A supported low-valent palladium single atom material and its preparation method and application

By doping phosphorus atoms on the carbon nitride support and reducing treatment, a load-type low-valent palladium single-atom material was prepared, which solved the problem of reduced catalytic activity caused by the agglomeration of palladium single-atoms on the support, and achieved efficient removal of halogenation Organic pollutants and reduce costs.

CN115722249BActive Publication Date: 2024-11-22ZHEJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211484591.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-24
Publication Date
2024-11-22
Estimated Expiration
2042-11-24

AI Technical Summary

Technical Problem

Traditional palladium nanomaterials have problems such as complex operation, difficulty in storage and transportation of hydrogen and high cost of precious metal materials when catalyzing reduction and degradation of halogenated organic matter. In addition, single palladium atoms are prone to agglomeration on the support, resulting in reduced catalytic activity and difficult to be applied on a large scale.

Method used

By doping phosphorus atoms on the carbon nitride support and performing reduction treatment, the valence state of the single palladium atom is regulated, so that it is dispersed in a zero-valence state or a low-valence state, improving catalytic activity and utilization rate, and preparing a load-type low-valence state, a high-valence state isolate, and a low-valence state isolate, a load-type low-valence state isolate, and a low-valence state isolate isolate, which can improve the catalytic activity and utilization rate. Palladium single atomic material.

Benefits of technology

It significantly improves the catalytic reduction activity of palladium single atoms and the removal effect of halogenated organic pollutants, reduces the cost of material use, and achieves good stability and recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003961480800000011
    Figure HDA0003961480800000011
  • Figure HDA0003961480800000012
    Figure HDA0003961480800000012
  • Figure HDA0003961480800000021
    Figure HDA0003961480800000021
Patent Text Reader

Abstract

The present invention discloses a supported low-valent palladium single atom material and a preparation method and application thereof, wherein cyanuric acid and melamine are dissolved in ultrapure water; palladium salt and organic acid are dissolved in ultrapure water and mixed with cyanuric acid solution; phosphoric acid is added to melamine solution; a mixed solution of cyanuric acid and organic palladium polymer is added to a phosphate melamine polymer solution and stirred; a reducing agent is added to the mixed solution and stirred until the reaction is complete; the obtained precipitate is washed and dried and then calcined in a tube furnace to obtain a supported low-valent palladium single atom material. The present invention prepares a supported low-valent palladium single atom material by introducing phosphorus and a reducing agent during the preparation process. The supported low-valent palladium single atom significantly improves the utilization rate of palladium atoms and the activity of catalyzing formic acid to degrade halogenated hydrocarbons, and can be used to catalyze the degradation of halogenated organic pollutants in wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of treatment of halogenated organic polluted wastewater, and specifically relates to a supported low-valent palladium single atom material and a preparation method and application thereof. Background Art

[0002] The pollution of halogenated organic matter in the environment caused by the abuse of halogenated organic solvents, pesticides, antibiotics, etc. has received widespread attention in recent years, and traditional treatment processes are difficult to effectively remove the above-mentioned halogenated organic pollutants. In recent years, studies have shown that the use of catalysts to catalyze the degradation of halogenated organic matter is one of the effective ways to repair halogenated organic pollution in the environment. For example, catalytic reduction technology (CRT) represented by palladium nanomaterials catalyzing hydrogen can achieve rapid reduction and degradation of a variety of halogenated organic pollutants, and has therefore been widely studied. However, this technology is complex to operate, and faces problems such as difficulties in hydrogen storage and transportation, and high costs of precious metal materials, making it difficult to apply on a large scale. At present, some studies have proposed that palladium single-atom catalytic materials can improve the efficiency of atomic utilization and the selectivity of atomic reactions, thereby achieving the goal of significantly reducing the cost of material use while improving the treatment effect of halogenated organic pollutants. Therefore, palladium single-atom catalysts have great application potential in the field of environmental remediation such as efficient removal of halogenated organic matter in water, and have attracted widespread attention from researchers.

[0003] Since metal single atoms such as palladium are thermodynamically unstable and easily aggregate into nanoclusters, resulting in a reduction in atomic utilization, it is necessary to load the single atoms onto a carrier to maintain their atomic-level dispersion. For example, carriers represented by carbon nitride contain a large number of nitrogen atoms with uncoordinated free electrons, which can be used as anchoring sites to fix dispersed metal atoms. However, while carriers such as carbon nitride anchor metal single atoms through strong interactions with metal atoms such as palladium and copper, they reduce the electron density of metal atoms, so that metal atoms are often loaded onto the carrier in the form of high-valent metal cations. The high valence of metal atoms significantly reduces the catalytic reduction activity of metal single atoms such as palladium, limiting their application scenarios in environmental remediation fields such as catalytic reduction degradation of halogenated organic matter. Therefore, reducing the valence state of palladium single atoms on the carrier is particularly important for improving the catalytic reduction activity of palladium single atoms. However, how to achieve the regulation of the valence state of supported metal single atoms is a huge challenge facing the current field of single-atom material preparation.

[0004] Therefore, it is urgent to develop a method for preparing a supported low-valent palladium single atom catalytic material, and prepare a supported low-valent palladium single atom catalytic material, so that palladium single atoms are dispersed on the carrier in the form of zero valence or low valence, thereby improving the utilization rate and catalytic reduction activity of palladium atoms, improving the removal effect of halogenated organic pollutants and reducing the cost of material use, and meeting the practical application needs of wastewater treatment containing halogenated organic pollutants. As an electron-rich element, phosphorus has a low electronegativity and a coordinated lone electron pair. In theory, phosphorus doping can regulate the coordination environment of palladium atoms on the carrier and increase the electron density of palladium single atoms in the carrier. Therefore, doping phosphorus atoms in the preparation process of supported palladium single atom precursors is expected to achieve the regulation of the valence state of supported palladium single atoms, thereby improving the catalytic reduction activity of supported palladium single atoms. In the process of preparing supported palladium single atom precursors, reduction treatment is carried out on them, and palladium single atoms can be made to participate in coordination in the form of zero valence during the self-assembly process of the carrier and the palladium single atom precursor, thereby facilitating the preparation of supported low-valent palladium single atom materials. Summary of the invention

[0005] The purpose of the present invention is to address the deficiencies of the prior art and provide a supported low-valent palladium single atom material and a preparation method and application thereof.

[0006] The objective of the present invention is achieved through the following technical solutions:

[0007] In a first aspect, the present invention provides a method for preparing a supported low-valent palladium single-atom material, comprising the following method:

[0008] S1: adding melamine and cyanuric acid to ultrapure water respectively, heating to 80-90° C. and stirring to obtain a melamine solution and a cyanuric acid solution; the concentration of the melamine solution is 0-60 mmol / L, and the concentration of the cyanuric acid solution is 0-60 mmol / L;

[0009] S2: dissolving an organic acid in ultrapure water, then adding a water-soluble palladium salt to the organic acid solution and stirring for 0.5-1h to obtain an organic palladium polymer solution; the molar ratio of the water-soluble palladium salt to the organic acid is 1:5-20;

[0010] S3: adding the organic palladium polymer solution prepared in step S2 to the cyanuric acid solution prepared in step S1 and stirring for 0.5-1h to obtain a mixed solution of cyanuric acid and organic palladium polymer; the molar ratio of cyanuric acid to water-soluble palladium salt is 50-1000:1;

[0011] S4: adding a palladium atomic valence regulator to the melamine solution prepared in step S1 and stirring for 0.5-1h to obtain a melamine polymer solution; the molar ratio of the palladium atomic valence regulator to melamine is 0.1-1:1;

[0012] S5: adding the mixed solution of cyanuric acid and organic palladium polymer prepared in step S3 to the melamine polymer solution prepared in step S4, and continuously stirring for 4-5 hours to obtain a supported palladium single atom precursor suspension;

[0013] S6: adding a reducing agent to the supported palladium single atom precursor suspension prepared in step S5, stirring for 0.5-1h to obtain a supported low-valent palladium single atom precursor suspension; the molar ratio of the reducing agent to melamine is 0.005-0.1:1;

[0014] S7: The supported low-valent palladium single atom precursor suspension obtained in step S6 is filtered and washed with deoxygenated ultrapure water, and then placed in a vacuum drying oven for vacuum drying at 60-90°C. After drying, the material is ground into powder and placed in a tubular furnace. Under argon protection, the furnace temperature is raised to 500-700°C at a heating rate of 5-10°C / min, and then calcined for 3-5h to obtain a supported low-valent palladium single atom material.

[0015] Furthermore, the organic acid is oxalic acid or acetic acid.

[0016] Furthermore, the water-soluble palladium salt is palladium nitrate or its hydrate, potassium chloropalladate or its hydrate, sodium chloropalladate or its hydrate, palladium chloride or its hydrate.

[0017] Furthermore, the palladium atom valence state regulator is phosphoric acid, phosphate or phosphate hydrate.

[0018] Furthermore, the reducing agent is sodium borohydride or potassium borohydride.

[0019] Furthermore, the flow rate of the argon gas is 5-50 mL / min.

[0020] In a second aspect, the present invention provides a supported low-valent palladium single atom material.

[0021] In the third aspect, the present invention provides an application of a supported low-valent palladium single atom material in catalyzing formic acid reduction to remove halogenated organic pollutants in water, comprising the following steps: adding the supported low-valent palladium single atom material and formic acid to water at a water temperature of 10-25°C, reacting for 1 hour, and completing the removal of halogenated organic pollutants in the water.

[0022] Furthermore, the water body is surface water, groundwater, municipal sewage or industrial wastewater, the dosage of the supported low-valent palladium single atom material is 0.1-1 g / L, the dosage of formic acid is 0.1-1 g / L, and the concentration of the halogenated organic pollutant is 0-0.3 mmol / L.

[0023] The beneficial effects of the present invention are as follows: the present invention prepares a supported low-valent palladium single-atom material with carbon nitride as a carrier by doping phosphorus in the process of assembling a carbon nitride carrier precursor and a palladium single-atom precursor to form a supported palladium single-atom precursor, and then reducing and calcining it. The supported low-valent palladium single-atom material prepared by the present invention is mainly dispersed on the carbon nitride carrier in the form of zero-valent palladium single atoms. The material can significantly improve the catalytic reduction activity of palladium single atoms while improving the utilization rate of palladium atoms, and realize the catalytic formic acid efficient degradation of various halogenated organic pollutants in water. The material has good stability and reusability (recycled more than 5 times, and the activity is not reduced). The supported low-valent palladium single-atom material prepared by the present invention significantly reduces the cost of wastewater treatment while improving the treatment capacity of halogenated organic polluted wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The present invention is a flow chart of a method for preparing a supported low-valent palladium single atom material;

[0025] Figure 2 This is a scanning electron microscope image of the supported low-valent palladium single atom material prepared in Example 1;

[0026] Figure 3 This is a transmission electron microscope dark field image of the supported low-valent palladium single atom material prepared in Example 1;

[0027] Figure 4 This is a carbon element distribution diagram after energy spectrum scanning of the supported low-valent palladium single atom material prepared in Example 1;

[0028] Figure 5 This is a nitrogen element distribution diagram after energy spectrum scanning of the supported low-valent palladium single atom material prepared in Example 1;

[0029] Figure 6 This is a palladium element distribution diagram after energy spectrum scanning of the supported low-valent palladium single atom material prepared in Example 1;

[0030] Figure 7 This is the X-ray diffraction pattern of the supported low-valent palladium single atom material prepared in Example 1;

[0031] Figure 8 This is a spherical aberration corrected scanning transmission electron microscopy image of the supported low-valent palladium single atom material prepared in Example 1;

[0032] Fig. 9 is the X-ray photoelectron spectrum, where Fig. 9 (a) is the X-ray photoelectron spectrum of conventional supported palladium single atom material. Fig. 9 (b) is an X-ray photoelectron spectrum of the supported low-valent palladium single atom material prepared in Example 1;

[0033] Fig.10 is the degradation diagram of florfenicol, where Fig.10 (a) is a graph showing the effect of formic acid degradation of florfenicol catalyzed by a carbon nitride carrier, a conventional supported palladium single atom material, and a supported low-valent palladium single atom material prepared in Example 3. Fig.10 (b) is a comparison chart of the reaction rates of formic acid degradation of florfenicol catalyzed by conventional supported palladium single atoms and supported low-valent palladium single atoms prepared in Example 3, Fig.10 (c) is a comparison chart of the dechlorination efficiency of conventional supported palladium single atoms and supported low-valent palladium single atom materials prepared in Example 3 in the degradation of florfenicol with formic acid, Fig.10 (d) is a comparison chart of the defluorination efficiency of conventional supported palladium single atoms and supported low-valent palladium single atom materials prepared in Example 3 in the degradation of florfenicol with formic acid;

[0034] Fig.11 This is a graph showing the recycling performance of the supported low-valent palladium single-atom material prepared in Example 3, wherein: Fig.11 (a) is a diagram showing the effect of the supported low-valent palladium single-atom material prepared in Example 3 on the cyclic catalysis of formic acid degradation of florfenicol. Fig.11 (b) is a reaction rate diagram of the cyclic catalytic degradation of florfenicol by formic acid using the supported low-valent palladium single atom material prepared in Example 3;

[0035] Fig.12 The effect diagram of conventional supported palladium single atom material and supported low-valent palladium single atom material prepared in Example 3 catalyzing formic acid to remove various halogenated organic pollutants in water, wherein: Fig.12 (a) is a diagram showing the effect of conventional supported palladium single atom material and supported low-valent palladium single atom material prepared in Example 3 catalyzing formic acid to remove gatifloxacin from water. Fig.12 (b) is a diagram showing the effect of conventional supported palladium single atom material and supported low-valent palladium single atom material prepared in Example 3 catalyzing formic acid to remove chloramphenicol from water. Fig.12 (c) is a diagram showing the effect of conventional supported palladium single atom material and supported low-valent palladium single atom material prepared in Example 3 catalyzing formic acid to remove 4-chlorophenol from water. Fig.12(d) is a diagram showing the effects of conventional supported palladium single atom material and supported low-valent palladium single atom material prepared in Example 3 catalyzing formic acid to remove 2,4-dichlorophenol from water. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0037] Example 1

[0038] The present invention provides Figure 1 The method for preparing a supported low-valent palladium single atom material shown comprises the following steps:

[0039] S1: Weigh 3.026 g of melamine and 2.9422 g of cyanuric acid, add them to 350 mL and 400 mL of ultrapure water respectively, heat to 80° C. in a water bath, and stir continuously to obtain a melamine solution and a cyanuric acid solution. The melamine and cyanuric acid are both used as carbon nitride carrier precursors.

[0040] S2: 0.3 mL of anhydrous acetic acid was measured and diluted to 40 mL with ultrapure water, and then 119.2 mg of palladium nitrate dihydrate was weighed and added to the acetic acid solution and stirred for 1 hour to obtain a palladium acetate polymer solution. The palladium nitrate dihydrate was used as a palladium source.

[0041] S3: injecting the palladium acetate polymer solution prepared in step S2 into the cyanuric acid solution prepared in step S1 and stirring for 1 hour to obtain a mixed solution of cyanuric acid and palladium acetate polymer.

[0042] S4: 1 mL of anhydrous phosphoric acid is measured and diluted to 10 mL with ultrapure water, and then added to the melamine solution prepared in step S1, and stirred for 1 hour to obtain a melamine phosphate polymer solution.

[0043] S5: adding the mixed solution of cyanuric acid and palladium acetate polymer prepared in step S3 to the melamine phosphate polymer solution prepared in step S4, stirring for 5 hours, and obtaining a supported palladium single atom precursor suspension.

[0044] S6: Weigh 89 mg of sodium borohydride and dissolve it in 20 mL of ultrapure water, add it to the supported palladium single atom precursor suspension prepared in step S5, and continue stirring for 0.5 h to obtain a supported low-valent palladium single atom precursor suspension.

[0045] S7: Filter the supported low-valent palladium single atom precursor suspension prepared in step S6 and wash it three times with ultrapure water, then place it in a vacuum drying oven and vacuum dry it at 60°C. After drying, grind the obtained material into powder and place it in a tubular furnace. Under the protection of argon at a flow rate of 5 mL / min, raise the furnace temperature to 600°C at a heating rate of 10°C / min, and then calcine for 4 hours to obtain the supported low-valent palladium single atom material.

[0046] Example 2

[0047] S1: Weigh 3.026 g of melamine and 2.9422 g of cyanuric acid, add them into 400 mL and 400 mL of ultrapure water respectively, heat to 85° C. in a water bath, and stir continuously to obtain a melamine solution and a cyanuric acid solution. The melamine and cyanuric acid are both used as carbon nitride carrier precursors.

[0048] S2: Weigh 27 mg of oxalic acid and dissolve it in 30 mL of ultrapure water, then weigh 39 mg of potassium chloropalladate and add it to the oxalic acid solution and stir for 0.5 h to obtain a palladium oxalate polymer solution. The potassium chloropalladate is used as a palladium source.

[0049] S3: adding the palladium oxalate polymer solution prepared in step S2 to the cyanuric acid solution prepared in step S1 and stirring for 0.5 h to obtain a mixed solution of cyanuric acid and palladium oxalate polymer.

[0050] S4: Dissolve 0.2 mL of anhydrous phosphoric acid in 10 mL of ultrapure water, then add the solution to the melamine solution prepared in step S1 and stir for 0.5 h to obtain a melamine phosphate polymer solution.

[0051] S5: Add the mixed solution of cyanuric acid and palladium oxalate polymer prepared in step S3 to the melamine phosphate polymer solution prepared in step S4, and stir for 4 hours to obtain a supported palladium single atom precursor suspension.

[0052] S6: Weigh 20 mg of sodium borohydride and dissolve it in 20 mL of ultrapure water, then add it to the supported palladium single atom precursor suspension prepared in step S5, and continue stirring for 0.5 h to obtain a supported low-valent palladium single atom precursor suspension.

[0053] S7: Filter the supported low-valent palladium single atom precursor suspension prepared in step S6 and wash it three times with deoxygenated ultrapure water, then place it in a vacuum drying oven and vacuum dry it at 60°C. After drying, grind the obtained material into powder and place it in a tubular furnace. Under the protection of argon at a flow rate of 10 mL / min, raise the furnace temperature to 600°C at a heating rate of 10°C / min and calcine for 4 hours to obtain a supported low-valent palladium single atom material.

[0054] Example 3

[0055] S1: Weigh 3.026 g of melamine and 2.9422 g of cyanuric acid, add them into 350 mL and 400 mL of ultrapure water respectively, heat to 85° C. in a water bath, and stir continuously to obtain a melamine solution and a cyanuric acid solution. The melamine and cyanuric acid are both used as carbon nitride carrier precursors.

[0056] S2: 0.3 mL of anhydrous acetic acid was measured and diluted to 30 mL with ultrapure water to obtain an acetic acid solution, and then 85 mg of palladium chloride was weighed and added to the acetic acid solution and stirred for 0.5 h to obtain a palladium acetate polymer solution. The palladium chloride was used as a palladium source.

[0057] S3: adding the palladium acetate polymer solution prepared in step S2 to the cyanuric acid solution prepared in step S1 and stirring for 1 hour to obtain a mixed solution of cyanuric acid and palladium acetate polymer.

[0058] S4: dilute 1 mL of anhydrous phosphoric acid to 10 mL with ultrapure water, then add it to the melamine solution prepared in step S1 and stir for 0.5 h to obtain a melamine phosphate polymer solution.

[0059] S5: adding the mixed solution of cyanuric acid and palladium acetate polymer prepared in step S3 to the melamine phosphate polymer solution prepared in step S4, stirring for 5 hours, to obtain a supported palladium single atom precursor suspension.

[0060] S6: Weigh 89 mg of sodium borohydride and dissolve it in 40 mL of ultrapure water, then add it to the supported palladium single atom precursor suspension prepared in step S5, and continue stirring for 1 hour to obtain a supported low-valent palladium single atom precursor suspension.

[0061] S7: Filter the supported low-valent palladium single atom precursor suspension prepared in step S6 and wash it three times with deoxygenated ultrapure water, then place it in a vacuum drying oven and vacuum dry it at 60°C. After drying, grind the obtained material into powder and place it in a tubular furnace. Under the protection of argon at a flow rate of 50 mL / min, raise the furnace temperature to 550°C at a heating rate of 10°C / min and calcine for 4 hours to obtain a supported low-valent palladium single atom material.

[0062] Figure 2 The figure shows a scanning electron microscope image of the supported low-valent palladium single atom material prepared in Example 1. The material morphology is a tubular material with a diameter of about 2 μm. Figure 3 The dark field image of a portion of the supported low-valent palladium single atom tubular material prepared in Example 1 is shown, and the scale bar in the figure is 50 nm. Figure 3Only the local morphology of the carrier was observed, and no obvious bright spots were observed, indicating that palladium was dispersed and loaded on the carrier at the atomic level. Figure 4-6 Shown is the pair Figure 3 Energy spectrum scanning diagram of supported low-valent palladium single atom material in the area shown, where Figure 4 Shown is the pair Figure 3 The carbon element distribution diagram of the supported low-valent palladium single atom material after energy spectrum scanning is shown. Figure 5 Shown Figure 3 The nitrogen element distribution diagram of the supported low-valent palladium single atom material after energy spectrum scanning is shown. Figure 6 for Figure 3 The palladium element distribution diagram of the supported low-valent palladium single atom material after energy spectrum scanning. Figure 4-6 The results show that the main components of the carrier in the supported low-valent palladium single atom material prepared in Example 3 are nitrogen and carbon, that is, a carbon nitride carrier is formed, and palladium atoms are uniformly loaded on the carrier.

[0063] Figure 7 The figure shows the X-ray diffraction pattern of supported low-valent palladium single atom material. Figure 7 It can be seen that the carbon nitride carrier (g-C3N4) and the supported low-valent palladium single atom material (Pd 1-red / g-C3N4) showed typical diffraction peaks of graphite phase carbon nitride, but no diffraction peaks of palladium were detected, indicating that the palladium in the prepared supported low-valent palladium single-atom material did not form a crystal structure, and the palladium element existed in the form of a single atom.

[0064] Figure 8 The spherical aberration-corrected scanning transmission electron micrograph of the supported low-valent palladium single atom material prepared in Example 1 is shown, and the scale bar shown in the figure is 5 nm. Figure 8 It can be seen that the palladium element is mainly dispersed on the carbon nitride carrier in the form of single atoms, which further indicates that the palladium element is dispersed and loaded on the carbon nitride carrier at the atomic level.

[0065] like Fig. 9 The figure shows the X-ray photoelectron spectroscopy (XPS) of palladium element in the supported palladium single atom material, where Fig. 9 a is the X-ray photoelectron spectrum of conventional supported palladium single atom material (Pd1 / g-C3N4), Fig. 9 b is the X-ray photoelectron spectrum of the supported low-valent palladium single atom material prepared in Example 1. Fig. 9 It can be seen that compared with conventional carbon nitride-supported palladium single atom materials, the vast majority of palladium atoms in the supported low-valent palladium single atom material are dispersed and supported on the carbon nitride carrier in a zero-valent form, that is, the supported low-valent palladium single atom material is successfully prepared using the present invention.

[0066] Application Example 1

[0067] Weigh 20 mg of carbon nitride carrier (g-C3N4), conventional supported palladium single atom material (Pd1 / g-C3N4) and supported low-valent palladium single atom material (Pd1 / g-C3N4) prepared in Example 3 respectively. 1-red / g-C3N4) was added to a 42mL serum bottle containing 17.5mL ultrapure water and ultrasonicated for 10min; then 0.5mL of 1mol / L formic acid solution and 2mL of 2.8mmol / L florfenicol solution were injected into the bottle respectively, and then covered with a rubber cover pad lined with polytetrafluoroethylene and mixed, so that the initial concentration of florfenicol in the reaction system was 0.28mmol / L.

[0068] The serum bottle was placed on a rotating incubator, the speed of the rotating incubator was set to 50 rpm, 100 μL of the solution was extracted with a glass injection needle at a preset time point and diluted to 1 mL, and then filtered with a 0.22 μm filter membrane; the filtered solution was subjected to liquid chromatography to detect the residual florfenicol content in the solution. The florfenicol content change curve during the reaction is as follows: Fig.10 As shown in a. Fig.10 It can be seen that compared with carbon nitride carriers and conventional supported palladium single-atom materials, supported low-valent palladium single-atom materials have a significant removal effect on florfenicol. After kinetic fitting of the reaction data, the reaction rate constants of conventional supported palladium single-atom materials and supported low-valent palladium single-atom materials catalyzing formic acid degradation of florfenicol were obtained, as shown in Fig.10 As shown in b. Fig.10 b It can be seen that the reaction rate of formic acid degradation of florfenicol catalyzed by conventional supported palladium single atom material is 0.7 L·g -1 ·h -1 The reaction rate of the supported low-valent palladium single-atom material prepared in Example 3 for catalyzing the degradation of florfenicol with formic acid was 1200 L·g -1 ·h -1 , which is more than 1,700 times faster than the reaction rate of conventional supported palladium single atom materials, indicating that reducing the valence state of palladium single atoms can significantly enhance the catalytic reduction activity of palladium single atoms.

[0069] After 1 hour of reaction, 1 mL of the serum bottle was sampled and then diluted to 10 mL. The diluted solution was filtered and pretreated with a 0.22 μm filter membrane, a C18 filter column, and a NA filter column, and then ion chromatography was performed to detect the content of chloride ions generated in the reaction system. Fig.10 As shown in c, from Fig.10c It can be seen that the dechlorination efficiency of conventional supported palladium single atom material for florfenicol is only 7.3%, while the dechlorination efficiency of supported low-valent palladium single atom material for florfenicol prepared in Example 3 reaches 100%.

[0070] After 5 hours of reaction, 1 mL of the serum bottle was sampled and then diluted to 10 mL. The diluted solution was filtered and pretreated with a 0.22 μm filter membrane, a C18 filter column, and a NA filter column, and then ion chromatography was performed to detect the content of fluoride ions generated in the reaction system. Fig.10 d, from Fig.10 d It can be seen that the conventional supported palladium single atom material cannot achieve the defluorination of florfenicol, while the supported low-valent palladium single atom material prepared in Example 3 has a defluorination efficiency of 35% for florfenicol after 5 hours of reaction.

[0071] Fig.10 It shows that compared with conventional supported palladium single atom materials, the supported low-valent palladium single atom material prepared in Example 3 significantly improves the reaction rate, dechlorination efficiency and defluorination efficiency of palladium single-atom catalytic degradation of florfenicol, indicating that by reducing the valence state of palladium single atoms on the carrier, the atomic utilization rate of palladium and the reaction performance of palladium single-atom catalytic formic acid reduction degradation of florfenicol can be significantly improved.

[0072] In order to verify the catalytic stability and recyclability of the supported low-valent palladium single-atom material, the supported low-valent palladium single-atom material prepared in Example 3 was subjected to 5 cycles of catalytic formic acid degradation of florfenicol: after the supported low-valent palladium single-atom material catalyzed the formic acid degradation of florfenicol for 1 hour, the supported low-valent palladium single-atom material and the solution in the solution were centrifuged; after the centrifugation was completed, the supernatant was poured out, and 17.5 mL of ultrapure water was added again and ultrasonicated for 10 minutes; after the ultrasonication was completed, 0.5 mL of 1 mol / L formic acid solution and 2 mL of 2.8 mmol / L florfenicol solution were injected again, and 100 μL of the sample was taken at a predetermined time point, diluted to 1 mL, and filtered through a 0.22 μm filter membrane. The residual florfenicol concentration in the solution was determined by liquid chromatography. The above experimental steps were repeated 5 times. The changes in the residual florfenicol in the solution during the cycle test are shown as follows. Fig.11 As shown in a, Fig.11 It can be seen that the supported low-valent palladium single atom material prepared in Example 3 always maintains an excellent degradation effect on florfenicol. The change in the catalytic degradation reaction rate of florfenicol by the supported low-valent palladium single atom prepared in Example 3 in 5 cycle tests is shown in FIG. Fig.11 As shown in b, Fig.11 b shows that the reaction rate of the supported low-valent palladium single atom material remained at 36 L·g in the five cycle tests.-1 ·min -1 . Fig.11 It shows that the supported low-valent palladium single atom material has good catalytic stability, so in actual wastewater treatment applications, the cost of wastewater treatment can be reduced by recycling the catalyst.

[0073] Application Example 2

[0074] 20 mg of conventional supported palladium single atom material and supported low-valent palladium single atom material prepared in Example 3 were weighed respectively, added into a 42 mL serum bottle containing 11.5 mL ultrapure water and ultrasonicated for 10 min; then 0.5 mL of 1 mol / L formic acid solution was injected into the bottle respectively;

[0075] 2 mL of gatifloxacin solution, chloramphenicol solution, 4-chlorophenol solution and 2,4-dichlorophenol solution were injected into the serum bottle respectively, and then covered with a rubber cover pad lined with polytetrafluoroethylene and mixed, so that the initial concentrations of gatifloxacin, chloramphenicol, 4-chlorophenol and 2,4-dichlorophenol in the reaction system were 0.28 mmol / L, respectively.

[0076] The serum bottle was placed on a rotating incubator, the speed of the rotating incubator was set to 50 rpm, 100 μL of the solution was extracted with a glass injection needle at a preset time point and diluted to 1 mL, and then filtered with a 0.22 μm filter membrane; the filtered solution was subjected to liquid chromatography to detect the content of residual halogenated organic pollutants. The content of residual halogenated organic matter in the solution during the reaction was as follows: Fig.12 The curve of the residual gatifloxacin content in the solution during the reaction is shown in FIG. Fig.12 As shown in a, the residual chloramphenicol content change curve in the solution is as follows Fig.12 As shown in b, the residual 4-chlorophenol content change curve in the solution is as follows Fig.12 c, the residual 2,4-dichlorophenol content variation curve in the solution is as follows Fig.12 d. Fig.12 It can be seen that compared with conventional supported palladium single atom materials, the supported low-valent palladium single atom material prepared in Example 3 has a significant removal effect on four halogenated organic pollutants, namely gatifloxacin, chloramphenicol, 4-chlorophenol and 2,4-dichlorophenol, indicating that by reducing the valence state of palladium single atoms on the carrier, the ability of palladium single atoms to catalyze formic acid to degrade various halogenated organic pollutants in water can be significantly improved.

[0077] Application Examples 1 and 2 show that the supported low-valent palladium single-atom material can be used to catalyze formic acid reduction to remove halogenated organic pollutants in water, which is characterized by comprising the following steps: adding the supported low-valent palladium single-atom material and formic acid to a water body containing halogenated organic pollutants, the water body temperature is 10-25°C, reacting for 1 hour, and completing the removal of halogenated organic pollutants in the water body. The water body is surface water, groundwater, municipal sewage or industrial wastewater, the dosage of the supported low-valent palladium single-atom material is 0.1-1g / L, the dosage of the formic acid is 0.1-1g / L, and the concentration of the halogenated organic pollutants is 0-0.3mmol / L.

[0078] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a supported low-valent palladium single-atom material, characterized in that: Includes the following methods: S1: adding melamine and cyanuric acid to ultrapure water respectively, heating to 80-90° C. and stirring to obtain a melamine solution and a cyanuric acid solution; the concentration of the melamine solution is 0-60 mmol / L, and the concentration of the cyanuric acid solution is 0-60 mmol / L; S2: dissolving an organic acid in ultrapure water, then adding a water-soluble palladium salt to the organic acid solution and stirring for 0.5-1h to obtain an organic palladium polymer solution; the molar ratio of the water-soluble palladium salt to the organic acid is 1:5-20; The water-soluble palladium salt is palladium nitrate or its hydrate, potassium chloropalladate or its hydrate, sodium chloropalladate or its hydrate, palladium chloride or its hydrate; S3: adding the organic palladium polymer solution prepared in step S2 to the cyanuric acid solution prepared in step S1 and stirring for 0.5-1h to obtain a mixed solution of cyanuric acid and organic palladium polymer; the molar ratio of cyanuric acid to water-soluble palladium salt is 50-1000:1; S4: adding a palladium atomic valence regulator to the melamine solution prepared in step S1 and stirring for 0.5-1h to obtain a melamine polymer solution; the molar ratio of the palladium atomic valence regulator to melamine is 0.1-1:1; The palladium atomic valence state regulator is phosphoric acid, phosphate or phosphate hydrate; S5: adding the mixed solution of cyanuric acid and organic palladium polymer prepared in step S3 to the melamine polymer solution prepared in step S4, and continuously stirring for 4-5 hours to obtain a supported palladium single atom precursor suspension; S6: adding a reducing agent to the supported palladium single atom precursor suspension prepared in step S5, stirring for 0.5-1h to obtain a supported low-valent palladium single atom precursor suspension; the molar ratio of the reducing agent to melamine is 0.005-0.1:1; S7: The supported low-valent palladium single atom precursor suspension obtained in step S6 is filtered and washed with deoxygenated ultrapure water, and then placed in a vacuum drying oven for vacuum drying at 60-90°C. After drying, the material is ground into powder and placed in a tubular furnace. Under argon protection, the furnace temperature is raised to 500-700°C at a heating rate of 5-10°C / min, and then calcined for 3-5h to obtain a supported low-valent palladium single atom material.

2. The method for preparing a supported low-valent palladium single-atom material according to claim 1, characterized in that: The organic acid is oxalic acid or acetic acid.

3. The method for preparing a supported low-valent palladium single-atom material according to claim 1, characterized in that: The reducing agent is sodium borohydride or potassium borohydride.

4. The method for preparing a supported low-valent palladium single-atom material according to claim 1, characterized in that: The flow rate of the argon gas is 5-50 mL / min.

5. A supported low-valent palladium single atom material prepared by any method of claims 1-4.

6. Use of the supported low-valent palladium single atom material according to claim 5 in catalyzing formic acid reduction to remove halogenated organic pollutants in water, characterized in that: The following steps are involved: The loaded low-valent palladium single atom material and formic acid are added into water at a temperature of 10-25°C and reacted for 1 hour to complete the removal of halogenated organic pollutants in the water.

7. The use according to claim 6, characterized in that: The water body is surface water, groundwater, municipal sewage or industrial wastewater, the dosage of the supported low-valent palladium single atom material is 0.1-1 g / L, the dosage of the formic acid is 0.1-1 g / L, and the concentration of the halogenated organic pollutant is 0-0.3 mmol / L.