Preparation method and application of mesoporous high entropy alloy catalyst

By preparing mesoporous high-entropy alloy catalysts, the problem of mesoporous intermetallic compounds synthesis is solved, the catalytic site efficiency is improved and the reaction stability is enhanced, suitable for large-scale production, and the raw material cost is reduced.

CN115763840BActive Publication Date: 2024-11-01SICHUAN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211560956.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-07
Publication Date
2024-11-01
Estimated Expiration
2042-12-07

AI Technical Summary

Technical Problem

The synthesis of mesoporous high entropy intermetallic compounds has not yet been achieved, resulting in the controllable macromorphology, orderly mesoporous structure and controllable atomic structure of mesoporous metal nanomaterials, which is still a challenge, limiting its in-catalytic field application.

Method used

A mesoporous high entropy alloy catalyst is prepared, including sodium chloropalladium chloroplatinate and potassium chloroplatinate being filled into the KIT-6 pore by reduced pressure, adding ascorbic acid for reduction, followed by addition of ferric chloride, cobalt chloride and Nickel chloride is calcined, and finally impurities and templates are removed with hydrochloric acid and hydrofluoric acid to obtain a mesoporous high entropy alloy catalyst.

Benefits of technology

This method realizes the preparation of mesoporous high-entropy alloy catalysts, combines the advantages of mesoporous and high-entropy intermetallic compounds, improves the utilization efficiency of catalytic sites, mass and area activity of the catalyst, and enhances the stability of the catalytic reaction , and reduces raw material costs, suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115763840B_ABST
    Figure CN115763840B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a mesoporous high entropy alloy catalyst, comprising the following steps: S1, filling sodium chloropalladate and potassium chloroplatinite into KIT-6 pores by decompression; S2, adding ascorbic acid for reduction, removing unreacted impurities by water washing, and drying to obtain Meso-PtPd / KIT-6; S3, adding ferric chloride to M-PtPd / KIT-6 for grinding, placing in a tubular furnace for calcination to obtain FCT-PtPdFe / KIT-6; S4, adding FCT-PtPdFe / KIT-6 to the catalyst; Cobalt chloride is added to T‑6 for grinding; FCT‑PtPdFeCo / KIT‑6 is obtained by calcining in a tubular furnace; S5, nickel chloride is added to FCT‑PtPdFeCo / KIT‑6 for grinding; FCT‑PtPdFeCoNi / KIT‑6 is obtained by calcining in a tubular furnace; S6, FCT‑PtPdFeCoNi / KIT‑6 needs to be soaked in hydrochloric acid to remove cobalt and nickel impurities that are not introduced into the crystalline phase, and the SiO2 template is removed by soaking in hydrofluoric acid to obtain a mesoporous high entropy alloy catalyst. The present invention provides a method for preparing a mesoporous high entropy alloy catalyst, which has the characteristics of simple process, mild reaction conditions, energy saving and emission reduction, good product morphology maintenance, and large-scale preparation. The present invention provides an application of a mesoporous high entropy alloy catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, and in particular to a preparation method of a mesoporous high entropy alloy catalyst and application thereof. Background Art

[0002] Mesoporous materials refer to materials containing pores with diameters between 2 and 50 nm. Since their first discovery in the early 1990s, functional mesoporous materials have received great attention and have become a research hotspot in the past 30 years. In the 30 years since the first report of the template method, great progress has been made in the development of functional mesoporous materials with various compositions, morphologies, mesoporous structures and pore sizes. They are widely used in adsorption, separation, sensors, catalysis, energy conversion and storage, biomedicine, electronic devices and other fields. In particular, the large pore size of mesopores can well meet the growing needs of application processes involving macromolecules or nanoparticles, such as drug delivery, petroleum and biomass conversion, etc. Compared with mature traditional nanoporous materials (such as silica, titania, transition metal oxides and carbon), more functional mesoporous metal / alloy materials with both metallic properties and mesoporous functions are more attractive. In particular, Pt-based alloy materials with both mesoporous framework stability and high-performance catalytic activity have received widespread attention in the field of catalysis and electrocatalysis. As the second generation of new mesoporous materials, the development of mesoporous metal single substances or alloys is relatively lagging. Mesoporous metals have multiple structural advantages over corresponding bulk and / or support materials. First, high mesoporosity gives mesoporous metals more catalytic active sites (higher than nanoparticles with the same surface area), exposing a large number of saturated sites, thereby significantly improving the utilization efficiency of precious metals and improving their catalytic mass activity. In addition, compared with discrete nanoparticles, the continuous mesoporous crystal framework can accelerate the transmission of electrons and inhibit the physical Ostwald ripening process, thereby activating and stabilizing mesoporous metals. Third, the concave / convex framework structure and confined environment can change the surface electronic structure of mesoporous metal nanocrystals, provide a "nano-clamp" environment for reactants, especially key intermediates, thereby changing the catalytic trend / barrier and possibly optimizing the catalytic selectivity for the target product. At present, the development of mesoporous metal / alloy nanomaterials has just started, and is limited to simple component regulation of nanomaterials and structural / morphological regulation of mesoporous particles and films, which is due to the difficulty in controlling the aqueous phase reduction kinetics and controllable crystal nucleation kinetics. The controllable preparation of mesoporous metal / alloy nanomaterials with controllable macroscopic morphology, ordered mesoscopic structure, and controllable atomic structure is still a challenge.

[0003] High entropy intermetallic compounds are a special class of alloy materials. They are a multi-component alloy composition formed by five or more metals. These high entropy intermetallic compounds exhibit very unique structural and chemical synergistic regulation, such as self-assembled long-range close-packed atomic ordered arrangement, sub-lattice occupancy of complex superlattices, and multi-element co-segregation and disordered phase transition at the interface nanoscale, thus showing many excellent physical and mechanical properties that traditional metal materials cannot possess, such as anomalous yield, high toughness, creep resistance, superelasticity, shape memory effect, etc. In the hot research field of catalysis and electrocatalysis, thanks to strong d orbital interactions and ordered stoichiometry, high entropy intermetallic compounds not only exhibit optimized electronic structures and expanded metal utilization efficiency to improve their mass activity, but also achieve "enthalpy" stability to improve long-term durability.

[0004] In recent years, the precise control of the size, shape, composition, structure and crystalline phase of high-entropy intermetallic compound nanocrystals has been widely studied in important technological applications. Different from single metal nanocrystals and other types of structured nanocrystals (such as core-shell and heterostructured nanocrystals), high-entropy intermetallic compound nanocrystals with precise structures have unique and interesting physicochemical properties and are ideal models for structure-property studies. However, the formation of intermetallic structures is highly dependent on harsh conditions (high temperature, high pressure, etc.), so most of the high-entropy intermetallic compound materials reported so far are irregular nanoparticles. So far, the synthesis of mesoporous high-entropy intermetallic compounds has not been achieved. Therefore, the design and synthesis of mesoporous high-entropy intermetallic compounds will be a new field, which is of great significance for expanding the synthesis of mesoporous metal nanomaterials. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a mesoporous high entropy alloy catalyst, which has the characteristics of simple process, mild reaction conditions, energy saving and emission reduction, good product morphology retention and large-scale preparation, and is suitable for large-scale production and application.

[0006] The technical solution adopted by the preparation method of a mesoporous high entropy alloy catalyst and its application disclosed in the present invention is:

[0007] A method for preparing a mesoporous high entropy alloy catalyst comprises the following steps:

[0008] S1, sodium chloropalladate and potassium chloroplatinite are filled into the pores of KIT-6 by decompression;

[0009] S2, adding ascorbic acid to reduce the product in step S1, removing unreacted impurities by washing with water, and drying to obtain solid powder Meso-PtPd / KIT-6;

[0010] S3, adding ferric chloride to the M-PtPd / KIT-6 obtained in step S2, grinding the mixture, and calcining the mixture in a tube furnace to obtain a mesoporous intermetallic compound FCT-PtPdFe / KIT-6 solid powder;

[0011] S4, adding cobalt chloride to the FCT-PtPdFe / KIT-6 solid powder obtained in step S3 for grinding; placing the solid powder in a tube furnace for calcination to obtain FCT-PtPdFeCo / KIT-6 solid powder;

[0012] S5, adding nickel chloride to the FCT-PtPdFeCo / KIT-6 solid powder obtained in step S4 for grinding; placing the solid powder in a tube furnace for calcination to obtain FCT-PtPdFeCoNi / KIT-6 solid powder;

[0013] S6, the obtained FCT-PtPdFeCoNi / KIT-6 needs to be soaked in hydrochloric acid to remove the cobalt and nickel impurities that are not introduced into the crystalline phase, and soaked in hydrofluoric acid to remove the SiO2 template, and finally a mesoporous high entropy alloy catalyst is obtained.

[0014] As a preferred embodiment, in step S1, the mass ratio of sodium chloropalladate, potassium chloroplatinite and KIT-6 is 1:2:15, and the sodium chloropalladate, potassium chloroplatinite and KIT-6 are all dissolved in water, and then dried under reduced pressure in a vacuum drying oven at 45-55°C for 1-1.5 hours.

[0015] As a preferred embodiment, the concentration of ascorbic acid added in step S2 is 0.25 mol / L.

[0016] As a preferred embodiment, the mass ratio of ferric chloride, cobalt chloride and nickel chloride is 9:8:5, and the mass ratio of nickel chloride to sodium chloropalladate is 1:4.

[0017] As a preferred embodiment, in the steps S3-S5, the calcination temperature is 400-500°C, the calcination time is 6-10 hours, the heating rate is 2-5°C / minute, and a reducing gas is introduced during the calcination process. The reducing gas is a H2 / N2 atmosphere in which the ratio of hydrogen to nitrogen is 5:95, the flow rate is 0.08-0.2L / min, and the pyrolysis temperature is 450-500°C.

[0018] As a preferred solution, in step S5, the concentration of the hydrochloric acid is 1 mol / L, and the concentration of the hydrofluoric acid used to etch the SiO2 template is 20%.

[0019] As a preferred embodiment, the mesoporous high entropy intermetallic compound with a component ratio of FCT-PtPdFeCoNi is obtained in step S5.

[0020] An application of a mesoporous high entropy alloy catalyst, comprising physically loading the above-mentioned mesoporous high entropy alloy catalyst and Vulcan XC-72 carbon black in a mass ratio of 1:1 and drop-coating the catalyst as a cathode catalyst on a clean rotating disk electrode, wherein the catalyst loading is 0.05 mg / cm 2 , and after drying, was applied to electrocatalytic oxygen reduction.

[0021] As a preferred solution, a three-electrode system is used, the catalyst is dripped onto a rotating disk electrode as a working electrode, a saturated silver / silver chloride electrode is used as a reference electrode, a carbon rod is used as a counter electrode, and a potassium hydroxide solution is used as an electrolyte. The potassium hydroxide concentration in the electrolyte is 0.1 mol / L. Before using the disk electrode, the electrode surface needs to be polished with aluminum oxide polishing powder to remove impurities from the pollution source. The particle size of aluminum oxide is 0.05 mm.

[0022] As a preferred embodiment, during the catalyst preparation process, ethanol:deionized water with a volume ratio of 4:1 is used as the solvent; the catalyst concentration is 1 mg / mL.

[0023] The beneficial effect of the preparation method of a mesoporous high entropy alloy catalyst disclosed in the present invention is that the mesoporous high entropy alloy catalyst prepared by the above preparation method combines the advantages of mesopores and high entropy metal intermetallic compound crystal structures: mesopores improve the utilization efficiency of catalytic sites, improve the mass activity and area activity of the catalyst; the stable mesoporous framework structure inhibits the Ostwald ripening process and enhances the stability of the catalytic reaction; the high entropy metal intermetallic compound has five specific atoms, the surface is highly heterogeneous, and a large number of different active sites are produced, which can accelerate the reaction kinetics; the high entropy metal intermetallic compound has the highest mixing enthalpy, which improves the structural stability of the catalyst during the catalytic process; the high entropy metal intermetallic compound has a specific structure and lattice constant, which is convenient for establishing the structure-activity relationship between the catalyst structure and the catalytic activity. Therefore, the use of the catalyst can not only improve the activity and stability of electrocatalytic oxygen reduction, but also clarify the relationship between the catalyst structure and the catalytic activity, improve the utilization rate of precious metals, and greatly reduce the cost of raw materials; and the one-step synthesis method is simple, easy to operate, can be prepared in large quantities, and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is the X-ray diffraction pattern (XRD) of the mesoporous high entropy metal FCT-PtPdFeCoNi catalyst prepared in Example 1 of the present invention and the comparative catalyst face-centered cubic high entropy alloy FCC-PtPdFeCoNi catalyst.

[0025] Figure 2 These are scanning electron microscope images (SEM) and transmission electron microscope images (TEM) of the mesoporous high entropy intermetallic FCT-PtPdFeCoNi catalyst prepared in Example 1 of the present invention.

[0026] Figure 3 It is the linear sweep voltammetry (LSV) curve of the mesoporous high entropy metal FCT-PtPdFeCoNi catalyst prepared in Example 1 of the present invention, the comparative catalyst face-centered cubic high entropy alloy FCC-PtPdFeCoNi catalyst and the commercial Pt / C catalyst.

[0027] Figure 4 It is a mass activity bar graph of the mesoporous high entropy metal FCT-PtPdFeCoNi catalyst prepared in Example 1 of the present invention, the comparative catalyst face-centered cubic high entropy alloy FCC-PtPdFeCoNi catalyst and the commercial Pt / C catalyst.

[0028] Figure 5 The LSV curves of the mesoporous high entropy intermetallic FCT-PtPdFeCoNi catalyst prepared in Example 1 of the present invention before and after 50,000 cyclic voltammetry (CV) tests.

[0029] Figure 6 It is the IT curve of the mesoporous high entropy intermetallic FCT-PtPdFeCoNi catalyst prepared in Example 1 of the present invention at a voltage of -0.3V (vs Ag / AgCl).

[0030] Figure 7 It is the LSV curve of the mesoporous high entropy intermetallic FCT-PtPdFeCoNi catalyst prepared in Example 1 of the present invention at 25-60°C. DETAILED DESCRIPTION

[0031] The present invention will be further described and illustrated below in conjunction with specific embodiments and accompanying drawings:

[0032] A method for preparing a mesoporous high entropy alloy catalyst comprises the following steps:

[0033] S1, sodium chloropalladate and potassium chloroplatinite are filled into the pores of KIT-6 by decompression;

[0034] In step S1, the mass ratio of sodium chloropalladate, potassium chloroplatinite and KIT-6 is 1:2:15, and sodium chloropalladate, potassium chloroplatinite and KIT-6 are all dissolved in water, and then dried under reduced pressure in a vacuum drying oven at 45-55° C. for 1-1.5 hours.

[0035] S2, adding ascorbic acid to the solution in step S1 for reduction, removing unreacted impurities by washing with water, and drying to obtain solid powder Meso-PtPd / KIT-6; the concentration of ascorbic acid is 0.25 mol / L, and the volume of the ascorbic acid solution is 2 mL.

[0036] S3, adding ferric chloride to the M-PtPd / KIT-6 obtained in step S2, grinding the mixture, and calcining the mixture in a tube furnace to obtain a mesoporous intermetallic compound FCT-PtPdFe / KIT-6 solid powder;

[0037] S4, adding cobalt chloride to the FCT-PtPdFe / KIT-6 solid powder obtained in step S3 for grinding; placing the solid powder in a tube furnace for calcination to obtain FCT-PtPdFeCo / KIT-6 solid powder;

[0038] S5, adding nickel chloride to the FCT-PtPdFeCo / KIT-6 solid powder obtained in step S4 for grinding; placing the solid powder in a tube furnace for calcination to obtain FCT-PtPdFeCoNi / KIT-6 solid powder;

[0039] The mass ratio of the above-mentioned ferric chloride, cobalt chloride and nickel chloride is 9:8:5, the mass ratio of nickel chloride to sodium chloropalladate is 1:4, and in steps S3-S5, the calcination temperature is 400-500°C, the calcination time is 6-10 hours, the heating rate is 2-5°C / minute, and a reducing gas is introduced during the calcination process. The reducing gas is a H2 / N2 atmosphere, in which the ratio of hydrogen to nitrogen is 5:95, the flow rate is 0.08-0.2L / min, and the pyrolysis temperature is 450-500°C.

[0040] S6, the obtained FCT-PtPdFeCoNi / KIT-6 needs to be soaked in hydrochloric acid to remove the cobalt and nickel impurities that are not introduced into the crystal phase, and soaked in hydrofluoric acid to remove the SiO2 template. The concentration of hydrochloric acid is 1 mol / L, and the concentration of hydrofluoric acid used to etch the SiO2 template is 20%, and finally a mesoporous high entropy alloy catalyst is obtained.

[0041] The obtained material in the above step S5 is a mesoporous high entropy intermetallic compound with a composition ratio of FCT-PtPdFeCoNi.

[0042] The mesoporous high entropy alloy catalyst prepared by the above preparation method combines the advantages of mesopores and high entropy metal intermetallic compound crystal structure: mesopores improve the utilization efficiency of catalytic sites, improve the mass activity and area activity of catalysts; the stable mesoporous framework structure inhibits the Ostwald ripening process and enhances the stability of catalytic reactions; high entropy metal intermetallic compounds have five specific atoms, highly heterogeneous surfaces, and produce a large number of different active sites, which can accelerate reaction kinetics; high entropy metal intermetallic compounds have the highest mixing enthalpy, which improves the structural stability of catalysts during catalysis; high entropy metal intermetallic compounds have specific structures and lattice constants, which facilitate the establishment of a structure-activity relationship between catalyst structure and catalytic activity. Therefore, the use of this catalyst can not only improve the activity and stability of electrocatalytic oxygen reduction, but also clarify the relationship between catalyst structure and catalytic activity, improve the utilization rate of precious metals, and greatly reduce the cost of raw materials; and the one-step synthesis method is simple, easy to operate, can be prepared in large quantities, and is suitable for large-scale industrial production.

[0043] An application of a mesoporous high entropy alloy catalyst, wherein the mesoporous high entropy alloy catalyst and Vulcan XC-72 carbon black are physically loaded in a mass ratio of 1:1 and are drop-coated on a clean rotating disk electrode as a cathode catalyst, and the catalyst loading is 0.05 mg / cm 2 , and after drying, was applied to electrocatalytic oxygen reduction.

[0044] In the above scheme, a three-electrode system is used, the catalyst is dripped on the rotating disk electrode as the working electrode, the saturated silver / silver chloride electrode is used as the reference electrode, the carbon rod is used as the counter electrode, and the potassium hydroxide solution is used as the electrolyte. The potassium hydroxide concentration in the electrolyte is 0.1 mol / L. Before the disk electrode is used, the electrode surface needs to be polished with aluminum oxide polishing powder to remove impurities from the pollution source. The particle size of aluminum oxide is 0.05 mm.

[0045] During the catalyst preparation process, ethanol: deionized water with a volume ratio of 4:1 was used as the solvent; the catalyst concentration was 1 mg / mL, and the disc electrode surface needed to be polished with alumina polishing powder before use to remove impurities from the pollution source. The alumina particle size was 0.05 mm, and the disc electrode area was 0.196 square centimeters. Oxygen was required to be passed to saturation before the electrochemical test and during the reduction process. The oxygen purity was above 99.999%. In the electrochemical test, the reaction potential was 0.2V-0.9V relative to the silver / silver chloride electrode, and the reaction temperature was 25°C.

[0046] Embodiment 1:

[0047] Preparation of KIT-6:

[0048] 7.9 g of hydrochloric acid was dissolved in 144 mL of deionized water, and then 4 g of Pluronic P123 (EO20PO70EO20, Aldrich) was added. After stirring and dissolving completely, 4 g of 1-butanol was added and stirred for 1 h. Then 8.6 g of tetraethyl orthosilicate was added to the above mixture and magnetically stirred at 30° C. for 24 h.

[0049] After the reaction was completed, the mixture was transferred to a hydrothermal reactor and hydrothermally heated at 75°C for 24 hours. After the hydrothermal treatment, the solid product was filtered and washed to recover, and after drying, it was placed in a muffle furnace and calcined at 550°C for 6 hours at a heating rate of 2°C per minute to obtain KIT-6.

[0050] Preparation of symbiotic template Meso-PtPd / KIT-6

[0051] Weigh 40 mg of potassium chloroplatinate and 20 mg of sodium chloropalladate and dissolve them in 2 mL of deionized water, then add 0.3 g of KIT-6, ultrasonically disperse and place in a vacuum oven to dry under reduced pressure. Then, 2.0 mL of freshly prepared L-ascorbic acid (AA) solution (0.25 M) was added dropwise to the solid powder, and the meso-Pt in the mesoporous KIT-6 began to crystallize. The reaction was carried out at room temperature for 10 hours. After washing with deionized water and drying, the symbiotic template Meso-PtPd / KIT-6 was obtained.

[0052] Preparation of face-centered tetragonal intermetallic phase FCT-PtPdFe / KIT-6

[0053] 10 mg of anhydrous FeCl3 was weighed and dissolved in 0.2 mL of anhydrous ethanol, and then added to a mortar containing 50 mg of Meso-PtPd / KIT-6. After grinding evenly, the mixture was placed in a tube furnace under a H2 / N2 atmosphere (5:95) at 0.1 L min -1 The mixture was treated at 470°C for 6 hours.

[0054] Preparation of Mesoporous Quaternary Metallic FCT-PtPdFeCo

[0055] 8 mg of CoCl2 was weighed and dissolved in 0.2 mL of anhydrous ethanol, and then added to the mortar containing FCT-PtPdFe / KIT-6. After grinding evenly, the mixture was placed in a tube furnace under a H2 / N2 atmosphere (5:95) at 0.08 L min -1 The mixture was treated at 470°C for 6 hours.

[0056] Preparation of Mesoporous High Entropy Intermetallic FCT-PtPdFeCoNi

[0057] 5 mg NiCl2 was weighed and dissolved in 0.2 mL anhydrous ethanol, and then added to the mortar containing FCT-PtPdFeCo / KIT-6. After grinding evenly, the mixture was placed in a tube furnace under H2 / N2 atmosphere (5:95) at 0.08 L min -1 The flow rate was 470 ° C for 6 hours. Finally, FCT-PtPdFeCoNi / KIT-6 was soaked in 1 mol / L HCl and 20% HF solution for two hours to remove impurities and SiO2 template, and washed with deionized water three times to obtain mesoporous high entropy metal FCT-PtPdFeCoNi.

[0058] Electrocatalytic oxygen reduction reaction

[0059] Electrochemical workstation (Chenhua 660e) was used for electrocatalytic oxygen reduction reaction. The test used a three-electrode system, with a rotating disk electrode as the working electrode, a saturated silver / silver chloride electrode as the reference electrode, and a carbon rod electrode as the counter electrode. 0.1 mol / L potassium hydroxide solution was used as the electrolyte. Before the electrochemical test and during the reduction process, argon gas with a purity of more than 99.9% was required to be passed to saturation. The test temperature was 25°C.

[0060] Comparative Example 1

[0061] Preparation of Mesoporous High Entropy Alloy FCC-PtPdFeCoNi

[0062] The mesoporous high entropy alloy FCC-PtPdFeCoNi comparative catalyst was synthesized as a comparison of catalytic properties. The preparation process of the mesoporous high entropy alloy FCC-PtPdFeCoNi catalyst is as follows: 8 mg of FeCl3 was weighed and dissolved in 0.2 mL of anhydrous ethanol and then added to a mortar containing 50 mg of Meso-PtPd / KIT-6. After grinding evenly, the mixture was placed in a tube furnace under a H2 / N2 atmosphere (5:95) at 0.1 L min -1 The mesoporous alloy FCC-PtPdFe / KIT-6 was obtained by treating at 400°C for 6 hours at a flow rate of . Subsequently, 8 mg CoCl2 and 6 mg NiCl2 were weighed in sequence to obtain the mesoporous quaternary alloy FCC-PtPdFeCo / KIT-6 and the mesoporous high entropy alloy FCC-PtPdFeCoNi / KIT-6 in the above method. Finally, FCC-PtPdFeCoNi / KIT-6 was soaked in 1 mol / L HCl and 20% HF solution for two hours to remove the SiO2 template, and the mesoporous high entropy alloy FCC-PtPdFeCoNi was obtained by washing with deionized water three times.

[0063] Comparative Example 2

[0064] Preparation of Pt nanoparticles (NPs)

[0065] The catalytic properties of commercial Pt / C catalysts were compared.

[0066] In the electrocatalytic oxygen reduction test, the current density (j) within the voltage range is recorded by linear sweep voltammetry (LSV), which can be used to characterize the electrochemical behavior within the voltage range, wherein the LSV scan rate is 10mV / s, and the scan voltage range is 0.1-1.2V relative to the standard hydrogen electrode; the constant voltage method can be used to record the current-time (It) curve under the applied potential to record the stability of the catalyst; the applied voltage range in the embodiment of the present application is 0.6V relative to the standard hydrogen electrode. The reaction temperature during the catalytic reaction is adjusted by a water bath; the range is 25-60°C.

[0067] The calculation method of mass activity (MA) is as follows:

[0068]

[0069] where i k is the oxygen reduction kinetic current of the tested LSV curve; m Pt is the mass of catalyst on the electrode surface normalized to Pt.

[0070] Kinetic current i k It can be calculated by the Koutecky Levich equation:

[0071]

[0072] where i and i L represent the measured current and the ultimate diffusion-limited current of the LSV curve, respectively.

[0073] Catalyst structure characterization and electrocatalytic oxygen reduction performance analysis of the examples:

[0074] Figure 1 a is the XRD spectrum of the mesoporous high entropy intermetallic FCT-PtPdFeCoNi catalyst prepared in Example 1 of the present invention, which reveals that FCT-PtPdFeCoNi has a face-centered tetragonal crystal structure with a P4 / mmm space group, which is consistent with the PtFe standard intermetallic phase (JCPDS No.65-1051), indicating that Co and Ni atoms selectively replace part of the Fe sites.

[0075] Figure 1b is the XRD spectrum of the mesoporous high entropy alloy FCC-PtPdFeCoNi prepared in Comparative Example 1 of the present invention, which reveals that FCC-PtPdFeCoNi has a face-centered cubic crystal structure of the Pm-3m space group, and all diffraction peak positions are positively shifted, which is caused by the alloying of Fe, Co, and Ni atoms with smaller radii with Pt and Pd.

[0076] Figure 2 The SEM and TEM images of the mesoporous high entropy intermetallic FCT-PtPdFeCoNi catalyst prepared in Example 1 of the present invention are shown in the figure. The catalyst is highly uniformly dispersed mesoporous nano-dodecahedrons with an average diameter of 240nm. There are abundant and highly permeable mesopores in the whole particle, with a mesopore size of 3.7-4.5nm and a skeleton thickness of 3.6-4.2nm.

[0077] Figure 3 The LSV curves of the mesoporous high entropy metal FCT-PtPdFeCoNi catalyst prepared in Example 1 of the present invention, the mesoporous high entropy alloy FCC-PtPdFeCoNi catalyst in Comparative Example 1, and the commercial Pt / C catalyst in the electrocatalytic oxygen reduction test. The figure shows that the oxygen reduction half-wave potential of FCT-PtPdFeCoNi can reach E 1 / 2 =0.91V, the limiting current density can reach 5.6mA / cm 2 , which is higher than the half-wave potential E of the FCC-PtPdFeCoNi catalyst 1 / 2 = 0.89 V and the half-wave potential E of the commercial Pt / C catalyst 1 / 2 =0.86V, which has great potential commercial value.

[0078] Figure 4 The mass activity comparison of the mesoporous high entropy metal FCT-PtPdFeCoNi prepared in Example 1 of the present invention, the mesoporous high entropy alloy FCC-PtPdFeCoNi catalyst in Comparative Example 1, and the commercial Pt / C catalyst at a voltage of 0.9V (relative to the standard hydrogen electrode) is shown in the figure. The oxygen reduction mass activity of the mesoporous high entropy metal FCT-PtPdFeCoNi catalyst is as high as 0.63A / mg PtPd , which is much higher than the mesoporous high entropy alloy FCC-PtPdFeCoNi catalyst (0.41A / mg PtPd ) and commercial Pt / C catalyst (0.11A / mg Pt ), indicating that the mesoporous high-entropy intermetallic FCT-PtPdFeCoNi catalyst has the best electrocatalytic oxygen reduction activity.

[0079] Figure 5The figure shows the LSV curves of the mesoporous high entropy metal intermetallic FCT-PtPdFeCoNi catalyst prepared in Example 1 of the present invention after 10,000, 20,000, 30,000, 40,000 and 50,000 cycles of accelerated durability tests. The figure shows that after 50,000 cycles of accelerated durability tests, the LSV curves of the mesoporous high entropy metal intermetallic FCT-PtPdFeCoNi catalyst are basically overlapped, with only a slight decrease in limiting current, indicating that the mesoporous high entropy alloy FCC-PtPdFeCoNi catalyst has the best electrocatalytic oxygen reduction stability.

[0080] Figure 6 This is a curve obtained by chronoamperometry at a voltage of 0.6 V (relative to the standard hydrogen electrode) for the mesoporous high entropy intermetallic FCT-PtPdFeCoNi catalyst prepared in Example 1 of the present invention. The figure shows that the current of the mesoporous high entropy intermetallic FCT-PtPdFeCoNi catalyst only decreased by 3% after 10 hours of electrolysis at a corresponding voltage of 0.6 V relative to the standard hydrogen electrode, once again demonstrating that the mesoporous high entropy intermetallic FCT-PtPdFeCoNi catalyst has the best electrocatalytic oxygen reduction stability.

[0081] Figure 7 This is the LSV curve of the mesoporous high entropy metal intermetallic FCT-PtPdFeCoNi catalyst prepared in Example 1 of the present invention in the range of 25°C-60°C (one LSV curve is tested for each 5°C increase). The figure shows that after increasing from 25°C to 60°C, the half-wave potential and limiting current of the LSV curve do not change significantly, indicating that the mesoporous high entropy metal intermetallic FCT-PtPdFeCoNi catalyst can be actually used in low-temperature proton exchange membrane fuel cells.

[0082] The present invention provides a method for preparing a mesoporous high entropy alloy catalyst. The mesoporous high entropy alloy catalyst prepared by the above preparation method combines the advantages of mesopores and high entropy metal intermetallic compound crystal structures: mesopores improve the utilization efficiency of catalytic sites, improve the mass activity and area activity of the catalyst; the stable mesoporous framework structure inhibits the Ostwald ripening process and enhances the stability of the catalytic reaction; the high entropy metal intermetallic compound has five specific atoms, the surface is highly heterogeneous, and a large number of different active sites are produced, which can accelerate the reaction kinetics; the high entropy metal intermetallic compound has the highest mixing enthalpy, which improves the structural stability of the catalyst during the catalytic process; the high entropy metal intermetallic compound has a specific structure and lattice constant, which is convenient for establishing the structure-activity relationship between the catalyst structure and the catalytic activity. Therefore, the use of the catalyst can not only improve the activity and stability of electrocatalytic oxygen reduction, but also clarify the relationship between the catalyst structure and the catalytic activity, improve the utilization rate of precious metals, and greatly reduce the cost of raw materials; and the one-step synthesis method is simple, easy to operate, can be prepared in large quantities, and is suitable for large-scale industrial production.

[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a mesoporous high entropy alloy catalyst, characterized in that: The steps include: S1, sodium chloropalladate and potassium chloroplatinite are filled into the pores of KIT-6 by decompression; S2, adding ascorbic acid to the reaction mixture in step S1 for reduction, removing unreacted impurities by washing with water, and drying to obtain a solid powder Meso-PtPd / KIT-6; S3, adding ferric chloride to the M-PtPd / KIT-6 obtained in step S2, grinding the mixture, and calcining the mixture in a tube furnace to obtain a mesoporous intermetallic compound FCT-PtPdFe / KIT-6 solid powder; S4, adding cobalt chloride to the FCT-PtPdFe / KIT-6 solid powder obtained in step S3 for grinding; placing the solid powder in a tube furnace for calcination to obtain FCT-PtPdFeCo / KIT-6 solid powder; S5, adding nickel chloride to the FCT-PtPdFeCo / KIT-6 solid powder obtained in step S4 for grinding; placing the solid powder in a tube furnace for calcination to obtain FCT-PtPdFeCoNi / KIT-6 solid powder; S6, the obtained FCT-PtPdFeCoNi / KIT-6 needs to be soaked in hydrochloric acid to remove the cobalt and nickel impurities that are not introduced into the crystalline phase, and soaked in hydrofluoric acid to remove the SiO2 template, and finally a mesoporous high entropy alloy catalyst is obtained.

2. The method for preparing a mesoporous high entropy alloy catalyst according to claim 1, characterized in that: In the step S1, the mass ratio of the sodium chloropalladate, potassium chloroplatinite and KIT-6 is 1:2:15, and the sodium chloropalladate, potassium chloroplatinite and KIT-6 are all dissolved in water, and then dried under reduced pressure in a vacuum drying oven at 45-55° C. for 1-1.5 hours.

3. The method for preparing a mesoporous high entropy alloy catalyst according to claim 2, characterized in that: The concentration of ascorbic acid added in step S2 is 0.25 mol / L.

4. The method for preparing a mesoporous high entropy alloy catalyst according to claim 1, characterized in that: The mass ratio of ferric chloride, cobalt chloride and nickel chloride is 9:8:5, and the mass ratio of nickel chloride to sodium chloropalladate is 1:

4.

5. The method for preparing a mesoporous high entropy alloy catalyst according to claim 1, characterized in that: In the steps S3-S5, the calcination temperature is 400-500°C, the calcination time is 6-10 hours, the heating rate is 2-5°C / minute, and a reducing gas is introduced during the calcination process. The reducing gas is a H2 / N2 atmosphere in which the ratio of hydrogen to nitrogen is 5:95, the flow rate is 0.08-0.2L / min, and the pyrolysis temperature is 450-500°C.

6. The method for preparing a mesoporous high entropy alloy catalyst according to claim 1, characterized in that: In the step S5, the concentration of the hydrochloric acid is 1 mol / L, and the concentration of the hydrofluoric acid used to etch the SiO2 template is 20%.

7. The method for preparing a mesoporous high entropy alloy catalyst according to claim 6, characterized in that: The obtained in step S5 is a mesoporous high entropy intermetallic compound with a component ratio of FCT-PtPdFeCoNi.

8. An application of a mesoporous high entropy alloy catalyst, characterized in that: The mesoporous high entropy alloy catalyst according to any one of claims 1 to 7 and Vulcan XC-72 carbon black are physically loaded in a mass ratio of 1:1 and are drop-coated on a clean rotating disk electrode as a cathode catalyst, and the catalyst loading is 0.05 mg / cm 2 , and after drying, was applied to electrocatalytic oxygen reduction.

9. The use of a mesoporous high entropy alloy catalyst as claimed in claim 8, characterized in that: A three-electrode system was adopted, and the catalyst was drop-coated on a rotating disk electrode as a working electrode, a saturated silver / silver chloride electrode was used as a reference electrode, a carbon rod was used as a counter electrode, and a potassium hydroxide solution was used as an electrolyte. The potassium hydroxide concentration in the electrolyte was 0.1 mol / L. Before use, the disk electrode surface needed to be polished with alumina polishing powder to remove impurities from pollution sources. The alumina particle size was 0.05 mm.

10. The use of a mesoporous high entropy alloy catalyst as claimed in claim 8, characterized in that: During the catalyst preparation process, ethanol:deionized water with a volume ratio of 4:1 was used as the solvent; the catalyst concentration was 1 mg / mL.

Citation Information

Cited By

  • Preparation method of nano-porous Cu6Sn5 type high-entropy intermetallic compound and application of nano-porous Cu6Sn5 type high-entropy intermetallic compound in electrocatalytic ammonia production

    CN119663090A