A method for resource utilization of fluorine in rare earth molten salt electrolytic slag
Through the coordinated roasting of aluminum sulfate and calcium oxide and acid leaching treatment, combined with rare earth compound salt precipitation and iron removal purification, fluorine is successfully recovered efficiently in rare earth molten salt electrolytic slag, and high value-added polymer-specific ice crystals are prepared, which solves fluorine resources The unused problem has achieved efficient and environmentally friendly rare earth and fluorine recycling, meeting the dual value of economy and environmental protection.
Patent Information
- Application Number
- CN202211423891.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-15
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-11-15
AI Technical Summary
Among the existing rare earth molten salt electrolytic slag recovery technology, the rare earth recovery rate is high but the fluorine resources are not effectively utilized, resulting in fluorine gas pollution and high recycling costs, and lack of environmentally friendly and economically beneficial solutions.
Aluminum sulfate and calcium oxide are used to jointly roast rare earth molten salt electrolytic slag, and rare earth and fluorine are separated and extracted through acid leaching and rare earth complex salt precipitation. After iron removal and pH adjustment, polymer-specific ice crystals are finally prepared to realize fluorine resources. Use.
While rare earth recycling, the fluorine recovery rate is greater than 90%, and there is no fluorine-containing pollutants. The prepared ice crystals meet national standards and have significant environmental protection and economic value.
Smart Images

Figure HDA0003943345420000011
Abstract
Description
Technical Field
[0001] The invention relates to a metallurgical secondary resource recycling technology, and in particular to a resource utilization method of fluorine in rare earth molten salt electrolytic slag. Background Art
[0002] At present, single rare earth metals and their alloys are mainly produced through the fluoride system molten salt electrolysis process. During the production process, the rare earth recovery rate is only 85-93%, and the residual rare earths are mainly present in the molten salt slag in the form of fluorides. The rare earth content in the slag can reach 20%-70% (calculated as REO), and the fluorine content is 8.28%-22.75%. The rare earth, fluorine and other valuable elements in the rare earth molten salt slag are of high grade. As we all know, rare earths and fluorine are both important strategic resources in my country. Therefore, rare earth molten salt electrolysis slag is an important secondary resource, and the recovery of rare earths and fluorine in it has great economic value.
[0003] At present, rare earth molten salt electrolytic slag is mainly used to recover rare earths in the slag, while fluorine in the slag is removed as an impurity, and the resource utilization of fluorine is not considered. When molten salt slag is treated with sulfuric acid roasting, sulfidation and nitration roasting, fluorine-containing gas will be generated, which pollutes the environment and corrodes equipment. At the same time, the fluorine-containing gas generated needs to be absorbed by alkali solution, which is costly; when calcium salt is used as a fluorine-fixing agent for roasting, calcium fluoride solid will be generated. When rare earths are extracted by acid leaching, calcium fluoride solid waste slag will be generated, forming polluting solid waste; when sodium salt is used for roasting, a large amount of sodium fluoride-containing wastewater will be generated during water washing and fluorine removal, and the recycling cost is high. Therefore, how to efficiently recover rare earths from rare earth molten salt electrolytic slag while recycling fluorine resources in the slag is a problem that needs to be solved in the current molten salt slag recovery technology. The solution to this problem has great environmental and economic value.
[0004] As a resource product of fluorine, cryolite is not only widely used, but also has high added value. Due to its excellent physical and chemical properties, high molecular weight cryolite is currently mainly used as a solvent in the aluminum electrolysis industry. 25 to 30 kilograms of cryolite are consumed for every ton of aluminum produced. Cryolite can also be used as an additive for grinding products, pesticides for crops, enamel whitening agents, etc. It is a compound with great application value. Depending on its quality, the price of cryolite can be as high as US$1,000 per metric ton. At the same time, fluorite, the raw material for synthesizing cryolite in industry, is currently facing a global resource shortage crisis. Therefore, the use of fluorine in molten salt slag to prepare synthetic cryolite has both environmental and economic benefits. Summary of the invention
[0005] The object of the present invention is to provide a method for resource utilization of fluorine in rare earth molten salt electrolytic slag. First, the rare earth molten salt electrolytic slag is co-roasted with aluminum sulfate and calcium oxide, and acid leached to obtain a solution containing rare earth and fluorine. Then, the rare earth is separated and extracted by a rare earth complex salt precipitation process, and the fluorine-containing solution is filtered to obtain a fluorine-containing solution. The fluorine-containing solution is purified by iron removal, and the pH value and component ratio are adjusted to finally prepare a high molecular weight cryolite, thereby realizing the resource utilization of fluorine in the molten salt slag.
[0006] The technical solution of the present invention:
[0007] A method for resource utilization of fluorine in rare earth molten salt electrolytic slag comprises the following steps:
[0008] (1) calcination; weighing rare earth molten salt electrolytic slag (hereinafter referred to as molten salt slag), aluminum sulfate and calcium oxide in a mass ratio of 1:0.5-2:0.1-0.5, and fully mixing them; placing the mixed materials in a ball mill in a ball-to-material mass ratio of 10:1, ball milling at a speed of 400 r / min for 1 hour, and passing the ball milled materials through a 200-mesh sieve; then placing the sieved materials in a corundum crucible, and then placing the corundum crucible in a muffle furnace for calcination at a temperature of 600-900° C. for 1-4 hours. After the calcination is completed, the corundum crucible is taken out and cooled, and the calcined products are ball milled and sieved to obtain calcined slag with a particle size of less than 75 μm;
[0009] (2) Leaching: taking the roasted slag with a particle size of less than 75 μm obtained in step (1) and placing it in a container, and pouring into a H2SO4 solution with a concentration of 1 to 4 mol / L, with a liquid-to-solid mass ratio of 7.5 to 15:1; then placing the container in a water bath at 70 to 95° C. and leaching for 1 to 4 hours, with a stirring speed of 300 r / min, to obtain an acid leaching solution containing rare earth and fluorine;
[0010] (3) rare earth separation: the acid leaching solution obtained in step (2) is transferred to a container, placed in a water bath and heated to 60-95° C., stirred at a speed of 200-400 r / min, the pH value of the solution is adjusted to 0.5-1.5 with 10 wt.% Na2CO3, anhydrous sodium sulfate is added, reacted for 0.5-2 h, and filtered while hot to obtain a rare earth complex salt filter cake and a fluorine-containing filtrate;
[0011] (4) iron removal purification: the fluorine-containing filtrate obtained in step (3) is placed in a container, and a 10 mol / L NaOH solution is added to the container under a stirring speed of 200 to 400 r / min to adjust the pH value to 1 to 2, and then 1.2 to 1.5 times the theoretical amount of H2O2 is added to the container, and stirred for 30 minutes to remove all Fe 2+ All oxidized to Fe 3+; After adjusting the pH value of the solution to 1.5-3 with 10wt.% Na2CO3, place the container in a water bath at 60-95°C and heat at a constant temperature; slowly add 10wt.% Na2CO3 to the solution using a constant pressure titration funnel, stirring while adding, and control the pH value of the solution between 2.5 and 3.5. After reacting for 1-4h, filter while hot to obtain an iron-containing filter cake and a fluorine-containing filtrate after iron removal and purification;
[0012] (5) preparing cryolite; taking the fluorine-containing filtrate obtained after iron removal and purification in step (4) and placing it in a container, and placing it in a water bath at 50°C for heating and stirring, adding a 30-45% by weight hydrofluoric acid solution to the solution to adjust the molar ratio of fluorine to aluminum ions in the solution to 1-7; adding a 10 wt.% Na2CO3 solution dropwise at a stirring speed of 200-400 r / min to adjust the pH value of the solution to 3-6, and then adding cryolite seeds at a rate of 0-10 g / L, reacting in a water bath at 30-90°C for 0.5-2.5 h, and then filtering while hot, and washing the filter cake with deionized water until the pH of the solution in the washing liquid is neutral, to obtain a cryolite filter cake.
[0013] In step (1), the mass ratio of molten salt slag, aluminum sulfate and calcium oxide is preferably 1:1.56:0.31, the roasting temperature is preferably 900° C., and the roasting time is preferably 2 h.
[0014] In step (2), the liquid-solid mass ratio of sulfuric acid to roasted slag is preferably 10:1, the sulfuric acid concentration is preferably 4 mol / L, the leaching temperature is preferably 90° C., and the leaching time is preferably 4 h.
[0015] In step (3), the stirring speed is preferably 300 r / min, the solution pH is preferably 0.8, and the reaction is preferably carried out at 90° C. for 1 h.
[0016] In step (4), preferably, NaOH solution is added under stirring speed of 300 r / min to adjust the pH value to 1.4-2; preferably 1.2 times the theoretical amount of H2O2 is added; preferably, the pH value of the solution is adjusted to 1.8 with 10 wt.% Na2CO3; preferably, the solution is heated at a constant temperature of 95°C in a water bath; 10 wt.% Na2CO3 is slowly added to the solution using a constant pressure titration funnel to control the pH value of the solution to preferably between 2.5 and 3, and the reaction is preferably carried out for 3-4 hours.
[0017] In step (5), the mass fraction of hydrofluoric acid is preferably 40 wt.%, the molar ratio of fluorine to aluminum ion is preferably 5-7, the pH is preferably 3-5, 5 g / L of cryolite seeds are preferably added, the stirring speed is preferably 300 r / min, and the reaction is preferably carried out at 75° C. for 1.5 h.
[0018] The present invention can efficiently recover rare earths from rare earth molten salt electrolytic slag and efficiently recycle fluorine in the slag, with a fluorine recovery rate of more than 90%. Fluorine is also used to prepare high-value-added high-molecular cryolite that meets national standards, and fluorine-containing washing water is circulated for preparing hydrofluoric acid solution. No fluorine-containing pollutants are generated in the entire process, solving the problem of fluorine-containing pollutants existing in the current rare earth molten salt electrolytic slag defluorination and rare earth recovery process and the fluorine in the slag not being utilized as a resource, and has great environmental and economic value. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The XRD spectrum of cryolite synthesized in Example 3 of the present invention is compared with the cryolite standard card. DETAILED DESCRIPTION
[0020] The present invention will be further described in detail below in conjunction with the examples to provide a better understanding of the content of the present invention, but the present invention is not limited to the following examples.
[0021] The present invention uses waste molten salt slag produced during the electrolysis of fluoride system rare earth molten salt as raw material, and the raw material composition is shown in Table 1.
[0022] Table 1 Main chemical composition of molten salt slag wt.%
[0023] Element TREO F <![CDATA[Li2O]]> <![CDATA[Fe2O3]]> <![CDATA[Al2O3]]> <![CDATA[SiO2]]> CaO MgO C content 34.75 18.72 4.91 13.45 5.24 7.26 1.19 0.38 31.2
[0024] Embodiment 1:
[0025] Weigh 20g of molten salt slag, 31.25g of aluminum sulfate and 6.25g of calcium oxide, mix them, put the mixed materials into a ball mill at a ball-to-material mass ratio of 10:1, ball mill at a speed of 400r / min for 1h, and pass the ball milled materials through a 200-mesh sieve. Then put the screened materials into a corundum crucible, and place the crucible in a muffle furnace for roasting at 900°C for 2h. After the roasting is completed, take out the crucible and cool it. The roasted product is ball milled and sieved to obtain a roasted slag with a particle size of less than 75μm.
[0026] Take 20g of ball-milled calcined slag with a particle size of less than 75μm and place it in a beaker, pour in a 3mol / L H2SO4 solution with a liquid-solid mass ratio of 10:1; place the beaker in a 90℃ water bath for 3h, stir at 300r / min, and obtain an acid leaching solution containing rare earth and fluorine. The leaching rates of rare earth and fluorine in the acid leaching solution are 95.83% and 95.45% respectively.
[0027] 150ml of the acid leaching solution was transferred to a three-necked flask, placed in a constant temperature water bath and heated to 85°C, stirred at 300r / min, and the pH value was adjusted to 0.8 with 10wt.% Na2CO3 solution, anhydrous sodium sulfate was added, and after reacting for 1.5h, it was filtered while hot to obtain a rare earth complex salt filter cake, and the filtrate was a fluorine-containing solution. The results showed that 99.76% of the rare earth in the acid leaching solution formed rare earth complex salt precipitation, and the precipitation loss rate of fluorine in the acid leaching solution was 2.27%.
[0028] Take 100 mL of the fluorine-containing filtrate in a three-necked flask, add 10 mol / L NaOH solution to the fluorine-containing filtrate at a stirring speed of 300 r / min to adjust the pH to 1.4, then add 1.2 times the theoretical amount of H2O2 to the three-necked flask and stir for 30 minutes to remove all Fe 2+ All oxidized to Fe 3+ . Adjust the pH value to 1.8 with 10wt.% Na2CO3 solution, and heat the three-necked flask in a water bath at 95℃. Use a constant pressure titration funnel to slowly add 10wt.% Na2CO3 to the solution, stirring while adding, and control the pH value of the solution to 3. React for 3h, filter while hot, and obtain an iron-containing filter cake and a purified fluorine-containing filtrate. The results show that the precipitation rate of iron is 96.69%, and the precipitation loss rate of fluorine in the filtrate is 1.87%.
[0029] Take 80ml of the purified fluorine-containing solution after iron removal into a beaker, place it in a 50℃ water bath with stirring and heating, and add 40% by mass hydrofluoric acid solution to the solution to adjust the molar ratio of fluorine to aluminum ions in the solution to 6. Add 10wt.% Na2CO3 solution dropwise at a stirring speed of 300r / min to adjust the pH value of the solution to 4.5, react in a 75℃ water bath for 1.5h, then filter while hot, and wash the filter cake with deionized water until the pH of the solution in the washing liquid is neutral to obtain a cryolite filter cake, which is used to prepare a hydrofluoric acid solution. The results show that the precipitation rate of fluorine in the solution is 98.32%,
[0030] In summary, the total recovery rate of fluorine in molten salt slag is 90.01%. The contents of Na, Al and F in the prepared cryolite are 32.78%, 13.23% and 53.75% respectively. The calculated product has nNa:nAl=2.83, which is a high molecular ratio cryolite and meets the national standard GB / T 4291-2017. The high molecular ratio cryolite can be efficiently recovered from rare earth molten salt electrolysis slag, and the fluorine in the slag can be efficiently recycled, and the high value-added high molecular ratio cryolite that meets the requirements of national standards can be prepared by using fluorine.
[0031] Embodiment 2:
[0032] Weigh 20g of molten salt slag, 31.25g of aluminum sulfate and 6.25g of calcium oxide, mix them, put the mixed materials into a ball mill at a ball-to-material mass ratio of 10:1, ball mill at a speed of 400r / min for 1h, and pass the ball milled materials through a 200-mesh sieve. Then put the screened materials into a corundum crucible, and place the crucible in a muffle furnace for roasting at 900°C for 2h. After the roasting is completed, take out the crucible and cool it. The roasted product is ball milled and sieved to obtain a roasted slag with a particle size of less than 75μm.
[0033] Take 20g of ball-milled calcined slag with a particle size of less than 75μm and place it in a beaker. Pour in a 4mol / L H2SO4 solution with a liquid-solid mass ratio of 10:1. Place the beaker in a 90℃ water bath for 4h with a stirring speed of 300r / min to obtain an acid leaching solution containing rare earth and fluorine. The leaching rates of rare earth and fluorine in the acid leaching solution are 95.83% and 96.85%, respectively.
[0034] 150ml of the acid extract was transferred to a three-necked flask, placed in a constant temperature water bath and heated to 95°C, stirred at 300r / min, and the pH value was adjusted to 0.8 with 10wt.% Na2CO3 solution, anhydrous sodium sulfate was added, reacted for 2h, and filtered while hot to obtain a rare earth complex salt filter cake, and the filtrate was a fluorine-containing solution. The results showed that 99.86% of the rare earth in the filtrate formed rare earth complex salt precipitation, and the precipitation loss rate of F in the solution was 2.17%.
[0035] Take 100 mL of the fluorine-containing filtrate in a three-necked flask, add 10 mol / L NaOH solution to the fluorine-containing filtrate at a stirring speed of 300 r / min to adjust the pH value to 1.4, add 1.4 times the theoretical amount of H2O2 to the three-necked flask, stir for 30 minutes, and remove all Fe 2+ All oxidized to Fe 3+ . Adjust the pH value to 2.0 with 10wt.% Na2CO3 solution, and heat the three-necked flask in a 90℃ water bath. Use a constant pressure titration funnel to slowly add 10wt.% Na2CO3 to the solution, control the pH value of the solution to 2.8, stir while adding, react for 3h, filter while hot, and obtain an iron-containing filter cake and a purified fluorine-containing filtrate. The results show that the precipitation rate of iron is 97.69%, and the precipitation loss rate of fluorine in the filtrate is 1.57%.
[0036] Take 80ml of the purified fluorine-containing solution after iron removal into a beaker, place it in a 50℃ water bath for heating and stirring, add 40% hydrofluoric acid solution by mass to the solution to adjust the molar ratio of fluorine to aluminum ions in the solution to 5. Add 10wt.% Na2CO3 solution dropwise at a stirring speed of 300r / min to adjust the pH value of the solution to 4, raise the water bath temperature to 75℃ for reaction for 1h, then filter while hot, and wash the filter cake with deionized water until the pH of the solution in the washing liquid is neutral to obtain a cryolite filter cake, and the washing liquid is used to prepare the hydrofluoric acid solution. The results show that the precipitation rate of fluorine in the solution is 97.22%.
[0037] In summary, the total recovery rate of fluorine in molten salt slag is 90.67%. The contents of Na, Al and F in the prepared cryolite are 32.75%, 13.46% and 53.5% respectively. The calculated product has nNa:nAl=2.81, which meets the national standard GB / T 4291-2017. The rare earth molten salt electrolysis slag can be efficiently recovered from rare earths, and fluorine in the slag can be efficiently recycled, and fluorine can be used to prepare high value-added high molecular weight cryolite that meets the requirements of national standards.
[0038] Embodiment 3:
[0039] Weigh 20g of molten salt slag, 31.25g of aluminum sulfate and 6.25g of calcium oxide, mix them, put the mixed materials into a ball mill at a ball-to-material mass ratio of 10:1, ball mill at a speed of 400r / min for 1h, and pass the ball-milled materials through a 200-mesh sieve. Then put the materials into a corundum crucible, place the crucible in a muffle furnace and roast it at 900°C for 2h. After the roasting is completed, take out the crucible and cool it. The roasted product is ball milled and sieved to obtain a roasted slag with a particle size of less than 75μm.
[0040] Take 20g of ball-milled calcined slag with a particle size of less than 75μm and place it in a beaker, pour in a 4mol / L H2SO4 solution with a liquid-solid mass ratio of 10:1, place the beaker in a 95℃ water bath for 4h, and stir at a speed of 300r / min to obtain an acid leaching solution containing rare earth and fluorine. The leaching rates of rare earth and fluorine in the acid leaching solution are 96.83% and 97.85%, respectively.
[0041] 150ml of the acid leaching solution was transferred to a three-necked flask, heated in a constant temperature water bath at 90°C, stirred at 300r / min, and the pH value was adjusted to 0.8 with a 10wt.% Na2CO3 solution. Anhydrous sodium sulfate was added, and after reacting for 1h, the solution was filtered while hot to obtain a rare earth complex salt filter cake, and the filtrate was a fluorine-containing solution. The results showed that 99.86% of the rare earth in the filtrate formed rare earth complex salt precipitation, and the precipitation loss rate of fluorine in the solution was 1.98%.
[0042] Take 100mL of fluorine-containing filtrate in a three-necked flask, add 10mol / LNaOH solution to the fluorine-containing filtrate at a stirring speed of 300r / min to adjust the pH of the filtrate to 1.4, then add 1.2 times the theoretical amount of H2O2 to the flask and stir for 30min to remove all Fe 2+ All oxidized to Fe 3+ . Adjust the pH value to 1.6 with 10wt.% Na2CO3 solution and heat it in a water bath at 95℃. Use a constant pressure titration funnel to slowly add 10wt.% Na2CO3 to the solution, control the pH value of the solution to 3, stir while adding, react for 3h, filter while hot to obtain an iron-containing filter cake and a purified fluorine-containing filtrate. The results show that the precipitation rate of iron is 98.69%, and the precipitation loss rate of fluorine in the filtrate is 1.37%.
[0043] Take 80ml of the purified fluorine-containing solution after iron removal into a beaker, place it in a 50℃ water bath for heating and stirring, add 40% hydrofluoric acid solution by mass to the solution to adjust the molar ratio of fluorine to aluminum ions in the fluorine-containing solution to 6. Add 10wt.% Na2CO3 solution dropwise at a stirring speed of 300r / min to adjust the solution pH to 4.5, add 5g / L cryolite seeds, react in a 75℃ water bath for 1h, then filter while hot, and wash the filter cake with deionized water until the pH of the solution in the washing liquid is neutral, to obtain a cryolite filter cake. The XRD spectrum of the filter cake is compared with the cryolite standard card. Figure 1 The washing liquid is used to prepare the hydrofluoric acid solution. The result analysis shows that the XRD spectrum of the generated product matches the spectrum of the cryolite standard card very well, indicating that the product is cryolite, and the precipitation rate of fluorine in the solution is 98.85%.
[0044] In summary, the total recovery rate of fluorine in molten salt slag is 93.51%. The contents of Na, Al and F in the prepared cryolite are 33.64%, 13.58% and 53.96% respectively. The calculated product has nNa:nAl=2.85, which is a high molecular ratio cryolite and meets the national standard GB / T4291-2017. It realizes the efficient recovery of rare earths in rare earth molten salt electrolysis slag, and the efficient resource recovery of fluorine in the slag, and uses fluorine to prepare high value-added high molecular ratio cryolite that meets the requirements of national standards.
Claims
1. A method for resource utilization of fluorine in rare earth molten salt electrolytic slag, characterized in that: The following steps are involved: (1) Calcination: Weigh rare earth molten salt electrolytic slag, aluminum sulfate and calcium oxide in a mass ratio of 1:0.5~2:0.1~0.5 and mix them thoroughly. Put the mixed materials into a ball mill in a ball-to-material mass ratio of 10:1 and ball mill them at a speed of 400 r / min for 1 h. The ball-milled materials are sieved with a 200-mesh sieve. Then, the sieved materials are placed in a corundum crucible, and the corundum crucible is placed in a muffle furnace for calcination at 600~900℃ for 1~4 h. After the calcination is completed, the corundum crucible is taken out and cooled. The calcined products are ball milled and sieved to obtain calcined slag with a particle size of less than 75 μm. (2) Leaching: Place the calcined slag with a particle size of less than 75 μm obtained in step (1) in a container, and pour in a H2SO4 solution with a concentration of 1 to 4 mol / L, with a liquid-to-solid mass ratio of 7.5 to 15:1; then place the container in a water bath at 70 to 95°C for 1 to 4 h, with a stirring speed of 300 r / min, to obtain an acid leaching solution containing rare earth and fluorine; (3) Rare earth separation: the acid leaching solution obtained in step (2) is transferred into a container, placed in a water bath and heated to 60-95°C, stirred at a speed of 200-400 r / min, the pH value of the solution is adjusted to 0.5-1.5 with 10 wt.% Na2CO3, anhydrous sodium sulfate is added, reacted for 0.5-2 h, and filtered while hot to obtain a rare earth complex salt filter cake and a fluorine-containing filtrate; (4) Iron removal purification: The fluorine-containing filtrate obtained in step (3) is placed in a container, and a 10 mol / L NaOH solution is added to the container under a stirring speed of 200-400 r / min to adjust the pH value to 1-2, and then 1.2-1.5 times the theoretical amount of H2O2 is added to the container, and stirred for 30 min to remove all Fe 2+ All oxidized to Fe 3+ ; After adjusting the pH value of the solution to 1.5-3 with 10wt.% Na2CO3, place the container in a water bath at 60-95°C and heat at a constant temperature; slowly add 10wt.% Na2CO3 to the solution using a constant pressure titration funnel, stirring while adding, and control the pH value of the solution between 2.5 and 3.
5. After reacting for 1-4h, filter while hot to obtain an iron-containing filter cake and a fluorine-containing filtrate after iron removal and purification; (5) Preparing cryolite; placing the fluorine-containing filtrate obtained after iron removal and purification in step (4) in a container, and heating and stirring in a water bath at 50°C, adding a 30-45% by mass hydrofluoric acid solution to the solution to adjust the molar ratio of fluorine to aluminum ions in the solution to 1-7; adding a 10 wt.% Na2CO3 solution dropwise at a stirring speed of 200-400 r / min to adjust the pH value of the solution to 3-6, and then adding cryolite seeds at a rate of 0-10 g / L, reacting in a water bath at 30-90°C for 0.5-2.5 h, and then filtering while hot, and washing the filter cake with deionized water until the pH value of the solution in the washing liquid is neutral, thereby obtaining a cryolite filter cake.
2. The method for resource utilization of fluorine in rare earth molten salt electrolytic slag according to claim 1, characterized in that: In step (1), the mass ratio of molten salt slag, aluminum sulfate and calcium oxide is 1:1.56:0.31, the roasting temperature is 900°C and the roasting time is 2 h.
3. The method for resource utilization of fluorine in rare earth molten salt electrolytic slag according to claim 1, characterized in that: In step (2), the liquid-solid mass ratio of sulfuric acid to roasted slag is 10:1, the sulfuric acid concentration is 4 mol / L, the leaching temperature is 90° C., and the leaching time is 4 h.
4. The method for resource utilization of fluorine in rare earth molten salt electrolytic slag according to claim 1, characterized in that: In step (3), the stirring speed is 300 r / min, the solution pH is 0.8, and the reaction is carried out at 90°C for 1 h.
5. The method for resource utilization of fluorine in rare earth molten salt electrolytic slag according to claim 1, characterized in that: In step (4), add NaOH solution under stirring speed of 300 r / min to adjust the pH value to 1.4-2; add 1.2 times the theoretical amount of H2O2; adjust the pH value of the solution to 1.8 with 10wt.% Na2CO3; heat at a constant temperature of 95°C in a water bath; use a constant pressure titration funnel to slowly add 10wt.% Na2CO3 to the solution to control the pH value of the solution to between 2.5 and 3, and react for 3-4h.
6. The method for resource utilization of fluorine in rare earth molten salt electrolytic slag according to claim 1, characterized in that: In step (5), the mass fraction of hydrofluoric acid is 40 wt.%, the molar ratio of fluorine to aluminum ion is 5-7, the pH value is 3-5, 5 g / L of cryolite seed is added, the stirring speed is 300 r / min, and the reaction is carried out at 75° C. for 1.5 h.
Citation Information
Patent Citations
Resource transforming method for separating rare earth from fluorine by utilizing rare earth ore concentrate hydrochloric leachate
CN102899488A
Preparation method of high-purity high-molecular-ratio cryolite
CN103101952A