A method for preparing polyacrylonitrile preoxidized fiber and obtained polyacrylonitrile preoxidized fiber

By using thermal oil to circulate the drying unit and combining saturated steam drafting and heat setting processes, the problems of poor draftability, more hairs and broken wires in the pre-oxidation process of polyacrylonitrile primary wire are solved, which significantly improves the The quality and stability of the fiber.

CN115707801BActive Publication Date: 2024-11-29CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202110958157.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-20
Publication Date
2024-11-29
Estimated Expiration
2041-08-20

AI Technical Summary

Technical Problem

In the prior art, polyacrylonitrile raw wire has poor drafting performance, many wool and many broken wires during pre-oxidation.

Method used

The drying and densification unit with a circulating heating medium as a thermal oil is used to control the ratio of the standard deviation of the average temperature of each section of the heat roller surface to the average temperature ≤8%, and then saturated steam drafting and heat setting are carried out in turn to prepare polyacrylonitrile Pre-oxidized fibers.

Benefits of technology

The tensile performance of polyacrylonitrile raw silk in the pre-oxidation process is improved, and even eliminated wool and broken silk are reduced and even eliminated, achieving good technical results.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115707801B_ABST
    Figure CN115707801B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing polyacrylonitrile preoxidized fibers, and mainly solves the problems of poor drawing performance, many hairy fibers and many broken fibers in the preoxidation process of polyacrylonitrile raw fibers in the prior art. The present invention adopts a drying and densifying unit whose circulating medium is heat transfer oil, and performs drying and densification on polyacrylonitrile fibers with a crystallinity of 45 to 70%, a grain size of 3 to 9 nm and a crystal orientation of 60 to 80% after oiling, and controls the circulating flow rate of the heat transfer oil to be 10 to 40 m / s. 3 / h, the temperature for drying and densification is between 70 and 180°C, the CV value of the surface temperature of the drying and densification hot roller is ≤7%, and then saturated steam drawing and heat setting are carried out in sequence to obtain polyacrylonitrile precursor for pre-oxidation and prepare polyacrylonitrile pre-oxidized fibers. The technical solution has solved the problem well and can be used in the preparation process of polyacrylonitrile pre-oxidized fibers and (or) polyacrylonitrile-based carbon fibers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyacrylonitrile-based carbon fiber preparation, and specifically relates to a method for preparing polyacrylonitrile pre-oxidized fibers and the obtained polyacrylonitrile pre-oxidized fibers. Background Art

[0002] PAN-based carbon fiber is a kind of artificially synthesized inorganic fiber. It is a fibrous polymer obtained by a series of processes such as polymerization, spinning, pre-oxidation and carbonization of acrylonitrile and comonomer. During the spinning process, the PAN molecules mainly undergo physical changes to form white fibrous precursors. During the pre-oxidation process, the PAN precursors gradually evolve into a certain heat-resistant oxygen-containing structure. After carbonization, carbon fibers with extremely high carbon content are obtained. Since carbon fibers have high specific strength, high specific modulus, high temperature resistance and chemical corrosion resistance, their application fields are very wide.

[0003] The preparation of polyacrylonitrile precursor involves two major processes: the preparation of the stock solution and the spinning of the stock solution. The preparation of the stock solution includes three processes: polymerization, de-singling and degassing. The spinning of the stock solution includes more than a dozen processes such as filtration, metering, coagulation, hot water drawing, washing, oiling, drying and densification, steam drawing, heat setting and winding. As mentioned above, the drawing processes used in the preparation of the precursor include hot water drawing and saturated water vapor drawing. The drawing process is the inevitable choice to achieve fine denier and high reinforcement of the precursor. High-quality PAN precursor is the first prerequisite for the manufacture of high-performance carbon fiber, and it is also one of the most critical factors affecting the quality of carbon fiber. The production of high-quality PAN precursor places high demands on spinning equipment and processes, especially on process parameters.

[0004] The drying and densification of polyacrylonitrile precursor is a very important link in the spinning process. Polyacrylonitrile precursor with good density is the prerequisite for the preparation of high-strength carbon fiber. The higher the degree of densification of polyacrylonitrile precursor, the better the mechanical properties of the prepared carbon fiber. Drying and densification are generally carried out by hot rollers. The lower the drying and densification temperature, the better, but if the temperature is too low, the pores in the fiber cannot be effectively weakened, resulting in a low degree of densification. Usually, a segmented drying and densification process is used to control the fiber drying to a moisture content of less than 2%. This slow densification of the fiber can prevent the formation of a skin-core structure and prevent the stranding.

[0005] During the production process of the raw silk, the fibers after boiling water drawing are in a swollen and porous state. This microstructure is not conducive to further high-multiple drawing. Through the drying and densification process under a certain tension, the pores can be closed and the fiber mesh structure becomes dense. This is an important and indispensable step to improve the mechanical properties of polyacrylonitrile-based carbon fibers. The drying and densification temperature must be higher than the glass transition temperature of the primary fiber, but lower than the thermochromic temperature (from white to slightly yellow). Generally, the drying and densification is carried out at 120℃~170℃ for 1~10min.

[0006] In the production of polyacrylonitrile precursor by dimethyl sulfoxide method, a multi-stage hot roller drying process is adopted. By optimizing the drying temperature of each stage, the formation of the skin-core structure is suppressed while ensuring the drying and densification of the fiber, thus solving the brittleness problem of the carbon fiber. The drying and densification temperature of polyacrylonitrile precursor has a certain influence on the bonding strength of the carbon fiber. When drying with a hot roller at one end, the drying temperature needs to be 140°C to achieve drying and densification. However, after the carbonization of the polyacrylonitrile precursor prepared by this process, the carbon fiber is relatively brittle, and its bonding strength value is in the range of 33N to 67N, and there are many hairy fibers. When drying with a multi-stage hot roller, the drying temperature can be 110°C to 120°C to achieve the drying and densification of the fiber, and the bonding strength value of the carbon fiber reaches 106N to 141N, reaching the level of general-grade carbon fiber products, and its brittleness has been significantly improved.

[0007] With the increase of drying temperature, the drying time can be appropriately shortened. At 120℃~150℃, it only takes 1min~1.5min to achieve the drying and densification of polyacrylonitrile precursor. The two drying modes of lower temperature-long residence time or higher temperature-short residence time drying have no obvious effect on the structural density of polyacrylonitrile precursor. The X-ray diffraction intensity of polyacrylonitrile precursor is higher under the lower temperature-long drying mode, indicating that the formed crystal structure is more perfect, which is conducive to improving the brittleness of carbon fiber.

[0008] Chinese patent CN102899743A discloses a drying and densification heating device for polyacrylonitrile-based carbon fiber precursor, wherein the gearbox is located in the middle of the main shaft, the roller and the slip ring are located on both sides of the gearbox, the roller is located at one end of the main shaft, the slip ring is fixed at the other end of the main shaft, and the gear is located in the gearbox near the slip ring. The connecting ring mounting sleeve of the roller is sleeved and fixed on the main shaft, and the heating tube sleeve is located between the shell of the roller and the connecting ring mounting sleeve, and sleeved on the connecting ring mounting sleeve. The outer connecting ring and the inner connecting ring are respectively fixed on the end face of the connecting ring mounting sleeve. A plurality of heating tube mounting holes and heat dissipation holes are evenly distributed on the end face of the heating tube sleeve. The above patent evenly distributes electric heating tubes with the same power in the roller, so that the roller surface temperature is uniform, the working temperature range is relatively wide, and it can meet the requirements of the drying and densification process of the precursor. The electrical system used in the above patent has low requirements, high control accuracy, good thermal stability, and improves the uniformity of the roller surface temperature, thereby effectively improving the quality and quality stability of the polyacrylonitrile precursor. The above patent adopts electric heating to heat the roller. Since the electrical system adopted has low requirements, high control accuracy and good thermal stability, the uniformity of roller surface temperature is improved, thereby effectively improving the quality and quality stability of polyacrylonitrile precursor. Compared with hot water, high-pressure steam and thermal oil as heat circulation media, the above patent adopts electric heating. The temperature uniformity of the surface of the electrically heated drying and densification hot roller is relatively poor. In addition, due to the unique structural design of the electrically heated drying and densification hot roller, some internal components are easily damaged and the replacement frequency is high. Summary of the invention

[0009] The technical problem to be solved by the present invention is that the polyacrylonitrile precursor in the prior art has poor stretchability, many hairy fibers and many broken fibers during the pre-oxidation process. A preparation method for polyacrylonitrile pre-oxidized fibers is provided, which adopts a drying and densification unit whose circulating heating medium is heat transfer oil, controls the ratio of the standard deviation of the average surface temperature of each section of hot roller during drying and densification to the average temperature to be ≤8%, and then sequentially performs saturated steam drawing and heat setting to obtain polyacrylonitrile precursor for pre-oxidation to prepare polyacrylonitrile pre-oxidized fibers.

[0010] One of the purposes of the present invention is to provide a method for preparing polyacrylonitrile pre-oxidized fibers, comprising subjecting polyacrylonitrile primary fibers to oiling, drying and densification, and pre-oxidation treatment to obtain polyacrylonitrile pre-oxidized fibers, wherein the ratio of the standard deviation of the average surface temperature of the drying and densification hot roller to the average temperature is ≤8%.

[0011] Specifically, the preparation method comprises: extruding and coagulating the polyacrylonitrile spinning stock solution to obtain polyacrylonitrile primary fibers, then subjecting the fibers to hot water drawing, water washing, oiling, drying and densification, steam drawing and heat setting to obtain polyacrylonitrile fiber precursors, and then subjecting the fibers to pre-oxidation treatment to obtain polyacrylonitrile pre-oxidized fibers.

[0012] In the above preparation method: the molecular weight of the polyacrylonitrile is 50,000 to 90,000, the molecular weight distribution is 2.0 to 5.0, and the viscosity at 60°C is 50 to 90 Pa·s; the filament bundle of the polyacrylonitrile primary fiber is 1 to 50K, preferably 1 to 12K, more preferably 1K, 3K, 6K or 12K. Correspondingly, a 1 to 50K spinneret, preferably a 1 to 12K spinneret, more preferably a 1K, 3K, 6K or 12K spinneret can be used in the coagulation molding step.

[0013] In the above preparation method:

[0014] The spinneret extrusion and coagulation molding can be completed using the equipment and process conditions commonly used in the art. Preferably, the spinneret extrusion temperature is 30-80°C, the coagulation molding temperature is 20-70°C, and the coagulation molding draft ratio is 0.5-1.5;

[0015] The temperature of the hot water drawing is 70-99°C, preferably 85-95°C; the total drawing ratio of the hot water drawing is 350-700%; the hot water drawing is performed in at least two stages, wherein the temperature of each hot water drawing is increased successively, and the drawing ratios are the same or different;

[0016] The water washing temperature is 40-80°C; the water washing is performed in at least two steps, and preferably, the water washing is performed in a step-by-step heating manner with a heating gradient of 4-20°C / step.

[0017] In the above preparation method:

[0018] The oiling process can be completed by using the commonly used equipment and oiling process in the art. Preferably, the mass concentration of the oil used is in the range of 0.5-5%, and the oiling operation is completed at room temperature.

[0019] In the oiling process, the width of the tow after oiling is greater than the width of the tow before oiling, and the ratio of the width of the tow after oiling to the width of the tow before oiling is greater than 1.5:1. Preferably, the ratio of the width of the tow after oiling to the width of the tow before oiling is greater than 2.0:1.

[0020] The crystallinity of the oiled polyacrylonitrile spun fibers is 45-70%, the grain size is 3-9 nm, and the crystal region orientation is 60-80%; preferably, the crystallinity of the oiled polyacrylonitrile spun fibers is 50-60%, the grain size is 5-8 nm, and the crystal region orientation is 65-75%; wherein the crystallinity and grain size are obtained by the analysis results of equatorial scanning in X-ray diffraction; the orientation refers to the crystal region orientation, which is obtained by the analysis results of azimuth scanning in X-ray diffraction;

[0021] The moisture content of the polyacrylonitrile primary fiber after oiling is 20-100%, preferably 30-50%; the oiling time is 0.2-3s, preferably 0.5-1s.

[0022] The present invention firstly adjusts the extrusion temperature, coagulation bath temperature and coagulation drawing ratio within the range according to different spinneret parameters during the spinning dope extrusion and coagulation forming process; and secondly adjusts the hot water drawing temperature, drawing ratio and water washing temperature and number of passes so that the obtained primary fiber has a grain size and crystal content within the specific range described in the present invention after oiling.

[0023] In the above preparation method:

[0024] The circulating heating medium used in the drying and densification is heat transfer oil;

[0025] The drying and densification is divided into at least two stages, the treatment temperature of each stage is 60-180°C, preferably 70-130°C; the treatment time of each stage is 40-180s, preferably 40-150s; the circulation flow rate of the heat transfer oil in each stage is 10-40m 3 / h, preferably 15 to 30 m 3 / h; the number of hot rollers used in each section is 3 to 12, preferably 5 to 10, more preferably 5, 7 or 9; the ratio of the standard deviation of the average temperature of the surface of each hot roller to the average temperature (CV value) is ≤8%, preferably ≤5%, wherein the surface temperature of the hot roller refers to the average temperature of the surfaces of 3 to 12 drying and densification hot rollers. The CV value can reflect the temperature uniformity of the drying and densification device, including the difference between the temperatures of the surfaces of the drying and densification hot rollers, or the difference between the temperatures of the rotating joint surfaces of the drying and densification hot rollers, or the difference between the temperatures of the heat transfer oil on the circulation branch at the outlet of the rotating joint connected to the drying and densification hot rollers. The surface temperature CV value of the drying and densification hot roller can be obtained by any of the above temperature differences.

[0026] In the above preparation method, the steam stretching and heat setting can be implemented using equipment and process conditions commonly used in the art. Preferably, the steam stretching pressure is 0.10-0.60 MPa, the stretching ratio is 1.0-4.0, the heat setting pressure is 0.05-0.40 MPa, and the heat setting ratio is 0.80-1.20.

[0027] In the above preparation method:

[0028] The pre-oxidation is provided with at least five temperature zones, and each temperature zone is completed in a normal pressure heat stabilization furnace in an air atmosphere;

[0029] The pre-oxidation temperature is 190-270°C, and the pre-oxidation temperature zone adopts a step-by-step heating method, with a temperature gradient of 10-30°C / pass. For example, five atmospheric pressure heat stabilization furnaces with air atmosphere are used, and the temperatures are 190-210°C, 210-215°C, 225-235°C, 245-255°C, and 260-265°C, respectively. The treatment time of each pre-oxidation temperature zone is 5-12 minutes; the pre-oxidation treatment time is 45-60 minutes;

[0030] The total drafting multiple of the polyacrylonitrile precursor in the pre-oxidation treatment stage is 2-10, preferably 4-8.

[0031] In the above preparation method, the fineness of the obtained polyacrylonitrile precursor is 0.5-1.5 dtex; the moisture content of the polyacrylonitrile precursor is 0.5-2%, and the oil content is 0.5-2%; preferably, the moisture content of the polyacrylonitrile precursor is 0.8-1.2%, and the oil content is 0.8-1.2%.

[0032] The second object of the present invention is to provide a polyacrylonitrile pre-oxidized fiber prepared by the above-mentioned preparation method.

[0033] The present invention adopts a drying and densification unit whose circulating heating medium is heat transfer oil, and controls the circulating flow rate of the heat transfer oil to be between 10 and 40 m 3 / h, the temperature for drying and densification is between 70 and 180°C, and the CV value of the surface temperature of the drying and densification hot roller is ≤7%, and then saturated steam drawing and heat setting are carried out in sequence to obtain polyacrylonitrile precursor for pre-oxidation to prepare polyacrylonitrile pre-oxidized fiber. Controlling the difference between the surface temperatures of the drying and densification hot rollers (i.e., the CV value) can improve the uniformity of the degree of drying and densification of the fibers, so that each fiber in the tow is dried and densified to a uniform degree. After drying and densification, the difference in the aggregated structure between each fiber in the original tow is minimal, and it is not easy to break and deform during the pre-oxidation process.

[0034] Furthermore, through research, it is found that the grain size and the content of the crystalline region of the primary fiber are closely related to the pre-oxidation process. During the pre-oxidation process, the drafting is carried out, and the pre-oxidation process first starts from the amorphous region and then slowly spreads to the crystalline region. The smaller the grains, the earlier the pre-oxidation process is carried out, the more and faster the channels for the pre-oxidation process to extend, and the more crystalline region content increases, which will inevitably increase the difficulty of the pre-oxidation process; and the crystalline region orientation of the primary fiber is more closely related to the pre-oxidation drafting. The larger the crystalline region orientation, the less likely it is to stretch during the pre-oxidation process, and the higher the probability of producing hairy and broken fibers. Therefore, the drying and densification step of the present invention with a drying temperature of 70 to 180°C and a CV value of the surface temperature of the drying and densification hot roller ≤7% for the polyacrylonitrile fiber with a crystallinity of 45 to 70% after oiling, a grain size of 3 to 9nm, and a crystalline region orientation of 60 to 80% can further effectively improve the quality and quality stability of the polyacrylonitrile precursor.

[0035] By adopting the technical solution provided by the present invention, the tensile properties of polyacrylonitrile precursor fibers during the pre-oxidation process can be improved, and the hairy fibers and (or) broken fibers of the polyacrylonitrile precursor fibers during the pre-oxidation process can be reduced or even eliminated, thereby achieving better technical effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 : is the equatorial scanning curve of the X-ray diffraction of the polyacrylonitrile nascent fiber obtained in Example 1, wherein the abscissa is the 2θ diffraction angle and the ordinate is the diffraction intensity of the equatorial scanning of the polyacrylonitrile nascent fiber. Figure 1 As shown, after Lorentz peak separation, three peak separation curves are obtained, namely curve a, curve b and curve c. The Lorentz peaks corresponding to the three curves are peak 1, peak 2 and peak 3, wherein peak 1 and peak 3 are crystalline peaks, and peak 2 is an amorphous peak.

[0037] Figure 2 This is an azimuth scanning curve of the X-ray diffraction of the polyacrylonitrile primary fiber obtained in Example 1, wherein the abscissa is the azimuth angle, and the ordinate is the diffraction intensity of the azimuth scanning of the polyacrylonitrile primary fiber. DETAILED DESCRIPTION

[0038] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the scope of protection of the present invention.

[0039] The test instruments and test conditions used in the examples are as follows:

[0040] CV value test:

[0041] The temperature uniformity of the drying and densification device mainly refers to the difference between the temperatures on the surface of the drying and densification hot roller, or the difference between the temperatures on the surface of the rotary joint of the drying and densification hot roller, or the difference between the temperatures of the heat transfer oil on the circulation branch at the outlet of the rotary joint connected to the drying and densification hot roller. The above temperature differences are all expressed by the CV value of the temperature. The surface temperature of the drying and densification hot roller is measured and recorded using a surface thermocouple (WRNM-201A, Shanghai Automation Instrument Factory No. 3) and a pocket temperature digital display (XMX-01, K = 0 ~ 1000 ° C, Shanghai Automation Instrument Factory No. 3). The surface temperature of the rotary joint of the drying and densification hot roller is measured and recorded using a portable infrared thermometer. The temperature of the heat transfer oil on the circulation branch at the outlet of the rotary joint connected to the drying and densification hot roller is measured and recorded using a PT100, 0 ~ 200 ° C, Class A precision armored platinum thermal resistor (with temperature sensor) Measure and record the temperature of the heat transfer oil on the circulation branch at the outlet of the rotary joint connected to the drying and densification hot roller.

[0042] Moisture content test:

[0043] Weigh a certain mass of polyacrylonitrile fiber (<3g), record the mass as m1, dry the polyacrylonitrile fiber in a blast oven at 80℃ for 1 hour, weigh the mass of the polyacrylonitrile fiber, record the mass as m2, the moisture content of the polyacrylonitrile fiber is equal to the ratio of (m1-m2) to m1, and the ratio is expressed as a percentage.

[0044] Oil content test:

[0045] Weigh a certain mass of polyacrylonitrile precursor (<3g), record the mass as m3, dry the polyacrylonitrile precursor in a blast oven at 80°C for 2 hours, weigh the mass of the polyacrylonitrile precursor, record the mass as m4, the moisture content of the polyacrylonitrile precursor is equal to the ratio of (m3-m4) to m3, and the ratio is expressed as a percentage. Perform Soxhlet extraction on the dried polyacrylonitrile precursor, the solvent is cyclohexane, reflux at 110°C for 3 hours, take it out and dry it in the air for 1 hour, then dry it in a blast oven at 105°C for 2 hours, weigh the mass of the dried polyacrylonitrile precursor, record the mass as m5, the oil content of the polyacrylonitrile precursor is equal to the ratio of (m4-m5) to m3, and the ratio is expressed as a percentage.

[0046] Crystallinity and grain size calculation:

[0047] The polyacrylonitrile spun fibers (filaments) were dehydrated and dried in a blast oven at 80°C for 1 hour. The dried polyacrylonitrile spun fibers (filaments) were subjected to X-ray diffraction (XRD) analysis. The test conditions were D8 Discover micro-focus spot diffractometer from Bruker, Germany, with micro-focus spot; voltage and current: 50KV×1000μA; angle reproducibility: 0.0001°; spot size: diameter 0.3-2mm. The polyacrylonitrile spun fibers (filaments) were bound to a fixture, and X-rays were used to scan the equatorial and meridian directions of the fibers, and the azimuth angle of the polyacrylonitrile spun fibers was scanned.

[0048] The equatorial scanning curve of the polyacrylonitrile nascent fiber is shown in the attached Figure 1 As shown, the horizontal axis is the 2θ diffraction angle, and the vertical axis is the diffraction intensity of the equatorial scanning of the polyacrylonitrile fiber. The equatorial scanning curve must be deducted from the air background curve. The equatorial scanning curve is divided into three peaks by using the Lorentz peak division method. The position of peak 1 is 16.8°±0.2°; the position of peak 2 is 27.5°±0.2°; the position of peak 3 is 29.3°±0.2°; peaks 1 and 3 are crystalline peaks, and peak 2 is a non-crystalline peak. The peak half-height width of peak 1 is used to calculate the grain size.

[0049] The calculation method of crystallinity is as follows: after Lorentz peak separation, the peak areas of peak 1, peak 2 and peak 3 are expressed as A1, A2 and A3 respectively, the crystallinity is the ratio between the sum of A1 and A3 (expressed as A1+A3) and the sum of A1, A2 and A3 (expressed as A1+A2+A3), and the crystallinity is expressed as a percentage.

[0050] The calculation method of grain size is as follows: after Lorentz peak separation, the position of peak 1 corresponds to a diffraction angle of 2θ (2θ is approximately equal to 16.8°±0.2°); the wavelength of X-rays is 0.1542nm; K is a constant, and its value is 0.89; the half-width at half maximum of peak 1 is β, and the grain size is the ratio of the product of K and the wavelength of X-rays (expressed as Kλ) and the product of the half-width at half maximum of peak 1 (expressed in radians) and the cosine value of half the diffraction angle (βcosθ), and the unit of grain size is nm.

[0051] Calculation of crystal orientation degree:

[0052] The azimuth scanning curve of the polyacrylonitrile primary fiber is shown in the attached Figure 2As shown, the horizontal axis is the azimuth angle, and the vertical axis is the diffraction intensity of the azimuth scanning of the polyacrylonitrile primary fiber. The azimuth scanning curve from 0° to 90° is subjected to Lorentz fitting. After fitting, the peak width height of the diffraction peak is obtained. The crystal area orientation degree of the polyacrylonitrile fiber is calculated using an empirical formula. The crystal area orientation degree is the ratio between the difference between 180 and the peak half-height width of the diffraction peak and 180, and the crystal area orientation degree is expressed as a percentage.

[0053] The raw materials used in the examples are all commercially available products.

[0054] [Example 1]

[0055] 1. Preparation of stock solution: Add distilled acrylonitrile (AN) and itaconic acid (IA) in a ratio of 97:3, solid content of 20%, azobisisobutyronitrile (AIBN) accounting for 0.4wt% of the comonomer, and dimethyl sulfoxide (DMSO) as solvent into a reactor, and react at a constant temperature of 59°C for 20 hours under nitrogen protection to obtain a binary acrylonitrile copolymer spinning solution. Then, after the spinning solution is decompressed to remove residual monomers and bubbles, it is filtered through a 5μm filter material to obtain an acrylonitrile copolymer spinning stock solution. The molecular weight is tested for the viscosity average molecular weight of polyacrylonitrile using an Ubbelohde viscometer, and the viscosity is tested using a RHEOLab QC viscometer produced by Anton Paar. After testing, the molecular weight is 80021, the molecular weight distribution is 3.34, and the viscosity is 75Pa·s at 60°C.

[0056] 2. Coagulation: The spinning solution is metered by a metering pump, filtered again, extruded through a spinneret, and then put into a coagulation bath for coagulation. The extrusion temperature is 65°C, the coagulation bath temperature is 50°C, and the draft ratio of coagulation is 0.6. The primary fiber is obtained using a 3K spinneret.

[0057] 3. Drawing and washing: After the raw fiber is coagulated, it is drawn in hot water for 3 times. The temperature of hot water drawing is 86℃, 90℃ and 95℃. The multiples of each hot water drawing can be the same or different. The total drawing multiple is controlled to be 4.2. After hot water drawing, the filaments are washed in 6 times. The temperature is increased in steps. No drawing is performed during the washing process. The washing temperatures are 45℃, 50℃, 55℃, 60℃, 70℃ and 80℃ respectively.

[0058] 4. Oiling: The washed polyacrylonitrile spun fibers are oiled with an oil concentration of 3% at room temperature. The excess oil is squeezed out by an extrusion roller. The obtained oiled polyacrylonitrile spun fibers have a crystallinity of 57%, a grain size of 6.9 nm, and a crystal orientation of 72%.

[0059] 5. Drying and densification: Dry and densify the oiled polyacrylonitrile primary fibers. The moisture content of the oiled polyacrylonitrile primary fibers is 40%. The drying and densification is divided into two stages. The first stage of drying and densification temperature is 90°C, and the circulation flow rate of the heat transfer oil is 25m 3 / h, the number of drying and densification hot rollers is 7, the surface temperature CV value is 2.0%, and the duration is 50s; the second stage drying and densification temperature is 120℃, and the circulation flow rate of the heat transfer oil is 25m 3 / h, there are 7 drying and densification hot rollers, the surface temperature CV value is 2.5%, and the duration is 50s.

[0060] 6. Steam drawing and heat setting: The dried and densified polyacrylonitrile fiber is steam drawn and heat set. The steam drawing pressure is 0.40 MPa, the drawing ratio is 2.6, the heat setting pressure is 0.1 MPa, and the heat setting ratio is 0.90 to obtain polyacrylonitrile precursor. The fineness of the polyacrylonitrile precursor is 0.9 dtex, the moisture content is 1.2%, and the oil content is 1.1%.

[0061] 7. Pre-oxidation: The polyacrylonitrile precursor was heat stabilized in five air heat stabilization furnaces at temperatures of 205°C, 215°C, 230°C, 250°C and 265°C, respectively. The constant temperature zone of each pre-oxidation furnace was of equal length. The heat treatment time was 10 min and the total heat treatment time was 50 min.

[0062] During the pre-oxidation process, the total drafting multiple of the polyacrylonitrile precursor was 10%, and the average number of hairy fibers in 10 meters of pre-oxidized fiber was 2 per meter.

[0063] The pre-oxidized fiber was carbonized to obtain carbon fiber. The carbonization conditions were as follows: carbonization was carried out in a nitrogen atmosphere, the temperature of low-temperature carbonization was 370°C, the time was 3 minutes, and the draft ratio was 2%, and the temperature of high-temperature carbonization was 1380°C, the time was 3 minutes, and the draft ratio was -3%. The mechanical properties of the carbon fiber were tested. The mechanical properties of the carbon fiber were a breaking strength of 5.3 GPa, an elongation at break of 1.9%, and a tensile modulus of 291 GPa.

[0064] [Example 2]

[0065] The preparation process is the same as in Example 1, except that:

[0066] 2. Solidification molding: using 1K spinneret.

[0067] 4. Oiling: After oiling, the crystallinity of the polyacrylonitrile primary fiber is 55%, the grain size is 6.6nm, and the degree of orientation of the crystal area is 70%.

[0068] 5. Drying and densification: The moisture content of the primary polyacrylonitrile fiber after oiling is 33%. The drying and densification is divided into two stages. The first stage of drying and densification temperature is 80℃, and the circulation flow rate of the heat transfer oil is 30m 3 / h, the number of drying and densification hot rollers is 7, the surface temperature CV value is 3.0%, and the duration is 60s; the second stage drying and densification temperature is 115℃, and the circulation flow rate of the heat transfer oil is 30m 3 / h, 7 drying and densification hot rollers, surface temperature CV value of 2.0%, duration of 60s, and other aspects are the same as in Example 1.

[0069] 6. Steam drawing and heat setting: The fineness of polyacrylonitrile raw yarn is 0.8dtex, the moisture content is 1.0%, and the oil content is 1.3%.

[0070] During the pre-oxidation process, the total drafting percentage of the polyacrylonitrile precursor can reach 10%, and the average number of hairs in 10 meters of pre-oxidized fiber is 2 per meter.

[0071] The pre-oxidized fiber was carbonized in a nitrogen atmosphere, with a low-temperature carbonization temperature of 370°C, a time of 3 min, and a draft ratio of 2%. The high-temperature carbonization temperature was 1380°C, a time of 3 min, and a draft ratio of -3%. The mechanical properties of the carbon fiber were as follows: a breaking strength of 5.6 GPa, an elongation at break of 2.1%, and a tensile modulus of 296 GPa.

[0072] [Example 3]

[0073] The preparation process is the same as in Example 1, except that:

[0074] 2. Solidification molding: using 6K spinneret.

[0075] 4. Oiling: After oiling, the crystallinity of the polyacrylonitrile primary fiber is 58%, the grain size is 7.3nm, and the degree of orientation of the crystal area is 75%.

[0076] 5. Drying and densification: The moisture content of the raw polyacrylonitrile fiber after oiling is 45%. The drying and densification is divided into two stages. The first stage of drying and densification temperature is 85℃, and the circulation flow rate of the heat transfer oil is 20m 3 / h, the number of drying and densification hot rollers is 5, the surface temperature CV value is 1.5%, and the duration is 45s; the second stage drying and densification temperature is 125℃, and the circulation flow rate of the heat transfer oil is 20m 3 / h, 5 drying and densification hot rollers, surface temperature CV value of 2.0%, duration of 45s, and other aspects are the same as in Example 1.

[0077] 6. Steam drawing and heat setting: The fineness of polyacrylonitrile raw yarn is 1.2dtex, the moisture content is 1.3%, and the oil content is 1.2%.

[0078] Other conditions are the same as in Example 1.

[0079] During the pre-oxidation process, the total drafting percentage of the polyacrylonitrile precursor can reach 10%, and the average number of hairy fibers in 10 meters of pre-oxidized fiber is 3 per meter.

[0080] After the pre-oxidized fibers are carbonized, they are carbonized in a nitrogen atmosphere. The low-temperature carbonization temperature is 370°C, the time is 3 minutes, and the draft ratio is 2%. The high-temperature carbonization temperature is 1380°C, the time is 3 minutes, and the draft ratio is -3%. The mechanical properties of the carbon fibers are as follows: a breaking strength of 3.8 GPa, an elongation at break of 2.2%, and a tensile modulus of 235 GPa.

[0081] [Example 4]

[0082] The preparation process is the same as in Example 1, except that:

[0083] 2. Solidification molding: using 12K spinneret.

[0084] 4. Oiling: After oiling, the crystallinity of the polyacrylonitrile primary fiber is 59%, the grain size is 7.3nm, and the degree of orientation of the crystal area is 75%.

[0085] 5. Drying and densification: After oiling, the moisture content of the primary polyacrylonitrile fiber is 40%. The drying and densification is divided into two stages. The first stage of drying and densification temperature is 80℃, and the circulation flow rate of the heat transfer oil is 18m 3 / h, the number of drying and densification hot rollers is 7, the surface temperature CV value is 4.0%, and the duration is 50s; the second stage drying and densification temperature is 120℃, and the circulation flow rate of the heat transfer oil is 18m 3 / h, 7 drying and densification hot rollers, surface temperature CV value of 2.0%, duration of 50s, and other aspects are the same as in Example 1.

[0086] 6. Steam drawing and heat setting: The fineness of polyacrylonitrile raw yarn is 1.0 dtex, the moisture content is 1.0%, and the oil content is 1.0%.

[0087] Other conditions are the same as in Example 1.

[0088] During the pre-oxidation process, the total drafting percentage of the polyacrylonitrile precursor can reach 10%, and the average number of hairs in 10 meters of pre-oxidized fiber is 2 per meter.

[0089] After the pre-oxidized fibers are carbonized, they are carbonized in a nitrogen atmosphere. The low-temperature carbonization temperature is 395°C, the time is 3 min, and the draft ratio is 2%. The high-temperature carbonization temperature is 1360°C, the time is 3 min, and the draft ratio is -3%. The mechanical properties of the carbon fibers are as follows: a breaking strength of 5.4 GPa, an elongation at break of 2.1%, and a tensile modulus of 289 GPa.

[0090] [Example 5]

[0091] The preparation process is the same as in Example 1, except that:

[0092] 2. Solidification molding: using 12K spinneret.

[0093] 4. Oiling: After oiling, the crystallinity of the polyacrylonitrile primary fiber is 58%, the grain size is 7.2nm, and the degree of orientation of the crystal area is 73%.

[0094] 5. Drying and densification: The moisture content of the raw polyacrylonitrile fiber after oiling is 40%. The drying and densification is divided into two stages. The first stage of drying and densification temperature is 80℃, and the circulation flow rate of the heat transfer oil is 25m 3 / h, the number of drying and densification hot rollers is 5, the surface temperature CV value is 2.0%, and the duration is 40s; the second stage drying and densification temperature is 120℃, and the circulation flow rate of the heat transfer oil is 30m 3 / h, 5 drying and densification hot rollers, surface temperature CV value of 1.0%, duration of 40s, and other aspects are the same as in Example 1.

[0095] 6. Steam drawing and heat setting: The fineness of polyacrylonitrile raw yarn is 0.9dtex, the moisture content is 1.2%, and the oil content is 1.2%.

[0096] Other conditions are the same as in Example 1.

[0097] During the pre-oxidation process, the total drafting percentage of the polyacrylonitrile precursor can reach 10%, and the average number of hairs in 10 meters of pre-oxidized fiber is 2 per meter.

[0098] After the pre-oxidized fiber is carbonized, it is carbonized in a nitrogen atmosphere. The low-temperature carbonization temperature is 395°C, the time is 3 min, and the draft ratio is 2%. The high-temperature carbonization temperature is 1360°C, the time is 3 min, and the draft ratio is -3%. The mechanical properties of the carbon fiber are as follows: breaking strength 5.3 GPa, breaking elongation 2.0%, and tensile modulus 292 GPa.

[0099] [Example 6]

[0100] The preparation process is the same as in Example 1, except that:

[0101] 2. Solidification molding: using 3K spinneret.

[0102] 4. Oiling: After oiling, the crystallinity of the polyacrylonitrile primary fiber is 56%, the grain size is 7.1nm, and the degree of orientation of the crystal area is 74%.

[0103] 5. Drying and densification: The moisture content of the raw polyacrylonitrile fiber after oiling is 40%. The drying and densification is divided into two stages. The first stage of drying and densification temperature is 80℃, and the circulation flow rate of the heat transfer oil is 15m 3 / h, the number of drying and densification hot rollers is 7, the surface temperature CV value is 3.0%, and the duration is 55s; the second stage drying and densification temperature is 110℃, and the circulation flow rate of the heat transfer oil is 25m 3 / h, 7 drying and densification hot rollers, surface temperature CV value of 3.0%, duration of 55s, and other aspects are the same as in Example 1.

[0104] 6. Steam drawing and heat setting: The fineness of polyacrylonitrile raw yarn is 1.3dtex, the moisture content is 1.3%, and the oil content is 1.2%.

[0105] Other conditions are the same as in Example 1.

[0106] During the pre-oxidation process, the total drafting percentage of the polyacrylonitrile precursor can reach 10%, and the average number of hairs in 10 meters of pre-oxidized fiber is 3 per meter.

[0107] After the pre-oxidized fibers are carbonized, they are carbonized in a nitrogen atmosphere. The low-temperature carbonization temperature is 395°C, the time is 3 min, and the draft ratio is 2%. The high-temperature carbonization temperature is 1360°C, the time is 3 min, and the draft ratio is -3%. The mechanical properties of the carbon fibers are as follows: a breaking strength of 3.6 GPa, an elongation at break of 2.2%, and a tensile modulus of 239 GPa.

[0108] [Example 7]

[0109] The preparation method is the same as in Example 1, except that:

[0110] 2. Solidification molding: using 6K spinneret.

[0111] 4. Oiling: After oiling, the crystallinity of the polyacrylonitrile primary fiber is 57%, the grain size is 7.3nm, and the degree of orientation of the crystal area is 74%.

[0112] 5. Drying and densification: The moisture content of the nascent polyacrylonitrile fiber after oiling is 45%. The drying and densification is divided into two stages. The first stage of drying and densification temperature is 70°C, and the circulation flow rate of the heat transfer oil is 20m 3 / h, the number of drying and densification hot rollers is 9, the surface temperature CV value is 3.0%, and the duration is 60s; the second stage drying and densification temperature is 110℃, and the circulation flow rate of the heat transfer oil is 25m 3 / h, 9 drying and densification hot rollers, surface temperature CV value of 3.0%, duration of 60s, and other aspects are the same as in Example 1.

[0113] 6. Steam drawing and heat setting: The fineness of polyacrylonitrile raw yarn is 1.2dtex, the moisture content is 1.2%, and the oil content is 1.3%.

[0114] Other conditions are the same as in Example 1.

[0115] During the pre-oxidation process, the total drafting percentage of the polyacrylonitrile precursor can reach 10%, and the average number of hairs in 10 meters of pre-oxidized fiber is 1 / meter.

[0116] After the pre-oxidized fiber is carbonized, it is carbonized in a nitrogen atmosphere. The low-temperature carbonization temperature is 395°C, the time is 3 minutes, and the draft ratio is 2%. The high-temperature carbonization temperature is 1360°C, the time is 3 minutes, and the draft ratio is -3%. The mechanical properties of the carbon fiber are as follows: breaking strength 3.6 GPa, breaking elongation 2.1%, and tensile modulus 238 GPa.

[0117] [Example 8]

[0118] The preparation process is the same as in Example 1, except that:

[0119] 2. Solidification molding: using 6K spinneret.

[0120] 4. Oiling: After oiling, the crystallinity of the polyacrylonitrile primary fiber is 58%, the grain size is 7.4nm, and the degree of orientation of the crystal area is 74%.

[0121] 5. Drying and densification: The moisture content of the primary polyacrylonitrile fiber after oiling is 45%. The drying and densification is divided into two stages. The first stage of drying and densification temperature is 80℃, and the circulation flow rate of the heat transfer oil is 20m 3 / h, the number of drying and densification hot rollers is 5, the surface temperature CV value is 1.0%, and the duration is 40s; the second stage drying and densification temperature is 120℃, and the circulation flow rate of the heat transfer oil is 15m 3 / h, 5 drying and densification hot rollers, surface temperature CV value of 1.0%, duration of 40s, and other aspects are the same as in Example 1.

[0122] 6. Steam drawing and heat setting: The fineness of polyacrylonitrile raw yarn is 0.8dtex, the moisture content is 1.0%, and the oil content is 0.9%.

[0123] Other conditions are the same as in Example 1.

[0124] During the pre-oxidation process, the total drafting percentage of the polyacrylonitrile precursor can reach 10%, and the average number of hairs in 10 meters of pre-oxidized fiber is 2 per meter.

[0125] After the pre-oxidized fibers are carbonized, they are carbonized in a nitrogen atmosphere. The low-temperature carbonization temperature is 395°C, the time is 3 min, and the draft ratio is 2%. The high-temperature carbonization temperature is 1360°C, the time is 3 min, and the draft ratio is -3%. The mechanical properties of the carbon fibers are as follows: a breaking strength of 5.4 GPa, an elongation at break of 2.3%, and a tensile modulus of 295 GPa.

[0126] [Comparative Example 1]

[0127] The preparation process is the same as in Example 1, except that:

[0128] 2. Coagulation molding: the extrusion temperature is 40°C, the coagulation bath temperature is 35°C, the coagulation draft ratio is 0.48, and a 3K spinneret is used.

[0129] 4. Oiling: After oiling, the crystallinity of the polyacrylonitrile primary fiber is 42%, the grain size is 2.8nm, and the degree of orientation of the crystal area is 71%.

[0130] 5. Drying and densification: The moisture content of the nascent polyacrylonitrile fiber after oiling is 40%. The drying and densification is divided into two stages. The first stage of drying and densification temperature is 90°C, and the circulation flow rate of the heat transfer oil is 25m 3 / h, the number of drying and densification hot rollers is 7, the surface temperature CV value is 2.0%, and the duration is 50s; the second stage drying and densification temperature is 120℃, and the circulation flow rate of the heat transfer oil is 25m 3 / h, 7 drying and densification hot rollers, surface temperature CV value of 2.5%, duration of 50s, and other aspects are the same as in Example 1.

[0131] 6. Steam drawing and heat setting: The fineness of polyacrylonitrile raw yarn is 0.9dtex, the moisture content is 1.0%, and the oil content is 1.3%.

[0132] During the pre-oxidation process, the total drafting percentage of the polyacrylonitrile precursor can reach 10%, and the average number of filaments in 10 meters of pre-oxidized fiber is 5 / meter.

[0133] The pre-oxidized fiber was carbonized under the following conditions: carbonization was carried out in a nitrogen atmosphere, the low-temperature carbonization temperature was 370°C, the time was 3 min, the draft ratio was 2%, the high-temperature carbonization temperature was 1380°C, the time was 3 min, the draft ratio was -3%, and the mechanical properties of the obtained carbon fiber were a breaking strength of 4.6 GPa, an elongation at break of 2.1%, and a tensile modulus of 240 GPa.

[0134] [Comparative Example 2]

[0135] The preparation process is the same as in Example 1, except that:

[0136] 2. Coagulation molding: The extrusion temperature is 68°C, the coagulation bath temperature is 71°C, the coagulation draft ratio is 0.90, and a 3K spinneret is used.

[0137] 4. Oiling: After oiling, the crystallinity of the polyacrylonitrile primary fiber is 72%, the grain size is 9.2nm, and the degree of orientation of the crystal area is 76%.

[0138] 5. Drying and densification: The moisture content of the nascent polyacrylonitrile fiber after oiling is 40%. The drying and densification is divided into two stages. The first stage of drying and densification temperature is 90°C, and the circulation flow rate of the heat transfer oil is 25m 3 / h, the number of drying and densification hot rollers is 7, the surface temperature CV value is 2.0%, and the duration is 50s; the second stage drying and densification temperature is 120℃, and the circulation flow rate of the heat transfer oil is 25m 3 / h, 7 drying and densification hot rollers, surface temperature CV value of 2.5%, duration of 50s, and other aspects are the same as in Example 1.

[0139] 6. Steam drawing and heat setting: The fineness of polyacrylonitrile raw yarn is 0.9dtex, the moisture content is 1.0%, and the oil content is 1.3%.

[0140] During the pre-oxidation process, the total drafting percentage of the polyacrylonitrile precursor can reach 5%, and the average number of filaments in 10 meters of pre-oxidized fiber is 6 per meter.

[0141] The pre-oxidized fiber was carbonized under the following conditions: carbonization was carried out in a nitrogen atmosphere, the low-temperature carbonization temperature was 370°C, the time was 3 min, the draft ratio was 2%, the high-temperature carbonization temperature was 1380°C, the time was 3 min, the draft ratio was -3%, and the mechanical properties of the obtained carbon fiber were a breaking strength of 4.5 GPa, an elongation at break of 2.0%, and a tensile modulus of 235 GPa.

[0142] [Comparative Example 3]

[0143] The preparation process is the same as in Example 1, except that:

[0144] 2. Solidification molding: using 3K spinneret.

[0145] 4. Oiling: After oiling, the crystallinity of the polyacrylonitrile primary fiber is 57%, the grain size is 6.9nm, and the degree of orientation of the crystal area is 72%.

[0146] 5. Drying and densification: The moisture content of the primary polyacrylonitrile fiber after oiling is 40%. The drying and densification is divided into two stages. The first stage of drying and densification temperature is 60℃, and the circulation flow rate of the heat transfer oil is 25m 3 / h, the number of drying and densification hot rollers is 7, the surface temperature CV value is 2.0%, and the duration is 50s; the second stage drying and densification temperature is 65℃, and the circulation flow rate of the heat transfer oil is 25m3 / h, 7 drying and densification hot rollers, surface temperature CV value of 2.5%, duration of 50s, and other aspects are the same as in Example 1.

[0147] 6. Steam drawing and heat setting: The fineness of polyacrylonitrile raw yarn is 0.9dtex, the moisture content is 1.0%, and the oil content is 1.3%.

[0148] During the pre-oxidation process, the total drafting percentage of the polyacrylonitrile precursor can reach 10%, and the average number of filaments in 10 meters of pre-oxidized fiber is 5 / meter.

[0149] The pre-oxidized fiber was carbonized under the following conditions: carbonization was carried out in a nitrogen atmosphere, the low-temperature carbonization temperature was 370°C, the time was 3 min, the draft ratio was 2%, the high-temperature carbonization temperature was 1380°C, the time was 3 min, the draft ratio was -3%, and the mechanical properties of the obtained carbon fiber were a breaking strength of 4.2 GPa, a breaking elongation of 2.0%, and a tensile modulus of 236 GPa.

[0150] [Comparative Example 4]

[0151] The preparation process is the same as in Example 1, except that:

[0152] 2. Solidification molding: using 3K spinneret.

[0153] 4. Oiling: After oiling, the crystallinity of the polyacrylonitrile primary fiber is 57%, the grain size is 6.9nm, and the degree of orientation of the crystal area is 72%.

[0154] 5. Drying and densification: The moisture content of the raw polyacrylonitrile fiber after oiling is 40%. The drying and densification is divided into two stages. The first stage of drying and densification temperature is 140℃, and the circulation flow rate of the heat transfer oil is 25m 3 / h, the number of drying and densification hot rollers is 7, the surface temperature CV value is 2.0%, and the duration is 50s; the second stage drying and densification temperature is 150℃, and the circulation flow rate of the heat transfer oil is 25m 3 / h, 7 drying and densification hot rollers, surface temperature CV value of 2.5%, duration of 50s, and other aspects are the same as in Example 1.

[0155] 6. Steam drawing and heat setting: The fineness of polyacrylonitrile raw yarn is 0.9dtex, the moisture content is 1.0%, and the oil content is 1.3%.

[0156] During the pre-oxidation process, the total drafting percentage of the polyacrylonitrile precursor can reach 10%, and the average number of filaments in 10 meters of pre-oxidized fiber is 8 per meter.

[0157] The pre-oxidized fiber was carbonized under the following conditions: carbonization was carried out in a nitrogen atmosphere, the low-temperature carbonization temperature was 370°C, the time was 3 min, the draft ratio was 2%, the high-temperature carbonization temperature was 1380°C, the time was 3 min, the draft ratio was -3%, and the mechanical properties of the obtained carbon fiber were a breaking strength of 4.0 GPa, an elongation at break of 2.1%, and a tensile modulus of 232 GPa.

[0158] [Comparative Example 5]

[0159] The preparation process is the same as in Example 1, except that:

[0160] 2. Solidification molding: using 3K spinneret.

[0161] 4. Oiling: After oiling, the crystallinity of the polyacrylonitrile primary fiber is 57%, the grain size is 6.9nm, and the degree of orientation of the crystal area is 72%.

[0162] 5. Drying and densification: The moisture content of the raw polyacrylonitrile fiber after oiling is 40%. The drying and densification is divided into two stages. The first stage of drying and densification temperature is 90℃, and the circulation flow rate of the heat transfer oil is 10m 3 / h, the number of drying and densification hot rollers is 7, the surface temperature CV value is 7.5%, and the duration is 50s; the second stage drying and densification temperature is 120℃, and the circulation flow rate of the heat transfer oil is 10m 3 / h, 7 drying and densification hot rollers, surface temperature CV value of 7.5%, duration of 50s, and other aspects are the same as in Example 1.

[0163] 6. Steam drawing and heat setting: The fineness of polyacrylonitrile raw yarn is 0.9dtex, the moisture content is 1.0%, and the oil content is 1.3%.

[0164] During the pre-oxidation process, the total drafting percentage of the polyacrylonitrile precursor can reach 10%, and the average number of filaments in 10 meters of pre-oxidized fiber is 6 per meter.

[0165] The pre-oxidized fiber was carbonized under the following conditions: carbonization was carried out in a nitrogen atmosphere, the low-temperature carbonization temperature was 370°C, the time was 3 min, the draft ratio was 2%, the high-temperature carbonization temperature was 1380°C, the time was 3 min, the draft ratio was -3%, and the mechanical properties of the obtained carbon fiber were a breaking strength of 3.6 GPa, an elongation at break of 2.2%, and a tensile modulus of 235 GPa.

[0166] [Comparative Example 6]

[0167] The preparation process is the same as in Example 1, except that:

[0168] 2. Solidification molding: using 3K spinneret.

[0169] 4. Oiling: After oiling, the crystallinity of the polyacrylonitrile primary fiber is 57%, the grain size is 6.9nm, and the degree of orientation of the crystal area is 72%.

[0170] 5. Drying and densification: After oiling, the moisture content of the polyacrylonitrile primary fiber is 40%. The drying and densification is divided into two stages. The first stage of drying and densification temperature is 90℃, and the circulation flow rate of the heat transfer oil is 35m 3 / h, the number of drying and densification hot rollers is 7, the surface temperature CV value is 5.5%, and the duration is 50s; the second stage drying and densification temperature is 120℃, and the circulation flow rate of the heat transfer oil is 35m 3 / h, 7 drying and densification hot rollers, surface temperature CV value of 5.5%, duration of 50s, and other aspects are the same as in Example 1.

[0171] 6. Steam drawing and heat setting: The fineness of polyacrylonitrile raw yarn is 0.9dtex, the moisture content is 1.0%, and the oil content is 1.3%.

[0172] During the pre-oxidation process, the total drafting percentage of the polyacrylonitrile precursor can reach 10%, and the average number of filaments in 10 meters of pre-oxidized fiber is 6 per meter.

[0173] The pre-oxidized fiber was carbonized under the following conditions: carbonization was carried out in a nitrogen atmosphere, the low-temperature carbonization temperature was 370°C, the time was 3 min, the draft ratio was 2%, the high-temperature carbonization temperature was 1380°C, the time was 3 min, the draft ratio was -3%, and the mechanical properties of the obtained carbon fiber were a breaking strength of 3.7 GPa, an elongation at break of 2.1%, and a tensile modulus of 245 GPa.

[0174] [Comparative Example 7]

[0175] The preparation process is the same as in Example 1, except that:

[0176] 2. Solidification molding: using 3K spinneret.

[0177] 4. Oiling: After oiling, the crystallinity of the polyacrylonitrile primary fiber is 56%, the grain size is 7.1nm, and the degree of orientation of the crystal area is 74%.

[0178] 5. Drying and densification: The moisture content of the raw polyacrylonitrile fiber after oiling is 40%. The drying and densification is divided into two stages. The first stage of drying and densification temperature is 80℃, and the circulation flow rate of the heat transfer oil is 15m 3 / h, the number of drying and densification hot rollers is 7, the surface temperature CV value is 12.0%, and the duration is 55s; the second stage drying and densification temperature is 110℃, and the circulation flow rate of the heat transfer oil is 25m 3 / h, 7 drying and densification hot rollers, surface temperature CV value of 10.0%, duration of 55s, and other aspects are the same as in Example 1.

[0179] 6. Steam drawing and heat setting: The fineness of polyacrylonitrile raw yarn is 1.3dtex, the moisture content is 1.3%, and the oil content is 1.2%.

[0180] Other conditions are the same as in Example 1.

[0181] During the pre-oxidation process, the total drafting percentage of the polyacrylonitrile precursor can reach 10%, and the average number of filaments in 10 meters of pre-oxidized fiber is 10 / meter.

[0182] After the pre-oxidized fibers are carbonized, they are carbonized in a nitrogen atmosphere. The low-temperature carbonization temperature is 395°C, the time is 3 min, and the draft ratio is 2%. The high-temperature carbonization temperature is 1360°C, the time is 3 min, and the draft ratio is -3%. The mechanical properties of the carbon fibers are as follows: a breaking strength of 2.8 GPa, an elongation at break of 2.7%, and a tensile modulus of 190 GPa.

[0183] It can be seen from Comparative Examples 1 to 6 and Example 1, as well as Comparative Example 7 and Example 6 that the preparation method of polyacrylonitrile pre-oxidized fiber provided by the present invention can improve the stretchability of polyacrylonitrile precursor, reduce or even eliminate the hairy fibers and / or broken fibers of the polyacrylonitrile pre-oxidized fiber, and achieve good technical effects.

Claims

1. A method for preparing polyacrylonitrile preoxidized fiber, comprising subjecting polyacrylonitrile primary fiber to oiling, drying and densification, and preoxidation treatment to obtain polyacrylonitrile preoxidized fiber, wherein the ratio of the standard deviation of the surface temperature of the drying and densification hot roller to the average temperature is ≤7%; the crystallinity of the polyacrylonitrile primary fiber after oiling is 50-60%, the grain size is 5-8nm, and the orientation degree of the crystal region is 65-75%; the drying and densification is divided into at least two stages, the treatment temperature of each stage of the drying and densification is 70-180°C, and the treatment time of each stage of the drying and densification is 40-180s; the circulating heating medium used in the drying and densification is heat transfer oil, and the circulation flow rate of the heat transfer oil in each stage of the drying and densification is 10-40m 3 / h.

2. The preparation method according to claim 1, characterized in that: The preparation method specifically comprises: extruding and coagulating the polyacrylonitrile spinning stock solution to obtain polyacrylonitrile primary fibers, then subjecting the fibers to hot water drawing, water washing, oiling, drying and densification, steam drawing, and heat setting to obtain polyacrylonitrile fiber precursors, and then subjecting the fibers to pre-oxidation treatment to obtain polyacrylonitrile pre-oxidized fibers.

3. The preparation method according to claim 2, characterized in that: The polyacrylonitrile has a molecular weight of 50,000 to 90,000, a molecular weight distribution of 2.0 to 5.0, and a viscosity of 50 to 90 Pa·s at 60°C; and / or The tow of the polyacrylonitrile primary fiber is 1-50K.

4. The preparation method according to claim 3, characterized in that: The tow of the polyacrylonitrile primary fiber is 1-12K.

5. The preparation method according to claim 2, characterized in that: The temperature of the hot water drawing is 70-99° C.; and / or, The total drafting ratio of the hot water drafting is 350-700%; and / or, The water washing temperature is 40-80°C; and / or, The water washing is performed at least twice.

6. The preparation method according to claim 5, characterized in that: The temperature of the hot water drawing is 85-95°C; and / or, The water washing adopts a step-by-step temperature increase method, and the temperature increase gradient is 4-20°C / step.

7. The preparation method according to claim 2, characterized in that: The moisture content of the oiled polyacrylonitrile primary fibers is 20-100%; and / or, The oiling time is 0.2-3s.

8. The preparation method according to claim 7, characterized in that: The moisture content of the oiled polyacrylonitrile primary fibers is 30-50%; and / or, The oiling time is 0.5-1s.

9. The preparation method according to claim 1, characterized in that: The treatment temperature of each stage of drying and densification is 80-130°C; and / or, The drying and densification treatment time for each stage is 40 to 150 seconds; and / or, The circulation flow rate of each section of the heat transfer oil in the drying and densification process is 15-30 m 3 / h; and / or, The number of hot rollers used in each drying and densification stage is 3 to 12; and / or, The ratio of the standard deviation of the surface temperature of each section of the hot roller for drying and densification to the average temperature is ≤5%.

10. The preparation method according to claim 9, characterized in that: The number of hot rollers used in each drying and densification stage is 5 to 10.

11. The preparation method according to claim 2, characterized in that: The fineness of the polyacrylonitrile precursor is 0.5-1.5 dtex; and / or, The water content of the polyacrylonitrile raw silk is 0.5-2%, and the oil content is 0.5-2%.

12. The preparation method according to claim 11, characterized in that: The water content of the polyacrylonitrile raw silk is 0.8-1.5%, and the oil content is 0.8-1.5%.

13. The preparation method according to claim 2, characterized in that: The pre-oxidation is provided with at least five temperature zones; and / or, The pre-oxidation temperature is 190-270°C; and / or, The pre-oxidation treatment time is 45 to 60 minutes.

14. The preparation method according to claim 13, characterized in that: The pre-oxidation temperature zone adopts a step-by-step heating method, with a temperature gradient of 10-30°C / step; and / or, The treatment time of each temperature zone of the pre-oxidation is 5 to 12 minutes.

15. The preparation method according to claim 2, characterized in that: The total drafting multiple of the polyacrylonitrile precursor in the pre-oxidation treatment stage is 2-10%.

16. The preparation method according to claim 15, characterized in that: The total drafting multiple of the polyacrylonitrile precursor in the pre-oxidation treatment stage is 4-8%.

17. A polyacrylonitrile pre-oxidized fiber, prepared by the preparation method according to any one of claims 1 to 16.

Citation Information

Patent Citations

  • Heating device for drying densification of polyacrylonitrile-based carbon fiber precursor

    CN102899743A

  • Preparation method of polyacrylonitrile-based carbon fiber

    CN112226851A

  • Chemical fiber heat setting device for spinning

    CN211199496U