Spherical crystalline silicon dioxide particles and method for producing the same
By mixing calcium and lithium in amorphous silica particles and performing heat treatment, spherical crystalline silica particles with high crystallization rate and high quartz ratio were successfully obtained, solving the problem of low dielectric loss and thermal expansion matching in the existing technology. problem, improving the dielectric properties and assembly reliability of semiconductor sealing materials.
Patent Information
- Application Number
- CN202180036714.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-05-20
- Filing Date
- 2021-05-20
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-05-20
AI Technical Summary
It is difficult to obtain spherical silica particles with low dielectric loss tangent in the millimeter-wave frequency band, and the crystallization rate and quartz ratio are insufficient, which affects the dielectric properties and thermal expansion matching of semiconductor sealing materials.
By mixing calcium and lithium raw materials into amorphous silica particles with a circularity of 0.80 or more, and performing heat treatment at 850°C to 1150°C to promote quartz crystallization, a spherical crystalline material with a high crystallization rate and a high quartz ratio is obtained. Silica particles.
Spherical silica particles with excellent dielectric properties in the millimeter-wave frequency band are realized, which reduces the dielectric loss tangent, matches the thermal expansion behavior of semiconductor components, and improves assembly reliability.
Smart Images

Figure CN115697907B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to spherical crystalline silica particles and a method for producing the same, and in particular to spherical crystalline silica particles having a high quartz ratio and a method for producing the same. Background Art
[0002] As the amount of information increases with the improvement of communication technology, and the use of millimeter wave bands such as millimeter wave radars is rapidly expanding, the frequency is becoming higher. The circuit substrate that transmits these high-frequency signals is composed of electrodes as circuit patterns and dielectric substrates. In order to suppress energy loss during high-frequency signal transmission, the dielectric loss tangent (tanδ) of the dielectric material must be small. In order to achieve low dielectric loss, the dielectric material must have low polarity and low dipole moment.
[0003] As dielectric materials, ceramic particles, resins, and composites thereof are mainly used. In particular, with the expansion of the use of millimeter wave bands in recent years, ceramic particles and resins with lower dielectric loss tangent (tanδ) are needed. Resins are suitable for high-frequency devices with relatively small relative dielectric constants (εr), but the dielectric loss tangent (tanδ) or thermal expansion coefficient is larger than that of ceramic particles. Therefore, in the composite of ceramic particles and resins for millimeter wave bands, it is suitable for (1) low dielectric loss tangent (tanδ) of the ceramic particles themselves and (2) high filling ceramic particles, thereby reducing the amount of resin exhibiting a large dielectric loss tangent (tanδ).
[0004] As ceramic particles, silicon dioxide (SiO2) particles are generally used. If the shape of the silicon dioxide particles is angular, the fluidity, dispersibility and filling property in the resin will deteriorate, and the wear of the manufacturing device will be accelerated. In order to improve it, spherical silicon dioxide particles are widely used. It is believed that the closer the spherical silicon dioxide particles are to a true sphere, the more they can improve the filling property, fluidity and wear resistance of the resin, so particles with high roundness have been sought. Furthermore, research on optimizing the particle size distribution of the particles to further improve the filling property has also been ongoing.
[0005] Generally, the melt-blowing method is used as a method for producing spherical silica. In melt-blowing, the particles are melted by passing them through a high temperature area such as a flame, and the shape of the particles becomes spherical due to surface tension. The melted spherical particles are transported and recovered by air flow to prevent the particles from fusing to each other, and the melt-blown particles are quenched. Since the silica is quenched from the molten state, it does not crystallize, but becomes glass-like particles with an amorphous structure, which are generally called quartz glass.
[0006] The spherical silica particles manufactured by the melt-blowing method are amorphous, so their thermal expansion coefficient and thermal conductivity are low. The thermal expansion coefficient of amorphous silica particles is 0.5ppm / K, and the thermal conductivity is 1.4W / mK. These properties are roughly the same as the thermal expansion coefficient of quartz glass, which has no crystalline structure and has an amorphous (amorphous) structure. In general, the thermal expansion coefficient of Si, the main raw material of the IC chip, is 3-5ppm / K, and the thermal expansion coefficient of the sealing resin used to seal the IC chip is much larger than that of Si. Therefore, due to the difference in the thermal expansion behavior of the two materials (Si and the sealing resin), warping will occur on the IC chip, which will affect the generation. On the other hand, when the spherical silica with a small thermal expansion coefficient is highly filled into the resin with a large thermal expansion coefficient, the effect of reducing the thermal expansion of the sealing material (composite of spherical silica and resin) itself can be obtained. By making the thermal expansion coefficient of the sealing material close to the value of Si, the deformation caused by the thermal expansion behavior when the IC chip is sealed can be suppressed.
[0007] As described above, the properties required of silica particles for sealing materials include excellent dielectric properties at high frequencies in the millimeter wave band, in addition to being able to maintain the performance of the composite by mixing a large amount of silica particles in the resin, fluidity, and wear resistance. Since dielectric properties are physical properties of the material, it is difficult to reduce the dielectric loss tangent of amorphous silica particles.
[0008] Patent document 1 describes a method for producing a porous powder whose main crystal phase is composed of quartz, which is characterized in that 0.5 mass % or more of a Zn compound is added in terms of ZnO to silica gel having an average particle size of 0.1 to 20 μm, and the mixture is heat treated at 900 to 1100°C.
[0009] Patent document 2 shows a method for producing spherical crystalline silica particles, characterized in that the method includes a step of heat treating the spherical silica particles at 800°C to 1300°C and cooling the heat-treated spherical silica particles, wherein the cooled spherical silica particles have a crystalline phase of 90% or more by mass, and quartz crystals account for 70% or more of the whole, wherein the spherical silica particles are mixed as follows: the alkali metal compound is mixed in a ratio of 0.4 to 5% by mass in terms of oxide conversion relative to the total mass of the mass of the amorphous spherical silica particles and the mass of the alkali metal after oxide conversion, or the alkaline earth metal oxide is mixed in a ratio of 1 to 5% by mass in terms of oxide conversion relative to the total mass of the mass of the amorphous spherical silica particles and the mass of the alkaline earth metal after oxide conversion. Wherein, when the amount of alkali metal added is less than 0.4% by mass and the amount of alkaline earth metal added is less than 1% by mass, the appearance rate of quartz will decrease.
[0010] In Non-Patent Document 1, alkali metal oxides were systematically added to synthesized amorphous spherical silica, and heat-treated after forming into particles, thereby studying the effect of additives on crystallization and phase transition. It can be seen that when the additive is lithium oxide (Li2O), if 0.5% by mass or more is added and fired at 800°C or above, quartz can be obtained.
[0011] The influence of cations on the crystallization and phase transition of silica materials is investigated in Non-Patent Document 2. It is disclosed that when 10% by mass of LiCl is added to synthesized amorphous silica and then heat-treated at 800°C, quartz appears as the most dominant phase.
[0012] Prior art literature
[0013] Patent Literature
[0014] Patent Document 1: Japanese Patent Application Publication No. 2002-20111
[0015] Patent Document 2: International Publication No. 2018 / 186308
[0016] Non-patent literature
[0017] Non-patent document 1: Journal of Ceramics Society of Japan 105[5]385-390(1997)
[0018] Non-patent document 2: Bulletin of the Faculty of Science, Kagoshima University, Earth Science and Biology, Vol. 24, pp. 1-22 (1991)
[0019] Non-patent document 3: High Pressure Research 28(4)641-650(2008) Summary of the invention
[0020] Technical problem to be solved by the invention
[0021] The present inventors aim to seek semiconductor sealing filler particles with excellent dielectric properties in the millimeter wave band of 30 GHz to 80 GHz, and to mix them into resin to make resin composites for high-frequency devices. As a result, it was found that in order to obtain a resin composite with a low dielectric loss tangent, first, heat-treating the spherical molten (amorphous) silica to crystallize it is very effective. That is, it can be confirmed that the dielectric loss tangent of crystalline silica in the millimeter wave band (30 GHz to 80 GHZ) is significantly reduced than that of amorphous silica that has been widely used. As a result, spherical crystalline silica particles become silica particles that show excellent dielectric properties for high-frequency equipment purposes. The crystalline silica obtained by heat treatment is quartz, cristobalite or a mixture thereof. Since quartz and cristobalite have differences in physical property values, when used as a filler, the phase of crystalline silica is preferably a single phase.
[0022] In addition, when crystallized into cristobalite, the coefficient of thermal expansion of cristobalite becomes more than 3 times that before heat treatment, and then, has an inflection point near 250 ° C, which will cause many problems in use. In particular, when used as a filler for semiconductor sealing, peeling occurs at the interface of the original part and the sealing material due to the mismatch with the thermal expansion behavior of the semiconductor original part. For this purpose, among crystalline silicon dioxide, quartz with an inflection point of thermal expansion outside the assembly temperature range is suitable. If quartz is used as a filler for semiconductor sealing, it is possible to seek the improvement of assembly reliability while seeking low dielectric loss and appropriate thermal expansion coefficient.
[0023] As a method for crystallizing spherical amorphous silicon dioxide to obtain quartz, Patent Document 1 discloses: adding 0.5% by mass or more of a zinc compound in terms of oxide, and heat treating the mixture at 900-1100°C. However, the results of the present inventors' reproduction test showed that at a heat treatment temperature below 950°C, the silicon dioxide itself did not crystallize, but remained amorphous silicon dioxide. When heat treated at a temperature exceeding 950°C, crystallization began to proceed, but the degree of crystallization stopped at about 20% even at 1100°C. Moreover, the crystalline phase that appeared was mainly cristobalite, and a single phase of quartz could not be obtained at a high content.
[0024] Patent document 2 shows a method for producing spherical crystalline silica particles, characterized in that it contains the following steps: for the total mass relative to the mass converted into oxides, alkaline earth metals are mixed at 1 to 5 mass% in oxide conversion, the mixed spherical silica particles are heat-treated at 800°C to 1300°C, and the heat-treated spherical silica particles are cooled; the cooled spherical silica particles have a crystalline phase of more than 90 mass%, and quartz crystals account for more than 70 mass% of the whole. Calcium is shown as an alkaline earth metal in the embodiment, but in the case of adding 0.5 mass% of calcium in oxide conversion and heat-treating at 1100°C as a comparative example, quartz appears as low as less than 30%. In addition, so far, spherical crystalline silica with a high quartz content has not been obtained when calcium is added in oxide conversion of less than 1 mass%.
[0025] In addition, in Patent Document 2, Non-Patent Document 1, and Non-Patent Document 2, lithium is also shown as a quartz crystallization promoting element. Patent Document 2 shows that lithium is mixed in a ratio of 0.4 to 5% by mass in terms of oxide, and heat-treated at 800°C to 1300°C. Non-Patent Document 1 shows that quartz can be obtained by adding 0.5% by mass or more of lithium oxide to synthetic amorphous spherical silica and firing it to 800°C or more. Furthermore, Non-Patent Document 2 shows that by adding 10% by mass of lithium chloride (LiCl) to synthetic amorphous silica and heat-treating it at 800°C, quartz will appear as the most dominant phase.
[0026] However, alkaline earth metals such as calcium and alkali metals such as lithium are not preferred as elements added to semiconductor sealing materials. In order to maintain normal operation of semiconductor components and assembly reliability, it is necessary to reduce the amount of alkaline earth metals and alkali metal elements added.
[0027] As factors that affect the crystallization of amorphous silicon dioxide, it is well known that there are temperature, pressure, and impurity elements. Regarding the influence of pressure, for example, it is recorded in non-patent document 3 that if heat treatment is carried out at 300°C to 1200°C under 20,000 to 30,000 atmospheres, quartz will be crystallized, but the pressurization device of tens of thousands of atmospheres has limitations in processing capacity, and it is difficult to carry out large-scale industrial production, so it is not preferred. So far, although there are many reports on crystallization experiments using temperature and impurity elements as variable factors, spherical crystalline silicon dioxide with a crystalline silicon dioxide content of more than 40% and a quartz ratio of more than 80% by mass in the crystalline silicon dioxide has not been obtained. From the viewpoint of maintaining the normal operation and assembly reliability of semiconductor components, it is expected to obtain silicon dioxide particles with a high crystallization rate and substantially composed of a single phase of quartz while reducing lithium and calcium to less than 0.40% and less than 1.0% by mass in terms of oxide conversion, respectively.
[0028] The present invention aims to provide: spherical silica particles suitable for use as fillers for semiconductor sealing materials with excellent dielectric properties in the millimeter wave band, that is, spherical crystalline silica particles with a high crystallization rate and a high proportion of quartz while suppressing the content of alkali metals and alkaline earth metals to a low level, and a method for producing the same.
[0029] Technical means for solving technical problems
[0030] The inventors of the present application have conducted in-depth research to solve the above problems. As a result, a mixed raw material powder formed by mixing a calcium raw material and a lithium raw material in a powder composed of amorphous silica particles with a circularity of 0.80 or more was heated at a heat treatment temperature of 850°C to 1150°C, thereby successfully lowering the content of each of lithium and calcium than the existing situation, while promoting quartz crystallization, wherein the calcium raw material contains 0.004 or more and less than 1.0% by mass of calcium in terms of oxide conversion, and the lithium raw material contains 0.02% by mass and less than 0.40% by mass of lithium in terms of oxide conversion. Without being bound by a specific theory, it is believed that by adding lithium metal and calcium metal to silica at the same time, a synergistic effect is exerted on quartz crystallization, and compared with the case where each element is added separately, the crystallization of quartz is promoted despite the reduced addition amount. The crystalline silica particles obtained by heat treatment at 850 to 1150°C contain a phase of crystalline silica, and the phase of the crystalline silica is essentially a single phase of quartz. The single phase mentioned here means that the ratio of quartz in the crystalline silica phase is 80 mass % or more, preferably 85.0 mass % or more, and more preferably 90.0 mass % or more.
[0031] The present invention provides the following spherical silica particles and a method for producing the same.
[0032] (1) A spherical crystalline silica particle having a circularity of 0.80 or more, containing 0.02 mass % or more and less than 0.40 mass % of lithium in terms of oxide, containing 0.004 mass % or more and less than 1.0 mass % of calcium in terms of oxide, and containing a crystalline silica phase; wherein the proportion of the crystalline silica phase in the spherical crystalline silica particle is 40.0% or more, and the proportion of quartz in the crystalline silica phase is 80.0 mass % or more.
[0033] (2) The spherical crystalline silica particles according to (1), wherein the ratio of the crystalline silica phase is 70.0% or more, and the ratio of quartz in the crystalline silica phase is 85.0% by mass or more.
[0034] (3) The spherical crystalline silica particles according to (2), wherein the ratio of the crystalline silica phase is 80.0% or more, and the ratio of quartz in the crystalline silica phase is 90.0% by mass or more.
[0035] (4) The spherical crystalline silica particles according to any one of (1) to (3) above, wherein the average particle size (D50) is 3 to 100 μm.
[0036] (5) A method for producing spherical crystalline silica particles as described in any one of (1) to (4), comprising: heat treating a mixed raw material powder obtained by mixing a calcium raw material and a lithium raw material into spherical amorphous silica particles having a circularity of 0.80 or more at 850°C to 1150°C.
[0037] (6) The method for producing spherical crystalline silica particles according to any one of (1) to (4), comprising:
[0038] A mixed raw material powder obtained by mixing a lithium raw material with spherical amorphous silica particles having a circularity of 0.80 or more and containing a calcium component is heat-treated at 850°C to 1150°C.
[0039] (7) The method for producing spherical crystalline silica particles according to any one of (1) to (4), comprising:
[0040] A mixed raw material powder obtained by mixing a calcium raw material with spherical amorphous silica particles having a circularity of 0.80 or more and containing a lithium component is heat-treated at 850°C to 1150°C.
[0041] (8) The method for producing spherical crystalline silica particles according to any one of (1) to (4), comprising:
[0042] Spherical amorphous silica particles having a circularity of 0.80 or more and containing a calcium component and a lithium component are heat treated at 850°C to 1150°C.
[0043] (9) The method for producing spherical crystalline silica particles according to any one of (5) to (8), wherein the temperature of the heat treatment is 875°C to 1110°C.
[0044] Effects of the Invention
[0045] According to the present invention, it is possible to provide: spherical silica particles that are preferred for use as fillers for semiconductor sealing materials having excellent dielectric properties in the millimeter wave band, that is, spherical crystalline silica particles that have a high crystallization rate and a high proportion of quartz while suppressing the content of alkali metals and alkaline earth metals to a low level, and a method for producing the same. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 These are XRD patterns of amorphous silicon dioxide before heat treatment and silicon dioxide (after heat treatment) according to one embodiment of the present invention. DETAILED DESCRIPTION
[0047] The spherical crystalline silica of one embodiment of the present invention is a spherical crystalline silica particle having a circularity of 0.80 or more, containing 0.02% by mass or more and less than 0.40% by mass of lithium in terms of oxide, containing 0.004% by mass or more and less than 1.0% by mass of calcium in terms of oxide, and containing a crystalline silica phase; the proportion of the crystalline silica phase in the spherical crystalline silica particle is 40.0% or more, and the proportion of quartz in the crystalline silica phase is 80.0% or more. The crystalline silica phase being 40.0% or more here refers to the proportion of the crystalline silica phase in the spherical crystalline silica particle, and the method for calculating the proportion is described below.
[0048] As the crystal structure of silicon dioxide (SiO2), there are cristobalite, quartz, etc. The silicon dioxide with these crystal structures has higher thermal conductivity than amorphous silicon dioxide. Therefore, in semiconductor sealing filler, by replacing amorphous silicon dioxide with crystalline silicon dioxide of suitable amount, it is possible to improve the heat dissipation of IC chip. And then due to the lower dielectric loss tangent of crystalline silicon dioxide in millimeter wave band, therefore in semiconductor sealing filler, the more amorphous silicon dioxide is replaced with crystalline silicon dioxide, the lower the dielectric loss tangent of semiconductor sealing material will be.
[0049] [Method for producing spherical crystalline silica particles]
[0050] The spherical crystalline silica particles of the present invention can also be produced by mixing spherical amorphous silica with both a calcium raw material and a lithium raw material, and heat-treating the mixture (also referred to as a mixed raw material).
[0051] According to one embodiment, the silica particles may be produced by heat-treating a mixed raw material obtained by mixing a lithium raw material with spherical amorphous silica particles containing a calcium component.
[0052] Alternatively, the silica particles may be produced by heat-treating a mixed raw material obtained by mixing a calcium raw material with spherical amorphous silica particles containing a lithium component.
[0053] Alternatively, it can also be produced by heat-treating spherical amorphous silica particles containing a calcium component and a lithium component.
[0054] (Spherical amorphous silica particles)
[0055] Amorphous spherical silica particles as raw materials can be produced by methods such as melt-blowing. In the melt-blowing method, natural silica powder that has been crushed and adjusted to a desired particle size is passed through a flame to melt the particles, and the shape of the particles becomes spherical due to surface tension. In this way, spherical amorphous silica particles with a circularity of 0.80 or more can be produced by the melt-blowing method.
[0056] The main component of the composition of the spherical amorphous silica particles is silicon dioxide, and there is no particular limitation as long as the spherical crystalline silica particles finally obtained are within the desired range. As one embodiment, the composition of the spherical amorphous silica particles can be: 98.0% by mass or more is silicon dioxide (SiO2), and as trace elements, Ca, Li, Al, Na, Mg, Ba, Zn, etc. can also be contained. In one embodiment, the composition of the spherical amorphous silica particles can also contain less than 0.5% by mass of Zn.
[0057] (Calcium raw materials)
[0058] The calcium raw material is mixed with the spherical amorphous silica particles and heat-treated. The composition and mixing amount of the calcium raw material are not particularly limited and can be appropriately adjusted as long as the spherical crystalline silica particles finally obtained are within the desired range. The calcium raw material can be calcium hydroxide or calcium oxide, etc., which are stably present in the atmosphere, or can be a natural mineral. In order for the calcium raw material to be uniformly mixed with the spherical amorphous silica particles, it can be added in a state such as a powder or an aqueous solution. In addition, at least a part of the calcium raw material is a trace element contained in the spherical amorphous silica particles. For example, as long as the spherical amorphous silica particles contain sufficient calcium and the desired calcium content is reached in the spherical crystalline silica particles finally obtained, the spherical amorphous silica particles can be used as the calcium raw material. In addition, in the case where the spherical amorphous silica particles contain calcium but are insufficient, in order to reach the desired calcium content in the spherical crystalline silica particles finally obtained, a calcium raw material can be added.
[0059] (Lithium raw materials)
[0060] The lithium raw material is mixed with the spherical amorphous silica particles and heat-treated. The composition and mixing amount of the lithium raw material are not particularly limited and can be appropriately adjusted as long as the spherical crystalline silica particles finally obtained are within the desired range. The lithium raw material is an oxide, a carbon oxide, a hydroxide, a nitrate oxide, etc., and the added form is not particularly limited. In order to be uniformly mixed with the amorphous spherical silica particles, it can be added in a state such as a powder or an aqueous solution. In addition, at least a part of the lithium raw material is also trace elements contained in the spherical amorphous silica particles. For example, as long as the spherical amorphous silica particles can contain sufficient lithium and the spherical crystalline silica particles finally obtained reach the desired lithium content, the spherical amorphous silica particles can be used as a lithium raw material. In addition, in the case where the spherical amorphous silica particles contain lithium but are insufficient, a calcium raw material can be added in order for the spherical crystalline silica particles finally obtained to reach the desired lithium content.
[0061] (mix)
[0062] Spherical amorphous silica particles are mixed with both calcium raw material and lithium raw material. It should be noted that calcium raw material and / or lithium raw material may also be contained in spherical amorphous silica. The mixing method is not particularly limited, as long as each raw material is uniformly dispersed and mixed in the mixture. Mixing can be carried out by a powder mixer. By mixing, the calcium raw material and the lithium raw material are in contact with at least a portion of the spherical amorphous silica, and in the subsequent heat treatment process, the crystallization of the spherical amorphous silica, especially the crystallization to quartz, is promoted.
[0063] During mixing, the raw materials are mixed so that the lithium contained in the manufactured spherical crystalline silica particles is 0.02 mass % or more and less than 0.40 mass % in terms of oxide conversion, and the calcium contained is 0.004 mass % or more and less than 1.0 mass % in terms of oxide conversion. It should be noted that since the total amount of the lithium raw material or calcium raw material to be mixed is not all contained in the manufactured spherical crystalline silica particles, it is preferred to mix them in consideration of the content ratio.
[0064] Note that mixing causes the calcium raw material and the lithium raw material to contact at least a part of the spherical amorphous silica, rather than promoting the pulverization of the spherical amorphous silica, and therefore the circularity thereof is hardly reduced before and after mixing.
[0065] (Heat Treatment)
[0066] The temperature at which the mixed raw material after mixing the spherical amorphous silica particles, the calcium raw material and the lithium raw material is heat-treated is in the temperature range of 850°C to 1150°C. The atmosphere during the heat treatment can be an oxidizing atmosphere such as air and an inert gas atmosphere such as nitrogen or argon. Since heat treatment is carried out in large quantities in industry, the atmospheric pressure is preferably atmospheric pressure. If the heat treatment temperature is lower than 850°C, crystallization cannot be carried out, or it slows down significantly. On the other hand, if it is higher than 1150°C, the crystallization of cristobalite will compete with the crystallization of quartz. As a result, spherical crystalline silica particles with a substantial quartz single phase cannot be obtained. Here, the substantial single phase refers to a state in which 80% or more of the crystalline silica phase contained in the spherical crystalline silica particles is a quartz phase. The preferred heat treatment temperature is 875°C to 1110°C.
[0067] In order to obtain the desired degree of crystallization, the time of heat treatment can be appropriately adjusted. If lithium and calcium are uniformly and simultaneously present in the spherical amorphous silica particles, the spherical amorphous silica particles can be crystallized into quartz by the synergistic effect of the two elements compared with the case where a single element exists. In one embodiment of the present invention, lithium can be added as a lithium raw material (lithium carbonate, etc.) during mixing, or it can be contained in the spherical amorphous silica particles in advance. In addition, calcium can be provided as a calcium raw material (calcium oxide, etc.) during mixing, or it can be contained in the spherical amorphous silica particles in advance. In order to make the lithium or calcium uniformly present in the spherical amorphous silica particles by diffusion during the heating process, it can be considered that the spherical amorphous silica particles are all crystallized into quartz. Therefore, the longer the heat treatment time, the more lithium or calcium diffuses in the spherical amorphous silica particles, and the more crystallization is carried out. Typically, in other words, when the heating and cooling rate is greater than 60 ° C / hour, the crystallization is actually determined by the heat treatment temperature, that is, the holding time at the maximum temperature. Therefore, the control of crystallization can be adjusted by adjusting the holding time at the maximum temperature. In this case, the heat treatment time can be adjusted in the range of approximately 1 hour to 48 hours. From the perspective of fully promoting crystallization, it can be more than 3 hours or more than 6 hours. In addition, even if the heat treatment time is excessively extended, the crystallinity will be saturated. Therefore, from the perspective of reducing costs, the heat treatment time can be less than 25 hours, less than 18 hours, or less than 12 hours.
[0068] In addition, if the heat treatment temperature becomes higher, the diffusion coefficient of lithium in the spherical amorphous silica particles will increase, causing the quartz to crystallize. However, if it exceeds 1150°C, the cristobalite phase will appear competitively and the quartz will no longer be a single phase, so there is an upper limit to the heat treatment temperature.
[0069] In addition, the degree of diffusion will vary with the type and amount of lithium raw material or calcium raw material added, so the appropriate heat treatment time and temperature can be selected accordingly.
[0070] It should be noted that, when heat treatment is performed in an electric furnace, the heating rate or cooling rate does not have a significant effect on the appearance of spherical crystalline silica particles.
[0071] The circularity of the spherical crystalline silica of the present invention hardly decreases before and after the heat treatment for crystallization. The spherical crystalline silica particles of the present invention become crystalline at a relatively low temperature during the heat treatment at 850°C to 1150°C, and the circularity hardly decreases within this temperature range. If it exceeds 1100°C, the amorphous silica particles may sometimes be combined by welding or sintering, and since the spherical crystalline silica particles of the present invention become crystalline (no longer amorphous) at 850°C to 1150°C, the combination between particles caused by welding or sintering can be completely suppressed.
[0072] [Spherical crystalline silica particles]
[0073] (Circularity)
[0074] The spherical crystalline silica particles of the present invention have a circularity of 0.80 or more.
[0075] If the circularity is less than 0.80, when used as silica particles of a resin composite composition for semiconductor sealing materials, the fluidity, dispersibility, and filling are insufficient, and there is a situation where the wear of the sealing material manufacturing machine is promoted. The average circularity of the spherical amorphous silica particles obtained by melt blowing can be above 0.80. Since the temperature in the heat treatment process for crystallization is 850-1150°C, the circularity of the silica particles is almost unchanged before and after the heat treatment. Moreover, if it is a melt-blowing method, particles with a high average circularity can be easily obtained. As a result, in the method of the present invention, spherical crystalline silica particles with a high desired circularity can be achieved. From the viewpoint of improving fluidity, dispersibility, filling or reducing machine wear, the higher the circularity, the more preferred it is, which can be above 0.85 or above 0.90. On the other hand, it is sometimes difficult to make the circularity 1.0, that is, a perfect circle, so the upper limit of the circularity can be set to below 0.99 or below 0.97.
[0076] The circularity is obtained by "the circumference of the circle equivalent to the projected area of the photographed particle ÷ the circumference of the photographed particle image". The closer the value is to 1, the closer it is to a true sphere. The circularity of the present invention is obtained by dynamic particle image analysis. In the dynamic particle image analysis method, spherical crystalline silica particles are flowed into a liquid, and then photographed as a still image of the particles. The obtained particle image is used as a reference for image analysis to obtain the circularity of the spherical crystalline silica particles. The average value of these multiple circularities is taken as the average circularity. When the average circularity is determined by the dynamic particle image analysis method, if the number of particles is too small, an accurate average value cannot be obtained. The number of particles needs to be at least 100, preferably more than 500, and more preferably more than 1000. In the present invention, a dynamic particle image analyzer "FPIA-3000" (manufactured by Spectris Co., Ltd.) and approximately 100 particles are used. It should be noted that the circularity of spherical amorphous silica particles is obtained in the same manner.
[0077] (composition)
[0078] The spherical crystalline silica particles of the present invention are based on the mass of the silica particles (100% by mass), and contain 0.02% by mass or more and less than 0.40% by mass of lithium as calculated by oxide, and contain 0.004% by mass or more and less than 1.0% by mass of calcium as calculated by oxide. The preferred lower limit of lithium is 0.05% by mass, more preferably 0.10% by mass, and further preferably 0.25% by mass. In addition, the preferred upper limit of lithium is less than 0.35% by mass, and more preferably less than 0.30% by mass. The preferred lower limit of calcium is 0.20% by mass, and more preferably 0.6% by mass. In addition, the preferred upper limit of calcium is 0.9% by mass, and more preferably 0.8% by mass. The content of lithium and calcium can be measured, for example, by atomic absorption spectrometry, ICP mass analysis (ICP-MS). Specifically, following JIS-K0133, ICP-MS (Agilent "7700X") is used for measurement. An aqueous solution in which silica particles are completely dissolved by hydrofluoric acid is used as a sample. Here, the content of impurity elements contained in the silica particles is taken as the content of impurity elements in the silica solution. The standard curve can also use a base solution containing only the reagent. By performing a specific heat treatment in a composition containing lithium and calcium in the above range, spherical crystalline silica particles composed of a single phase with a high crystallization rate and a high actual quartz ratio can be obtained. Lithium and calcium are almost completely present in the form of oxides through heat treatment in the temperature range of 850 to 1150°C for crystallization, and then react with silica to allow lithium or calcium to enter the silica structure, so that their content remains almost unchanged before and after the heat treatment in the above temperature range. When the content of lithium and calcium changes before and after the heat treatment, the composition of the raw material can be appropriately adjusted to achieve the predetermined lithium and calcium content in the finally obtained spherical crystalline silica particles, taking into account the degree of change.
[0079] (Properties of crystals)
[0080] The spherical crystalline silica particles of the present invention contain a crystalline silica phase, wherein the ratio of the crystalline silica phase in the spherical crystalline silica particles is 40.0% or more, and the ratio of quartz in the crystalline silica phase is 80.0% or more by mass.
[0081] In the case where the silica particles obtained by heat treatment are composed of amorphous and crystalline silica, the existence ratio of amorphous and crystalline silica (i.e., "degree of crystallinity", which is referred to as such in this specification) and the type and ratio of crystalline silica can be obtained by XRD. In the XRD measurement, the ratio of the crystalline phase can be calculated by the following formula from the sum of the integrated intensity of the crystalline peak (Ic) and the integrated intensity of the amorphous halo portion (Ia). More specifically, the ratio of the crystalline silica phase contained in the spherical crystalline silica particles can be obtained.
[0082] X (crystal phase ratio) = Ic / (Ic+Ia)×100(%)
[0083] In the present invention, XRD measurement is performed in the range of 2θ = 10° to 90°. The crystal phase ratio is obtained from the sum of the crystalline peak intensities appearing in the 2θ measurement range and the integrated intensity of the broad halo-shaped portion due to amorphous phase appearing near 2θ = 22°.
[0084] Furthermore, the types of crystalline phases such as cristobalite and quartz and their respective proportions (mass %) can be obtained by quantitative analysis by X-ray diffraction. In the present invention, the quantitative analysis by X-ray refraction uses an analytical method by the Rietveld method, and quantitative analysis is performed without using a standard sample. In the present invention, an X-ray diffraction device "D2PHASER" (manufactured by BRUKER CORPORATION) is used. The quantitative analysis of the crystalline phase by the Rietveld method is performed by a crystal structure analysis software "TOPAS" (manufactured by BRUKER CORPORATION).
[0085] The spherical crystalline silica particles of the present invention contain a crystalline silica phase, and the ratio of the crystalline silica phase in the spherical crystalline silica particles is 40.0% or more, that is, the spherical crystalline silica particles have a high crystallinity of 40.0% or more, and the dielectric loss tangent is significantly lower than that of amorphous silica, which is preferred. From the viewpoint of reducing the dielectric loss tangent, the higher the crystallinity, the more preferred, and it can be 70.0% or more, and more preferably 80.0% or more.
[0086] The spherical crystalline silica particles of the present invention contain a phase of crystalline silica, in which the proportion of quartz in the phase of the crystalline silica is high, being 80.0% by mass or more, and being substantially a single phase of quartz. Therefore, many characteristics such as the coefficient of thermal expansion and thermal conductivity of the spherical crystalline silica particles are substantially determined by the characteristics of quartz, i.e., they will not change, and are preferably used for fillers. From the above viewpoint, the higher the proportion of quartz, the more preferred it is, and it can be 85.0% by mass or more, and more preferably, it can be 90.0% by mass or more.
[0087] (Average particle size)
[0088] In one embodiment of the present invention, the average particle size (D50) of the spherical crystalline silica particles can be 3 to 100 μm. If the average particle size is less than 3 μm, the agglomeration of the particles becomes larger and the fluidity is significantly reduced, so it is not preferred. If the average particle size exceeds 100 μm, gaps are likely to remain between the particles, making it difficult to improve the filling property, so it is not preferred. The average particle size in the range of 10 to 80 μm is more preferred. The particle size of the spherical amorphous silica particles before heat treatment hardly changes before and after heat treatment in the temperature range of 850 to 1150°C.
[0089] The average particle size (D50) is measured by a laser diffraction / scattering particle size distribution measurement method to obtain the median particle size D50 at a cumulative volume of 50% in a volume-based particle size distribution. It should be noted that the laser diffraction / scattering particle size distribution measurement method is a method of irradiating a dispersion liquid in which spherical crystalline silica particles are dispersed with a laser, and obtaining the particle size distribution from the intensity distribution pattern of the diffraction / scattered light emitted by the dispersion liquid. In the present invention, a laser diffraction / scattering particle size distribution measuring device "CILAS920" (manufactured by Silas Corporation) is used. It should be noted that the average particle size of spherical amorphous silica particles can also be obtained in the same manner.
[0090] (Application example)
[0091] According to the present invention, a composite composition of finally obtained spherical crystalline silica particles and a resin can be produced, and further, a resin composite body obtained by curing the resin composite composition can be produced. The composition of the resin composite composition will be described below.
[0092] By using a slurry composition containing spherical crystalline silica particles and a resin, a resin composite composition such as a semiconductor sealing material (especially a solid sealing material) and an interlayer insulating film can be obtained. Furthermore, by curing these resin composite compositions, a resin composite such as a sealing material (cured body) and a semiconductor package substrate can be obtained.
[0093] When manufacturing the resin composite composition, for example, in addition to the spherical crystalline silica particles and the resin, a curing agent, a curing accelerator, a flame retardant, a silane coupling agent, etc. are mixed as needed and compounded by a known method such as kneading. Then, the composite composition is formed into a granular form, a film form, etc. according to the application.
[0094] Furthermore, when the resin composite composition is cured to produce a resin composite, for example, the resin composite composition is heated and melted, and a shape is processed according to the application, and a higher heat than when it is melted is applied to completely cure it. In this case, a known method such as transfer molding can be used.
[0095] For example, when manufacturing semiconductor-related materials such as encapsulation substrates or interlayer insulating films, as the resin used for the resin composite composition, known resins can be used, but epoxy resins are preferably used. The epoxy resin is not particularly limited, and for example: bisphenol A type epoxy resin, bisphenol F type epoxy resin, biphenyl type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, naphthalene type epoxy resin, phenoxy type epoxy resin, etc. can be used. One type thereof can be used alone, or two or more types with different molecular weights can be used in combination. Among them, from the viewpoints of curability, heat resistance, etc., an epoxy resin having two or more epoxy groups in one molecule is preferred. Specifically, for example, biphenyl epoxy resins, phenol novolac epoxy resins, o-cresol novolac epoxy resins, phenol and aldehyde novolac resins epoxidized products, glycidyl ester epoxy resins obtained by reacting glycidyl ethers such as bisphenol A, bisphenol F and bisphenol S, polyacids such as phthalic acid or dimer acid with epichlorohydrin, linear aliphatic epoxy resins, alicyclic epoxy resins, heterocyclic epoxy resins, alkyl-modified multifunctional epoxy resins, β-naphthol novolac epoxy resins, 1,6-dihydroxynaphthalene epoxy resins, 2,7-dihydroxynaphthalene epoxy resins, dihydroxybiphenyl epoxy resins, and epoxy resins into which halogens such as bromine are introduced for imparting flame retardancy, etc. Among these epoxy resins having two or more epoxy groups in a single molecule, bisphenol A epoxy resins are particularly preferred.
[0096] In addition, resins other than epoxy resins are also applicable for uses other than composite materials for semiconductor sealing materials, such as resins for prepreg materials for printed boards, various engineering plastics and other resin composite compositions. Specifically, in addition to epoxy resins, for example, polyamides such as silicone resins, phenolic resins, melamine resins, urea-formaldehyde resins, unsaturated polyesters, fluororesins, polyimides, polyamide-imides, polyether-imides, etc.; polyesters such as polybutylene terephthalate and polyethylene terephthalate; polyphenylene sulfide, aromatic polyesters, polysulfones, liquid crystal polymers, polyether sulfones, polycarbonates, maleimide-modified resins, ABS resins, AAS (acrylonitrile-butyl acrylate-styrene) resins, and AES (acrylonitrile-EPDM rubber-styrene) resins.
[0097] As a curing agent for the resin composite composition, in order to cure the resin, a known curing agent can be used, for example, a phenolic curing agent can also be used. As a phenolic curing agent, phenol novolac resin, alkylphenol novolac resin, polyvinylphenol, etc. can be used alone, or two or more thereof can be used in combination.
[0098] The phenol curing agent is preferably blended in an equivalent ratio (phenolic hydroxyl equivalent / epoxy equivalent) of 0.1 or more and less than 1.0 to the epoxy resin. This prevents unreacted phenol curing agent from remaining and improves moisture absorption and heat resistance.
[0099] The amount of spherical crystalline silica particles added to the resin composite composition of the present invention is preferably more than 70% by mass and less than 95% by mass from the viewpoint of heat resistance and thermal expansion coefficient, preferably more than 80% by mass and less than 95% by mass, and more preferably more than 85% by mass and less than 95% by mass. The reason is that if the amount of silica powder is too small, it is difficult to obtain the effect of improving the strength of the sealing material or inhibiting thermal expansion. In addition, if it is too much, regardless of the surface treatment of the silica powder, segregation caused by the agglomeration of silica powder in the composite material is more likely to occur, thereby making the viscosity of the composite material too large. Because of these problems, it is difficult to be practical as a sealing material.
[0100] As the silane coupling agent, a known silane coupling agent can be used, and a silane coupling agent having an epoxy functional group is preferred.
[0101] Example
[0102] The present invention is explained by the following examples and comparative examples, but the present invention is not limited to the following examples.
[0103] (Example 1 to Example 3)
[0104] Amorphous silica particles containing calcium are prepared by melt-blowing. After mixing lithium carbonate particles with the spherical amorphous silica particles, they are filled into an aluminum container and heat-treated in an atmospheric atmosphere (atmospheric pressure) using an electric furnace SUPER-BURN (manufactured by MOTOYAMA Co., Ltd.). Relative to the total mass of the mass of the spherical amorphous silica and the mass of lithium converted to oxide, the mixing amount of lithium carbonate is set to 0.25% by mass in terms of oxide conversion, and the calcium contained in the amorphous silica particles is set to 0.004% by mass in terms of oxide conversion. The temperature is raised to 900°C (Example 1), 1000°C (Example 2), and 1100°C (Example 3) at a heating rate of 300°C / hour and maintained for 6 hours. Thereafter, it is cooled to room temperature at a cooling rate of approximately 100°C / hour.
[0105] (Example 4 to Example 6)
[0106] Amorphous silica particles containing calcium are prepared by melt-blowing. The calcium contained in the amorphous silica particles is set to 0.0040 mass%. Relative to the total mass of the mass of the spherical amorphous silica and the mass of lithium converted to oxide, lithium carbonate is mixed in oxide conversion at 0.10 mass% (Example 4), 0.07 mass% (Example 5), and 0.05 mass% (Example 6). The temperature is raised to 930°C (Example 4), 1030°C (Example 5), and 1130°C (Example 6) at a heating rate of 300°C / hour and maintained for 6 hours. Then, it is cooled to room temperature at a heating rate of 100°C / hour.
[0107] (Example 7 to Example 9)
[0108] Amorphous silica particles containing calcium were prepared by melt-blowing. Relative to the total mass of the mass of spherical amorphous silica and the mass of lithium converted to oxide, 0.25 mass% of lithium carbonate particles were mixed in terms of oxide, and the calcium contained in the amorphous silica particles was 0.24 mass% in terms of oxide. The temperature was raised to 900°C (Example 7), 1000°C (Example 8), and 1100°C (Example 9) at a heating rate of 300°C / hour and maintained for 6 hours. Otherwise, heat treatment was performed in the same manner as in Example 1.
[0109] (Example 10 to Example 12)
[0110] Amorphous silica particles containing calcium were prepared by melt-blowing. Relative to the total mass of the mass of spherical amorphous silica and the mass of lithium converted to oxide, 0.25% by mass of lithium carbonate particles were mixed in terms of oxide, and the calcium contained in the amorphous silica particles was 0.66% by mass in terms of oxide. Then, the temperature was raised to 900°C (Example 10), 1000°C (Example 11), and 1100°C (Example 12) at a heating rate of 300°C / hour and maintained for 6 hours. Then, the mixture was cooled to room temperature at a cooling rate of approximately 100°C / hour.
[0111] (Example 13, Example 14)
[0112] Amorphous silica particles containing calcium were prepared by melt-blowing. Relative to the total mass of the mass of spherical amorphous silica and the mass of lithium converted to oxide, 0.05 mass% of lithium carbonate particles were mixed in terms of oxide, and the calcium contained in the amorphous silica particles was 0.66 mass% in terms of oxide. Then, the temperature was raised to 925°C in Example 13 and to 1080°C in Example 14 at a heating rate of 300°C / hour. Then, the temperature was maintained for 6 hours in Example 13 and for 24 hours in Example 14, and heat treatment was performed in the same manner as in Example 1 except that the temperature was maintained for 6 hours in Example 13 and for 24 hours in Example 14.
[0113] (Example 15, Example 16)
[0114] Amorphous silica particles containing calcium were prepared by melt-blowing. Relative to the total mass of the mass of spherical amorphous silica and the mass of lithium converted to oxide, lithium carbonate particles were mixed in an oxide conversion of 0.10 mass% (Example 15) and 0.02 mass% (Example 16), and the calcium contained in the amorphous silica particles was 0.66 mass% in oxide conversion. Then, the temperature was raised to 925°C in Example 15 and to 950°C in Example 16 at a heating rate of 300°C / hour. Then, the temperature was maintained for 6 hours, and heat treatment was performed in the same manner as in Example 1 except for this.
[0115] (Example 17 to Example 20)
[0116] Amorphous silica particles are prepared by melt-blowing. After mixing calcium hydroxide particles and lithium carbonate particles into the spherical amorphous silica particles, they are filled into an aluminum container and heat-treated in an atmospheric atmosphere (atmospheric pressure) using an electric furnace SUPER-BURN (manufactured by MOTOYAMA Co., Ltd.). Relative to the mass of the spherical amorphous silica and the total mass of the mass of calcium converted to oxide and the mass of lithium converted to oxide, the mixed amount of calcium hydroxide is 0.48% by mass in terms of oxide, and the mixed amount of lithium carbonate is 0.04% by mass (Example 17), 0.06% by mass (Example 18), 0.08% by mass (Example 19), and 0.10% by mass (Example 20) in terms of oxide. The temperature is raised to 925°C at a heating rate of 300°C / hour and maintained for 12 hours. Thereafter, the mixture is cooled to room temperature at a cooling rate of approximately 100°C / hour.
[0117] (Example 21, Example 22)
[0118] Amorphous silica particles containing calcium and lithium were prepared by melt-blowing. The spherical amorphous silica particles were filled into an aluminum container and heat-treated in an atmospheric atmosphere (atmospheric pressure) using an electric furnace SUPER-BURN (manufactured by MOTOYAMA Co., Ltd.). The amorphous silica particles contained 0.82% by mass of calcium in terms of oxide and 0.08% by mass of lithium in terms of oxide. The temperature was raised to 950°C (Example 21) and 1050°C (Example 22) at a heating rate of 300°C / hour and maintained for 24 hours. Thereafter, the mixture was cooled to room temperature at a cooling rate of approximately 100°C / hour.
[0119] In addition, amorphous silica particles containing lithium were prepared by melt-blowing. After the calcium compound particles were mixed with the spherical amorphous silica particles, the spherical amorphous silica particles were filled into an aluminum container and heat-treated at 850° C. to 1150° C. in an air atmosphere (atmospheric pressure) using an electric furnace SUPER-BURN (produced by MOTOYAMA Co., Ltd.).
[0120] (Comparative Example 1)
[0121] Amorphous silica particles containing 0.004 mass % of calcium in terms of oxide were prepared by melt-blowing. The spherical amorphous silica particles were not mixed with lithium carbonate particles, and then heated to 900° C. at a heating rate of 300° C. / hour and maintained for 6 hours, and were heat-treated in the same manner as in Example 1.
[0122] (Comparative Example 2)
[0123] Amorphous silica particles containing calcium were prepared by melt-blowing. Relative to the total mass of the mass of spherical amorphous silica and the mass of lithium converted to oxide, 0.25 mass % of lithium carbonate particles were mixed in terms of oxide, and 0.004 mass % of calcium contained in the amorphous silica particles was converted to oxide, and then the temperature was raised to 1200° C. at a heating rate of 300° C. / hour and maintained for 6 hours. Except for this, the heat treatment was performed in the same manner as in Example 1.
[0124] (Comparative Example 3, Comparative Example 4)
[0125] Amorphous silica particles containing calcium were prepared by melt-blowing. Relative to the total mass of the mass of spherical amorphous silica and the mass of lithium converted to oxide, 0.25 mass % of lithium carbonate particles were mixed in terms of oxide, and 0.24 mass % of calcium contained in the amorphous silica particles was converted to oxide, and then the temperature was raised to 1200°C (Comparative Example 3) and 800°C (Comparative Example 4) at a heating rate of 300°C / hour and maintained for 6 hours. Otherwise, heat treatment was performed in the same manner as in Example 1.
[0126] (Comparative Example 5)
[0127] Amorphous silica particles containing calcium were prepared by melt-blowing. 0.25% by mass of lithium carbonate particles were mixed in terms of oxides relative to the total mass of the mass of spherical amorphous silica and the mass of lithium converted to oxides, and 0.0014% by mass of calcium contained in the amorphous silica particles was converted to oxides, and then the temperature was raised to 900° C. at a heating rate of 300° C. / hour and maintained for 6 hours. Except for this, the heat treatment was performed in the same manner as in Example 1.
[0128] (Comparative Example 6)
[0129] Amorphous silica particles containing calcium were prepared by melt-blowing. 0.01% by mass of lithium carbonate particles were mixed in terms of oxide relative to the total mass of the mass of spherical amorphous silica and the mass of lithium converted to oxide, and 0.66% by mass of calcium contained in the amorphous silica particles was converted to oxide, and then the temperature was raised to 925° C. at a heating rate of 300° C. / hour and maintained for 6 hours. Except for this, the heat treatment was performed in the same manner as in Example 1.
[0130] (Comparative Example 7)
[0131] Amorphous silica particles containing 0.66% by mass of calcium in terms of metal were prepared by melt-blowing. The spherical amorphous silica particles were not mixed with lithium carbonate particles, and then heated to 1100° C. at a heating rate of 300° C. / hour for 6 hours, and otherwise heat treated in the same manner as in Example 1.
[0132] The ratio of amorphous and crystalline silica in the silica particles obtained by heat treatment, as well as the type and ratio of crystalline silica, are determined by XRD. In the present invention, an X-ray diffraction apparatus "D2 PHASER" (manufactured by BRUKER CORPORATION) is used. Quantitative analysis of the crystalline phase by the Rietveld method is performed by a crystal structure analysis software "TOPAS" (manufactured by BRUKER CORPORATION).
[0133] The circularity is determined by dynamic particle image analysis. In the present invention, a dynamic particle image analyzer "FPIA-3000" (manufactured by Spectris Co., Ltd.) is used.
[0134] The content of impurity elements such as lithium and calcium in the spherical silica particles of the present invention is measured by ICP mass analysis (ICP-MS). Specifically, the measurement is performed using ICP-MS ("7700X" manufactured by Agilent) in accordance with JIS-K0133. An aqueous solution in which the silica particles are completely dissolved by hydrofluoric acid is used as a sample. Here, the content of impurity elements contained in the silica particles is taken as the content of impurity elements in the silica solution. The standard curve uses a base solution containing only the reagent.
[0135] The average particle size (D50) of the spherical quartz particles is measured by a laser diffraction / scattering particle size distribution measuring method. In the present invention, a laser diffraction / scattering particle size distribution measuring apparatus "CILAS920" (manufactured by Silas Corporation) is used.
[0136] The spherical crystalline silica particles obtained in the examples of the present invention have a lithium content in the range of 0.02 mass % or more and less than 0.40 mass % in terms of oxide conversion, and contain a crystalline silica phase, the proportion of the crystalline silica phase in the spherical crystalline silica particles is 40.0% or more, and the proportion of quartz in the crystalline silica phase is 80 mass % or more. The circularity of the spherical crystalline silica particles in the examples of the present invention is 0.83 to 0.95.
[0137] The average particle size of the spherical amorphous silica particles containing 0.004 mass % of calcium in terms of oxide is 35.1 μm, whereas the average particle size of the spherical crystalline silica particles of the present invention using this raw material is 35.2 μm to 35.6 μm.
[0138] The average particle size of the spherical amorphous silica particles containing 0.24 mass % of calcium was 33.8 μm, whereas the average particle size of the spherical crystalline silica particles of the present invention using this raw material was 33.3 μm to 33.9 μm.
[0139] The spherical amorphous silica particles containing 0.66 mass % of calcium in terms of oxide had a size of 41.1 μm, whereas the spherical crystalline silica particles of the present invention using this raw material had a size of 40.9 μm to 41.5 μm.
[0140] In addition, when a mixed raw material powder obtained by mixing a calcium raw material containing 0.48 mass % of calcium as oxide and a lithium raw material containing 0.04 to 0.10 mass % of lithium as oxide into amorphous silica particles is heat treated, the average particle size of the spherical amorphous silica particles is 32.3 μm, while the average particle size of the spherical crystalline silica particles of the present invention using the mixed raw material powder is 31.6 μm to 35.1 μm.
[0141] Furthermore, the average particle size of the spherical amorphous silica particles containing 0.82 mass % and 0.08 mass % of calcium and lithium respectively in terms of oxides was 21.5 μm, whereas that of the spherical crystalline silica particles of the present invention using the same raw materials was 20.3 μm and 21.9 μm.
[0142] Comparing Example 1 and Example 7 with Comparative Example 5, it can be seen that although the lithium content is the same as 0.25 mass%, the calcium content is higher than 0.004 mass% in terms of oxide conversion, so that the proportion of the crystalline silica phase in the spherical crystalline silica particles exceeds 40.0%. It can be seen that the synergistic effect of the coexistence of calcium and lithium elements is exhibited, and crystallization is promoted. Further observing Comparative Example 1, even if it contains 0.004 mass% of calcium in terms of oxide conversion, crystallization cannot be carried out if lithium is not added. It can be seen that the coexistence of lithium and calcium is necessary.
[0143] Comparison of Examples 4 to 6 and Examples 13 to 16 with Comparative Examples 6 and 7 revealed that the lower limit of the amount of lithium added is 0.02 mass %.
[0144] Comparing Examples 1 to 3 with Comparative Example 2, and comparing Examples 7 to 9 with Comparative Example 3, it can be seen that if the heat treatment temperature is high, the cristobalite content will increase, and the proportion of quartz in the crystalline silica phase will be less than 80% by mass at 1200°C. Furthermore, comparing Examples 7 to 9 with Comparative Example 4, it can be seen that when the heat treatment temperature is 800°C, crystallization does not proceed, and the proportion of the crystalline silica phase in the spherical crystalline silica particles is less than 40%. The preferred heat treatment temperature is 850°C to 1150°C. The more preferred temperature range is 875°C to 1100°C.
[0145] Comparing Example 12 with Comparative Example 7, even if the content of calcium is 0.66% or more in terms of oxide conversion, if the amount of lithium added is not added, the proportion of the crystalline silica phase in the spherical crystalline silica particles is 11.4%, which is less than 40.0%. When lithium is 0.02% or more in terms of oxide conversion, the proportion of the crystalline silica phase in the spherical crystalline silica particles exceeds 40%, and the proportion of quartz in the crystalline silica phase exceeds 80% by mass. It can be seen that the high quartz crystallization rate is a synergistic effect brought about by the coexistence of calcium and lithium. It should be noted that even if the content of lithium or calcium is increased (0.02% or more in terms of lithium oxide conversion, 0.004% or more in terms of calcium oxide conversion), there will be no problem in terms of crystallinity & quartzization, and the proportion of the crystalline silica phase in the spherical crystalline silica particles is 40.0% or more, and the proportion of quartz in the crystalline silica phase exceeds 80% by mass.
[0146] The zinc content of the spherical crystalline silica particles of the examples and comparative examples of the present invention is less than 1.0 ppm in terms of metal conversion, and the total of alkali metals (K and Na) other than lithium is 24 to 36 ppm in terms of metal conversion, the total of alkaline earth metals (Mg + Ba) other than calcium is 1.8 to 42 ppm, and the metal aluminum is 90 to 4552 ppm. These metal impurities other than lithium and calcium may be contained in silica within a range that does not affect crystallization.
[0147] Table 1
[0148]
[0149] Table 2
[0150]
[0151] Table 3
[0152]
[0153] Table 4
[0154]
[0155] Industrial application possibilities
[0156] The spherical crystalline silica particles of the present invention are not limited to semiconductor sealing materials, but can also be used for other purposes. Specifically, they can also be used as prepreg materials for printed boards or various engineering plastics.
Claims
1. A spherical crystalline silica particle having a circularity of 0.80 or more, containing 0.02 mass % or more and less than 0.40 mass % of lithium in terms of oxide, containing 0.004 mass % or more and less than 1.0 mass % of calcium in terms of oxide, and containing a crystalline silica phase, wherein: In the spherical crystalline silica particles, the ratio of the crystalline silica phase is 40.0% or more, and the ratio of quartz in the crystalline silica phase is 80.0% by mass or more. 2 . The spherical crystalline silica particles according to claim 1 , wherein the ratio of the crystalline silica phase is 70.0% or more, and the ratio of quartz in the crystalline silica phase is 85.0% by mass or more. 3 . The spherical crystalline silica particles according to claim 2 , wherein the ratio of the crystalline silica phase is 80.0% or more, and the ratio of quartz in the crystalline silica phase is 90.0% by mass or more. 4 . The spherical crystalline silica particles according to claim 1 , wherein the average particle size D50 is 3 to 100 μm.
5. The method for producing spherical crystalline silica particles according to any one of claims 1 to 4, comprising: A mixed raw material powder obtained by mixing a calcium raw material and a lithium raw material into spherical amorphous silica particles having a circularity of 0.80 or more is heat-treated at 850°C to 1150°C.
6. The method for producing spherical crystalline silica particles according to any one of claims 1 to 4, comprising: A mixed raw material powder obtained by mixing a lithium raw material with spherical amorphous silica particles having a circularity of 0.80 or more and containing a calcium component is heat-treated at 850°C to 1150°C.
7. The method for producing spherical crystalline silica particles according to any one of claims 1 to 4, comprising: A mixed raw material powder obtained by mixing a calcium raw material with spherical amorphous silica particles having a circularity of 0.80 or more and containing a lithium component is heat-treated at 850°C to 1150°C.
8. The method for producing spherical crystalline silica particles according to any one of claims 1 to 4, comprising: Spherical amorphous silica particles having a circularity of 0.80 or more and containing a calcium component and a lithium component are heat treated at 850°C to 1150°C. 9 . The method for producing spherical crystalline silica particles according to claim 5 , wherein the temperature of the heat treatment is 875° C. to 1110° C.
Citation Information
Patent Citations
Porous powder and method for producing the same
JP2002020111A
Spherical crystalline silica particles and method for producing same
WO2018186308A1
Silica powder, silica container, and method for producing the silica powder and container
CN102482137A
Preparation method of monocrystalline spherical silicon dioxide particles
CN103114333A
Silica-based composite fine particle dispersion and method for manufacturing same
CN109155246A