A high-efficiency anti-fouling emulsion separation material and its preparation method and application
The material, which forms a water-oil dual-channel structure by intertwining collagen and polypropylene, solves the problem of trapped phase contamination of traditional emulsion separation materials, achieves efficient and long-term stable emulsion separation, and improves separation throughput and anti-fouling properties.
Patent Information
- Application Number
- CN202211589703.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-12
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-12
AI Technical Summary
Traditional emulsion separation materials have problems with trapped phase contamination during the separation process, resulting in reduced separation flux and performance degradation, limiting their use in practical applications.
By intertwining collagen and polypropylene to form a material with a water-oil dual channel structure, the significant difference in wettability of hydrophilic collagen and hydrophobic polypropylene is used to build a stable water and oil transmission channel to avoid the generation of trapped phases and achieve high efficiency. , long-term stable emulsion separation.
It achieves high separation efficiency and large separation flux, avoids trapped phase contamination, ensures long-term stability and anti-fouling properties of emulsion separation, and significantly enhances the application value of the material.
Smart Images

Figure CN115671797B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of emulsion separation, and in particular to a high-efficiency anti-fouling emulsion separation material and a preparation method and application thereof. Background Art
[0002] A large amount of emulsion wastewater is generated during the production and processing of industries such as oil extraction, cosmetics production, pharmaceuticals, food processing, textile dyeing and finishing, and leather manufacturing. Direct discharge without treatment poses a huge potential threat to the ecological environment and human health. Superwetting materials have extreme wettability and have completely different extreme affinities for oil and water. They only allow one phase in the emulsion to pass through while strictly rejecting the other phase. This single-channel separation strategy achieves ultra-high selectivity for emulsion separation (Wang B, Liang W, Guo Z, et al. Biomimetic super-lyophobic and super-lyophilic materials applied for oil / water separation: a new strategy beyond nature[J]. Chemical Society Reviews, 2015, 44(1): 336-361.). The separation process does not rely on pore screening mechanism and therefore has excellent separation efficiency and separation flux (Zhang W, Shi Z, Zhang F, et al. Superhydrophobic and superoleophilic PVDF membranes for effective separationof water-in-oil emulsions with high flux[J]. Advanced materials, 2013, 25(14): 2071-2076.). However, the selectively rejected trapped phase continues to accumulate on the surface of the superwetting material, greatly weakening the extreme wettability of the superwetting material and reducing the mass transfer kinetics of the permeating phase, which causes the separation flux of the superwetting material to decrease rapidly in the early stage of separation. As the separation proceeds further, the trapped phase will even form a barrier layer, preventing the surface of the superwetting material from contacting the emulsion, completely destroying the separation performance of the superwetting material. This shortcoming significantly and greatly hinders the application of superwetting materials in actual oily wastewater treatment (Tummons E, Han Q, Tanudjaja HJ, et al.Membrane fouling by emulsified oil: A review[J]. Separation and Purification Technology, 2020, 248: 116919.).
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] In order to solve the pollution problem of intercepted relative separation materials in the emulsion separation process of traditional emulsion separation materials in the background technology, the first purpose of the present invention is to provide a high-efficiency anti-fouling emulsion separation material, which has outstanding characteristics such as large separation flux, high separation efficiency, strong anti-fouling, and long-term stable separation, and has significant application value.
[0005] The second object of the present invention is to provide a method for preparing an efficient antifouling emulsion separation material, which overcomes the technical difficulty that hydrophilic collagen and hydrophobic polypropylene with opposite wettability are difficult to entangle with each other. In addition, the method has a simple preparation route, and the prepared efficient antifouling emulsion separation material retains the original wettability of hydrophilic collagen and hydrophobic polypropylene.
[0006] The third object of the present invention is to provide an application of a highly efficient anti-fouling emulsion separation material.
[0007] To achieve the above object, the first technical solution adopted by the present invention is:
[0008] The invention discloses a highly effective antifouling emulsion separation material, which is a material having a water-oil dual-channel structure formed by the mutual entanglement of collagen and polypropylene.
[0009] Preferably, the mass ratio of collagen to polypropylene is 5:1-5:7.
[0010] The high-efficiency anti-fouling emulsion separation material of the present invention utilizes hydrophilic collagen and hydrophobic polypropylene to be entangled with each other to construct an emulsion that can be efficiently demulsified, and provides a water transmission channel and an oil transmission channel for the water phase and the oil phase formed by the demulsification, respectively; at the same time, the water channel and the oil channel formed by the entanglement of hydrophilic collagen and hydrophobic polypropylene repel each other due to the significant difference in wettability between the two. This strong repulsive effect makes the water channel and the oil channel highly stable, thereby ensuring that the water phase and the oil phase formed by the subsequent demulsification and separation can transfer mass along the channels constructed by collagen and polypropylene respectively for a long time and stably without interfering with each other. No trapped phase is generated during the emulsion separation process using the separation material, and there is no trapped phase pollution problem, so the emulsion can be separated stably for a long time. Compared with traditional emulsion separation materials, the material has outstanding characteristics such as large separation flux, high separation efficiency, strong anti-fouling property, and long-term stable separation, and has significant application value.
[0011] The second technical solution adopted by the present invention is:
[0012] A method for preparing an efficient antifouling emulsion separation material comprises the following steps:
[0013] Collagen and polypropylene are placed in an organic solution, sheared and mixed at high speed, and then dried.
[0014] There is no particular limitation on the organic solvent in the present invention. Theoretically, all organic solvents can achieve the technical effect of the present invention. In the embodiment of the present invention, ethanol and N,N-dimethylformamide are preferred.
[0015] The third technical solution adopted by the present invention is:
[0016] Application of any of the above-mentioned high-efficiency anti-fouling emulsion separation materials in emulsion separation.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1. The high-efficiency anti-fouling emulsion separation material prepared by the present invention has a water-oil dual-channel structure. After the emulsion is demulsified and separated by mutually entangled collagen and polypropylene, the formed water phase and oil phase are transmitted through the water channel and oil channel constructed by hydrophilic collagen and hydrophobic polypropylene respectively, and no trapped phase is generated. The high-efficiency anti-fouling emulsion separation material avoids the generation of trapped phases and solves the problem of trapped phase contamination of materials that has long existed in traditional emulsion separation materials. The high-efficiency anti-fouling emulsion separation material can achieve long-term and stable separation of emulsions while ensuring high separation efficiency and high separation flux.
[0019] 2. The high-efficiency anti-fouling emulsion separation material prepared by the present invention does not have the problem of interception and clogging of the separation channel, and thus has the characteristic of large separation flux.
[0020] 3. The preparation method provided by the present invention overcomes the technical difficulty that two materials with significantly different wettability are difficult to entangle with each other, and has the characteristics of simple and efficient operation. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a photo of the high-efficiency antifouling emulsion separation material prepared in Example 1 of the present invention;
[0022] Figure 2 This is a photo of collagen in the highly efficient antifouling emulsion separation material prepared in Example 1 of the present invention;
[0023] Figure 3 This is a photo of the polypropylene fiber in the high-efficiency anti-fouling emulsion separation material prepared in Example 1 of the present invention;
[0024] Figure 4 , 5 6 are field emission scanning electron microscope images of the high-efficiency antifouling emulsion separation material, skin collagen and polypropylene fiber prepared in Example 1, respectively;
[0025] Figure 7 The contact angle image of the highly efficient antifouling emulsion separation material prepared in Implementation 1 is shown in 2.0 μL water in dodecane medium;
[0026] Figure 8 The contact angle image of the highly efficient antifouling emulsion separation material prepared in Implementation 1 is shown in FIG. 1 when 2.0 μL dodecane is infiltrated in water medium;
[0027] Fig. 9 This is the underwater contact angle image of 2.0 μL chloroform on the collagen surface;
[0028] Fig.10 This is the contact angle image of 2.0 μL water in air on the polypropylene surface;
[0029] Fig.11 is the particle size distribution diagram of emulsion E1;
[0030] Fig.12 This is a particle size distribution diagram of emulsion E1 after separation by the high-efficiency antifouling emulsion separation material prepared in Example 1;
[0031] Fig.13 are photos and fluorescence micrographs of emulsion E4;
[0032] Fig.14 The photograph and fluorescence micrograph of emulsion E4 after separation by the high-efficiency antifouling emulsion separation material prepared in Example 1;
[0033] Fig.15 This is a fluorescence micrograph of the high-efficiency antifouling emulsion separation material prepared in Example 1 after separating emulsion E4;
[0034] Fig.16 The relationship curve between separation efficiency, COD and time during the continuous separation of emulsions E1, E2 and E3 by the high-efficiency anti-fouling emulsion separation material prepared in Example 1 for 20 h;
[0035] Fig.17 The curve of the relationship between separation flux and time during the continuous separation of emulsions E1, E2 and E3 by the high-efficiency antifouling emulsion separation material prepared in Example 1 for 20 h;
[0036] Fig.18 This is a photograph of the mass transfer and migration of dodecane (red) in the separation material during the continuous separation of Sudan III-dyed emulsion E1 by the high-efficiency antifouling emulsion separation material prepared in Example 1;
[0037] Fig.19 This is a particle size distribution diagram of emulsion E1 after separation by the polypropylene emulsion separation material prepared in Comparative Example 2;
[0038] Fig. 20 This is the particle size distribution diagram of emulsion E1 after separation from control material-1 prepared in comparative example 3. DETAILED DESCRIPTION
[0039] The present invention is described in detail below through examples, and the technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.
[0040] It is necessary to point out here that this embodiment is only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above-mentioned invention content are also regarded as falling within the scope of protection of the present invention.
[0041] The present invention provides a high-efficiency anti-fouling emulsion separation material and a preparation method and application thereof. The specific implementation scheme is as follows:
[0042] Example 1
[0043] (1) Preparation of highly efficient antifouling emulsion separation material: 5.0 g of skin collagen and 7.0 g of polypropylene fiber were added to 200 mL of anhydrous ethanol in sequence. The mixture was stirred at 4000 rpm for 10.0 min and then placed in a perforated plate for molding. After drying at 60 °C, a highly efficient antifouling emulsion separation material was obtained.
[0044] Figure 1 This is a photo of the high-efficiency antifouling emulsion separation material prepared in this example. Figure 2 For photos of leather and glue raw materials, Figure 3 This is a photo of polypropylene fiber. Figure 4 , 5 6 are field emission scanning electron microscope images of high-efficiency antifouling emulsion separation material, collagen and polypropylene fiber respectively. Figure 4 It can be seen that skin collagen and polypropylene are entangled with each other, forming a highly efficient antifouling emulsion separation material.
[0045] After testing, the high-efficiency antifouling emulsion separation material prepared in this embodiment has unique underwater lipophilicity and oil-underwater hydrophilicity. Figure 7 As shown in FIG. 1 , in the dodecane medium, the time it takes for a 2.0 μL water droplet to completely wet the surface of the high-efficiency antifouling emulsion separation material prepared in this embodiment is 85.994 s. Figure 8 As shown in FIG. 1 , in an aqueous medium, the time it takes for a 2.0 μL dodecane droplet to completely wet the surface of the highly efficient antifouling emulsion separation material prepared in this embodiment is 9.930 s. Fig. 9 As shown in FIG. 1 , the collagen fibers used in preparing the highly effective antifouling emulsion separation material of this embodiment have underwater superoleophobicity, and the contact angle is 156°. Fig.10 As shown, the polypropylene fiber used to prepare the high-efficiency anti-fouling emulsion separation material of this embodiment has super hydrophobicity and a contact angle of 154°.
[0046] (2) Preparation of water-in-oil emulsion: 20 mL of dodecane solution was added to 2000 mL of deionized water, stirred at 3000 rpm for 1.0 h, and then ultrasonically treated for 2.0 min to obtain a water-in-dodecane emulsion, which was recorded as E1. 20 mL of kerosene was added to 2000 mL of deionized water, stirred at 3000 rpm for 1.0 h, and then ultrasonically treated for 2.0 min to obtain a water-in-kerosene emulsion, which was recorded as E2. 20 mL of n-octane solution was added to 2000 mL of deionized water, stirred at 3000 rpm for 1.0 h, and then ultrasonically treated for 2.0 min to obtain a water-in-octane emulsion, which was recorded as E3. 10 mL of 1,2-dichloroethane solution containing 0.01 g of rhodamine B was added to 100 mL of 1,2-dichloroethane solution containing 0.05 g of sodium dodecyl sulfonate (SLS) and 0.01 g of fluorescein isothiocyanate (FITC). mL of deionized water was stirred at 3000 rpm for 1.0 h to obtain a 1,2-dichloroethane-in-water emulsion stained with rhodamine B and FITC, which was recorded as E4.
[0047] (3) Separating the above-prepared emulsions using the high-efficiency anti-fouling emulsion separation material prepared in this example: 2.0 g of the high-efficiency anti-fouling emulsion separation material prepared in this example was loaded into a column, wherein the column inner diameter was 1.6 cm and the bed height was 5.0 cm. The four types of water-in-oil emulsions prepared in (2) were separated using a column separation method. A constant flow pump was used to control the emulsion inlet speed, and the filtrate was collected for analysis.
[0048] The experimental results show that the high-efficiency antifouling emulsion separation material prepared in this example exhibits excellent separation performance for the four water-in-oil emulsions (E1, E2, E3, and E4) prepared in (2), and the four emulsions become clear and transparent after separation. The particle size distribution of the obtained filtrate was measured by a dynamic light scattering particle size analyzer (DLS). Before separation, the water-in-oil emulsion E1 had a particle size distribution in the range of 301.27-341.89 nm ( Fig.11 ), while the filtrate collected after separation by the high-efficiency antifouling emulsion separation material prepared in this embodiment has no particle size distribution ( Fig.12 ). The emulsion E4 was observed under an inverted fluorescence microscope before and after separation of the high-efficiency antifouling emulsion separation material prepared in this example. Before separation, the emulsion E4 had significant fluorescence ( Fig.13 ) and the filtrate after separation has no fluorescence ( Fig.14 The separation efficiency of the high-efficiency antifouling emulsion separation material prepared in this example for three kinds of oil-in-water emulsions (E1, E2, and E3) was 99.21%, 99.14%, and 98.82%, respectively, and the separation flux was 2617.44, 2638.63, and 2716.74 L m -2 h -1The high-efficiency antifouling emulsion separation material prepared in this example has the characteristics of high separation efficiency and large flux for the separation of oil-in-water emulsion.
[0049] It is worth noting that the high-efficiency antifouling emulsion separation material prepared in this example after separation of E4 is placed under an inverted fluorescence microscope for observation, and the green fluorescence and red fluorescence partitions are clearly visible, and the formation of the two fluorescence regions is complementary ( Fig.15 ), these results show that oil and water transfer mass through their own channels inside the high-efficiency anti-fouling emulsion separation material prepared in this embodiment, and the high-efficiency anti-fouling emulsion separation material prepared in this embodiment has a unique water-oil dual-channel structure.
[0050] The high-efficiency antifouling emulsion separation material prepared in this example was used to continuously separate the three oil-in-water emulsions (E1, E2, and E3) prepared in (2) for 20 h. The relationship between the chemical oxygen demand (COD) of the filtrate, the separation efficiency, and the separation flux and time is shown in the following figure: Fig.16 , Fig.17 The experimental results show that the separation efficiency of the high-efficiency antifouling emulsion separation material prepared in this example for the three kinds of water-in-oil emulsions prepared in (2) after separation for 20 h is 99.72%, 99.79% and 99.43%, respectively, and the separation flux is 1975.52, 1851.11 and 2542.79 L m -2 h -1 , indicating that the high-efficiency anti-fouling emulsion separation material can perform long-term and stable separation of water-in-oil emulsions, and has excellent anti-fouling properties and long-term performance.
[0051] It is worth noting that during the long-term separation of the three water-in-oil emulsions prepared in (2) by the high-efficiency anti-fouling emulsion separation material prepared in this example, floating oil began to be collected in the filtrate after a certain period of separation, indicating the formation of a water-oil dual channel in the high-efficiency anti-fouling emulsion separation material. Taking the separation of E1 as an example, the distribution of Sudan III-dyed dodecane in the bed of the high-efficiency anti-fouling emulsion separation material gradually moved downward as the separation time went by until it penetrated the bed of the high-efficiency anti-fouling emulsion separation material ( Fig.18 ). These results show that the highly efficient anti-fouling emulsion separation material still retains a stable oil channel underwater, and the oil phase produced after the emulsion is demulsified is transferred in the oil channel. No trapped phase is produced in the separation process, which has solved the bottleneck problem of trapped phase pollution in the separation process of traditional emulsion separation materials.
[0052] Example 2
[0053] (1) Preparation of highly efficient antifouling emulsion separation material: 5.0 g of skin collagen and 5.0 g of polypropylene fiber were added to 200 mL of anhydrous ethanol in sequence. The mixture was stirred at 4000 rpm for 10.0 min and then placed in a perforated plate for molding. After drying at 60 °C, a highly efficient antifouling emulsion separation material was obtained.
[0054] (2) The emulsion E1 in Example 1 was separated using the high-efficiency anti-fouling emulsion separation material prepared in this example: 2.0 g of the high-efficiency anti-fouling emulsion separation material prepared in this example was loaded into a column having an inner diameter of 1.6 cm and a bed height of 5.0 cm. The emulsion E1 was separated using a column separation method. A constant flow pump was used to control the emulsion inlet speed, and the filtrate was collected for analysis.
[0055] The test results show that the high-efficiency antifouling emulsion separation material prepared in this example exhibits excellent separation performance for emulsion E1, with a separation efficiency of 99.11% and a separation flux of 2369.42 L m -2 h -1 .
[0056] Example 3
[0057] (1) Preparation of highly efficient antifouling emulsion separation material: 5.0 g of skin collagen and 3.0 g of polypropylene fiber were added to 200 mL of anhydrous ethanol in sequence. The mixture was stirred at 4000 rpm for 10.0 min and then placed in a perforated plate for molding. After drying at 60 °C, a highly efficient antifouling emulsion separation material was obtained.
[0058] (2) The emulsion E1 in Example 1 was separated using the high-efficiency anti-fouling emulsion separation material prepared in this example: 2.0 g of the high-efficiency anti-fouling emulsion separation material prepared in this example was loaded into a column having an inner diameter of 1.6 cm and a bed height of 5.0 cm. The emulsion E1 was separated using a column separation method. A constant flow pump was used to control the emulsion inlet speed, and the filtrate was collected for analysis.
[0059] The test results show that the high-efficiency antifouling emulsion separation material prepared in this example exhibits excellent separation performance for emulsion E1, with a separation efficiency of 99.40% and a separation flux of 1360.77 L m -2 h -1 .
[0060] Example 4
[0061] (1) Preparation of highly efficient antifouling emulsion separation material: 5.0 g of skin collagen and 1.0 g of polypropylene fiber were added to 200 mL of anhydrous ethanol in sequence. The mixture was stirred at 4000 rpm for 10.0 min and then placed in a perforated plate for molding. After drying at 60 °C, a highly efficient antifouling emulsion separation material was obtained.
[0062] (2) The emulsion E1 in Example 1 was separated using the high-efficiency anti-fouling emulsion separation material prepared in this example: 2.0 g of the high-efficiency anti-fouling emulsion separation material prepared in this example was loaded into a column having an inner diameter of 1.6 cm and a bed height of 5.0 cm. The emulsion E1 was separated using a column separation method. A constant flow pump was used to control the emulsion inlet speed, and the filtrate was collected for analysis.
[0063] The test results show that the high-efficiency antifouling emulsion separation material prepared in this example exhibits excellent separation performance for emulsion E1, with a separation efficiency of 99.42% and a separation flux of 931.63 L m -2 h -1 .
[0064] Example 5
[0065] (1) Preparation of highly efficient antifouling emulsion separation material: 5.0 g of skin collagen and 7.0 g of polypropylene fiber were added to 200 mL of N,N-dimethylformamide. The mixture was stirred at 4000 rpm for 10.0 min and then placed in a perforated plate for molding. After drying at 60 °C, a highly efficient antifouling emulsion separation material was obtained.
[0066] (2) The emulsion E1 in Example 1 was separated using the high-efficiency anti-fouling emulsion separation material prepared in this example: 2.0 g of the high-efficiency anti-fouling emulsion separation material prepared in this example was loaded into a column having an inner diameter of 1.6 cm and a bed height of 5.0 cm. The emulsion E1 was separated using a column separation method. A constant flow pump was used to control the emulsion inlet speed, and the filtrate was collected for analysis.
[0067] The test results show that the high-efficiency antifouling emulsion separation material prepared in this example exhibits excellent separation performance for emulsion E1, with a separation efficiency of 99.37% and a separation flux of 2536.12 L m -2 h -1 .
[0068] Comparative Example 1
[0069] (1) Preparation of skin collagen emulsion separation material: 5.0 g of skin collagen was added to 200 mL of anhydrous ethanol, stirred at 4000 rpm for 10.0 min, and then placed in a perforated plate for molding. After drying at 60°C, the skin collagen emulsion separation material was obtained.
[0070] (2) The emulsion E1 prepared in Example 1 was separated using the skin collagen emulsion separation material prepared in this comparative example: 2.0 g of the skin collagen emulsion separation material prepared in this comparative example was loaded into a column having an inner diameter of 1.6 cm and a bed height of 5.0 cm. The emulsion E1 was separated using a column separation method. A constant flow pump was used to control the emulsion inlet speed, and the filtrate was collected for analysis.
[0071] The test results show that the separation efficiency of the collagen emulsion separation material prepared in this comparative example for emulsion E1 is 99.43%, and the separation flux is 340.19 L m -2 h -1 However, after 2.0 h of continuous separation, the separation flux decreased to 113.40 Lm -2 h -1 , which indicates that the skin collagen emulsion separation material cannot achieve high-throughput stable separation.
[0072] Comparative Example 2
[0073] (1) Preparation of polypropylene emulsion separation material: 5.0 g of polypropylene fiber was added to 200 mL of anhydrous ethanol, stirred at 4000 rpm for 10.0 min, and then placed in a perforated plate for molding. After drying at 60 °C, the polypropylene emulsion separation material was obtained.
[0074] (2) The emulsion E1 in Example 1 was separated using the polypropylene emulsion separation material prepared in this comparative example: 2.0 g of the polypropylene emulsion separation material prepared in this comparative example was loaded into a column having an inner diameter of 1.6 cm and a bed height of 5.0 cm. The emulsion E1 was separated using a column separation method. A constant flow pump was used to control the emulsion inlet speed, and the filtrate was collected for analysis.
[0075] The particle size distribution of the obtained filtrate was measured by DLS. After the emulsion E1 was separated by the polypropylene emulsion separation material prepared in this comparative example, there were still particles with a diameter in the range of 186.03-207.13 nm ( Fig.19 ), which indicates that the polypropylene emulsion separation material cannot effectively separate emulsion E1.
[0076] Comparative Example 3
[0077] (1) Preparation of control material-1: 1.0 g of dermal collagen and 5.0 g of polypropylene fiber were added to 200 mL of anhydrous ethanol in sequence. The mixture was stirred at 4000 rpm for 10.0 min and then placed in a perforated plate for molding. After drying at 60°C, control material-1 was obtained.
[0078] (2) Using the control material-1 prepared in this comparative example to separate the emulsion E1 in Example 1: 2.0 g of the control material-1 prepared in this comparative example was loaded into a column having an inner diameter of 1.6 cm and a bed height of 5.0 cm. The emulsion E1 was separated by a column separation method. A constant flow pump was used to control the emulsion inlet speed, and the filtrate was collected for analysis.
[0079] The particle size distribution of the obtained filtrate was measured by DLS. After the emulsion E1 was separated by the control material-1 prepared in this comparative example, there were still particles with a diameter in the range of 142.92-207.13 nm ( Fig. 20 ), which indicates that Control Material-1 cannot effectively separate Emulsion E1.
[0080] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the above embodiments, it should be understood by those skilled in the art that the technical solutions described in the above embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A highly efficient antifouling emulsion separation material, characterized in that: The material having a water-oil double channel structure is formed by irregular entanglement of skin collagen and polypropylene; the mass ratio of the skin collagen to the polypropylene is 5:1-5:
7.
2. A method for preparing the high-efficiency antifouling emulsion separation material according to claim 1, characterized in that: The following steps are involved: The collagen and polypropylene are placed in an organic solution and mixed at high speed by shearing, and then dried.
3. Use of the high-efficiency anti-fouling emulsion separation material as claimed in claim 1 in emulsion separation.
Citation Information
Patent Citations
Preparation and application of underwater super-oleophobic and under-oil hydrophilic emulsion separation functional fibers
CN112095337A
Sorbent for collecting oil and oil products and method of its production
RU2461421C1
Method and device for deep oil removal from wastewater containing low concentration dirty oil
US20170088441A1