A method for preparing heat-resistant and aging-resistant degradable aliphatic polyester
By performing prepolymerization and final polymerization in a static mixer and combined with negative pressure heating treatment, the problems of cyclic ester monomer residue and high temperature polymerization are solved, and the molecular weight distribution and material properties of the degradable aliphatic polyester are improved, thus achieving the Improved heat aging resistance and mechanical strength.
Patent Information
- Application Number
- CN202110850638.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-07-27
AI Technical Summary
In the preparation of degradable aliphatic polyesters, the residue of cyclic ester monomers and high-temperature polymerization leads to a decline in material properties, affecting the mechanical strength and aging resistance, and the high-temperature polymerization process consumes energy and widens the molecular weight distribution, limiting the material. scope of application and service life.
Prepolymerization and final polymerization are carried out using a static mixer, combined with negative pressure heating treatment, and the activation energy of ring-opening polymerization is reduced through reaction aids such as catalysts, polyols and dehydrating agents, reducing the residue of cyclic ester monomers, and promoting polymerization through tackification equipment. The preparation of polyhydroxycarboxylic acids with high molecular weight and narrow molecular weight distribution is achieved.
It effectively reduces the residue of cyclic ester monomers, avoids high-temperature polymerization, improves the molecular weight and molecular weight distribution uniformity of polyester, improves the mechanical strength and heat-resistant aging performance of the material, reduces energy consumption, and expands the application range of the material.
Smart Images

Figure BDA0003182352570000091 
Figure BDA0003182352570000101 
Figure BDA0003182352570000111
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer preparation, and in particular to a method for preparing heat-resistant, aging-resistant and degradable aliphatic polyester. Background Art
[0002] Degradable aliphatic polyesters, such as polyglycolic acid, polylactic acid, polyglycolic acid-lactic acid copolymers, etc., can be decomposed by microorganisms or enzymes existing in the soil, rivers or seas, and therefore, they have attracted much attention as biodegradable polymer materials with low environmental load. Degradable aliphatic polyesters can be synthesized by dehydration polycondensation of α-hydroxycarboxylic acids such as glycolic acid and lactic acid, but the polymer obtained by direct dehydration polycondensation has a low molecular weight and poor melt processing strength. In order to efficiently synthesize polymers with higher molecular weights, dimeric cyclic esters of α-hydroxycarboxylic acids can be synthesized first, and then the cyclic esters can be ring-opened polymerized. For example, glycolide of dimeric cyclic esters of glycolic acid can be ring-opened polymerized to prepare high molecular weight polyglycolic acid, or lactide of dimeric cyclic esters of lactic acid can be ring-opened polymerized to prepare high molecular weight polylactic acid. However, in the ring-opening polymerization process of cyclic esters, unreacted cyclic ester monomers will inevitably remain in the final polyester product. These residual monomers will induce side reactions such as thermal degradation of the polymer under the influence of high temperature during the subsequent polyester melt molding process, which will seriously affect the performance of the final material (such as mechanical strength, aging resistance, etc.). In addition, the existing reactive extrusion equipment (such as reactive twin-screw extruder) for preparing aliphatic polyesters such as polyglycolic acid usually requires the glycolide to be polymerized at a higher reaction temperature (such as 220-240° C.) in actual application to obtain a product with a higher molecular weight. However, a higher reaction temperature not only means high energy consumption, but also easily leads to a greater degree or serious thermal degradation of the generated polyglycolic acid, which is not conducive to the improvement of the molecular weight of the final product, and also causes the molecular weight distribution of the final product to become wider, which has an adverse effect on the mechanical properties and aging resistance of the material, not only increasing the uncertainty of the material life cycle, but also greatly limiting the application range and service life of the material.
[0003] Therefore, there is an urgent need in the art to provide a method for preparing a degradable aliphatic polyester that can effectively reduce residual cyclic ester monomers and avoid high-temperature polymerization. Summary of the invention
[0004] The present invention aims to provide a method for preparing degradable aliphatic polyester.
[0005] The present invention provides a method for preparing a heat-resistant and ageing-resistant degradable aliphatic polyester, the method comprising the steps of:
[0006] (1) prepolymerizing a molten material of a cyclic ester monomer in a static mixer to obtain a hydroxycarboxylic acid prepolymer;
[0007] (2) subjecting the hydroxycarboxylic acid prepolymer to final polymerization through a viscosity increasing device, and granulating to obtain granulated polyhydroxycarboxylic acid; and
[0008] (3) subjecting the granulated polyhydroxycarboxylic acid to negative pressure heating treatment to obtain a heat-resistant, aging-resistant, and degradable aliphatic polyester.
[0009] In another embodiment, the molten material of the cyclic ester monomer in step (1) contains a reaction aid, and the reaction aid includes a catalyst, a polyol and a dehydrating agent.
[0010] In another embodiment, based on the mass of the cyclic ester monomer, the amount of the catalyst is 0.001-1 wt %, the amount of the polyol is 0.01-0.1 wt %, and the amount of the dehydrating agent is 0.1-2 wt %.
[0011] In another embodiment, the catalyst is selected from at least one of tin compounds, antimony compounds or zinc compounds; the dehydrating agent is selected from at least one of carbodiimide, polycarbodiimide or carbodiimide-based compounds.
[0012] In another embodiment, the polyol is selected from at least one of 1,4-butanediol, glycerol, pentaerythritol, xylitol, sorbitol, 1,6-hexanediol, triethylene glycol and dipropylene glycol.
[0013] In another embodiment, the static mixer used in step (1) adopts at least two stages of gradient temperature increase, the temperature range of the first stage is between 120-180°C, and the temperature range of the last stage is between 180-200°C.
[0014] In another embodiment, the temperature of the second section of the static mixer is 10-80° C. higher than that of the first section; and the temperature of the last section is 0-20° C. higher than that of the previous adjacent section.
[0015] In another embodiment, the viscosity increasing device in step (2) is devolatilized at an absolute pressure of ≤500 Pa and a temperature of 220-250°C.
[0016] In another embodiment, the particle size of the granulated polyhydroxycarboxylic acid obtained in step (2) is ≤10 mm.
[0017] In another embodiment, the negative pressure heating treatment in step (3) is performed under conditions of absolute pressure ≤ 1 kPa and temperature of 100-220°C.
[0018] Accordingly, the present invention provides a method for preparing a degradable aliphatic polyester which can effectively reduce residual cyclic ester monomers and avoid high-temperature polymerization. DETAILED DESCRIPTION
[0019] After extensive and in-depth research, the inventors conducted the polymerization reaction in a static mixer, which minimized the influence of oxygen and moisture on the polymerization reaction and enabled the molecular chain to maintain stable growth for a longer time in the polymerization reaction; the activation energy of the ring-opening polymerization reaction of the cyclic ester monomer was reduced by compounding the catalyst with the polyol and the dehydrating agent to form a reaction aid, so that the ring-opening polymerization reaction of the cyclic ester could occur in the reaction system at a relatively low temperature to generate polyhydroxycarboxylic acid with a high molecular weight and a relatively narrow molecular weight distribution, and was conducive to reducing the content of residual cyclic ester monomers in the polyhydroxycarboxylic acid product; finally, the polyhydroxycarboxylic acid obtained by final polymerization through a viscosity increasing device was granulated and then subjected to negative pressure heating treatment, and the residual cyclic ester monomers were removed from the product particles in time under the action of negative pressure, which could further reduce the content of residual cyclic ester monomers in the polyhydroxycarboxylic acid product. On this basis, the present invention was completed.
[0020] definition
[0021] The "viscosity-increasing device" in the present invention plays a devolatilization role, which can promote the further polymerization of the hydroxycarboxylic acid prepolymer and remove the generated small molecules from the system in time, so that the molecular weight of the polymer is further improved, and the corresponding polymer viscosity will also be further increased; the "viscosity-increasing device" in the present invention can be, for example but not limited to, a twin-screw extruder with only a devolatilization section.
[0022] As used in the present invention, "cyclic ester monomer" refers to a cyclic ester or lactone between two molecules of an α-hydroxycarboxylic acid, such as, but not limited to, glycolide, a cyclic ester between two molecules of glycolic acid, lactide, a cyclic ester between two molecules of lactic acid, β-butyrolactone, δ-valerolactone, ε-caprolactone, etc., or a mixture of two or more thereof.
[0023] As used herein, "hydroxycarboxylic acid" refers to α-hydroxycarboxylic acids, such as, but not limited to, glycolic acid, lactic acid, α-hydroxybutyric acid, α-hydroxyvaleric acid, α-hydroxycaproic acid, and the like.
[0024] As used in the present invention, "polyhydroxycarboxylic acid" refers to a polymer prepared by ring-opening polymerization of cyclic ester and / or lactone monomers, such as but not limited to polyglycolic acid, polylactic acid, polyglycolic acid-lactic acid copolymer, polyε-caprolactone, polyglycolic acid-ε-caprolactone copolymer, etc.
[0025] Preparation method
[0026] The present invention provides a method for preparing a heat-resistant and ageing-resistant degradable aliphatic polyester, comprising the steps of:
[0027] The first step is to add the cyclic ester monomer into a melting mixing kettle, and after the cyclic ester monomer is completely melted, add a reaction aid into the melting mixing kettle to mix the molten cyclic ester monomer and the reaction aid uniformly to obtain a molten material of the cyclic ester monomer;
[0028] The second step is to introduce the molten material of the cyclic ester monomer into a static mixer for prepolymerization to obtain a hydroxycarboxylic acid prepolymer;
[0029] The third step is to subject the hydroxycarboxylic acid prepolymer to final polymerization in a viscosity increasing device to generate polyhydroxycarboxylic acid, and the granulated polyhydroxycarboxylic acid obtained by granulation is subjected to negative pressure heating treatment to obtain the product of the present invention, namely, heat-resistant and aging-resistant degradable aliphatic polyester.
[0030] In the first step, the purity of the cyclic ester monomer used is not less than 98%, preferably not less than 98.5%, and the acidity is not more than 20 mmol / kg. In one embodiment of the present invention, glycolide is used in the first step.
[0031] In the first step, the melting temperature is selected according to the cyclic ester monomer. In one embodiment of the present invention, glycolide is completely melted at 90-120°C.
[0032] The reaction aid used in the first step comprises a catalyst, a polyol and a dehydrating agent; in terms of the amount of the reaction aid, the amount of the catalyst is about 0.001-1wt% of the mass of the cyclic ester monomer, the amount of the polyol is about 0.01-0.1wt% of the mass of the cyclic ester monomer, and the amount of the dehydrating agent is about 0.1-2wt% of the mass of the cyclic ester monomer.
[0033] The catalyst may be selected from at least one of tin compounds, antimony compounds or zinc compounds, such as but not limited to stannous octoate, stannous chloride, tin lactate, antimony trioxide, diethyl zinc or zinc acetate dihydrate.
[0034] The polyol may be selected from one or more of 1,4-butanediol, glycerol, pentaerythritol, xylitol, sorbitol, 1,6-hexanediol, triethylene glycol and dipropylene glycol.
[0035] The dehydrating agent may be selected from carbodiimide, polycarbodiimide or carbodiimide-based compounds (such as but not limited to N,N′-diisopropylcarbodiimide, dicyclohexylcarbodiimide, etc.).
[0036] In order to prevent the local concentration of the reaction aid in the molten glycolide from being too high, in one embodiment of the present invention, the reaction aid can be added dropwise into the molten mixing kettle by injection.
[0037] As an embodiment, the molten material of the cyclic ester monomer described in the first step can be obtained by the following method: introducing the cyclic ester monomer into a molten mixing kettle, heating it to make it completely melted, and then adding a reaction aid to the molten mixing kettle while stirring, so that the molten cyclic ester monomer and the reaction aid are evenly mixed.
[0038] The static mixer in the second step adopts at least 2 stages of gradient temperature increase, for example, 2-10 stages of gradient temperature increase; preferably 3-7 stages.
[0039] In one embodiment of the present invention, the temperature range of the first section of the static mixer is between 120-180°C, such as but not limited to 140-170°C, 150-180°C, etc.; the temperature range of the last section is between 180-200°C, such as but not limited to 180-190°C, 190-200°C, etc.
[0040] In one embodiment of the present invention, the temperature of the second section of the static mixer is increased by 10-80°C than that of the first section, such as but not limited to 40-50°C, 20-70°C, 30-60°C, etc.; the temperature of the last section is increased by 0-20°C than that of the previous adjacent section, such as but not limited to 0-15°C, 5-10°C, etc.
[0041] In one embodiment of the present invention, the static mixer is provided with three sections, the temperature of the first section is set at 120-180°C, the temperature of the second section is set at 180-190°C, and the temperature of the third section is set at 190-200°C.
[0042] In one embodiment of the present invention, the static mixer has four sections, the temperature of the first section is set at 120-150°C, the temperature of the second section is set at 150-180°C, the temperature of the third section is set at 180-190°C, and the temperature of the fourth section is set at 190-200°C.
[0043] In one embodiment of the present invention, the static mixer is provided with five sections, the temperature of the first section is set at 120-150°C, the temperature of the second section is set at 150-170°C, the temperature of the third section is set at 170-180°C, the temperature of the fourth section is set at 180-190°C, and the temperature of the fifth section is set at 190-200°C.
[0044] In one embodiment of the present invention, under working conditions, the total time that the material stays in the static mixer is generally not more than 150 minutes, for example but not limited to, 60-90 minutes.
[0045] The weight average molecular weight of the hydroxycarboxylic acid prepolymer obtained in the second step is about 50,000 to 150,000.
[0046] In the third step, the viscosity increasing device may be, for example, a twin-screw extruder provided only with a devolatilization section, and the final polymerization conditions are an absolute pressure of ≤500Pa and a temperature of 220-250°C for devolatilization to remove the residual cyclic ester monomers, so that the content of the residual cyclic ester monomers is reduced to 0.3-1wt% (calculated by dividing the mass of glycolide remaining in the polymer obtained by the final polymerization by the mass of the polymer obtained by the final polymerization).
[0047] It should be noted that the viscosity increasing device in the present invention plays a devolatilization role, which can promote the further polymerization of the hydroxycarboxylic acid prepolymer and remove the generated small molecules from the system in time, so that the molecular weight of the polymer can be further increased.
[0048] In the third step, conventional methods in the art may be used for granulation, such as, but not limited to, conventional extrusion granulation, underwater pelletizing, and the like.
[0049] In one embodiment of the present invention, the particle size of the granulated polyhydroxycarboxylic acid in the third step is ≤10 mm.
[0050] In one embodiment of the present invention, the granulated polyhydroxycarboxylic acid in the third step is subjected to negative pressure heating in a vacuum pressure vessel (such as but not limited to a vacuum pressure tank, etc.), and the negative pressure heating conditions are: controlling the absolute pressure ≤ 1 kPa and the temperature to be 100-220°C.
[0051] The molecular weight distribution index of the heat-aging-resistant degradable aliphatic polyester prepared by the method of the present invention is no more than about 1.6, for example but not limited to, about 1.2-1.5.
[0052] The heat-aging-resistant and degradable aliphatic polyester product prepared by the method of the present invention has a residual cyclic ester monomer content of no more than 0.1 wt % based on the total mass of the product.
[0053] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0054] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0055] In this article, all features defined in the form of numerical ranges or percentage ranges, such as values, quantities, contents and concentrations, are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0056] As used herein, when the term "about" is used to modify a numerical value, it indicates an error tolerance of measurement within ±5% of the numerical value.
[0057] The above-mentioned features mentioned in the present invention or the features mentioned in the embodiments can be combined in any way. All the features disclosed in the specification of this case can be used in combination with any combination form. As long as there is no contradiction in the combination of these features, all possible combinations should be considered to be within the scope of this specification. Each feature disclosed in the specification can be replaced by any alternative feature that can provide the same, equal or similar purpose. Therefore, unless otherwise specified, the disclosed features are only general examples of equal or similar features.
[0058] The main advantages of the present invention are:
[0059] 1. The present invention couples a melt mixing kettle with a static mixer, firstly mixes the cyclic ester (such as glycolide) and the reaction aid uniformly through the melt mixing kettle to obtain a premix, and then introduces the premix into the static mixer for prepolymerization, creatively utilizing efficient mixing to achieve low shear and high dispersion of the premix, which is beneficial to preventing and eliminating heat accumulation in local areas of the material, and effectively preventing the occurrence of side reactions such as excessively high temperatures in local areas and thermal degradation caused by uneven heating in the material, thereby ensuring that the cyclic ester (such as glycolide) can undergo a good prepolymerization reaction to obtain a hydroxyl radical with a certain molecular weight. Carboxylic acid prepolymer (such as glycolic acid prepolymer), and then introducing hydroxycarboxylic acid prepolymer (such as glycolic acid prepolymer) into a viscosity increasing device (such as a twin-screw extruder with only a devolatilization section) for final polymerization can effectively shorten the time that the material is subjected to high shear in the viscosity increasing device, which is not only beneficial to inhibiting the occurrence of side reactions such as thermal degradation, but also beneficial to inhibiting the occurrence of ester exchange reactions, thereby reducing the content of oligomers and / or low molecular weight chain substances in the system. The obtained polyhydroxycarboxylic acid (such as polyglycolic acid) can not only have a significantly improved molecular weight, but also a relatively small molecular weight distribution index and a more uniform molecular weight distribution.
[0060] 2. The present invention introduces a molten fluid premix of cyclic ester (e.g. glycolide) into a static mixer, and uses a cross-flow method to strengthen the mixing effect between the cyclic ester (e.g. glycolide) and the reaction aid, so that the reaction aid can be more evenly dispersed in the reaction system. At the same time, a gradient heating method is used to firstly induce the ring-opening polymerization reaction of the cyclic ester (e.g. glycolide) at a relatively low temperature and in a relatively short time, and then the temperature is appropriately increased and the time is appropriately extended to form a relatively stable and reactive hydroxycarboxylic acid molecular chain (e.g. glycolic acid molecular chain) in the reaction system, and then the hydroxycarboxylic acid molecular chain (e.g. glycolic acid molecular chain) is further promoted to grow at a relatively high temperature and in a relatively long time to obtain a hydroxycarboxylic acid prepolymer (e.g. glycolic acid prepolymer) with a certain molecular weight. The gradient heating process of the static mixer is conducive to suppressing the rapid change of the viscosity of the reaction system, and can effectively avoid the occurrence of excessive heat accumulation and coking and slagging due to the rapid change of the local viscosity of the reaction system.
[0061] 3. In the aspect of reaction aids, the present invention compounded the catalyst with the polyol and the dehydrating agent, wherein the introduction of the polyol is conducive to reducing the activation energy of the ring-opening polymerization reaction of the cyclic ester (such as glycolide), so that the reaction system can undergo the ring-opening polymerization reaction of the cyclic ester (such as glycolide) at a relatively low temperature (compared with the usual temperature of 220-230° C. for the ring-opening polymerization of glycolide) to generate polyhydroxycarboxylic acid (such as polyglycolic acid) with a high molecular weight and a narrow molecular weight distribution, which is conducive to improving the monomer conversion rate, and can effectively reduce the polymerization energy consumption, and realize low carbonization generation. Moreover, the relatively low polymerization reaction temperature is conducive to reducing or inhibiting the thermal degradation degree of the polyhydroxycarboxylic acid (such as polyglycolic acid) generated during the polymerization process, so that the finally obtained polyhydroxycarboxylic acid (such as polyglycolic acid) has good mechanical strength and heat aging resistance.
[0062] 4. The main polymerization reaction of the present invention is carried out in a static mixer. Compared with the twin-screw extruder in the dynamic mixing category, the static mixer has better air tightness and can minimize the influence of oxygen and moisture on the polymerization reaction. In addition, the present invention utilizes the good uniform heat transfer effect of the static mixer to enable the molecular chain in the polymerization reaction to maintain stable growth for a longer time. However, in the reactive twin-screw extruder, the local temperature of the reaction system caused by the high shearing effect rises too fast, and it is more likely to cause side reactions such as thermal degradation in advance, which is not conducive to the increase of the molecular weight of the final product and will also cause the molecular weight distribution of the final product to become wider, which will have a negative impact on the processing of the material and its mechanical properties and heat aging resistance.
[0063] 5. In the present invention, the polyhydroxycarboxylic acid (e.g., polyglycolic acid) obtained by final polymerization in a viscosity increasing device (e.g., a twin-screw extruder with only a devolatilization section) is granulated and then subjected to negative pressure heating treatment. The residual monomers (e.g., residual glycolide) in the product particles are heated and removed from the product particles in a timely manner under the action of negative pressure, thereby obtaining a granulated polyhydroxycarboxylic acid product with the residual monomers (e.g., residual glycolide) reduced as much as possible, which is beneficial to further improve the heat aging resistance of the material.
[0064] 6. The device provided by the present invention is suitable for industrial scale-up production, and existing production equipment can be used to transform the production line. It has good flexibility and applicability, and can achieve stable output of polyhydroxycarboxylic acid (such as polyglycolic acid) products, realize low-carbon production, and has good economic benefits.
[0065] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods for which specific conditions are not specified in the following examples are usually performed under normal conditions or according to the conditions recommended by the manufacturer. Unless otherwise specified, all percentages, ratios, proportions, or parts are by weight. The units in the weight volume percentages in the present invention are well known to those skilled in the art, for example, refer to the weight (grams) of the solute in 100 ml of solution. Unless otherwise defined, all professional and scientific terms used in the text have the same meaning as those familiar to those skilled in the art. In addition, any method and material similar or equivalent to the recorded content can be applied to the method of the present invention. The preferred implementation methods and materials described in the text are for demonstration purposes only.
[0066] The cyclic ester reaction materials (eg glycolide) used in the following examples can be measured for glycolide content by gas chromatography known in the art, and the acidity by potentiometric titration known in the art (eg, using an automatic potentiometric titrator).
[0067] The content of residual monomer (i.e. glycolide) in the obtained polyglycolic acid is determined by the following method:
[0068] About 300 mg of the sample was dissolved in about 6 g of dimethyl sulfoxide (DMSO) at 150°C for about 10 min, cooled to room temperature, and then filtered. A certain amount of internal standard 4-chlorobenzophenone and acetone were added to the filtrate. 2 μl of the solution was measured and injected into a gas chromatograph for measurement.
[0069] As used herein, "distribution index" is a parameter D that represents the width of molecular weight distribution, D = M(w) / M(n), where M(w) is the weight average molecular weight, M(n) is the number average molecular weight, and when D = 1, it is a polymer with uniform molecular weight. The larger the value of D is than 1, the wider the molecular weight distribution is, and the greater the degree of polydispersity is. The determination method generally adopts gel permeation chromatography (GPC) to measure the M(w) and M(n) of the sample, and then calculates the ratio of the two.
[0070] The molecular weight and distribution of polyglycolic acid were tested by gel permeation chromatography (GPC), as follows:
[0071] Take 0.2g PGA sample, dissolve it in 100mL hexafluoroisopropanol solution with a sodium trifluoroacetate content of 5mmol / L, filter it through a polytetrafluoroethylene filter membrane with a pore size of 0.4μm, take 20μL and add it to the "LC-20AD GPC" injector made by Shimadzu (Japan), test conditions: column temperature 40℃; eluent: hexafluoroisopropanol dissolved with 5mmol / L sodium trifluoroacetate; flow rate 1mL / min; detector: RI detector; calibration: use five different standard polymethyl methacrylates with molecular weights ranging from 7000 to 200000 for molecular weight calibration.
[0072] The following Examples 1-6 are described by taking the preparation of polyglycolic acid as an example, and the preparation method is as follows:
[0073] Step 1): glycolide (D 90 ≤200 μm, purity ≥98.5%, acidity ≤20 mmol / kg) is added into a melt mixing kettle, heated at 90-120° C. to completely melt it, then a reaction aid is added into the melt mixing kettle while stirring, so that the molten cyclic ester and the reaction aid are evenly mixed to obtain a molten material of glycolide, and the molten material of glycolide is introduced into a static mixer for prepolymerization to obtain a glycolic acid prepolymer with a certain molecular weight;
[0074] Step 2): The glycolic acid prepolymer obtained in step 1) is subjected to final polymerization in a viscosity increasing device, and the generated polyglycolic acid is subjected to conventional extrusion granulation to obtain granular polyglycolic acid with a particle size of ≤10 mm, which is then subjected to negative pressure heating treatment.
[0075] In the above step 1), in order to prevent the local concentration of the reaction aid in the molten glycolide from being too high, the reaction aid can be added dropwise into the molten mixing kettle by injection.
[0076] The addition amount of the reaction aid in Example 1-6 is shown in the following Table 1-1.
[0077] Table 1-1
[0078]
[0079] The types of reaction aids selected in Examples 1-6 are shown in Table 1-2 below.
[0080] Table 1-2
[0081]
[0082] The heating temperatures of the melt mixing kettle in Examples 1-6 are shown in Table 1-3 below.
[0083] Table 1-3
[0084] project Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Temperature(℃) Approx. 90 Approx. 110 Approx. 120 Approx. 115 Approx. 118 Approx. 106
[0085] Note: The time from each batch of glycolide powder entering the melting mixer to obtaining the premix is about 20 minutes.
[0086] The temperature parameters of each section in the static mixer in Examples 1-6 are shown in Table 2-1 below:
[0087] Table 2-1
[0088] project Static mixer Paragraph 1 Paragraph 2 Paragraph 3 Paragraph 4 Paragraph 5 Example 1 Three sections About 120℃ About 180℃ About 190℃ / / Example 2 Three sections About 178℃ About 190℃ About 200℃ / / Example 3 Four sections About 120℃ About 150℃ About 180℃ About 198℃ / Example 4 Four sections About 150℃ About 160℃ About 190℃ About 200℃ / Example 5 Five sections About 125℃ About 165℃ About 175℃ About 180℃ About 195℃ Example 6 Five sections About 152℃ About 170℃ About 180℃ About 190℃ About 200℃
[0089] The time required for the material in the static mixer to pass through each section in Examples 1-6 is shown in Table 2-2 below:
[0090] Table 2-2
[0091] project Static mixer Paragraph 1 Paragraph 2 Paragraph 3 Paragraph 4 Paragraph 5 Example 1 Three sections About 5 minutes About 15 minutes About 70 minutes / / Example 2 Three sections About 5 minutes About 15 minutes About 70 minutes / / Example 3 Four sections About 5 minutes About 10 minutes About 15 minutes About 60 minutes / Example 4 Four sections About 5 minutes About 10 minutes About 15 minutes About 60 minutes / Example 5 Five sections About 5 minutes About 5 minutes About 10 minutes About 15 minutes About 55 minutes Example 6 Five sections About 5 minutes About 5 minutes About 10 minutes About 15 minutes About 55 minutes
[0092] The viscosity increasing equipment used in Examples 1-6 is a twin-screw extruder provided with only a devolatilization section, and the parameter settings of the devolatilization section are shown in Table 3-1 below:
[0093] Table 3-1
[0094] project Temperature(℃) Absolute pressure(Pa) Screw aspect ratio Screw speed (r / min) Example 1 Approx. 220 Approx. 200 55 30 Example 2 Approx. 228 Approx. 120 50 45 Example 3 Approx. 230 Approx. 150 50 40 Example 4 Approx. 236 Approx. 250 55 35 Example 5 Approx. 250 Approx. 500 60 50 Example 6 Approx. 240 Approx. 100 50 45
[0095] Note: The time for the material to pass through the devolatilization section of the viscosity increasing equipment is controlled to be about 15 minutes
[0096] The residual glycolide monomer content of the polyglycolic acid produced by the final polymerization in the viscosity increasing device in Example 1-6 is shown in Table 3-2 below: (the content is based on the total mass of the polyglycolic acid obtained by the final polymerization)
[0097] Table 3-2
[0098]
[0099] The process parameters of the negative pressure heating treatment in Examples 1-6 are shown in Table 4 below:
[0100] Table 4
[0101]
[0102] The weight average molecular weight of the glycolic acid prepolymer formed by the static mixer in Examples 1-6, the number average molecular weight, weight average molecular weight, molecular weight distribution index and residual glycolide content of the polyglycolic acid finally obtained are shown in Table 5 below:
[0103] Table 5
[0104]
[0105] Comparative Example 1
[0106] This comparative example is basically the same as Example 6, except that the reaction aid used only includes a catalyst (i.e., stannous octoate and antimony trioxide are mixed in a mass ratio of 2:1), and the amount of the catalyst used is the same as that in Example 6.
[0107] Comparative Example 2
[0108] This comparative example is basically the same as Example 6, except that the reaction aid used only includes a catalyst (i.e., a mixture of stannous octoate and antimony trioxide in a mass ratio of 2:1) and a dehydrating agent (i.e., carbodiimide), and the amounts of the catalyst and the dehydrating agent are the same as those in Example 6.
[0109] Comparative Example 3
[0110] This comparative example is basically the same as Example 6, except that no negative pressure heating treatment is performed, and the rest is the same as Example 6.
[0111] Comparative Example 4
[0112] This comparative example uses glycolide powder (D 90 ≤200 μm, purity ≥98.5%, acidity ≤20 mmol / kg), polyglycolic acid was prepared by a conventional reactive twin-screw extruder (without using a static mixer), the reaction aids used and their amounts were the same as in Example 6, and the polyglycolic acid pellets (particle size ≤10 mm) obtained by the reactive twin-screw extruder were treated at an absolute pressure of 100 Pa and 218° C. for 3 h.
[0113] In this comparative example, the specific process conditions of the reactive twin-screw extruder are shown in Table 6-1 below.
[0114] Table 6-1
[0115]
[0116] Note: In Comparative Example 4, glycolide powder and reaction aid were added from the beginning of the first section of the mixing section, and the absolute pressure of the devolatilization section was controlled to be 100P. a
[0117] Comparative Example 5
[0118] This comparative example uses glycolide powder (D 90 ≤200 μm, purity ≥98.5%, acidity ≤20 mmol / kg), polyglycolic acid was prepared by a conventional reactive twin-screw extruder (without using a static mixer), wherein the reaction aid used only contained a catalyst (i.e., stannous octoate and antimony trioxide were mixed in a mass ratio of 2:1), and the amount of the catalyst was the same as that in Example 6, and the polyglycolic acid pellets (particle size ≤10 mm) obtained by the reactive twin-screw extruder were treated at an absolute pressure of 100 Pa and 218° C. for 3 h.
[0119] In this comparative example, the specific process conditions of the reactive twin-screw extruder are shown in Table 6-2 below.
[0120] Table 6-2
[0121]
[0122] Note: In Comparative Example 5, glycolide powder and reaction aid were added from the beginning of the first section of the mixing section, and the absolute pressure of the devolatilization section was controlled to be 100P. a
[0123] In the above comparative examples 4 and 5, the screw aspect ratios and screw speeds of each section in the conventional reactive twin-screw extruder are shown in Table 6-3 below.
[0124] Table 6-3
[0125] project Screw length-diameter ratio of mixing section Screw aspect ratio in the reaction section Screw length-diameter ratio of devolatilization section <![CDATA[Screw rotation speed ( r / m i n )]]> Reactive twin screw extruder 35 70 54 45
[0126] The number average molecular weight, weight average molecular weight, molecular weight distribution index and residual glycolide content of the polyglycolic acid obtained in the above Comparative Examples 1-5 are shown in Table 7 below.
[0127] Table 7
[0128]
[0129] Performance Testing
[0130] The tensile strength and elongation at break of the PGA prepared in Examples 1-6 and Comparative Examples 1-5 were measured according to the GB / T 1040.1-2006 test standard. The specific test results are shown in Table 8 below:
[0131] Table 8 Test results
[0132]
[0133] Note: The tensile speed in the above tensile test is 50 mm / min
[0134] Based on the test results in Table 8 above, the data of Example 6 and Comparative Examples 1-5 are compared. As shown in Table 8, the tensile strength and elongation at break of the polyglycolic acid material obtained in Example 6 decreased by about 4.7% and 12.5% respectively after the hot air aging test. The tensile strength and elongation at break of the polyglycolic acid material obtained in Comparative Example 3, which is closest to Example 6, decreased by about 11.3% and 19.0% respectively after the hot air aging test, which is significantly higher than the results of Example 6; this may be due to the fact that the granulated polyglycolic acid is subjected to negative pressure heating treatment in Example 6, which can effectively remove the residual glycolide in the polyglycolic acid product, thereby reducing the influence of the residual glycolide on the heat aging resistance of the PGA product as much as possible, which can be specifically reflected in the ability to better maintain the mechanical strength of the material without causing the mechanical strength of the material to deteriorate rapidly.
[0135] As for Comparative Examples 1 and 2, compared with Example 6, the reaction aid in Comparative Example 1 only contains a catalyst, and the reaction aid in Comparative Example 2 only contains a catalyst and a dehydrating agent. No polyol is added to the reaction aid in the two comparative examples, which may be unfavorable for reducing the activation energy of the glycolide ring-opening polymerization reaction, so that the reaction degree is reduced compared with Example 6, which is not conducive to the increase of the product molecular weight. This also makes the mechanical strength of the PGA products obtained in Comparative Examples 1 and 2 lower than that in Example 6; in addition to this influence, it may also be unfavorable for reducing the residual glycolide content in the final PGA product. Compared with Example 6, the residual glycolide content in the PGA products of Comparative Examples 1 and 2 is higher, which may cause the mechanical strength of the material to deteriorate significantly under relatively high temperature and humidity conditions.
[0136] Compared with Example 6, Comparative Examples 4 and 5 both use a conventional reactive twin-screw extruder to prepare polyglycolic acid (without using a static mixer). From the comparison of the test results in Table 8, it can be seen that the mechanical strength and heat aging resistance of the PGA material obtained by the conventional reactive twin-screw extruder are significantly weaker than those of Example 6. This may be due to the poor air tightness and heat transfer effect of the conventional reactive twin-screw extruder, and its high shear effect easily causes the local temperature of the reaction system to rise too fast, resulting in premature side reactions such as thermal degradation, which is not conducive to the increase of the molecular weight of the final product, and also causes the molecular weight distribution of the final product to become wider, which results in a significant decrease in the mechanical strength and heat aging resistance of the final PGA material.
[0137] The materials obtained in Example 6 and Comparative Examples 1-5 were subjected to thermal gravimetric tests using a thermal analyzer (model: NETZSCH STA 2500) (purge atmosphere: nitrogen 20 ml / min; crucible: Al2O3 without cover; heating rate: 5°C / min), and the temperatures corresponding to 3% mass loss of the materials were measured. The test results are shown in Table 9 below.
[0138] Table 9 Material thermal weight loss test results
[0139]
[0140] It can be seen from the test results in Table 9 that the polyglycolic acid product obtained in Example 6 based on the method of the present invention has excellent heat aging resistance, and the temperature corresponding to a 3% mass loss is about 283°C, while the temperature corresponding to a 3% mass loss of the polyglycolic acid material obtained in Comparative Example 3, which is closest to Example 6, is about 271°C, which is about 12°C lower than that of Example 6. The reason for this phenomenon may be that Example 6 uses negative pressure heating treatment to remove residual monomers (i.e., residual glycolide) in the polyglycolic acid product as much as possible, which is beneficial to improving the heat aging resistance of the material.
[0141] In addition, the temperatures corresponding to the 3% mass loss of the polyglycolic acid materials obtained in Comparative Examples 1 and 2 are about 256°C and 262°C, respectively, which are significantly lower than those in Example 6. Compared with Example 6, the reaction aid used in Comparative Example 1 only includes a catalyst, and the reaction aid used in Comparative Example 2 only includes a catalyst and a dehydrating agent. The corresponding residual monomer (i.e., residual glycolide) contents in the polyglycolic acid products obtained in Comparative Examples 1 and 2 are 0.25% and 0.14%, respectively. It can be seen that compounding the catalyst with the polyol and the dehydrating agent as a reaction aid is beneficial to reducing the residual glycolide content in the polyglycolic acid product, which is also beneficial to improving the heat aging resistance of the material.
[0142] Compared with Example 6, Comparative Example 4 uses a conventional reaction-type twin-screw extruder to prepare polyglycolic acid (without a static mixer). Due to the high shearing effect of the conventional reaction-type twin-screw extruder, the local temperature of the reaction system easily rises too fast, thereby causing more serious side reactions such as thermal degradation, which is not conducive to reducing the residual glycolide content in the polyglycolic acid product, and also causes the molecular weight distribution of the polyglycolic acid product to become wider, so that the heat aging resistance of the product is greatly reduced, which can be reflected in that the temperature corresponding to the 3% mass loss of the polyglycolic acid material obtained in Comparative Example 4 is only about 244°C. Compared with Comparative Example 4, the reaction aid used in Comparative Example 5 only includes a catalyst, and the temperature corresponding to the 3% mass loss of the polyglycolic acid material obtained in Comparative Example 5 is lower, only about 232°C, which may be due to the excessive residual glycolide content in the polyglycolic acid product obtained in Comparative Example 5.
[0143] The above description is only a preferred embodiment of the present invention and is not intended to limit the scope of the substantial technical content of the present invention. The substantial technical content of the present invention is broadly defined in the scope of the claims of the application. Any technical entity or method completed by others, if it is exactly the same as that defined in the scope of the claims of the application or an equivalent variation, will be deemed to be included in the scope of the claims.
Claims
1. A method for preparing a heat-resistant and ageing-resistant degradable aliphatic polyester, characterized in that: The method comprises the steps of: (1) adding a cyclic ester monomer into a melting and mixing kettle, and after the cyclic ester monomer is completely melted at 90-120° C., adding a reaction aid into the melting and mixing kettle, and uniformly mixing the molten cyclic ester monomer and the reaction aid, to obtain a molten material of the cyclic ester monomer; the reaction aid comprises a catalyst, a polyol and a dehydrating agent; the dehydrating agent is selected from at least one of carbodiimide, polycarbodiimide or a carbodiimide-based compound; and the amount of the polyol is 0.01-0.1 wt % based on the mass of the cyclic ester monomer; (2) prepolymerizing the molten material of the cyclic ester monomer in a static mixer to obtain a hydroxycarboxylic acid prepolymer; (3) subjecting the hydroxycarboxylic acid prepolymer to final polymerization through a viscosity increasing device, and obtaining granulated polyhydroxycarboxylic acid through granulation, wherein the viscosity increasing device is a twin-screw extruder provided with only a devolatilization section; the particle size of the obtained granulated polyhydroxycarboxylic acid is ≤10 mm; (4) subjecting the granulated polyhydroxycarboxylic acid to negative pressure heating treatment to obtain a heat-resistant and aging-resistant degradable aliphatic polyester; The static mixer used in step (2) adopts at least two stages of gradient temperature increase, the temperature range of the first stage is between 120-180°C, and the temperature range of the last stage is between 180-200°C; the total time of the material in the static mixer is 60-90 minutes; The viscosity increasing device in step (3) is devolatilized at an absolute pressure of ≤500Pa and a temperature of 220-250°C for 15min; the content of the residual cyclic ester monomer is 0.3-1wt% based on the mass of the polymer obtained by the final polymerization; The negative pressure heating treatment conditions in step (4) are absolute pressure ≤ 1 kPa and temperature 100-220° C.; the molecular weight distribution index of the heat-resistant aging-degradable aliphatic polyester obtained in step (4) is not more than 1.6; based on the total mass of the heat-resistant aging-degradable aliphatic polyester obtained in step (4), the content of residual cyclic ester monomer is not more than 0.1 wt %.
2. The preparation method according to claim 1, characterized in that Based on the mass of the cyclic ester monomer, the amount of the catalyst used is 0.001-1wt%, and the amount of the dehydrating agent used is 0.1-2wt%.
3. The preparation method according to claim 1, characterized in that: The catalyst is selected from at least one of tin compounds, antimony compounds or zinc compounds.
4. The preparation method according to claim 1, characterized in that: The polyol is selected from at least one of 1,4-butanediol, glycerol, pentaerythritol, xylitol, sorbitol, 1,6-hexanediol, triethylene glycol and dipropylene glycol.
5. The preparation method according to claim 1, characterized in that: The temperature of the second section of the static mixer is 10-80° C. higher than that of the first section; the temperature of the last section is 0-20° C. higher than that of the previous adjacent section.
6. The preparation method according to claim 1, characterized in that: The static mixer used in step (2) adopts a 3-7 stage gradient heating method.
7. The preparation method according to claim 1, characterized in that: The weight average molecular weight of the hydroxycarboxylic acid prepolymer obtained in step (2) is 50,000-150,000.