A method for improving the density consistency of double-sided film layers on quartz wafers
By performing multiple temperature preheating and degassing treatments before film formation on both sides of the quartz MEMS device, the problem of inconsistent density on both sides of the quartz MEMS device is solved, significantly reducing size differences and improving device accuracy.
Patent Information
- Application Number
- CN202211139409.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-19
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-09-19
AI Technical Summary
The difference in double-sided dimensions in quartz MEMS devices leads to a decrease in structural accuracy. The main reason is that the density of the metal film layers on both sides of the quartz surface is inconsistent, which affects the coating and etching processes.
By preheating at two different temperatures before film formation on both sides, the temperature of the substrate is precisely controlled to ensure that the temperatures on both sides are consistent before deposition, thereby improving the consistency of the film layer density. The specific steps include first preheating, degassing, first side deposition, second preheating, second degassing and second side deposition.
It effectively reduces the size difference between the front and back sides of the quartz MEMS device, improves device accuracy, and significantly improves the test indicators after packaging.
Smart Images

Figure CN115747735B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to quartz materials, and in particular to a method for improving the density consistency of double-sided film layers of a quartz wafer. Background Art
[0002] Quartz material, due to its unique piezoelectric properties, has become an ideal material for a variety of sensors, filters and other devices. The process of processing quartz from raw materials into miniaturized, high-performance devices is called the quartz MEMS process, which is opposite to the traditional silicon MEMS process (Micro-Electro-Mechanical System). Similar to the semiconductor manufacturing process, the quartz MEMS process also includes processes such as coating, photolithography, etching, and packaging. A typical quartz structure processing process includes: depositing a film layer (usually metal, which may be single-sided or double-sided) on the quartz surface, transferring the pattern to the film layer through photolithography, and finally etching (usually wet method) to form a specific structure.
[0003] Different from IC manufacturing process, some quartz MEMS sensors have strict requirements on the consistency of their double-sided dimensions. The difference in double-sided dimensions will cause the structure to deviate from the design, which will lead to a decrease in device accuracy. This difference in double-sided dimensions is common in quartz MEMS devices. Summary of the invention
[0004] The present invention aims to solve at least one of the above technical problems.
[0005] The present invention has found that one of the important reasons for the size difference on both sides of the quartz MEMS device is the difference in density of the metal film layer on the surface of both sides of the quartz. On the one hand, due to the different densities of the film layer itself, its etching rate is different, resulting in size differences in the mask patterns on both sides of the wafer after the photolithography is completed; on the other hand, when the quartz is etched using metal films of different densities as masks, the rates are also different. Furthermore, the difference in density is caused by the degassing step in the coating process, which is usually completed by heating with an irradiation lamp before coating. Before the wafer is coated, if the other side of the wafer has been coated, the irradiation lamp will reflect the irradiation light, weakening its heating effect, resulting in a significant difference in the substrate temperature before the deposition step, which leads to the above-mentioned problems.
[0006] The present invention firstly provides a method for improving the density consistency of double-sided film layers of a quartz wafer, by performing two additional preheatings at different temperatures before film formation on both sides, accurately controlling the substrate temperature and thus improving the density consistency of the double-sided film layers.
[0007] Specifically, a method for improving the density consistency of double-sided film layers of a quartz wafer includes:
[0008] S1. Preheat the quartz wafer for the first time at temperature T1 for a period of time t1;
[0009] S2. Degassing, set temperature T2, duration t2;
[0010] S3. Deposition is performed on one side of the quartz wafer;
[0011] S4. The quartz wafer after the first deposition is taken out and preheated for a second time at a temperature T3 for a duration of t3;
[0012] S5. Degassing, setting temperature T4, duration t4;
[0013] S6. Deposition is performed on the other side of the quartz wafer.
[0014] In some embodiments, the quartz wafer in step S1 is wet cleaned and dried in advance.
[0015] In some embodiments, the thickness of the quartz wafer in step S1 is 100-700 μm, for example, 200-500 μm.
[0016] In some embodiments, the temperature T1 is 80-150°C, for example, 100-120°C. Studies have found that preheating at this temperature can bring the wafer to a suitable initial temperature. When the set temperature is too low (less than 80°C), the temperature during deposition will be more affected by the degassing temperature T2, resulting in poor preheating effect; if it is too high (i.e., higher than the degassing temperature, a typical value of 140°C), the degassing step will not be ideal. In addition to the degassing itself, the degassing step also has the function of accurately controlling and adjusting the wafer temperature in a vacuum environment. If the wafer temperature exceeds the degassing temperature before degassing, the adjustment effect is poor and the wafer temperature cannot be accurately controlled.
[0017] In some embodiments, the duration t1 is 20-40 minutes, for example, 20-30 minutes. Studies have found that preheating under this duration can make the actual temperature of the wafer close to or equal to the preheating temperature setting value, and the degassing time should be long enough. Considering the wafer thickness and preheating temperature, 20 minutes can ensure that the temperature reaches the set value; if the time is too long (to more than 40 minutes), there will be no additional effect on the preheating effect, but the efficiency will be reduced due to the extension of time.
[0018] In some specific embodiments, the thickness of the quartz wafer is 500 μm, the temperature T1 is 100° C., and the time t1 is 30 min.
[0019] In some specific embodiments, the thickness of the quartz wafer is 200 μm, the temperature T1 is 120° C., and the time t1 is 30 min.
[0020] In some embodiments, the temperature T2 is 100-150° C. In order to remove as much water vapor as possible in a short time, the temperature should be greater than 100° C. After exceeding 150° C., further increasing the temperature has little effect on the water removal effect.
[0021] In some embodiments, the time t2 is 3-10 minutes, for example, 3-8 minutes. Studies have shown that if the degassing time is too short, the gas cannot be completely removed, and if it is too long, it will not be helpful for precise temperature control and water removal.
[0022] In some embodiments, the duration t2 is less than or equal to 1 / 10 of the duration t1. Studies have shown that if the duration t2 is too long, the temperature control effect of t1 will be affected.
[0023] In some embodiments, the degassing temperature T2 in step S2 is higher than the preheating temperature T1 in step S1, for example, the temperature T2 is 20-50° C. higher than the temperature T1, specifically, for example, higher than 50° C. Studies have found that if the wafer temperature exceeds the degassing temperature before degassing, the adjustment effect is poor and the wafer temperature cannot be accurately controlled.
[0024] In some embodiments, step S3 deposits metal on one side of the quartz wafer to form a metal film layer. Specifically, the metal includes one or more of chromium, nickel, titanium, silver, tungsten, gold, etc., and can be deposited by conventional methods in the art such as magnetron sputtering, evaporation coating, etc. The metal film layer formed by deposition can be determined according to needs.
[0025] In some embodiments, the temperature T3 is 130-150°C. Studies have found that preheating at this temperature can bring the wafer to a suitable initial temperature. When the set temperature is too low (less than 130°C), the temperature during deposition will be more affected by the degassing temperature T4, resulting in poor preheating effect; if it is too high (i.e., higher than the degassing temperature, a typical value of 150°C), the degassing step will not be ideal. In addition to the degassing itself, the degassing step also has the function of accurately controlling and adjusting the wafer temperature in a vacuum environment. If the wafer temperature exceeds the degassing temperature before degassing, the adjustment effect is poor and the wafer temperature cannot be accurately controlled.
[0026] In some embodiments, the time t3 is 20-30 minutes. Studies have found that preheating under this time can make the actual temperature of the wafer close to or equal to the preheating temperature setting value, and the degassing time should be long enough. Considering the wafer thickness and preheating temperature, 20 minutes can ensure that the temperature reaches the set value; if the time is too long (to more than 40 minutes), there will be no additional effect on the preheating effect, but the efficiency will be reduced due to the extension of time.
[0027] In some embodiments, the preheating temperature T1 in step S1 is different from the preheating temperature T3 in step S4. As described above, without preheating, the substrate temperature is actually different before the two depositions start. In order to make the above temperatures the same, differentiated preheating should be performed.
[0028] In some embodiments, the preheating temperature T3 in step S4 is higher than the preheating temperature T1 in step S1, for example, temperature T3 is 10-30° C. higher than temperature T1, specifically, for example, higher than 30° C. It is found that this can keep the substrate temperature consistent before two depositions.
[0029] In some embodiments, the temperature T4 is 100-150° C. In order to remove as much water vapor as possible in a short time, the temperature should be greater than 100° C. After exceeding 150° C., further increasing the temperature has little effect on the water removal effect.
[0030] In some embodiments, the time t4 is 3-10 minutes, for example 3-8 minutes. Studies have shown that if the degassing time is too short, the gas cannot be completely removed, and if it is too long, it will not be helpful for precise temperature control and water removal.
[0031] In some embodiments, the temperature and duration of the degassing in step S2 and step S4 are the same.
[0032] In some embodiments, the duration t4 is less than or equal to 1 / 10 of the duration t3. Studies have shown that if the duration t4 is too long, the temperature control effect of t3 will be affected.
[0033] In some embodiments, the other side in step S6 refers to the side opposite to the side of the quartz wafer in step S4.
[0034] The invention also provides a double-sided film layer quartz wafer, which is prepared by the method.
[0035] The present invention also provides a quartz MEMS sensor, which is made of the above-mentioned double-sided film layer quartz wafer. The specific preparation method can refer to the existing technology.
[0036] The present invention heats the quartz wafer to be plated twice with different parameters before film formation on both sides, ensuring that the substrate temperature is constant before deposition begins, thereby improving the film layer difference on both sides of the wafer and obtaining a device with better dimensional consistency between the front and back sides. The quartz MEMS device manufactured using the method of the present invention has significantly reduced dimensional differences between the front and back sides compared to the traditional process; and its related indicators are also significantly improved in post-packaging testing. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 : Schematic diagram of a method for improving the density consistency of double-sided film layers on a quartz wafer according to an embodiment of the present invention. DETAILED DESCRIPTION
[0038] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the art or the product instructions are used. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased through regular channels.
[0039] This embodiment provides a method for improving the density consistency of the double-sided film layer of a quartz wafer, such as Figure 1 It includes the following steps:
[0040] S1. Preheat the wet-cleaned and dried quartz wafer for the first time at a temperature T1 for a duration of t1.
[0041] S2. Perform degassing, set temperature T2, duration t2.
[0042] S3. Depositing the first side.
[0043] S4. Take out the quartz wafer that has completed the first deposition, and preheat it for a second time at a temperature T3 for a duration of t3.
[0044] S5. Perform degassing, set temperature T4, duration t4.
[0045] S6. Depositing the second side.
[0046] In some embodiments, the above method requires preheating the substrate twice before two film formations, and T1≠T3.
[0047] In some examples, the single preheating time of the above method should be greater than 20 minutes, that is, t1>20min, t3>20min.
[0048] In some examples, the degassing time of the aforementioned method should not be greater than 1 / 10 of the corresponding preheating time.
[0049] In some examples, the degassing temperature of the aforementioned method should be higher than the preheating temperature.
[0050] Example 1
[0051] A 500nm chromium layer was prepared on both sides of a 500μm thick quartz wafer by magnetron sputtering. The process includes: using a mixed solution of concentrated sulfuric acid and hydrogen peroxide (7:3, v / v) to clean and dry the wafer; turning on the hot plate oven, setting the temperature to 100℃, and performing the first preheating after the oven temperature stabilizes, placing the wafer on the hot plate and controlling the gap between the wafer and the hot plate to be less than 2mm; closing the hot plate oven door and keeping it for 30 minutes to make the wafer temperature uniform and stable; taking out the wafer after the preheating is completed, and putting it into the sputtering coating machine as soon as possible; performing the first degassing, setting the temperature to 150℃, and the duration for 3 minutes; depositing a chromium layer on the first side; adjusting the hot plate oven temperature, setting it to 130℃, and performing a second preheating according to the first preheating method, and keeping it for 30 minutes; preparing for the second deposition after the completion, and performing the second degassing according to the first degassing parameters; depositing a chromium layer on the second side.
[0052] Example 2
[0053] A 500nm nickel layer was prepared on both sides of a 500μm thick quartz wafer by evaporation coating. The difference between this process and Example 1 is that: the temperature of the first preheating is 100℃, and the duration is 30min; the temperature of the first degassing is 150℃, and the duration is 3min; the nickel layer is deposited on the first side; the temperature of the second preheating is 130℃, and the duration is 30min; the temperature of the second degassing is 150℃, and the duration is 3min; and the nickel layer is deposited on the second side.
[0054] Example 3
[0055] A 200 nm chromium layer was prepared on both sides of a 200 μm thick quartz wafer by magnetron sputtering. The difference between this process and Example 1 is that the first preheating temperature is 120° C. and the duration is 30 min; the second preheating temperature is 130° C. and the duration is 30 min.
[0056] Comparative Example 1
[0057] The only difference from Example 1 is that two preheating steps are not included.
[0058] Comparative Example 2
[0059] The only difference from Example 1 is that the preheating parameters are the same for the two times.
[0060] Comparative Example 3
[0061] The only difference from Example 1 is that the second preheating step is not included.
[0062] Experimental example
[0063] As mentioned above, the density and consistency of the film layer will affect the etching time. The better the consistency of the film layer on both sides of the wafer, the closer the etching time. This experiment evaluates the properties of the film layer by etching time.
[0064] Take the wafer with both sides coated, immerse it vertically in the etching solution (mixed solution of hydrochloric acid, nitric acid, and hydrogen peroxide) and keep it still, record the time from the beginning of etching to complete dissolution (i.e. etching time) on both sides, and calculate the difference between the two. For the convenience of operation, during the experiment, the wafer is taken out and observed every 5 seconds of etching, so the results are all multiples of 5.
[0065] The results are as follows:
[0066] sample Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Etching time 10 seconds 10 seconds 15 seconds 25 seconds 25 seconds 35 seconds
[0067] It can be seen from the above results that the method of the present invention can effectively improve the density consistency of the film layers on both sides of the wafer.
[0068] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A method for improving the density consistency of double-sided film layers on a quartz wafer, characterized in that: include: S1. Preheat the quartz wafer for the first time at temperature T1 for a period of time t1; The temperature T1 is 80-150°C; the time t1 is 20-40min; S2. Degassing is performed, and the temperature T2 and the duration t2 are set; the temperature T2 is 100-150°C; the duration t2 is 3-10min; the duration t2 is less than or equal to 1 / 10 of the duration t1; the temperature T2 is 20-50°C higher than the temperature T1; S3. Deposition is performed on one side of the quartz wafer; S4. Take out the quartz wafer after the first deposition, and preheat it for the second time at temperature T3 for a time period t3; the temperature T3 is 130-150° C.; the time period t3 is 20-30 minutes; the temperature T3 is 10-30° C. higher than the temperature T1; S5. Degassing is performed, and the temperature T4 and the duration t4 are set; the temperature T4 is 100-150°C; the duration t4 is 3-10min; the temperature and duration of degassing in step S2 and step S5 are the same; the duration t4 is less than or equal to 1 / 10 of the duration t3; S6. Deposition is performed on the other side of the quartz wafer.
2. The method for improving the density consistency of double-sided film layers of quartz wafer according to claim 1, characterized in that: The thickness of the quartz wafer in step S1 is 100-700 μm.
3. The method for improving the density consistency of double-sided film layers of quartz wafer according to claim 2, characterized in that: The thickness of the quartz wafer in step S1 is 200-500 μm.
4. The method for improving the density consistency of double-sided film layers of a quartz wafer according to any one of claims 1 to 3, characterized in that: The temperature T1 is 100-120° C.; the time t1 is 20-30 min.
5. The method for improving the density consistency of double-sided film layers of quartz wafer according to claim 4, characterized in that: The thickness of the quartz wafer is 500 μm, the temperature T1 is 100° C., and the duration t1 is 30 min; or, The thickness of the quartz wafer is 200 μm, the temperature T1 is 120° C., and the time t1 is 30 min.
6. The method for improving the density consistency of double-sided film layers of a quartz wafer according to any one of claims 1 to 3, characterized in that: The duration t2 is 3-8 minutes.
7. The method for improving the density consistency of double-sided film layers of a quartz wafer according to any one of claims 1 to 3, characterized in that: The temperature T2 is 50° C. higher than the temperature T1.
8. The method for improving the density consistency of double-sided film layers of a quartz wafer according to any one of claims 1 to 3, characterized in that: Step S3 is to deposit metal on one side of the quartz wafer to form a metal film layer.
9. The method for improving the density consistency of double-sided film layers of a quartz wafer according to claim 8, characterized in that: The metal includes one or more of chromium, nickel, titanium, silver, tungsten and gold.
10. The method for improving the density consistency of double-sided film layers of a quartz wafer according to any one of claims 1 to 3, characterized in that: The temperature T3 is 30° C. higher than the temperature T1.
11. The method for improving the density consistency of double-sided film layers of a quartz wafer according to any one of claims 1 to 3, characterized in that: The duration t4 is 3-8 minutes.
12. A double-sided film-layer quartz wafer, characterized in that: Prepared by the method according to any one of claims 1 to 11.
13. A quartz MEMS sensor, characterized in that: Made from the double-sided film layer quartz wafer as described in claim 12.
Citation Information
Patent Citations
Preparation method of quartz pendulous reed
CN111847847A
Wax spraying method for reducing corrosion scattering difference of quartz WAFER sheet
CN113463027A