A welding wire suitable for Al-Li-Cu-Mg-Zn alloy welding and a preparation method thereof

By using TiB2 micron-sized welding wire in Al-Li-Cu-Mg-Zn alloy welding, the crack problem during welding is solved, the strength and plasticity of the welding head are improved, and high-strength and low-crack sensitivity are achieved. Effect, suitable for industrial applications of high-strength aluminum lithium alloys.

CN115709350BActive Publication Date: 2024-11-05AEROSPACE RES INST OF MATERIAL & PROCESSING TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211177463.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-26
Publication Date
2024-11-05
Estimated Expiration
2042-09-26

AI Technical Summary

Technical Problem

When welding, Al-Li-Cu-Mg-Zn alloys have poor weldability and easy to form crystalline cracks and liquefied cracks. The welding head has low strength and cannot meet the needs of engineering applications.

Method used

Welding wire containing TiB2 micron-scale particles is used to form micron-scale TiB2 particles by in-situ self-generating method, and disperse it in high-temperature stirring. Combined with gas refining and heat treatment processes, high-strength and low crack sensitivity welding wire was prepared.

Benefits of technology

It significantly reduces the sensitivity of welding cracks, improves the room temperature mechanical properties of the welding head, solves the welding problem of high-strength aluminum lithium alloys, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115709350B_ABST
    Figure CN115709350B_ABST
Patent Text Reader

Abstract

The invention discloses a welding wire suitable for Al-Li-Cu-Mg-Zn alloy welding, comprising the following components in percentage by mass: Cu: 5.8% to 6.8%; Ag: 0.05% to 0.3%; TiB2: 1.5% to 2.5%; Cr: 0.1% to 0.2%; Be: 0.0003% to 0.001%; ​​Al: balance. The invention also discloses a method for preparing a welding wire suitable for Al-Li-Cu-Mg-Zn alloy welding, comprising: smelting aluminum, copper, silver, Al-5Cr master alloy and Al-3Be master alloy; adding boron salt and titanium salt during the smelting process, continuing smelting and stirring; refining, standing and casting the melt obtained after smelting in sequence to obtain an ingot; extruding, annealing and drawing the ingot in sequence to obtain the welding wire. The invention is beneficial to improving the mechanical properties and crack resistance of fusion welding joints, is suitable for Al-Li-Cu-Mg-Zn alloy welding, and is a welding wire that can be industrially produced on a large scale to promote the engineering application of high-strength aluminum-lithium alloys.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a welding wire suitable for high-strength Al-Li-Cu-Mg-Zn alloy welding and a preparation method thereof, belonging to the technical field of metal connection. Background Art

[0002] Reducing structural weight and increasing payload have always been important research directions in the aerospace field, so the application of new lightweight and high-strength structural materials is crucial. Aluminum-lithium alloy (Al-Li) is a type of aluminum alloy with lithium added, which has the advantages of low density, high elastic modulus, high specific strength and specific stiffness, and high toughness. Using aluminum-lithium alloy to replace traditional aluminum alloy materials can reduce the weight of structural parts by 10-15% and increase stiffness by 15%-20%. NASA uses aluminum-lithium alloy to replace 2219 aluminum-copper alloy as the structural material of the new generation of tanks, which reduces the overall weight of the tank by 3405kg and improves the carrying capacity of the space shuttle. Therefore, aluminum-lithium alloy has broad application prospects in the aerospace field.

[0003] Al-Li-Cu-Mg-Zn series lightweight and high-strength aluminum-lithium alloy is based on 2195 aluminum-lithium alloy, with the addition of micro-alloying elements such as Mn and Zn, which can effectively control the grain size and organizational structure of the alloy and promote the precipitation of S phase and T1 phase. As the third-generation aluminum-lithium alloy, its strength can exceed 600Mpa, and its elongation can reach 10%, which has better solved the problems of poor plasticity and toughness and severe anisotropy of the second-generation aluminum-lithium alloy. However, Al-Li-Cu-Mg-Zn series alloy has poor weldability. When welding with existing welding wire, crystallization cracks and liquefaction cracks are easily formed. The softening of the weld joint causes the strength to be far lower than the strength of the parent material, which cannot be applied in engineering. At present, there is no welding wire that meets the requirements.

[0004] Therefore, it is necessary to develop a welding wire that can improve the microstructure of the fusion weld joint while improving the mechanical properties and crack resistance of the fusion weld joint. The welding wire is suitable for Al-Li-Cu-Mg-Zn alloy welding and can be industrially produced on a large scale to promote the engineering application of high-strength aluminum-lithium alloys. Summary of the invention

[0005] The purpose of the present invention is to overcome the above defects, provide a welding wire suitable for Al-Li-Cu-Mg-Zn alloy welding and a preparation method thereof, and solve the technical problem of poor weldability of existing Al-Li-Cu-Mg-Zn alloys. The present invention is conducive to reducing the sensitivity of welding cracks, improving the normal temperature performance of the welding head, and is suitable for large-scale industrial production.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] A welding wire suitable for Al-Li-Cu-Mg-Zn alloy welding, comprising the following components in percentage by mass:

[0008]

[0009] Furthermore, TiB2 is in the form of micron-sized particles.

[0010] A method for preparing a welding wire suitable for Al-Li-Cu-Mg-Zn alloy welding, comprising:

[0011] Aluminum, copper, silver, Al-5Cr master alloy and Al-3Be master alloy are melted;

[0012] Add boron salt and titanium salt during smelting, continue smelting and stirring;

[0013] The melt obtained after smelting is successively refined, allowed to stand and cast to obtain an ingot;

[0014] The ingot is sequentially extruded, annealed and drawn to obtain welding wire.

[0015] Furthermore, the boron salt and titanium salt added during the smelting process are KBF4 and K2TiF6, respectively.

[0016] Furthermore, the purity of aluminum is ≥99.999%, the purity of copper is ≥99.999%, and the purity of silver is ≥99.999%; and the alloying of the Al-5Cr master alloy and the Al-3Be master alloy is ≤5%.

[0017] Furthermore, the melting temperature before adding the boron salt and the titanium salt is 760-820°C, and the melting temperature after adding the boron salt and the titanium salt is 820-860°C.

[0018] Further, the melt obtained after smelting is refined by gas refining method, and the specific method is: using Ar-Cl2 mixed gas, refining for 10 to 20 minutes;

[0019] After refining, the melt is allowed to stand for 15 to 20 minutes.

[0020] Furthermore, the temperature for casting the melt is 780-840° C., and the speed of pulling the ingot out of the crystallizer during casting is 80-90 mm / min.

[0021] Furthermore, when the ingot is extruded, the temperature of the extrusion die is 440-480° C. The ingot is placed in the extrusion die and extruded after being kept warm for 4-6 hours.

[0022] Furthermore, the ingot is annealed at a temperature of 480-530°C.

[0023] Compared with the prior art, the present invention has at least one of the following beneficial effects:

[0024] (1) The present invention creatively proposes a combination of components in a welding wire suitable for Al-Li-Cu-Mg-Zn alloy welding, and the content of grain refiner TiB2 in the welding wire is high, which is beneficial to reduce the sensitivity of welding cracks and improve the normal temperature performance of the welding joint;

[0025] (2) The present invention uses an in-situ autogenous method instead of a preparation method that directly adds Ti and B to form micron-sized TiB2 particles, and effectively disperses the micron-sized TiB2 particles by stirring and increasing the melting temperature. The dispersed micron-sized TiB2 particles can effectively refine the weld structure and improve the strength and plasticity;

[0026] (3) The welding wire obtained by the present invention has good melt-casting wire making performance, is suitable for large-scale industrial production, and is used for the fusion welding of high-strength aluminum-lithium alloys. It has low welding crack sensitivity and excellent room temperature performance of the welding joint, which solves the problems of poor weldability, easy formation of crystal cracks and liquefaction cracks, and joint softening that occur during the fusion welding of high-strength aluminum-lithium alloys. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the microstructure of the fusion welded joint in Example 1 of the present invention;

[0028] Figure 2 This is the microstructure of the fusion welded joint in Example 2 of the present invention;

[0029] Figure 3 This is the microstructure of the fusion welded joint in Comparative Example 1. DETAILED DESCRIPTION

[0030] The following detailed description of the present invention will make the features and advantages of the present invention more clear and explicit.

[0031] The word "exemplary" is used exclusively herein to mean "serving as an example, embodiment, or illustration." Any embodiment described herein as "exemplary" is not necessarily to be construed as preferred or advantageous over other embodiments. Although various aspects of the embodiments are shown in the drawings, the drawings are not necessarily drawn to scale unless otherwise noted.

[0032] Al-Li-Cu-Mg-Zn series lightweight and high-strength aluminum-lithium alloy is based on 2195 aluminum-lithium alloy, with the addition of micro-alloying elements such as Mn and Zn. Its strength can exceed 600Mpa, and its elongation can reach 10%, which has effectively solved the problems of poor plasticity and toughness, severe anisotropy, etc. of the second-generation aluminum-lithium alloy. However, Al-Li-Cu-Mg-Zn series alloy has poor weldability, and is very easy to form crystal cracks and liquefaction cracks during welding. The softening of the weld joint causes the strength to be far lower than that of the parent material, and it cannot be applied in engineering. At present, there is no welding wire that meets the requirements. To solve these problems, the present invention has developed a new type of welding wire, which has good manufacturing processability and is suitable for fusion welding of high-strength aluminum-lithium alloys. The crack sensitivity K1=0%, K2=0%, the repair welding crack sensitivity K1=0%, K2=0%, excellent mechanical properties at room temperature, the fusion welding joint strength coefficient exceeds 0.55, and the elongation exceeds 4%. It can be used as a welding wire for Al-Li-Cu-Mg-Zn alloys, and can be extended to the fusion welding of 2195 aluminum-lithium alloys, 2219 aluminum alloys and 2A14 aluminum alloys.

[0033] The present invention discloses a welding wire suitable for Al-Li-Cu-Mg-Zn alloy welding, the components of which include Cu, Ag, Ti, B, Cr, Be and Al, and the mass content of each component is:

[0034] The Cu content is 5.8% to 6.8%, the Ag content is 0.05% to 0.3%, the TiB2 content is 1.5% to 2.5%, the Cr content is 0.1% to 0.2%, the Be content is 0.0003% to 0.001%, and the rest is Al.

[0035] The present invention discloses a method for preparing a ceramic aluminum welding wire suitable for Al-Li-Cu-Mg-Zn alloy welding, which solves the agglomeration and segregation problem of high TiB2 welding wire and forms an aluminum alloy welding wire reinforced with micron-sized TiB2 particles. The method is characterized by the following steps:

[0036] Step 1: Ingredients: The ingredients include high-purity aluminum, pure copper, pure silver, Al-5Cr master alloy, Al-3Be master alloy, KBF4 and K2TiF6 mixed salt. The master alloys are all low-alloyed master alloys to avoid agglomeration and segregation of precipitated phases. High-purity aluminum, pure copper, pure silver, Al-5Cr master alloy and Al-3Be master alloy are added first;

[0037] Step 2: Melting, the melting temperature is 760-820℃;

[0038] Step 3: Add KBF4 and K2TiF6 mixed salt;

[0039] Step 4: Melting. In order to make the in-situ self-generated TiB2 distributed finely and evenly, the melting temperature is increased to 820-860℃ and stirred continuously;

[0040] Step 5: Degassing and slag removal: gas refining method, using Ar-Cl2 mixed gas, refining for 15 minutes, and letting the melt stand for 15 minutes;

[0041] Step 6: Casting, the casting temperature is 780-840℃; the ingot is pulled out of the crystallizer at a speed of 80-90mm / min;

[0042] Step 7: Cut the head and tail and peel the skin;

[0043] Step 8: Extrusion, the ingot temperature is 460-490℃, the extrusion die temperature is 440-480℃, and hot extrusion is performed after keeping warm for 4-6 hours;

[0044] Step 9: Annealing, the annealing temperature is 480-530℃;

[0045] Step 10: Perform the pull.

[0046] The welding wire of the present invention has a high content of TiB2, a grain refiner, which exceeds the TiB2 content of the existing Al-Cu welding wire. An in-situ autogenous method is used instead of a preparation method of directly adding Ti and B to form micron-sized TiB2 particles, which are effectively dispersed by stirring and increasing the melting temperature. The dispersed micron-sized TiB2 particles can effectively refine the weld structure and improve the strength and plasticity. The welding wire uses a micro-alloyed combination of Ti-B-Cr-Ag-Be for the first time.

[0047] The welding wire of the invention is suitable for fusion welding of aluminum-lithium alloy (belonging to Al-Li-Cu-Mg-Zn alloy) with a strength exceeding 600MPa.

[0048] Example 1

[0049] In this embodiment, a welding wire suitable for Al-Li-Cu-Mg-Zn alloy welding is prepared. The welding wire contains micron-level in-situ self-generated TiB2 particles. The composition of the welding wire is composed of Cu, Ag, Ti, B, Cr, Be and Al.

[0050] The specific steps of the preparation method are:

[0051] Step 1: Ingredients: The ingredients include high-purity aluminum, pure copper, pure silver, Al-5Cr master alloy, Al-3Be master alloy, KBF4 and K2TiF6 mixed salt. The master alloys are all low-alloyed master alloys to avoid agglomeration and segregation of precipitated phases. High-purity aluminum, pure copper, pure silver, Al-5Cr master alloy and Al-3Be master alloy are added first;

[0052] Step 2: Melting, the melting temperature is 780℃;

[0053] Step 3: Add KBF4 and K2TiF6 mixed salt;

[0054] Step 4: Melting. In order to make the in-situ self-generated TiB2 distributed finely and evenly, the melting temperature is increased to 835°C and stirred continuously;

[0055] Step 5: Degassing and slag removal: gas refining method, using Ar-Cl2 mixed gas, refining for 15 minutes, and letting the melt stand for 15 minutes;

[0056] Step 6: Casting, the casting temperature is 820°C; the ingot is pulled out of the crystallizer at a speed of 85 mm / min;

[0057] Step 7: Cut the head and tail and peel the skin;

[0058] Step 8: Extrusion, the ingot temperature is 470℃, the extrusion die temperature is 450℃, and hot extrusion is performed after keeping warm for 4-6 hours;

[0059] Step 9: Annealing, the annealing temperature is 500°C;

[0060] Step 10: Perform the pull.

[0061] Press while stretching The process produced 200 kg of oil seal welding wire with a diameter of 3.0 mm. The chemical composition is as follows: Cu content is 6.07%, Ag content is 0.20%, TiB2 content is 1.62%, Cr content is 0.1%, Be content is 0.0004%, and the rest is Al.

[0062] Pickling before welding, used for welding high-strength Al-Li-Cu-Mg-Zn alloy with a thickness of 6.0 mm, the weld is well formed, the internal quality of the joint meets the requirements of QJ-2698A I-level weld, the welding crack sensitivity crystallization crack sensitivity rate K1 = 0%, liquefaction crack sensitivity rate K2 = 0%, repair welding crack sensitivity K1 = 0%, K2 = 0%, Table 1 is the room temperature mechanical properties table of fusion welding joints, where sample numbers 1 to 5 represent 5 sub-samples respectively. According to Table 1, the tensile strength σ of the fusion welding joint is b It is 362MPa and the elongation δ is 4.5%. Figure 1 This is the microstructure of the fusion welded joint. It can be seen that the TiB2 particles are dispersed relatively evenly and the particle size is 5-10μm.

[0063] Table 1 Mechanical properties of fusion welded joints at room temperature using welding wire from Example 1

[0064]

[0065]

[0066] Example 2

[0067] In this embodiment, a welding wire suitable for Al-Li-Cu-Mg-Zn alloy welding is prepared. The welding wire contains micron-level in-situ self-generated TiB2 particles. The composition of the welding wire is composed of Cu, Ag, Ti, B, Cr, Be and Al.

[0068] The steps of the preparation method are:

[0069] Step 1: Ingredients: The ingredients include high-purity aluminum, pure copper, pure silver, Al-5Cr master alloy, Al-3Be master alloy, KBF4 and K2TiF6 mixed salt. The master alloys are all low-alloyed master alloys to avoid agglomeration and segregation of precipitated phases. High-purity aluminum, pure copper, pure silver, Al-5Cr master alloy and Al-3Be master alloy are added first;

[0070] Step 2: Melting, the melting temperature is 780℃;

[0071] Step 3: Add KBF4 and K2TiF6 mixed salt;

[0072] Step 4: Melting. In order to make the in-situ self-generated TiB2 distributed finely and evenly, the melting temperature is increased to 845°C and stirred continuously;

[0073] Step 5: Degassing and slag removal: gas refining method, using Ar-Cl2 mixed gas, refining for 15 minutes, and letting the melt stand for 15 minutes;

[0074] Step 6: Casting, the casting temperature is 830°C; the ingot is pulled out of the crystallizer at a speed of 87 mm / min;

[0075] Step 7: Cut the head and tail and peel the skin;

[0076] Step 8: Extrusion, the ingot temperature is 480℃, the extrusion die temperature is 460℃, and hot extrusion is performed after keeping warm for 4-6 hours;

[0077] Step 9: Annealing, the annealing temperature is 510°C;

[0078] Step 10: Perform the pull.

[0079] When stretching The process produced 150 kg of oil seal welding wire with a diameter of 3.0 mm. The chemical composition is: Cu content is 5.83%, Ag content is 0.15%, TiB2 content is 1.98%, Cr content is 0.12%, Be content is 0.0005%, and the rest is Al. Pickling before welding, used for welding Al-Li-Cu-Mg-Zn alloy with a thickness of 6.0 mm, the weld is well formed, the internal quality of the joint meets the requirements of QJ-2698A Class I weld, the welding crack sensitivity crystallization crack sensitivity K1=0%, liquefaction crack sensitivity K2=0%, repair welding crack sensitivity K1=0%, K2=0%, as shown in Table 2 Fusion welding joint tensile strength σ b It is 366MPa and the elongation δ is 4.8%. Figure 2 This is the microstructure of the fusion welded joint. It can be seen that the TiB2 particles are dispersed relatively evenly and the particle size is 5-10μm.

[0080] Table 2 Mechanical properties of fusion welded joints at room temperature using welding wire from Example 2

[0081] Sample No. <![CDATA[σ b (MPa)]]> δ(%) 1 362 5 2 359 4 3 367 5 4 371 5 5 371 5 average value 366 4.8

[0082] Comparative Example 1

[0083] In this comparative example, a welding wire suitable for Al-Li-Cu-Mg-Zn alloy welding is prepared. The welding wire contains micron-level in-situ self-generated TiB2 particles. The composition of the welding wire is composed of Cu, Ag, Ti, B, Cr, Be and Al.

[0084] The steps of the preparation method are:

[0085] Step 1: Ingredients: The ingredients include high-purity aluminum, pure copper, pure silver, Al-5Cr master alloy, Al-3Be master alloy, KBF4 and K2TiF6 mixed salt. The master alloys are all low-alloyed master alloys to avoid agglomeration and segregation of precipitated phases. High-purity aluminum, pure copper, pure silver, Al-5Cr master alloy and Al-3Be master alloy are added first;

[0086] Step 2: Melting, the melting temperature is 780℃;

[0087] Step 3: Add KBF4 and K2TiF6 mixed salt;

[0088] Step 4: Melting. In order to make the in-situ self-generated TiB2 distributed finely and evenly, the melting temperature is increased to 845°C and stirred continuously;

[0089] Step 5: Degassing and slag removal: gas refining method, using Ar-Cl2 mixed gas, refining for 15 minutes, and letting the melt stand for 15 minutes;

[0090] Step 6: Casting, the casting temperature is 830°C; the ingot is pulled out of the crystallizer at a speed of 87 mm / min;

[0091] Step 7: Cut the head and tail and peel the skin;

[0092] Step 8: Extrusion, the ingot temperature is 480℃, the extrusion die temperature is 460℃, and hot extrusion is performed after keeping warm for 4-6 hours;

[0093] Step 9: Annealing, the annealing temperature is 510°C;

[0094] Step 10: Perform the pull.

[0095] When stretching The process produced 150 kg of oil seal welding wire with a diameter of 3.0 mm. The chemical composition is: Cu content is 6.12%, Ag content is 0.14%, TiB2 content is 2.96%, Cr content is 0.13%, Be content is 0.0005%, and the rest is Al. Pickling before welding, used for welding Al-Li-Cu-Mg-Zn alloy with a thickness of 6.0 mm, the weld is well formed, the internal quality of the joint meets the requirements of QJ-2698A Class I weld, the welding crack sensitivity crystallization crack sensitivity K1 = 1.1%, liquefaction crack sensitivity K2 = 0.5%, repair welding crack sensitivity K1 = 1.4%, K2 = 1.0%, as shown in Table 3 Fusion welding joint tensile strength σ b The tensile strength is 342MPa, the elongation δ is 2.9%, and the comprehensive performance cannot meet the use requirements. Figure 3 The microstructure of the fusion welded joint shows that the TiB2 particles are coarse and the particle size exceeds 50 μm. This is because the TiB2 content in this comparative example exceeds the content range given in the present invention, resulting in agglomeration of the TiB2 particles.

[0096] Table 3 Mechanical properties of fusion welded joints at room temperature using welding wire from Comparative Example 1

[0097] Sample No. <![CDATA[σ b (MPa)]]> δ(%) 1 345 3.5 2 340 2.5 3 325 2 4 355 3 5 345 3 average value 342 2.9

[0098] Comparative Example 2:

[0099] The remaining conditions of this comparative example are consistent with those of Example 2. The added raw materials are high-purity aluminum, pure copper, pure silver, pure boron, Al-5Cr master alloy, Al-3Ti master alloy, and Al-3Be master alloy. The welding crack sensitivity of the present invention is K1=2.1%, K2=1.1%, and the repair welding crack sensitivity is K1=3.2%, K2=2.3%. As shown in Table 4, the tensile strength σ of the fusion welded joint is bThe tensile strength is 344 MPa and the elongation is 3.3%, which cannot meet the use requirements. This is because the raw materials in this comparative example cannot generate fine and uniformly distributed TiB2 in situ, but generate coarse Al3Ti phase.

[0100] Table 4 Mechanical properties of fusion welding joints obtained by welding wire of comparative example 2 at room temperature

[0101] Sample No. <![CDATA[σ b (MPa)]]> δ(%) 1 350 3 2 340 4 3 325 2.5 4 360 3 5 345 4 average value 344 3.3

[0102] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

[0103] The contents not described in detail in the specification of the present invention belong to the common knowledge of those skilled in the art.

Claims

1. A welding wire suitable for welding Al-Li-Cu-Mg-Zn alloy, characterized in that: The following components are included in percentage by mass: TiB2 is micron-sized particles; The welding wire is prepared by the following method: aluminum, copper, silver, Al-5Cr master alloy and Al-3Be master alloy are smelted; Add boron salt and titanium salt during smelting, continue smelting and stirring; The melt obtained after smelting is successively refined, allowed to stand and cast to obtain an ingot; The ingot is sequentially extruded, annealed and drawn to obtain welding wire; The purity of aluminum is ≥99.999%, the purity of copper is ≥99.999%, the purity of silver is ≥99.999%; the alloying of Al-5Cr master alloy and Al-3Be master alloy is ≤5%; The melting temperature before adding the boron salt and the titanium salt is 760-820°C, and the melting temperature after adding the boron salt and the titanium salt is 820-860°C; When the ingot is extruded, the extrusion die temperature is 440-480°C, the ingot is placed in the extrusion die, and extrusion is performed after keeping the temperature for 4-6 hours; The ingot is annealed at a temperature of 480 to 530°C.

2. The method for preparing a welding wire suitable for Al-Li-Cu-Mg-Zn alloy welding according to claim 1, characterized in that: include: Aluminum, copper, silver, Al-5Cr master alloy and Al-3Be master alloy are melted; Add boron salt and titanium salt during smelting, continue smelting and stirring; The melt obtained after smelting is successively refined, allowed to stand and cast to obtain an ingot; The ingot is sequentially extruded, annealed and drawn to obtain welding wire.

3. The method for preparing a welding wire suitable for Al-Li-Cu-Mg-Zn alloy welding according to claim 2, characterized in that: The boron salt and titanium salt added during the smelting process are KBF4 and K2TiF6 respectively.

4. The method for preparing a welding wire suitable for Al-Li-Cu-Mg-Zn alloy welding according to claim 2, characterized in that: The melt obtained after smelting is refined by gas refining method, and the specific method is: using Ar-Cl2 mixed gas, refining for 10 to 20 minutes; After refining, the melt is allowed to stand for 15 to 20 minutes.

5. The method for preparing a welding wire suitable for Al-Li-Cu-Mg-Zn alloy welding according to claim 2, characterized in that: The temperature for casting the melt is 780-840°C, and the speed at which the ingot is pulled out of the crystallizer is 80-90 mm / min.