Polyimide composite gas separation membrane, its preparation method and application

By coating polyimide material on the base membrane and preparing it by the dry-wet phase inversion method, the problem of both selectivity and permeability of the polyimide gas separation membrane is solved, the mechanical strength is improved and gas separation is achieved. Performance improvements.

CN115770494BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202111042410.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-07
Publication Date
2024-10-15
Estimated Expiration
2041-09-07

AI Technical Summary

Technical Problem

Existing polyimide gas separation membranes cannot take into account both gas selectivity and permeability, and delamination and peeling of the separation layer and the base membrane often occur during the preparation process, resulting in insufficient mechanical strength.

Method used

The polyimide material is compounded on the base membrane of the porous support layer using a coating method, and a polyimide composite gas separation membrane with an ultra-thin separation layer and porous structure is prepared through a dry-wet phase conversion method to improve the mechanical strength and reduce the Amount of selective separation layer material.

Benefits of technology

It achieves a gas separation membrane with high selectivity and high permeability, improves the mechanical strength of the membrane, and simplifies the preparation process. It is suitable for the purification of helium and hydrogen and the separation of gas mixtures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115770494B_ABST
    Figure CN115770494B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of polymer membrane materials and membrane separation, and discloses a polyimide composite gas separation membrane and a preparation method and application thereof. The composite gas separation membrane comprises a support layer and a separation layer, and the material of the separation layer contains a structure shown in formula (I): m and n are each independently an integer of 5 to 2000; X has a structure shown in any one of formulas (X1) to (X3); Y has a structure shown in any one of formulas (Y1) to (Y5); Z and Z' each independently have a structure shown in formula (Z1) or (Z2); #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer membrane materials and membrane separation, and in particular to a polyimide composite gas separation membrane and a preparation method and application thereof. Background Art

[0002] Gas separation membranes use the differences in the speed of dissolution and diffusion of different gases in membrane materials to achieve separation and concentration of different gases. The main separation function of gas separation membranes is a dense selective skin layer, and the separation performance depends on the bulk performance of the material and the thickness of the skin layer. In order to design new materials with excellent separation performance, researchers have invented a variety of new gas separation materials, but these materials are usually relatively expensive, which increases the cost of gas separation membranes. Compared with the preparation of membranes with integrated skin layers, composite gas separation membranes with ultra-thin selective skin layers can reduce the amount of casting liquid. In addition to saving material costs, this method also provides more options and advantages in the preparation of membranes with various morphologies and uses. Composite gas separation membranes contain more than one material, and the support layer usually uses porous polymers or inorganic materials as the base membrane, and a selective separation layer is constructed on the base membrane. The selective layer of the composite gas separation membrane in this technical field can be prepared by different methods, including interfacial polymerization, coating, and deposition. The selective separation layer material of the gas separation membrane requires the polymer material to be soluble in a suitable solvent to prepare a homogeneous casting liquid, and the casting liquid is required to have good processability. At the same time, it is required that the base membrane as the support layer can be well combined with the separation layer, but in actual use, delamination and peeling of the separation layer and the base membrane often occur. The preparation of a gas separation membrane with an ultra-thin defect-free selective separation layer and a porous support layer is a technical difficulty, which puts forward high requirements on the formulation of the casting liquid, the membrane making process, including the pretreatment of the base membrane. The existing public technology involves very little on the control of the selective separation layer of the polyimide gas separation membrane and the technology for simultaneously improving the permeation rate, and it is not yet possible to take into account both gas selectivity and permeation rate. The mixed matrix membrane prepared by adding porous inorganic materials to the polymer matrix often has a reduced selectivity of the mixed matrix membrane due to the compatibility between the polymer matrix and the porous inorganic filler and the interface defects.

[0003] Therefore, it is of great significance to devote oneself to the research and development of a polyimide composite gas separation membrane. Summary of the invention

[0004] The purpose of the present invention is to overcome the defect that the polyimide gas separation membrane in the prior art cannot take into account both gas selectivity and permeability at the same time, and to provide a polyimide composite gas separation membrane and a preparation method and application thereof. The polyimide composite gas separation membrane has high selectivity and permeability performance and can also improve the mechanical strength of the membrane.

[0005] In order to achieve the above-mentioned object, the first aspect of the present invention provides a polyimide composite gas separation membrane, wherein the composite gas separation membrane is a sheet structure, and the composite gas separation membrane comprises a support layer and a separation layer attached to the outer surface of the support layer, the material of the separation layer contains a polyimide random copolymer, and the polyimide random copolymer has a structure shown in formula (I):

[0006]

[0007] In formula (I), m and n are each independently an integer of 5-2000;

[0008] X has a structure represented by any one of formula (X1) to formula (X3);

[0009]

[0010] In formula (X1) to formula (X3), R 1 , R 2 , R 3 , R 4 , R 5 and R 6 Each is independently H, C1-C4 alkyl, C6-C10 aryl, amino, hydroxyl or carboxyl;

[0011] Y has a structure represented by any one of formula (Y1) to formula (Y5);

[0012]

[0013] In formula (Y1) to formula (Y5), R 7 , R 8 , R 9 , R 10 , R 11 , R 12 , R 13 , R 14 , R 15 and R 16 Each is independently H, C1-C4 alkyl, C6-C10 aryl, amino, hydroxyl or carboxyl;

[0014] Z and Z' each independently have a structure represented by formula (Z1) or formula (Z2);

[0015]

[0016] In formula (Z2), Ra and Rb are each independently H, C1-C4 alkyl or C1-C4 halogenated alkyl.

[0017] A second aspect of the present invention provides a method for preparing a polyimide composite gas separation membrane, wherein the preparation method comprises:

[0018] (1) mixing a polyimide random copolymer and a diluent to prepare a film casting solution;

[0019] (2) coating the casting solution on a base film and performing a heat treatment to obtain a film precursor;

[0020] (3) solidifying, extracting and drying the membrane precursor to obtain a polyimide composite gas separation membrane;

[0021] Wherein, the polyimide random copolymer has a structure shown in formula (I):

[0022]

[0023] In formula (I), m and n are each independently an integer of 5-2000;

[0024] X has a structure represented by any one of formula (X1) to formula (X3);

[0025]

[0026] In formula (X1) to formula (X3), R 1 , R 2 , R 3 , R 4 , R 5 and R 6 Each is independently H, C1-C4 alkyl, C6-C10 aryl, amino, hydroxyl or carboxyl;

[0027] Y has a structure represented by any one of formula (Y1) to formula (Y5);

[0028]

[0029] In formula (Y1) to formula (Y5), R 7 , R 8 , R 9 , R 10 , R 11 , R 12 , R 13 , R 14 , R 15 and R 16 Each is independently H, C1-C4 alkyl, C6-C10 aryl, amino, hydroxyl or carboxyl;

[0030] Z and Z' each independently have a structure represented by formula (Z1) or formula (Z2);

[0031]

[0032] In formula (Z2), Ra and Rb are each independently H, C1-C4 alkyl or C1-C4 halogenated alkyl.

[0033] The third aspect of the present invention provides a polyimide-based composite gas separation membrane prepared by the aforementioned preparation method.

[0034] A fourth aspect of the present invention provides an application of the aforementioned polyimide-based composite gas separation membrane in one or more of gas separation, hydrogen concentration and helium extraction from natural gas.

[0035] Through the above technical scheme, the present invention uses a coating method to composite a polyimide material with a selective separation layer on a base membrane of a porous support layer, and obtains a polyimide composite gas separation membrane by a dry-wet phase conversion method. The polyimide composite gas separation membrane has an ultra-thin separation layer and a porous support layer, which not only improves the mechanical strength of the membrane, but also reduces the amount of selective separation layer material. The ultra-thin selective separation layer can effectively reduce resistance and improve the permeation rate of the membrane. The preparation method provided by the present invention is simple and easy to carry out industrial implementation. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a scanning electron microscope image of a cross section of the polyimide composite gas separation membrane prepared in Example 1, magnified 1000 times;

[0037] Figure 2 This is a scanning electron microscope image of a cross section of the polyimide composite gas separation membrane prepared in Example 1, magnified 10,000 times;

[0038] Figure 3 This is a scanning electron microscope image of a cross section of the polyimide composite gas separation membrane prepared in Example 1, magnified 20,000 times;

[0039] Figure 4 This is a scanning electron microscope image of a cross section of the polyimide composite gas separation membrane prepared in Example 2, magnified 1000 times;

[0040] Figure 5 This is a scanning electron microscope image of a cross section of the polyimide composite gas separation membrane prepared in Example 2, magnified 2000 times;

[0041] Figure 6 This is a scanning electron microscope image of a cross section of the polyimide composite gas separation membrane prepared in Example 3, magnified 1000 times;

[0042] Figure 7 This is a scanning electron microscope image of a cross section of the polyimide composite gas separation membrane prepared in Example 3, magnified 1000 times;

[0043] Figure 8This is a scanning electron microscope image of a cross section of the polyimide composite gas separation membrane prepared in Comparative Example 1, magnified 500 times;

[0044] Fig. 9 This is a surface scanning electron microscope image of the polyimide composite gas separation membrane prepared in Comparative Example 1 magnified 20,000 times. DETAILED DESCRIPTION

[0045] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0046] In the present invention, "C1-C4 alkyl" includes methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl and tert-butyl.

[0047] "C6-C10 aromatic group" includes benzene, toluene, xylene (o-, m-, p-), ethylbenzene, methylethylbenzene, etc.

[0048] The "C1-C4 haloalkyl group" includes monofluoromethyl, difluoromethyl, trifluoromethyl, monofluoroethyl, difluoroethyl, trifluoroethyl, monochloromethyl, dichloromethyl, trichloromethyl, etc.

[0049] The "C1-C4 saturated monohydric alcohol" includes methanol, ethanol, n-propanol, isopropanol, n-butanol and isobutanol.

[0050] "C3-C5 alkanes" include straight-chain alkanes (such as n-propane, isopropane, n-pentane, isopentane, etc.), branched alkanes or cycloalkanes (cyclopropane, cyclobutane, cyclopentane) with 3-5 carbon atoms. "C5-C7 alkanes" are similar.

[0051] The first aspect of the present invention provides a polyimide composite gas separation membrane, wherein the composite gas separation membrane is a sheet structure, and the composite gas separation membrane comprises a support layer and a separation layer attached to the outer surface of the support layer, the material of the separation layer contains a polyimide random copolymer, and the polyimide random copolymer has a structure shown in formula (I):

[0052]

[0053] In formula (I), m and n are each independently an integer of 5-2000;

[0054] X has a structure represented by any one of formula (X1) to formula (X3);

[0055]

[0056] In formula (X1) to formula (X3), R 1 , R 2 , R 3 , R 4 , R 5 and R 6 are independently H, C1-C4 alkyl, C6-C 10 an aryl, amino, hydroxyl or carboxyl group;

[0057] Y has a structure represented by any one of formula (Y1) to formula (Y5);

[0058]

[0059]

[0060] In formula (Y1) to formula (Y5), R 7 , R 8 , R 9 , R 10 , R 11 , R 12 , R 13 , R 14 , R 15 and R 16 are independently H, C1-C4 alkyl, C6-C 10 an aryl, amino, hydroxyl or carboxyl group;

[0061] Z and Z' each independently have a structure represented by formula (Z1) or formula (Z2);

[0062]

[0063] In formula (Z2), Ra and Rb are each independently H, C1-C4 alkyl or C1-C4 halogenated alkyl.

[0064] The inventor of the present invention unexpectedly discovered that the polyimide composite gas separation membrane provided by the present invention has an ultra-thin dense layer (separation layer) and a support layer with a sponge pore structure. The support layer with a higher porosity and the ultra-thin separation layer can effectively reduce resistance and increase the permeation rate of the membrane; in addition, the mechanical strength (such as compressive strength) is also high. In the method provided by the present invention, a polyimide material (especially a polyimide random copolymer provided by the present invention) is used, and the molecular structure level of the polyimide can be regulated by changing the synthesis conditions, adjusting the packing density and free volume of the polymer molecular chain, and obtaining a bimodal pore size distribution to achieve accurate screening of gas molecules. An asymmetric ultra-thin polyimide composite gas separation membrane (dense layer thickness less than 1000nm, preferably, can be controlled at 500-1000nm) and a support layer with high porosity prepared by a dry-wet spinning phase conversion method; specifically, preferably, a diluent (specific type and ratio) and an additive are added to the polyimide to form a homogeneous casting solution, which enters the air and a specific coagulation bath to undergo phase separation, and is extracted and dried to form a polyimide composite gas separation membrane with an ultra-thin dense skin asymmetric structure, the preparation method is simple, and it is easy to carry out industrial implementation, and the prepared polyimide composite gas separation membrane has excellent selectivity and permeation rate. In addition, the polyimide composite gas separation membrane provided by the present invention is preferably suitable for the purification of helium and hydrogen, and is also suitable for the separation of gas mixtures, including but not limited to the separation of CO2 and CH4, O2 and N2, He and N2, He and CH4, CO2 and N2, He and CO2, H2 and N2, H2 and CH4, H2 and CO2, etc.

[0065] According to the present invention, preferably, the X has one of the following structures:

[0066]

[0067] According to the present invention, Y has one of the following structures,

[0068]

[0069] According to the present invention, Z and Z' both have the structure shown by Z1 or Z3,

[0070]

[0071] According to the present invention, preferably, X is Xa, Y is Ya, and Z and Z' are both Z1;

[0072] Alternatively, X is Xa, Y is Yb, and Z and Z' are both Z1;

[0073] Or, X is Xa, Y is Yd, and Z and Z' are both Z1;

[0074] Or, X is Xb, Y is Ya, and Z and Z' are both Z1;

[0075] Or, X is Xb, Y is Yb, and Z and Z' are both Z1;

[0076] Or, X is Xb, Y is Yd, and Z and Z' are both Z1;

[0077] Or, X is Xc, Y is Ya, and Z and Z' are both Z1;

[0078] Alternatively, X is Xc, Y is Yb, and Z and Z' are both Z1;

[0079] Or, X is Xc, Y is Yc, and Z and Z' are both Z1;

[0080] Alternatively, X is Xc, Y is Y4, and Z and Z' are both Z1;

[0081] Or, X is Xc, Y is Yd, and Z and Z' are both Z1;

[0082] Or, X is Xb, Y is Ya, and Z and Z' are both Z3;

[0083] Or, X is Xb, Y is Yb, and Z and Z' are both Z3;

[0084] Or, X is Xb, Y is Yd, and Z and Z' are both Z3;

[0085] Or, X is Xc, Y is Ya, and Z and Z' are both Z3;

[0086] Or, X is Xc, Y is Yb, and Z and Z' are both Z3;

[0087] Alternatively, X is Xc, Y is Yd, and Z and Z' are both Z3.

[0088] Although according to a preferred embodiment of the present invention, X, Y, and Z have a specific structure, the present invention does not exclude the situation that "X is taken from two or three different structures, Y is taken from two, three, four or five different structures, and Z is taken from two different structures".

[0089] According to the present invention, the separation layer has a dense structure, and the thickness of the separation layer is ≤1000nm, preferably 500-1000nm (such as 500nm, 600nm, 700nm, 800nm, 900nm or any value therebetween).

[0090] According to the present invention, the separation layer further contains an additive, and the additive is selected from one or more of a metal organic framework compound, lithium nitrate and lithium chloride; preferably, the metal organic framework compound is selected from UiO-66 and / or ZIF-8. In the present invention, UiO-66 is formed by the coordination connection of the regular octahedral secondary structural unit of Zr [Zr6O4(OH)4] and 12 organic ligands of terephthalic acid. ZIF-8, a zeolite imidazole ester framework, is formed by the coordination connection of metal ions and imidazole ligands. A typical representative is ZIF-8, which has a cage-shaped pore structure.

[0091] According to the present invention, the support layer is an organic porous ultrafiltration membrane having a porous structure. Preferably, the support layer is selected from one or more of polyvinylidene fluoride, polypropylene, polyether sulfone, polysulfone, cellulose acetate, polyacrylonitrile, polyethylene, polytetrafluoroethylene and non-woven fibers.

[0092] According to the present invention, the porosity of the composite gas separation membrane is 50-80%, preferably 50-75%, and more preferably 55-65%.

[0093] In the present invention, it should be noted that the porosity of the support layer is greater than the porosity of the separation layer (dense layer). The porosity of the separation layer (dense layer) cannot be characterized by mercury intrusion.

[0094] According to the present invention, preferably, m and n are each independently an integer of 50-1000.

[0095] According to the present invention, 0.9≥n / (m+n)≥0.3, preferably, 0.7≥n / (m+n)≥0.5.

[0096] According to the present invention, the weight average molecular weight of the polyimide random copolymer is 120,000-600,000, preferably 200,000-450,000.

[0097] In the present invention, based on the principle of firstly subjecting a dianhydride monomer (dianhydride shown in formula (II) and dianhydride shown in formula (III)) and a diamine monomer to polycondensation to obtain polyamic acid, and then imidizing (intramolecular dehydration) the polyamic acid, the dianhydride monomer and the diamine monomer can be subjected to polycondensation to obtain polyamic acid by a one-pot method, or the dianhydride monomer (i.e., the dianhydride shown in formula (II) and the dianhydride shown in formula (III)) can be uniformly mixed before being subjected to polycondensation with the diamine monomer. However, in order to better control the reaction, it is preferred to react in the latter manner.

[0098] Therefore, the present invention also provides a method for preparing a polyimide random copolymer, the method comprising the following steps:

[0099] (S1) in the presence of a first solvent, mixing a mixture of a dianhydride monomer represented by formula (II) and a dianhydride monomer represented by formula (III) with a diamine monomer to carry out a polycondensation reaction to obtain a material containing polyamic acid,

[0100]

[0101] (S2) imidizing the material containing polyamic acid obtained in step (S1) to cause intramolecular dehydration of the polyamic acid to obtain a polyimide random copolymer;

[0102] In formula (II), X has a structure represented by any one of formulas (X1) to (X3);

[0103]

[0104] In formula (X1) to formula (X3), R 1 , R 2 , R 3 , R 4 , R 5 and R 6 Each is independently H, C1-C4 alkyl, C6-C10 aryl, amino, hydroxyl or carboxyl;

[0105] In formula (III), Y has a structure represented by any one of formulas (Y1) to (Y5);

[0106]

[0107] In formula (Y1) to formula (Y5), R 7 , R 8 , R 9 , R 10 , R 11 , R 12 , R 13 , R 14 , R 15 and R 16 Each is independently H, C1-C4 alkyl, C6-C10 aryl, amino, hydroxyl or carboxyl;

[0108] The diamine monomer is selected from at least one of the compounds having a structure such as H2N-Zp-NH2, wherein Zp has a structure as shown in formula (Z1) or (Z2),

[0109]

[0110] In formula (Z2), Ra and Rb are each independently H, C1-C4 alkyl or C1-C4 halogenated alkyl.

[0111] In the present invention, in formula (II), X has one of the following structures:

[0112]

[0113] And / or, in formula (III), Y has one of the following structures,

[0114]

[0115] and / or, Zp is Z1 or Z3,

[0116]

[0117] In the present invention, X is Xa, Y is Ya, and Zp is Z1;

[0118] Alternatively, X is Xa, Y is Yb, and Zp is Z1;

[0119] Or, X is Xa, Y is Yd, and Zp is Z1;

[0120] Or, X is Xb, Y is Ya, and Zp is Z1;

[0121] Or, X is Xb, Y is Yb, and Zp is Z1;

[0122] Or, X is Xb, Y is Yd, and Zp is Z1;

[0123] Or, X is Xc, Y is Ya, and Zp is Z1;

[0124] Or, X is Xc, Y is Yb, and Zp is Z1;

[0125] Or, X is Xc, Y is Yc, and Zp is Z1;

[0126] Or, X is Xc, Y is Y4, and Zp is Z1;

[0127] Or, X is Xc, Y is Yd, and Zp is Z1;

[0128] Or, X is Xb, Y is Ya, and Zp is Z3;

[0129] Or, X is Xb, Y is Yb, and Zp is Z3;

[0130] Or, X is Xb, Y is Yd, and Zp is Z3;

[0131] Or, X is Xc, Y is Ya, and Zp is Z3;

[0132] Or, X is Xc, Y is Yb, and Zp is Z3;

[0133] Alternatively, X is Xc, Y is Yd, and Zp is Z3.

[0134] In the present invention, the molar amounts of the dianhydride monomer represented by formula (II) and the dianhydride monomer represented by formula (III) are defined as M and N, respectively, and the ratio of M to N is (10-2000):(10-2000), more preferably 1:(0.5-15), and further preferably 1:(1-9).

[0135] In the present invention, m and n satisfy 0.9≥n / (m+n)≥0.3, preferably, 0.7≥n / (m+n)≥0.5.

[0136] In the present invention, the molar ratio of the total amount of the dianhydride monomer represented by formula (II) and the dianhydride monomer represented by formula (III) to the diamine monomer is 1:(0.6-1.5), preferably 1:(0.8-1.2).

[0137] In the present invention, in step (S1), the polycondensation reaction conditions may include: reaction temperature of -20°C to 60°C, preferably -10°C to 40°C; reaction time of 5-30h, preferably 8-24h.

[0138] In the present invention, the polycondensation reaction is carried out under an inert atmosphere, which is preferably provided by nitrogen.

[0139] In the present invention, the first solvent can be selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide and N-methylpyrrolidone (NMP), preferably selected from N-methylpyrrolidone and / or N,N-dimethylformamide.

[0140] In the present invention, the usage of the first solvent is 1000-3000 mL relative to 1 mmol of the diamine monomer.

[0141] In the present invention, the dianhydride monomer represented by formula (II) and the dianhydride monomer represented by formula (III) can be mixed to obtain a mixture by the following methods: mechanical stirring, shaking or ultrasound. The mechanical stirring conditions may include: 20-40°C, 2000-15000rpm, 2-12h; the ultrasound conditions may include: 20-40°C, 0.5-2.0h; the shaking conditions may include: 20-40°C, 260-800rpm, 12-36h.

[0142] In the present invention, the imidization treatment is carried out by adding a dehydrating agent and a catalyst to the amic acid-containing material obtained in step (S1), and reacting at 170-200° C. for 12-24 hours.

[0143] In the present invention, the dehydrating agent is selected from at least one of dichlorobenzene, toluene, acetic anhydride and xylene.

[0144] In the present invention, the catalyst is selected from pyridine and / or diquinoline.

[0145] In the present invention, the amount of the dehydrating agent used may be 2-15 mol, preferably 3-8 mol, relative to 1 mol of the diamine monomer.

[0146] In the present invention, the amount of the catalyst used may be 2-15 mol, preferably 3-8 mol, relative to 1 mol of the diamine monomer.

[0147] In the present invention, the method further comprises: before obtaining the polyimide copolymer, the material after the imidization treatment in step (S2) is diluted and contacted with a precipitant to obtain the polyimide copolymer. Wherein, the precipitant can be a poor solvent for polyimide, selected from at least one of ethanol, acetone and water, and more preferably selected from at least two of ethanol, acetone and water. Equivalent to 1 mol of diamine monomer, the total amount of the precipitant can be 10-50L. Wherein, the solvent for dilution can be N-methylpyrrolidone. Preferably, relative to 1 mol of diamine monomer, the amount of the solvent for dilution can be 5-8L.

[0148] In the present invention, there is no particular limitation on the manner in which the imidization-treated material in step (S2) is contacted with the precipitant, as long as the requirements of the present invention are met. For example, the following manner may be used: the imidization-treated material in step (S2) (after dilution) is added to the precipitant to precipitate the polyimide, and then the precipitated polyimide is eluted with the precipitant (the elution may be 3-5 times), and finally filtered and dried (70-150° C., 24-48 hours) to obtain a polyimide random copolymer.

[0149] A second aspect of the present invention provides a method for preparing a polyimide composite gas separation membrane, wherein the preparation method comprises:

[0150] (1) mixing a polyimide random copolymer and a diluent to prepare a film casting solution;

[0151] (2) coating the casting solution on a base film and performing a heat treatment to obtain a film precursor;

[0152] (3) solidifying, extracting and drying the membrane precursor to obtain a polyimide composite gas separation membrane;

[0153] Wherein, the polyimide random copolymer has a structure shown in formula (I):

[0154]

[0155] In formula (I), m and n are each independently an integer of 5-2000;

[0156] X has a structure represented by any one of formula (X1) to formula (X3);

[0157]

[0158] In formula (X1) to formula (X3), R 1 , R 2 , R 3 , R 4 , R 5 and R 6 are independently H, C1-C4 alkyl, C6-C 10 an aryl, amino, hydroxyl or carboxyl group;

[0159] Y has a structure represented by any one of formula (Y1) to formula (Y5);

[0160]

[0161] In formula (Y1) to formula (Y5), R 7 , R 8 , R 9 , R 10 , R 11 , R 12 , R 13 , R 14 , R 15 and R 16 are independently H, C1-C4 alkyl, C6-C 10 an aryl, amino, hydroxyl or carboxyl group;

[0162] Z and Z' each independently have a structure represented by formula (Z1) or formula (Z2);

[0163]

[0164] In formula (Z2), Ra and Rb are each independently H, C1-C4 alkyl or C1-C4 halogenated alkyl.

[0165] According to the present invention, preferably, the X has one of the following structures:

[0166]

[0167] According to the present invention, preferably, Y has one of the following structures,

[0168]

[0169] According to the present invention, preferably, Z and Z' both have the structure shown by Z1 or Z3,

[0170] Preferably, X is Xa, Y is Ya, and Z and Z' are both Z1;

[0171] Alternatively, X is Xa, Y is Yb, and Z and Z' are both Z1;

[0172] Or, X is Xa, Y is Yd, and Z and Z' are both Z1;

[0173] Or, X is Xb, Y is Ya, and Z and Z' are both Z1;

[0174] Or, X is Xb, Y is Yb, and Z and Z' are both Z1;

[0175] Or, X is Xb, Y is Yd, and Z and Z' are both Z1;

[0176] Or, X is Xc, Y is Ya, and Z and Z' are both Z1;

[0177] Alternatively, X is Xc, Y is Yb, and Z and Z' are both Z1;

[0178] Or, X is Xc, Y is Yc, and Z and Z' are both Z1;

[0179] Alternatively, X is Xc, Y is Y4, and Z and Z' are both Z1;

[0180] Or, X is Xc, Y is Yd, and Z and Z' are both Z1;

[0181] Or, X is Xb, Y is Ya, and Z and Z' are both Z3;

[0182] Or, X is Xb, Y is Yb, and Z and Z' are both Z3;

[0183] Or, X is Xb, Y is Yd, and Z and Z' are both Z3;

[0184] Or, X is Xc, Y is Ya, and Z and Z' are both Z3;

[0185] Or, X is Xc, Y is Yb, and Z and Z' are both Z3;

[0186] Alternatively, X is Xc, Y is Yd, and Z and Z' are both Z3.

[0187] According to the present invention, preferably, m and n are each independently an integer of 50-1000.

[0188] According to the present invention, preferably, 0.9≥n / (m+n)≥0.3, preferably, 0.7≥n / (m+n)≥0.5.

[0189] According to the present invention, the weight average molecular weight of the polyimide random copolymer is 120,000-600,000, preferably 200,000-450,000.

[0190] According to the present invention, in step (1), the casting solution further contains additives; preferably, based on the total weight of the casting solution, the content of the polyimide is 18-35wt%, the content of the diluent is 60-77wt%, and the content of the additive is 0.5-5wt%; preferably, based on the total weight of the casting solution, the content of the polyimide is 25-35wt%, the content of the diluent is 63-70wt%, and the content of the additive is 1-5wt%. In the present invention, the total amount of the polyimide, the diluent and the additive is 100%.

[0191] According to the present invention, in order to obtain better effects, the present invention has certain requirements on the dosage ratio of the compound A, compound B and compound C. Preferably, the diluent includes compound A, compound B and compound C, and the mass ratio of the compound A, the compound B and the compound C is 1:(0.1-0.5):(0.1-0.5), preferably 1:(0.15-0.3):(0.15-0.3).

[0192] According to the present invention, the compound A is selected from one or more of N-methylpyrrolidone (NMP), N,N-dimethylacetamide and N,N-dimethylacetamide.

[0193] According to the present invention, the compound B is selected from one or more of ethanol, gamma-butyrolactone and water.

[0194] According to the present invention, the compound C is selected from one or more of tetrahydrofuran (THF), pentane, ethyl chloride and acetone.

[0195] According to the present invention, the additive is selected from one or more of lithium nitrate, lithium chloride and metal organic framework compounds. In the invention, the metal organic framework compound is UiO-66 and / or ZIF-8.

[0196] According to the present invention, in step (1), the casting solution is prepared according to a method comprising the following steps: polyimide, a diluent and an additive are stirred at a stirring rate of 100-1200 r / min for 12-48 h at 20-70° C., and then vacuum degassing is performed, and then impurities are removed by filtering through a 0.45-5 μm filter screen; preferably, the casting solution is stirred at a stirring rate of 200-900 r / min for 24-36 h at 40-60° C., and then vacuum degassing is performed and then impurities are removed by filtering through a 1-2 μm filter screen.

[0197] According to the present invention, the conditions for vacuum degassing include: pressure of -0.1MPa to -0.095MPa, temperature of 20-30°C, rotation speed of 1-10r / min, and time of 12-24h; preferably, pressure of -0.08MPa to -0.09MPa, temperature of 25-30°C, rotation speed of 2-5r / min, and time of 12-16h.

[0198] According to the present invention, in step (2), the coating thickness is 50-300 μm, preferably 100-200 μm.

[0199] According to the present invention, the heat treatment conditions include: temperature of 70-150° C., preferably 80-120° C.; time of 1-5 min, preferably 2-4 min.

[0200] According to the present invention, in step (2), the base film is also pretreated; preferably, the pretreatment includes: infiltrating the base film with a pretreatment solution; more preferably, the pretreatment solution is selected from one or more of ethylenediamine, ethanol and acetone; in addition, the infiltration time is 5-60s, preferably 30-60s.

[0201] According to the present invention, the base membrane is an organic porous ultrafiltration membrane. Preferably, the base membrane is selected from one or more of polyvinylidene fluoride, polypropylene, polyethersulfone, polysulfone, cellulose acetate, polyacrylonitrile, polyethylene, polytetrafluoroethylene and non-woven fibers; more preferably, the base membrane is selected from one or more of non-woven fibers, polyvinylidene fluoride, polyethersulfone, polysulfone and cellulose acetate.

[0202] According to the present invention, in step (3), the coagulation bath used for coagulation is water and / or C 1- C4 saturated monohydric alcohol; preferably, the temperature of the coagulation bath is 40-70°C, preferably 50-60°C.

[0203] According to the present invention, the extractant used for extraction is selected from at least one of water, C1-C4 saturated monohydric alcohols and C5-C7 alkanes; preferably, the C1-C4 saturated monohydric alcohols are selected from one or more of methanol, ethanol and isopropanol; preferably, the C5-C7 alkanes are n-hexane or cyclohexane.

[0204] According to the present invention, the extraction conditions include: temperature of 20-35°C, time of 3-48h; preferably, temperature of 30-35°C, time of 6-24h.

[0205] According to the present invention, the extraction further includes a drying step; preferably, the drying conditions include: a temperature of 20-35°C and a time of 2-15h; preferably, a temperature of 25-30°C and a time of 4-10h.

[0206] The third aspect of the present invention also provides a polyimide-based composite gas separation membrane prepared by the aforementioned preparation method.

[0207] A fourth aspect of the present invention provides an application of the aforementioned polyimide-based composite gas separation membrane in one or more of gas separation, hydrogen concentration and helium extraction from natural gas.

[0208] In the present invention, among gas separations, separation of acidic gases is preferred.

[0209] In the present invention, the meanings of abbreviations are:

[0210] PMDA: Pyromellitic anhydride

[0211] BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride

[0212] ODPA: 4,4'-diphenyl ether dianhydride

[0213] 6FDA: 4,4'-(Hexafluoroisopropylene) diphthalic anhydride

[0214] BTDA: 3,3',4,4'-Benzophenone tetracarboxylic dianhydride

[0215] TPDAn (a compound represented by formula (III), wherein Y is Yd): triptylenyl dianhydride (prepared by referring to “LUO SJ, WIEGAND JR, KAZANOWSKA B, et al. Finely Tuning the Free Volume Architecture in Iptycene-Containing Polyimides for Highly Selective and Fast Hydrogen Transport. Macromolecules 2016, 49, (9): 3395-3405”)

[0216] mPDA: meta-phenylenediamine

[0217] PPDA (structural formula: ): pentiptycene diamine (prepared with reference to “LUO SJ, LIU Q, ZHANG BH, et al. Pentiptycene-based polyimides with hierarchically controlled molecular cavity architecture for efficient membrane gasseparation. J Membrane Sci 2015, 480: 20-30”).

[0218] The present invention will be described in detail below through examples.

[0219] In the following examples and comparative examples:

[0220] The important performance indicators of gas separation membranes include permeability coefficient (P), permeation rate (R) and separation coefficient (α). The unit of gas permeability coefficient is Barrer (1 Barrer = 10 -10 cm 3 (STP)cm / (cm 2 s cmHg)) indicates the difficulty of gas permeation through the membrane and is used to characterize the gas permeability of the membrane material itself. For composite gas separation membranes, the gas permeation rate is usually used to express the membrane's permeability performance. The unit of gas permeation rate is GPU (1GPU = 10 -6 cm 3 (STP) / (cm 2 ·s·cmHg)) reflects the speed of gas component penetration in the membrane and is used to characterize the gas permeability during membrane application; measurement method: at room temperature 20°C, measure the gas flow rate permeating per unit membrane area per unit time under a certain pressure difference. The separation coefficient α is dimensionless and is used to characterize the selective permeability of gas components in the membrane. The separation coefficient is the ratio of the permeation rates of two gases in the membrane.

[0221] The porosity of polyimide-based composite gas separation membranes was measured by mercury intrusion porosimetry;

[0222] The thickness of the polyimide-based composite gas separation membrane was measured by scanning electron microscopy.

[0223] Preparation Example 1

[0224] (1) Under nitrogen protection, 200 mL of anhydrous N-methylpyrrolidone and m-phenylenediamine (10.81 g, 0.1 mmol) were added to a 1 L three-necked flask in sequence, and stirred until the materials were completely dissolved; 4,4-diphenyl ether dianhydride (ODPA) (0.01 mmol) and 4,4'-(hexafluoroisopropylene) diphthalic anhydride (6FDA) (0.09 mmol) were mixed under mechanical stirring, and then added to the above system at 0°C, and polycondensation reaction was carried out for 12 hours to obtain a material containing polyimide acid;

[0225] (2) Add a mixture of acetic anhydride (0.36 mmol) and pyridine (0.36 mmol) to the polyimide acid material obtained in step (1), and perform intramolecular dehydration at 200°C for 24 hours to obtain a material containing polyimide; then add 600 mL of N-methylpyrrolidone (NMP) to the polyimide-containing material for dilution, and pour the diluted material into a mixed solvent of water and ethanol (500 mL: 500 mL) under stirring to precipitate polyimide to obtain polyimide, and then rinse with a mixed solution of water and ethanol (1500 mL: 1500 mL) (3 times), and obtain a polyimide random copolymer after suction filtration and drying, which is calculated as PI-1. Infrared test table PI-1 has a structure shown in formula (I), wherein X is Xc, Y is Ya, and Z and Z' are both Z1. In addition, no raw materials can be detected in the remaining liquid phase after the polyimide is precipitated, indicating that all raw materials participate in the reaction.

[0226] The polyimide (PI-1) obtained above was used to prepare a gas separation membrane:

[0227] PI-1 was added to NMP at a solid content of 40 wt%, and stirred in a shaking table at 50°C until PI-1 was completely dissolved to obtain a uniform and stable casting liquid; the casting liquid was cooled to room temperature, ultrasonically degassed, and then uniformly coated on the surface of a clean glass plate, placed in a 70°C forced air oven for 6 hours to remove a large amount of solvent, and then moved to a vacuum oven (dried at 120°C for 12 hours) to further remove the solvent; after cooling to room temperature, the glass plate with the membrane was immersed in deionized water until the membrane fell off the surface of the glass plate to obtain a gas separation membrane, which was calculated as S1.

[0228] Preparation Example 2

[0229] (1) Under nitrogen protection, 200 mL of anhydrous N-methylpyrrolidone and m-phenylenediamine (10.81 g, 0.1 mmol) were added to a 1 L three-necked flask in sequence, and stirred until the materials were completely dissolved; 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) (0.02 mmol) and 4,4'-(hexafluoroisopropylene) diphthalic anhydride (6FDA) (0.08 mmol) were mixed under shaking conditions, and then added to the above system at -10°C, and polycondensation reaction was carried out for 18 hours to obtain a material containing polyimide acid;

[0230] (2) Add a mixture of acetic anhydride (0.4 mmol) and pyridine (0.4 mmol) to the polyimide acid material obtained in step (1), and perform intramolecular dehydration at 200°C for 24 hours to obtain a material containing polyimide; then add 600 mL of N-methylpyrrolidone (NMP) to the polyimide-containing material for dilution, and pour the diluted material into a mixed solvent of water and ethanol (500 mL: 500 mL) under stirring to precipitate polyimide to obtain polyimide, and then rinse with a mixed solution of water and ethanol (1500 mL: 1500 mL) (3 times), and obtain a polyimide random copolymer after suction filtration and drying, which is calculated as PI-2. Infrared test table PI-2 has a structure shown in formula (I), wherein X is Xb, Y is Ya, and Z and Z' are both Z1. In addition, no raw materials can be detected in the remaining liquid phase after the polyimide is precipitated, indicating that all raw materials participate in the reaction.

[0231] The polyimide (PI-2) obtained above was used to prepare a gas separation membrane:

[0232] PI-2 was added to NMP at a solid content of 25 wt%, and stirred in a shaker at 50°C until PI-2 was completely dissolved to obtain a uniform and stable casting liquid; the casting liquid was cooled to room temperature, ultrasonically degassed, and then uniformly coated on the surface of a clean glass plate, placed in a 70°C forced air oven for 6 hours to remove a large amount of solvent, and then moved to a vacuum oven (dried at 120°C for 12 hours) to further remove the solvent; after cooling to room temperature, the glass plate with the membrane was immersed in deionized water until the membrane fell off the surface of the glass plate to obtain a gas separation membrane, which was calculated as S2.

[0233] Preparation Example 3

[0234] (1) Under nitrogen protection, 200 mL of anhydrous N-methylpyrrolidone and m-phenylenediamine (10.81 g, 0.1 mmol) were added to a 1 L three-necked flask in sequence, and stirred until the materials were completely dissolved; 3,3',4,4'-biphenyltetracarboxylic dianhydride (0.01 mmol) and 4,4'-(hexafluoroisopropylene) diphthalic anhydride (6FDA) (0.09 mmol) were mixed under shaking conditions, and then added to the above system at -10°C, and polycondensation reaction was carried out for 18 hours to obtain a material containing polyimide acid;

[0235] (2) A mixture of acetic anhydride (0.4 mmol) and pyridine (0.4 mmol) was added to the polyimide acid material obtained in step (1), and intramolecular dehydration was performed at 200° C. for 24 h to obtain a material containing polyimide; then 600 mL of N-methylpyrrolidone (NMP) was added to the polyimide-containing material for dilution, and the diluted material was poured into a mixed solvent of water and ethanol (500 mL: 500 mL) under stirring to precipitate polyimide to obtain polyimide, and then the mixture was rinsed with a mixed solution of water and ethanol (1500 mL: 1500 mL) (3 times), and after suction filtration and drying, a polyimide random copolymer was obtained, which was designated as PI-3. The polyimide random copolymer was subjected to infrared testing using a Fourier transform infrared spectrometer (Thermo Nicolet 380), and the infrared spectrum was shown in FIG. Figure 4 Infrared test table PI-3 has a structure shown in formula (I), wherein X is Xb, Y is Ya, and Z and Z' are both Z1. In addition, no raw materials are detected in the remaining liquid phase after the polyimide is precipitated, indicating that all raw materials participate in the reaction.

[0236] FTIR infrared test, 1785cm -1 and 1730cm -1 The peaks at 1357 cm-1 are the symmetric stretching vibration peaks and asymmetric stretching vibration peaks of the two carbonyl groups on the five-membered imine ring in polyimide. -1 is the stretching vibration of CN in polyimide, 721 cm -1 is the deformation vibration peak of the imine ring, 1255cm -1 The stretching vibration of the ether bond in aromatic ether is 1144 cm -1 The peak at is the stretching vibration peak of CF, that is, the appearance of the above characteristic peaks indicates the successful synthesis of PI-3.

[0237] The obtained polyimide (PI-3) is used to prepare a gas separation membrane:

[0238] PI-3 was added to NMP at a solid content of 25 wt%, and stirred in a shaker at 50°C until PI-3 was completely dissolved to obtain a uniform and stable casting liquid; the casting liquid was cooled to room temperature, ultrasonically degassed, and then uniformly coated on the surface of a clean glass plate, placed in a 70°C forced air oven for 6 hours to remove a large amount of solvent, and then moved to a vacuum oven (dried at 120°C for 24 hours) to further remove the solvent; after cooling to room temperature, the glass plate with the membrane was immersed in deionized water until the membrane fell off the surface of the glass plate to obtain a gas separation membrane, which was calculated as S3.

[0239] Preparation Example 4

[0240] (1) Under nitrogen protection, 200 mL of anhydrous N-methylpyrrolidone and m-phenylenediamine (10.81 g, 0.1 mmol) were added to a 1 L three-necked flask in sequence and stirred until the materials were completely dissolved; pyromellitic dianhydride (PMDA) (0.03 mmol) and 4,4'-(hexafluoroisopropylene) diphthalic anhydride (6FDA) (0.07 mmol) were mixed under ultrasonic conditions, and then added to the above system at 25° C. and polycondensed for 12 h to obtain a material containing polyimide acid;

[0241] (2) Add a mixture of acetic anhydride (0.4 mmol) and pyridine (0.4 mmol) to the polyimide acid material obtained in step (1), and perform intramolecular dehydration at 170°C for 18 hours to obtain a material containing polyimide; then add 600 mL of N-methylpyrrolidone (NMP) to the polyimide-containing material for dilution, and pour the diluted material into a mixed solvent of water and ethanol (500 mL: 500 mL) under stirring to precipitate polyimide to obtain polyimide, and then rinse with a mixed solution of water and ethanol (1500 mL: 1500 mL) (3 times), and obtain a polyimide random copolymer after suction filtration and drying, which is calculated as PI-4. Infrared test table PI-4 has a structure shown in formula (I), wherein X is Xa, Y is Ya, and Z and Z' are both Z1. In addition, no raw materials can be detected in the remaining liquid phase after the polyimide is precipitated, indicating that all raw materials participate in the reaction.

[0242] The polyimide (PI-4) obtained above was used to prepare a gas separation membrane:

[0243] PI-4 was added to NMP at a solid content of 15 wt%, and stirred in a shaking table at 50°C until PI-4 was completely dissolved to obtain a uniform and stable casting liquid; the casting liquid was cooled to room temperature, ultrasonically degassed, and then uniformly coated on the surface of a clean glass plate, placed in a 70°C forced air oven for 6 hours to remove a large amount of solvent, and then moved to a vacuum oven (dried at 120°C for 24 hours) to further remove the solvent; after cooling to room temperature, the glass plate with the membrane was immersed in deionized water until the membrane fell off the surface of the glass plate to obtain a gas separation membrane, which was calculated as S4.

[0244] Example 1

[0245] This example is to illustrate the preparation of the polyimide composite gas separation membrane of the present invention.

[0246] (1) 30 wt % of the random copolymer of polyimide prepared in Preparation Example 1, 48 wt % of N-methylpyrrolidone (NMP), 10 wt % of THF, 9 wt % of ethanol, and 3 wt % of LiNO3 were added to a liquid kettle and stirred at 50° C. for 24 h, and then allowed to stand and degas at -0.1 MPa for 24 h to obtain a casting liquid for preparing a separation layer of a gas separation membrane; and then filtered through a 0.45 μm filter to obtain a casting liquid;

[0247] (2) The polyvinylidene fluoride film was infiltrated with ethylenediamine solution for 30 seconds, and the casting solution was continuously scraped on the base film, and the scraper thickness was controlled to be 200 μm;

[0248] (3) The film precursor after scraping is irradiated with an infrared heating lamp at 150°C for 1 min, and then immersed in a water coagulation bath to cause phase inversion and curing.

[0249] (4) Then the membrane is sequentially soaked in water for 12 hours, ethanol for 12 hours, and n-hexane for 1 hour to extract the diluent added to the casting solution. The extracted membrane is dried under ventilation and room temperature conditions to obtain a polyimide composite gas separation membrane. The polyimide composite gas separation membrane is a sheet structure, and the composite gas separation membrane includes a support layer and a separation layer attached to the outer surface of the support layer, the thickness of the separation layer is 958nm, and the porosity of the composite gas separation membrane is 66%.

[0250] The cross-sectional structure of the obtained polyimide composite gas separation membrane is as follows: Figure 1 , Figure 2 and Figure 3 As shown, Figure 1 This is a SEM photo of the flat membrane cross section magnified 1000 times. Figure 2 This is a SEM photo of the flat membrane cross section magnified 10,000 times. Figure 3 This is a SEM photo of a flat membrane cross section magnified 20,000 times. Figure 1 , Figure 2 and Figure 3 It can be seen that the membrane cross section has a dense surface cortex and a porous support layer, and is tightly bonded to the basement membrane.

[0251] The gas permeation properties of the prepared composite gas separation membranes are shown in Table 1.

[0252] Example 2

[0253] This example is to illustrate the preparation of the polyimide composite gas separation membrane of the present invention.

[0254] (1) 35 wt% of the random copolymer of polyimide prepared in Preparation Example 2, 44 wt% of NMP, 10 wt% of ethylene monochloride, 9 wt% of ethanol, 1 wt% of LiNO3, and 1 wt% of UiO-66 were added to a liquid kettle and stirred at 60°C for 24 hours, and then allowed to stand and degas at -0.1 MPa for 24 hours to obtain a casting solution for preparing a separation layer of a gas separation membrane; and then filtered through a 0.45 μm filter to obtain a casting solution;

[0255] (2) The polyvinylidene fluoride film was infiltrated with acetone solution for 30 seconds, and the casting solution was continuously scraped on the base film, and the scraper thickness was controlled to be 200 μm;

[0256] (3) The film precursor after knife coating was irradiated with an infrared heating lamp at 150°C for 3 min, and then immersed in a water coagulation bath to cause phase inversion and curing;

[0257] (4) Then, the membrane is sequentially soaked in water for 12 hours, ethanol for 12 hours, and n-hexane for 1 hour to extract the diluent added to the casting solution. The extracted membrane is dried under ventilation and room temperature conditions to obtain a polyimide composite gas separation membrane.

[0258] The polyimide composite gas separation membrane is a sheet structure, and the composite gas separation membrane includes a support layer and a separation layer attached to the outer surface of the support layer. The thickness of the separation layer is 850 nm, and the porosity of the composite gas separation membrane is 62%.

[0259] Figure 4 and Figure 5 is a cross-sectional scanning electron microscope image of the polyimide composite gas separation membrane prepared in Example 2; wherein, Figure 4 To magnify 1000 times, Figure 5 Magnified 2000 times. Figure 4 and Figure 5 It can be seen that the membrane cross section has a dense surface cortex and a porous support layer, and is tightly bonded to the basement membrane.

[0260] Results The gas permeation properties of the prepared composite gas separation membranes are shown in Table 1.

[0261] Example 3

[0262] This example is to illustrate the preparation of the polyimide composite gas separation membrane of the present invention.

[0263] (1) 25 wt% of the random copolymer of polyimide prepared in Preparation Example 3, 45 wt% of NMP, 15 wt% of THF, 10 wt% of ethanol, 3 wt% of LiNO3, and 2 wt% of ZIF-8 were added to a liquid kettle and stirred at 65°C for 24 hours, and then allowed to stand and degas at -0.1 MPa for 24 hours to obtain a casting liquid for preparing a separation layer of a gas separation membrane; and then filtered through a 0.45 μm filter to obtain a casting liquid;

[0264] (2) The polyvinylidene fluoride film was soaked in an ethanol solution for 60 seconds, and the casting solution was continuously scraped on the base film, and the scraper thickness was controlled to be 200 μm;

[0265] (3) The film precursor after knife coating is irradiated with an infrared heating lamp at 100°C for 1 min, and then immersed in a water coagulation bath to cause phase inversion and curing;

[0266] (4) Then the membrane is sequentially soaked in water for 12 hours, ethanol for 12 hours, and n-hexane for 1 hour to extract the diluent added to the casting solution. The extracted membrane is dried under ventilation and room temperature conditions to obtain a polyimide composite gas separation membrane. The polyimide composite gas separation membrane is a sheet structure, and the composite gas separation membrane includes a support layer and a separation layer attached to the outer surface of the support layer, the thickness of the separation layer is 780nm, and the porosity of the composite gas separation membrane is 60%.

[0267] Figure 6 and Figure 7 is a cross-sectional scanning electron microscope image of the polyimide composite gas separation membrane prepared in Example 3; wherein, Figure 6 To magnify 1000 times, Figure 7 The magnification is 1000 times. Figure 6 and Figure 7 It can be seen that the membrane section has a dense surface skin layer and a porous support layer, and is tightly bonded to the base membrane. Results The gas permeability of the prepared composite gas separation membrane is shown in Table 1.

[0268] Comparative Example 1

[0269] A polyimide composite gas separation membrane was prepared in the same manner as in Example 1, except that lithium nitrate was not added in step (1), heat treatment was not performed in step (2), 30 wt % polyimide resin, 48 wt % NMP, 10 wt % THF, and 9 wt % ethanol were added, and a scanning electron microscope image of the cross section of the polyimide composite membrane was obtained. Figure 4 It can be seen that the membrane prepared in Comparative Example 1 has more pores on the surface.

[0270] in addition, Figure 8 This is a cross-sectional scanning electron microscope image of the polyimide composite gas separation membrane prepared in Comparative Example 1. Fig. 9 This is a surface scanning electron microscope image of the polyimide composite gas separation membrane prepared in Comparative Example 1. Figure 8 and Fig. 9 It can be seen that: membrane section ( Figure 8 ) No dense cortex was formed, and the surface ( Fig. 9 ) When magnified 20,000 times, micropores can be seen and the membrane has no ability to separate gases.

[0271] Comparative Example 2

[0272] A polyimide composite gas separation membrane was prepared in the same manner as in Example 1, except that in step (2), the polyvinylidene fluoride-based membrane was not soaked with ethylenediamine solution for 30 seconds, but the casting solution was directly scraped onto the base membrane. The prepared membrane coating was peeled off from the base membrane, and a composite gas separation membrane could not be formed.

[0273] Comparative Example 3

[0274] A polyimide composite gas separation membrane was prepared in the same manner as in Example 1, except that in step (3), the film precursor after scraping was irradiated by an infrared heating lamp at 200°C.

[0275] The separation layer of the prepared membrane had a thickness of 5 μm and a relatively small gas permeation rate.

[0276] Table 1

[0277]

[0278] Note: In Table 1, "polyimide" represents polyimide random copolymer, "solvent 1" represents compound A, "solvent 2" represents compound B, and "solvent 3" represents compound C; "thickness" represents the thickness of the separation layer in the polyimide composite gas separation membrane; "porosity" represents the porosity of the support layer in the polyimide composite gas separation membrane.

[0279] Test Example 1

[0280] The performance of the composite gas separation membranes prepared in the above examples and comparative examples was tested.

[0281] The test method of permeation rate (GPU): at room temperature 20℃, measure the gas flow rate per unit membrane area per unit time under a pressure difference of 0.1MPa. The separation coefficient α is dimensionless and is used to characterize the selective permeation ability of gas components in the membrane. The separation coefficient is the ratio of the permeation rates of two gases in the membrane. The test results are shown in Table 4. Among them, 1GPU = 10 -6 cm 3 (STP) / (cm 2 ·s·cmHg).

[0282] Table 2

[0283]

[0284] Note: The numbers refer to the serial numbers of the embodiments and comparative examples.

[0285] From the above results, it can be seen that the composite gas separation membranes prepared by using Examples 1-3 of the present invention have a high separation coefficient and a high permeation flux for the separation of hydrogen and helium, and have significantly better effects than Comparative Examples 1-3. In addition, the composite gas separation membranes prepared by using Examples 1-3 of the present invention can improve the mechanical strength of the membrane.

[0286] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A polyimide composite gas separation membrane, It is characterized in that The composite gas separation membrane is a sheet structure, and the composite gas separation membrane includes a support layer and a separation layer attached to the outer surface of the support layer. The material of the separation layer contains a polyimide random copolymer, and the polyimide random copolymer has a structure shown in formula (I): (I), In formula (I), m and n are each independently an integer of 5-2000; X has a structure represented by any one of formula (X1) to formula (X3); (X1)、 (X2)、 (X3), In formula (X1)-formula (X3), R 1 , R 2 , R 3 , R 4 , R 5 and R 6 Each is independently H, C1-C4 alkyl, C6-C10 aryl, amino, hydroxyl or carboxyl; Y has a structure represented by any one of formula (Y1) to formula (Y5); <h2 style=";text-align:left;direction:ltr"> <h2 style=";text-align:left;direction:ltr"> (Y1)<h2 style=";text-align:left;direction:ltr"> <h2 style=";text-align:left;direction:ltr"> (Y2)<h2 style=";text-align:left;direction:ltr"> <h2 style=";text-align:left;direction:ltr"> (Y3) (Y4) (Y5), In formula (Y1) to formula (Y5), R 7 , R 8 , R 9 , R 10 , R 11 , R 12 , R 13 , R 14 , R 15 and R 16 Each is independently H, C1-C4 alkyl, C6-C10 aryl, amino, hydroxyl or carboxyl; Z and Z' each independently have a structure represented by formula (Z1) or formula (Z2); (Z1)、 (Z2), In formula (Z2), Ra and Rb are each independently H, C1-C4 alkyl or C1-C4 halogenated alkyl.

2. The composite gas separation membrane according to claim 1, in, The X has one of the following structures, 、 、 ; And / or, Y has one of the following structures, 、 、 、 、 ; and / or, Z and Z' both have the structure shown by Z1 or Z3, 、 。 3. The composite gas separation membrane according to claim 1 or 2, in, X is Xa, Y is Ya, and Z and Z' are both Z1; Alternatively, X is Xa, Y is Yb, and Z and Z' are both Z1; Or, X is Xa, Y is Yd, and Z and Z' are both Z1; Or, X is Xb, Y is Ya, and Z and Z' are both Z1; Or, X is Xb, Y is Yb, and Z and Z' are both Z1; Or, X is Xb, Y is Yd, and Z and Z' are both Z1; Or, X is Xc, Y is Ya, and Z and Z' are both Z1; Alternatively, X is Xc, Y is Yb, and Z and Z' are both Z1; Or, X is Xc, Y is Yc, and Z and Z' are both Z1; Alternatively, X is Xc, Y is Y4, and Z and Z' are both Z1; Or, X is Xc, Y is Yd, and Z and Z' are both Z1; Or, X is Xb, Y is Ya, and Z and Z' are both Z3; Or, X is Xb, Y is Yb, and Z and Z' are both Z3; Or, X is Xb, Y is Yd, and Z and Z' are both Z3; Or, X is Xc, Y is Ya, and Z and Z' are both Z3; Or, X is Xc, Y is Yb, and Z and Z' are both Z3; Alternatively, X is Xc, Y is Yd, and Z and Z' are both Z3.

4. The composite gas separation membrane according to claim 1, in, The separation layer further contains an additive, wherein the additive is selected from one or more of a metal organic framework compound, lithium nitrate and lithium chloride; And / or, the separation layer has a dense structure, and the thickness of the separation layer is ≤1000 nm; And / or, the support layer is an organic porous ultrafiltration membrane; And / or, the porosity of the composite gas separation membrane is 50-80%.

5. The composite gas separation membrane according to claim 4, in, The metal organic framework compound is selected from UiO-66 and / or ZIF-8; And / or, the support layer is selected from one or more of polyvinylidene fluoride, polypropylene, polyether sulfone, polysulfone, cellulose acetate, polyacrylonitrile, polyethylene, polytetrafluoroethylene and non-woven fabric fibers.

6. The composite gas separation membrane according to claim 1, in, m and n are each independently an integer of 50-1000.

7. The composite gas separation membrane according to claim 1 or 6, in, 0.9≥n / (m+n)≥0.

3.

8. The composite gas separation membrane according to claim 7, in, 0.7≥n / (m+n)≥0.

5.

9. The composite gas separation membrane according to claim 1, in, The weight average molecular weight of the polyimide random copolymer is 120,000-600,000.

10. The composite gas separation membrane according to claim 9, in, The weight average molecular weight of the polyimide random copolymer is 200,000-450,000.

11. A method for preparing a polyimide composite gas separation membrane, It is characterized in that The preparation method comprises: (1) mixing a polyimide random copolymer and a diluent to prepare a casting solution; (2) coating the casting solution on a base film and performing a heat treatment to obtain a film precursor; (3) solidifying, extracting and drying the membrane precursor to obtain a polyimide composite gas separation membrane; Wherein, the polyimide random copolymer has a structure shown in formula (I): (I), In formula (I), m and n are each independently an integer of 5-2000; X has a structure represented by any one of formula (X1) to formula (X3); (X1)、 (X2)、 (X3), In formula (X1)-formula (X3), R 1 , R 2 , R 3 , R 4 , R 5 and R 6 Each is independently H, C1-C4 alkyl, C6-C10 aryl, amino, hydroxyl or carboxyl; Y has a structure represented by any one of formula (Y1) to formula (Y5); <h2 style=";text-align:left;direction:ltr"> <h2 style=";text-align:left;direction:ltr"> (Y1)<h2 style=";text-align:left;direction:ltr"> <h2 style=";text-align:left;direction:ltr"> (Y2)<h2 style=";text-align:left;direction:ltr"> <h2 style=";text-align:left;direction:ltr"> (Y3) (Y4) (Y5), In formula (Y1) to formula (Y5), R 7 , R 8 , R 9 , R 10 , R 11 , R 12 , R 13 , R 14 , R 15 and R 16 Each is independently H, C1-C4 alkyl, C6-C10 aryl, amino, hydroxyl or carboxyl; Z and Z' each independently have a structure represented by formula (Z1) or formula (Z2); (Z1)、 (Z2), In formula (Z2), Ra and Rb are each independently H, C1-C4 alkyl or C1-C4 halogenated alkyl.

12. The preparation method according to claim 11, in, The X has one of the following structures, 、 、 ; And / or, Y has one of the following structures, 、 、 、 、 ; and / or, Z and Z' both have the structure shown by Z1 or Z3, 、 ; Alternatively, X is Xa, Y is Yb, and Z and Z' are both Z1; Or, X is Xa, Y is Yd, and Z and Z' are both Z1; Or, X is Xb, Y is Ya, and Z and Z' are both Z1; Or, X is Xb, Y is Yb, and Z and Z' are both Z1; Or, X is Xb, Y is Yd, and Z and Z' are both Z1; Or, X is Xc, Y is Ya, and Z and Z' are both Z1; Alternatively, X is Xc, Y is Yb, and Z and Z' are both Z1; Or, X is Xc, Y is Yc, and Z and Z' are both Z1; Alternatively, X is Xc, Y is Y4, and Z and Z' are both Z1; Or, X is Xc, Y is Yd, and Z and Z' are both Z1; Or, X is Xb, Y is Ya, and Z and Z' are both Z3; Or, X is Xb, Y is Yb, and Z and Z' are both Z3; Or, X is Xb, Y is Yd, and Z and Z' are both Z3; Or, X is Xc, Y is Ya, and Z and Z' are both Z3; Or, X is Xc, Y is Yb, and Z and Z' are both Z3; Alternatively, X is Xc, Y is Yd, and Z and Z' are both Z3.

13. The preparation method according to claim 12, in, X is Xa, Y is Ya, and Z and Z' are both Z1.

14. The preparation method according to claim 11, in, m and n are each independently an integer of 50-1000.

15. The preparation method according to claim 11 or 14, in, 0.9≥n / (m+n)≥0.

3.

16. The preparation method according to claim 15, in, 0.7≥n / (m+n)≥0.

5.

17. The preparation method according to claim 11, in, The weight average molecular weight of the polyimide random copolymer is 120,000-600,000.

18. The preparation method according to claim 17, in, The weight average molecular weight of the polyimide random copolymer is 200,000-450,000.

19. The preparation method according to claim 11, in, In step (1), the casting solution further contains additives.

20. The preparation method according to claim 19, in, Based on the total weight of the casting solution, the content of the polyimide is 18-35wt%, the content of the diluent is 60-77wt%, and the content of the additive is 0.5-5wt%.

21. The preparation method according to claim 20, in, Based on the total weight of the casting solution, the content of the polyimide is 25-35wt%, the content of the diluent is 63-70wt%, and the content of the additive is 1-5wt%.

22. The preparation method according to claim 11, in, The diluent includes compound A, compound B and compound C, and the mass ratio of compound A, compound B and compound C is 1:(0.1-0.5):(0.1-0.5).

23. The preparation method according to claim 22, in, The mass ratio of the compound A, the compound B and the compound C is 1:(0.15-0.3):(0.15-0.3).

24. The preparation method according to claim 22 or 23, in, The compound A is selected from one or more of N-methylpyrrolidone, N,N-dimethylacetamide and N,N-dimethylacetamide; And / or, the compound B is selected from one or more of ethanol, γ-butyrolactone and water; And / or, the compound C is selected from one or more of tetrahydrofuran, pentane, ethyl chloride and acetone.

25. The preparation method according to any one of claims 19 to 21, in, The additive is selected from one or more of lithium nitrate, lithium chloride and metal organic framework compounds.

26. The preparation method according to claim 25, in, The metal organic framework compound is selected from UiO-66 and / or ZIF-8.

27. The preparation method according to claim 11, in, The base membrane is an organic porous ultrafiltration membrane.

28. The preparation method according to claim 27, in, The base film is selected from one or more of polyvinylidene fluoride, polypropylene, polyether sulfone, polysulfone, cellulose acetate, polyacrylonitrile, polyethylene, polytetrafluoroethylene and non-woven fabric fibers.

29. The preparation method according to claim 11, in, In step (1), the casting solution is prepared according to a method comprising the following steps: stirring polyimide, a diluent and an optional additive at 20-70° C. for 12-48 hours, then vacuum degassing, and then filtering through a 0.45-5 μm filter to remove impurities.

30. The preparation method according to claim 29, in, The vacuum degassing conditions include: pressure of -0.1 MPa to -0.095 MPa, temperature of 20-30° C., and time of 12-24 h.

31. The preparation method according to claim 11, in, In step (2), the coating thickness is 50-300 μm.

32. The preparation method according to claim 11, in, In step (2), the heat treatment conditions include: temperature of 70-150° C. and time of 1-5 min.

33. The preparation method according to claim 32, in, In step (2), the heat treatment conditions include: temperature of 80-100°C and time of 2-4 minutes.

34. The preparation method according to claim 11, in, In step (2), the base film is also pretreated.

35. The preparation method according to claim 34, in, The pretreatment includes: soaking the base film with a pretreatment solution.

36. The preparation method according to claim 35, in, The pretreatment solution is selected from one or more of ethylenediamine, ethanol and acetone; And / or, the infiltration time is 5-60s.

37. The preparation method according to claim 11, in, In step (3), the coagulation bath used for coagulation is water and / or a C1-C4 saturated monohydric alcohol; And / or, the extractant used for extraction is selected from at least one of water, C1-C4 saturated monohydric alcohol and C5-C7 alkane; And / or, the extraction conditions include: temperature of 20-35°C and time of 3-48h; And / or, the extraction further includes a drying step.

38. The preparation method according to claim 37, in, The temperature of the coagulation bath is 40-70°C; And / or, the C1-C4 saturated monohydric alcohol is selected from one or more of methanol, ethanol and isopropanol; And / or, the C5-C7 alkane is n-hexane or cyclohexane; And / or, the drying conditions include: temperature of 20-35° C. and time of 2-15 h.

39. A polyimide-based composite gas separation membrane prepared by the preparation method according to any one of claims 11 to 38.

40. Use of the polyimide-based composite gas separation membrane according to any one of claims 1 to 10 and 39 in one or more of gas separation, hydrogen concentration and helium extraction from natural gas.

Citation Information

Cited By

  • Method and system for separating and purifying helium in natural gas