A method for preparing PVA coarse denier fibers by melt plasticization-wet spinning
By adopting the melt plasticizing-wet spinning process in the PVA fiber spinning process, and using the method of combining composite plasticizer and wet spinning, the existing technology solves the long process, large pollution and increased pollution of the PVA fiber spinning process. The problem of plastic residue has been solved, and the effects of process shortening, environmental protection and fiber performance improvement have been achieved.
Patent Information
- Application Number
- CN202211529756.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-30
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-11-30
AI Technical Summary
The existing spinning process of PVA fiber has problems such as long process, high pollution and limited performance. In particular, water-based wet spinning has difficulties in dehydration and floating yarn problems when preparing PVA coarse denier fiber. Melt spinning has problems due to plasticizer residue. This results in lower fiber mechanical properties and difficulty in plasticizer removal.
Using the melt plasticization-wet spinning process, by adding a composite plasticizer to the PVA resin, using a screw extruder for plasticization, combined with the wet spinning process to remove the plasticizer, including air cooling, moist heat After stretching, oil bath, drying, hot stretching and other steps, PVA coarse denier fiber is finally produced, and all organic solvents can be recycled.
It achieves shortened process flow, environmentally friendly production, increased fiber draw ratio, solves the problem of plasticizer residue, reduces production costs, and eliminates the need to use boric acid and acetic acid, improves the on-site operating environment, and improves fiber performance.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of PVA fiber spinning and manufacturing, and in particular to a method for preparing PVA coarse-denier fibers by melt plasticization-wet spinning. Background Art
[0002] Polyvinyl alcohol (PVA) fiber is a synthetic fiber made from PVA resin as the main raw material. It has the advantages of high strength and modulus, good weather resistance, wear resistance and good moisture absorption. It meets the characteristics of new materials and environmental protection requirements and is widely used in construction, clothing, military industry, medical and other fields.
[0003] The preparation process of PVA fiber includes the steps of stock solution preparation, spinning, drying, and drawing. Spinning is the key to PVA fiber forming. At present, the most mature and industrially applied spinning methods of PVA fiber are mainly water-based wet spinning, including conventional water-based wet spinning and water-based wet spinning with boron cross-linking. However, the process of water-based wet spinning is long, the "three wastes" pollution is large, the on-site working environment is harsh, and the performance of the prepared PVA fiber is limited: for example, water-based wet spinning has the problems of difficult dehydration and floating fibers when preparing PVA coarse denier fibers.
[0004] In response to the problems of water-based wet spinning, people have explored different spinning methods, of which two are representative: one is Kuraray's "solvent wet cooling gel spinning" process. Kuraray's "KURALON K-Ⅱ" new PVA fiber prepared using this process has been commercialized, and the product models include three types: easily water-soluble (water-soluble temperature 0-100℃), high-strength (strength 14.6cN / dtex) and easy fibrillation. However, the "solvent wet cooling gel spinning" process has not been industrialized in China due to factors such as the large amount of organic solvents used and production equipment.
[0005] The other is the melt spinning of PVA. Since the melting temperature and decomposition temperature of PVA are close, PVA decomposes while melting and cannot be directly melt processed. In order to achieve the melt processing of PVA, it is usually necessary to add a plasticizer. Plasticizing modifiers that have been reported to be used for PVA include polyols, inorganic salts, water, ionic liquids, etc. Melt spinning of PVA is an effective method for preparing PVA coarse denier fibers. Although PVA plasticized melt spinning does not need to consider the dissolution of raw materials and solvent recovery, the residual plasticizer causes the fiber to have a low stretch multiple and low mechanical properties. Therefore, the removal of plasticizers has always been an unresolved problem.
[0006] PVA coarse denier fiber can effectively solve the problem of poor dispersion and easy agglomeration of high-strength and high-modulus PVA coarse denier fiber in concrete. At present, most of the PVA coarse denier fibers on the market rely on foreign imports. Therefore, it is of great significance to realize the localization of PVA coarse denier. Summary of the invention
[0007] Aiming at the advantages and disadvantages of aqueous wet boron cross-linking spinning, organic solvent gel spinning and melt spinning for preparing PVA coarse denier fibers, the invention proposes a method for preparing PVA coarse denier fibers by melt plasticization-wet spinning, which has a short process flow, is green and environmentally friendly, and is easy to industrialize.
[0008] In order to achieve the purpose, the present invention adopts the following technical scheme:
[0009] A method for preparing PVA coarse denier fibers by melt plasticization-wet spinning, comprising the following steps:
[0010] S1, melt plasticization step:
[0011] Adding plasticizer to PVA resin, then plasticizing and melting it through a screw extruder, and then metering and pressurizing it to a spinning assembly through a metering pump to obtain PVA primary fibers;
[0012] S2, wet spinning steps:
[0013] The PVA primary fiber is cooled by air and then put into an organic solvent to remove the plasticizer; then it is subjected to wet heat stretching, oil bath, drying, hot stretching, oiling, cutting, and packaging processes to finally obtain the PVA coarse denier fiber.
[0014] Furthermore, in step S1, the PVA resin has a degree of polymerization of 1700-5000 and a degree of alcoholysis of ≥99.0%.
[0015] Furthermore, in step S1, the plasticizer is a composite plasticizer, which uses small molecule glycerol as a main plasticizer and at least one of polyols, inorganic salts, and polyphenols as an auxiliary plasticizer.
[0016] Furthermore: the polyol is at least one of 1,4-butanediol, 1,5-pentanediol, 1,4-cyclohexanedimethanol, sorbitol, isosorbide and polyethylene glycol; the inorganic salt is at least one of lithium salt, potassium salt and sodium salt; the polyphenol is at least one of phenol, ellagic acid, chlorogenic acid and tannic acid.
[0017] Furthermore, in step S1, the amount of the plasticizer added is 5%-50% of the mass of the PVA resin, preferably 5%-30%.
[0018] Furthermore, the mass percentage of glycerol in the composite plasticizer is 60%-90%.
[0019] Furthermore, in step S1, the temperature of the screw extruder is set as follows: 110-120°C in the first feeding zone; 130-135°C in the second compression zone; 140-155°C in the third melting zone; 155-165°C in the fourth homogenizing metering zone; and 120-140°C in the spinning assembly.
[0020] Furthermore, the organic solvent in step S2 is one of methanol, ethanol, isopropanol and acetone.
[0021] Furthermore, all the organic solvents used in step S2 can be recycled, thereby reducing production costs.
[0022] Further: in step S2, the temperature of the organic solvent is -30°C to 10°C, the wet heat stretching temperature is 50-92°C, and the oil bath temperature is 30-40°C; in step S2, the heating method of the drying process is quartz tube electric heating or microwave heating, and the drying process is a three-stage drying process, the temperature of the first stage is 50-70°C, the drying time is 120-180 seconds, the temperature of the second stage is 85-90°C, the drying time is 150-200 seconds, and the temperature of the third stage is 100-120°C, and the drying time is 240-300 seconds.
[0023] The beneficial effects of the present invention are embodied in:
[0024] 1. Compared with the method for preparing PVA coarse denier fiber by aqueous wet boron cross-linking spinning, the present invention does not require the use of boric acid and acetic acid, no acetic acid vapor is generated during the production process, and the on-site operating environment is good;
[0025] 2. Compared with the method for preparing PVA coarse denier fiber by aqueous wet boron cross-linking spinning, the present invention does not require the steps of dissolving, degassing and washing PVA, and the production process is significantly shortened;
[0026] 3. The present invention introduces organic solvents into the nascent fibers, and the plasticizers in the raw materials can be effectively removed, which is convenient for increasing the fiber stretching multiples in the later stage, and solves the problem of difficulty in recovering plasticizers in melt spinning. Moreover, the organic solvents are fully recovered after use, and no wastewater is generated, which is a major improvement in environmental protection. DETAILED DESCRIPTION
[0027] The embodiments of the present invention are described in detail below. The following embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following embodiments.
[0028] Example 1
[0029] The PVA resin used in this embodiment has a degree of polymerization of 1700 and a degree of alcoholysis of 99%, and is used in an amount of 20 kg.
[0030] The composite plasticizer used in this embodiment is composed of glycerol and sorbitol, wherein the mass of glycerol is 2.8 kg and the mass of sorbitol is 1.2 kg.
[0031] The method steps for preparing PVA coarse denier fibers by melt plasticization-wet spinning in this embodiment are as follows:
[0032] S1, melt plasticization step:
[0033] The PVA resin and the composite plasticizer are mixed evenly, fed into the feed port after granulation, and then plasticized and melted through a screw extruder, and the temperature is set as follows: 115°C in the first feeding zone; 130°C in the second compression zone; 140°C in the third melting zone; 155°C in the fourth homogenization metering zone; and 130°C in the spinning assembly. After plasticization and melting, the resin passes through a spinneret with a micropore diameter of 1 mm to obtain PVA primary fibers.
[0034] S2, wet spinning steps:
[0035] The PVA nascent fibers are air-cooled and then placed in methanol to remove the plasticizer. The temperature of the methanol is -10°C. The filaments out of the methanol are subjected to wet heat stretching (the wet heat stretching temperature is 65°C), and then passed through an oil bath (the oil bath temperature is 35°C) and dried. The drying method is quartz tube heating drying. The drying process is a three-stage drying process. The first stage drying temperature is 60°C and the drying time is 150 seconds. The second stage drying temperature is 90°C and the drying time is 180 seconds. The third stage drying temperature is 110°C and the drying time is 240 seconds.
[0036] The dried filament bundle is subjected to heat stretching, oiling, cutting and packaging processes to obtain the finished PVA coarse denier fiber.
[0037] The main technical quality indicators of the PVA coarse denier fiber in this embodiment are shown in Table 1:
[0038] Table 1
[0039] index Measured value Denier / dtex 40 Breaking strength / (cN / dtex) 13.58 Initial modulus / (cN / dtex) 270.00 Elongation at break / % 6.5
[0040] Example 2
[0041] The PVA resin used in this embodiment has a degree of polymerization of 2400 and a degree of alcoholysis of 99%, and is used in an amount of 20 kg.
[0042] The composite plasticizer used in this embodiment is composed of glycerol, sodium chloride and phenol, wherein the mass of glycerol is 2.4 kg, the mass of sodium chloride is 0.1 kg, and the mass of phenol is 0.5 kg.
[0043] The method steps for preparing PVA coarse denier fibers by melt plasticization-wet spinning in this embodiment are as follows:
[0044] S1, melt plasticization step:
[0045] The PVA resin and the composite plasticizer are mixed evenly, granulated and fed into the feed port, and then plasticized and melted through a screw extruder, and the temperature is set as follows: 115°C in the first feeding zone; 130°C in the second compression zone; 145°C in the third melting zone; 155°C in the fourth homogenization metering zone; and 120°C in the spinning assembly. After plasticization and melting, the resin passes through a spinneret with a micropore diameter of 0.8 mm to obtain PVA primary fibers.
[0046] S2, wet spinning steps:
[0047] The PVA nascent fibers are air-cooled and then placed in ethanol to remove the plasticizer. The ethanol temperature is 0°C. The filaments out of ethanol are subjected to wet heat stretching (wet heat stretching temperature is 65°C), and then passed through an oil bath (oil bath temperature is 35°C) and dried. The drying method is quartz tube heating drying. The drying process is a three-stage drying process. The first stage drying temperature is 60°C and the drying time is 150 seconds. The second stage drying temperature is 90°C and the drying time is 180 seconds. The third stage drying temperature is 110°C and the drying time is 240 seconds.
[0048] The dried filament bundle is subjected to heat stretching, oiling, cutting and packaging processes to obtain the finished PVA coarse denier fiber.
[0049] The main technical quality indicators of the PVA coarse denier fiber in this embodiment are shown in Table 2:
[0050] Table 2
[0051] index Measured value Denier / dtex 25 Breaking strength / (cN / dtex) 12.47 Initial modulus / (cN / dtex) 290.00 Elongation at break / % 5.0
[0052] The above description is only an exemplary embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing PVA coarse denier fibers by melt plasticization-wet spinning, characterized in that: The steps include: S1, melt plasticization step: 20kg of PVA resin with a polymerization degree of 1700 and an alcoholysis degree of 99% and a composite plasticizer consisting of 2.8kg of glycerol and 1.2kg of sorbitol were mixed uniformly, granulated and fed into a feed port, and then plasticized and melted through a screw extruder, and the temperature was set as follows: 115°C in the first feeding zone; 130°C in the second compression zone; 140°C in the third melting zone; 155°C in the fourth homogenization metering zone; 130°C in the spinning assembly; after plasticization and melting, the fibers passed through a spinneret with a micropore diameter of 1mm to obtain PVA primary fibers; S2, wet spinning steps: The PVA nascent fibers were cooled by air and then placed in methanol to remove the plasticizer. The temperature of the methanol was -10°C. The filaments out of methanol were subjected to wet heat stretching at 65°C. They were then placed in an oil bath at 35°C and dried. The drying method was quartz tube heating drying. The drying process was a three-stage drying process. The first stage was at 60°C and the drying time was 150 seconds. The second stage was at 90°C and the drying time was 180 seconds. The third stage was at 110°C and the drying time was 240 seconds. The dried filament bundle is subjected to heat stretching, oiling, cutting and packaging processes to obtain the finished PVA coarse denier fiber.
Citation Information
Patent Citations
Method for preparing water soluble polyvinyl alcohol fiber through melt spinning
CN103409837A
Method for preparing polyvinyl alcohol coarse denier fiber through melt spinning
CN110205696A
Anti-counterfeiting fiber preparation method and anti-counterfeiting fiber
CN113308752A
High-tenacity and high-modulus PVA fiber and production thereof
JP1987085013A
Polyvinyl alcohol-based fiber
JP2005281900A