric according to claim 1, having a g / m 2 Total fabric weight.

26. The woven fabric according to claim 1, having a g / m 2 Total fabric weight.

27. The woven fabric according to claim 1, having a thickness of 170 to 225 g / m 2 Total fabric weight within the range.

28. The woven fabric according to claim 1, having a g / m 2 Total fabric weight.

29. The woven fabric according to claim 1, having a g / m 2 Total fabric weight.

30. The woven fabric of claim 1, wherein: The yarn has from 90 to 300 ends / dm.

31. The woven fabric of claim 1, wherein: The yarn has from 160 to 240 ends / dm.

32. The woven fabric of claim 1, wherein: The polyamide is nylon-6,6.

33. The woven fabric of claim 1, wherein: The yarn has a mass density per unit length in the range from 150 to 940 dtex.

34. The woven fabric of claim 1, wherein: The yarn has a mass density per unit length in the range of 150 to 750 dtex.

35. The woven fabric of claim 1 having an overall thickness of no greater than 0.40 mm.

36. The woven fabric of claim 1, wherein: When the fabric is not aged, the fabric has a tear strength of at least 120N in both the warp and weft directions.

37. The woven fabric of claim 1, wherein: When the fabric is not aged, the fabric has a tear strength of at least 150 N in both the warp and weft directions.

38. The woven fabric of claim 1, wherein: When the fabric is not aged, the fabric has a tear strength of at least 170N in both the warp and weft directions.

39. The woven fabric of claim 1, wherein: The fabric exhibits no more than 6.0 1 / dm 2 / minute static air permeability.

40. The woven fabric of claim 1, wherein: The fabric exhibits no more than 5.0 l / dm 2 / minute static air permeability.

41. The woven fabric of claim 1, wherein: The fabric exhibits no more than 4.0 l / dm 2 / minute static air permeability.

42. The woven fabric of claim 1, wherein: The fabric exhibits no more than 3.0 l / dm 2 / minute.

43. The woven fabric of claim 1, wherein: The fabric exhibits no more than 2.0 l / dm 2 / minute static air permeability.

44. The woven fabric of claim 1, wherein: The fabric exhibits a dynamic air permeability of not more than 700 mm / s.

45. The woven fabric of claim 1, wherein: The fabric exhibits a dynamic air permeability of not more than 600 mm / s.

46. ​​The woven fabric of claim 1, wherein: The fabric exhibits a dynamic air permeability of not more than 500 mm / s.

47. The woven fabric of claim 1, wherein: The fabric exhibits a dynamic air permeability of not more than 400 mm / s.

48. The woven fabric of claim 1, wherein: The fabric exhibits a dynamic air permeability of not more than 300 mm / s.

49. The woven fabric of claim 1, wherein: The fabric exhibits a dynamic air permeability of not more than 200 mm / s.

50. The woven fabric of claim 1, wherein: The fabric is uncoated.

51. The woven fabric of claim 1, wherein: The density of the fabric does not exceed 750kg / m 3 .

52. An article made from the woven fabric of any one of claims 1-51.

53. The article of claim 52, wherein: The article is an air bag.

54. A method of making a woven fabric according to any one of claims 1 to 51, comprising the steps of weaving a spun synthetic polyamide yarn and scouring the yarn during or after weaving so that the polyamide yarn in the woven fabric exhibits a formic acid relative viscosity of at least 70, a halogen:copper molar ratio of at least 2.0:1 and a sodium metal content of not more than 25 ppm.

55. The method of claim 54, comprising: The severity of the scouring process is controlled by controlling one or more of the volume, temperature, pH, residence time and nature of the alkali of the water used in the scouring process.

56. The method of claim 55, wherein: The temperature in the scouring step is lower than 95°C; and / or the final pH of the scouring bath is at least 10; and / or the residence time in the scouring bath is no more than 5 minutes / m 2 and / or the concentration of sodium ions in the scouring bath or fluid is less than 35 ppm; and / or the scouring bath contains potassium hydroxide but not sodium hydroxide.

57. The method of claim 55, wherein: The temperature in the scouring step is lower than 75°C; and / or the final pH of the scouring bath is at least 11; and / or the residence time in the scouring bath is no more than 3 minutes / m 2 and / or the concentration of sodium ions in the scouring bath or fluid is less than 10 ppm; and / or the scouring bath contains potassium hydroxide but not sodium hydroxide.

58. A method according to claim 57, wherein the residence time in the scouring bath does not exceed 2 minutes / m 2 A fabric made of scoured yarn.

59. The method of claim 54, comprising: The halogen loading in the raw yarn from which the woven fabric is made is controlled.

60. The method of claim 59, wherein: The halogen loading in the raw yarn is such that the molar ratio of halogen:copper in the raw yarn is at least 4.0:

1.

61. The method of claim 59, wherein: The halogen loading in the raw yarn is such that the molar ratio of halogen:copper in the raw yarn is at least 8.0:

1.

62. The method of claim 59, wherein: The halogen loading in the raw yarn is such that the molar ratio of halogen:copper in the raw yarn is at least 10.0:

1.

63. The method of claim 59, wherein: The halogen loading in the raw yarn is such that the molar ratio of halogen:copper in the raw yarn is at least 12.0:

1.

64. The method of claim 54, comprising: The concentration of sodium in the woven fabric is controlled by controlling the sodium content of the water supply used in the weaving and / or scouring steps.

65. The method of claim 54, comprising: The sodium concentration in the woven fabric is controlled by controlling the sodium content of the water supply by a membrane reverse osmosis system capable of rejecting at least 90% of the sodium ions in the water supply used in the weaving and / or scouring process steps.