Powder composition, waterproof slurry and preparation method thereof
Through the combination of fast hard cement and modified fly ash and other materials, the problem of slow hydration and flash setting of waterproof slurry is solved, rapid hydration and water resistance are achieved, construction time is extended, construction efficiency is improved and construction efficiency is improved. Water resistance.
Patent Information
- Application Number
- CN202211422554.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-15
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-11-15
AI Technical Summary
The existing waterproof slurry is slow to hydrate, resulting in relatively slow strength development, long maintenance time, and prone to flash settling or stability problems of operation time, which affects construction efficiency.
Fast hard cement and modified fly ash are used as cementitious materials, combined with retarder, quartz sand, cellulose ether, early strength agent and water reducing agent to form a powder composition, and with polymer emulsion and hydrophobic agent , mix bacterial and defoaming agents to prepare waterproof slurry, improve hydration speed and water resistance, avoid flash condensation, and extend construction time.
It realizes rapid hydration of waterproof slurry, improves compressive strength, flexural strength and water resistance, extends construction time, avoids flash condensation, and improves construction efficiency and water resistance.
Smart Images

Figure BDA0003942976920000151 
Figure BDA0003942976920000152 
Figure BDA0003942976920000161
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a powder composition, a waterproof slurry and a preparation method thereof. Background Art
[0002] Waterproof slurry is an indispensable protective material for building decoration. It can effectively prevent accidents such as water leakage that cause damage to other rooms. The current waterproof slurry is basically based on ordinary Portland cement as the gelling material, compounded with some fillers and additives and polymer emulsion. Due to the limitation of the hydration speed of ordinary Portland cement itself, the strength development is relatively slow and the required curing time is relatively long.
[0003] In the related art, the cement hydration rate is usually accelerated by significantly increasing the early hydration heat of ordinary Portland cement or compounding ordinary Portland cement into a ternary system or a binary system. However, flash setting is very likely to occur or the stability problem of the operable time may occur. Summary of the invention
[0004] Based on this, it is necessary to provide a powder composition, a waterproof slurry and a preparation method thereof that can accelerate the hydration rate of the slurry and prevent the slurry from flashing and prolong the construction time.
[0005] The first aspect of the present invention provides a powder composition, which comprises, by weight, 35 to 50 parts of rapid-hardening cement, 10 to 25 parts of functional materials, 35 to 60 parts of quartz sand, 0.05 to 0.2 parts of cellulose ether, 0.05 to 0.4 parts of retarder, 0.05 to 0.3 parts of early strength agent and 0.05 to 0.5 parts of water reducing agent; wherein the functional material comprises modified fly ash.
[0006] In some embodiments, the modified fly ash satisfies the following
[0007] At least one of the following conditions:
[0008] I. The average particle size D50 of the modified fly ash is ≤3 μm;
[0009] II. The modified fly ash is obtained by modifying fly ash with phosphoric acid and sulfate;
[0010] Optionally, the sulfate includes one or more of aluminum sulfate, sodium sulfate, calcium sulfate and iron sulfate.
[0011] In some embodiments, the functional material further comprises steel slag powder, and the mass ratio of the modified fly ash to the steel slag powder is (1-2):1;
[0012] Optionally, the specific surface area of the steel slag powder is 750-800m2 / kg.
[0013] In some embodiments, the retarder includes one or more of sodium citrate and sodium gluconate;
[0014] Optionally, when the retarder is a mixture of sodium citrate and sodium gluconate, the mass ratio of the sodium citrate to the sodium gluconate is (1-2):1.
[0015] In some embodiments, the rapid-hardening cement includes magnesite cement, and the mass ratio of light-burned magnesium oxide to magnesium chloride used in the preparation process of the magnesite cement is 1:(0.44-0.55).
[0016] In some embodiments, the quartz sand includes quartz sand with a particle size of 40 to 70 mesh, quartz sand with a particle size of 70 to 100 mesh, and quartz sand with a particle size of 100 to 180 mesh in a mass ratio of (1 to 1.5):(2 to 3):(0 to 1).
[0017] In some embodiments, the cellulose ether includes one or more of hydroxyethyl cellulose and hydroxypropyl methyl cellulose; the early strength agent includes a magnesia early strength agent; and the water reducer includes one or more of a polycarboxylate water reducer and a sulfonated melamine high-efficiency water reducer.
[0018] The second aspect of the present invention provides a waterproof slurry, comprising the powder composition of the first aspect of the present invention, and also comprising a liquid composition;
[0019] In parts by weight, the liquid composition comprises 38 to 50 parts of polymer emulsion, 58 to 78 parts of water, 0.1 to 0.8 parts of water repellent, 0.1 to 0.5 parts of bactericide and 0.1 to 0.8 parts of defoaming agent.
[0020] In some embodiments, the waterproof slurry meets one or more of the following conditions:
[0021] (1) The polymer emulsion includes one or more of vinyl acetate-ethylene copolymer emulsion, styrene-acrylate copolymer emulsion, and butadiene-styrene copolymer emulsion;
[0022] (2) The water repellent comprises an organosilicon water repellent;
[0023] (3) The defoamer includes one or more of a mineral oil defoamer, a silicone defoamer and a polyether defoamer;
[0024] (4) The fungicide includes one or more of Kasone, BIT fungicide and composite fungicide SIG;
[0025] Optionally, the composite fungicide SIG is a mixture of (1,2-benzisothiazolin-3-one) and 2-methyl-4-isothiazolin-3-one.
[0026] In some embodiments, the waterproof slurry satisfies at least one of the following conditions:
[0027] (1) The construction time of the waterproof slurry is 60 to 150 minutes;
[0028] (2) The waterproof slurry is subjected to a water-tightness test 4 to 6.5 hours after construction, and there is no leakage after 48 hours;
[0029] (3) The anti-seepage pressure of the waterproof slurry is 0.7-0.8 MPa;
[0030] (4) The lateral deformation capacity of the waterproof slurry after hydration is 2.4 to 3.0 mm;
[0031] (5) The compressive strength of the waterproof slurry after hydration is 24 to 31 MPa;
[0032] (6) The flexural strength of the waterproof slurry after hydration is 7 to 11 MPa;
[0033] (7) The shrinkage rate of the waterproof slurry after hydration is 0.2 to 0.26%;
[0034] (8) After the waterproof slurry is hydrated, the bonding strength in the untreated state is 1.3 to 1.8 MPa, the bonding strength on the wet base is 1.6 to 2.2 MPa, the bonding strength after alkali treatment is 1.6 to 2.2 MPa, and the bonding strength after immersion treatment is 1.7 to 2.5 MPa.
[0035] The third aspect of the present invention provides a method for preparing a waterproof slurry, comprising the following steps:
[0036] Mixing rapid-hardening cement, functional materials, quartz sand, cellulose ether, retarder, early strength agent and water reducing agent to prepare a powder composition;
[0037] The polymer emulsion, the water repellent, the bactericide, the defoamer and water are mixed to prepare a liquid material composition.
[0038] The powder composition, waterproof slurry and preparation method thereof provided above adopt quick-hardening cement to prepare the powder composition, and the powder composition also includes a retarder; when the above-mentioned powder composition is used in the waterproof slurry, the hydration rate of the waterproof slurry can be increased, and the addition of the retarder can effectively avoid the flash setting of the waterproof slurry and increase the construction time of the waterproof slurry during use.
[0039] In addition, the powder composition also includes modified fly ash. When the powder composition is used in waterproof slurry, during the hydration process of the waterproof slurry, the active silicon dioxide in the modified fly ash can react with the magnesium oxide in the magnesite cement to generate a water-insoluble hydration product, magnesium silicate; at the same time, the active aluminum oxide in the modified fly ash can generate aluminum hydroxide colloid to block the capillary pores of the magnesite cement and reduce the water absorption rate; thereby effectively improving the water resistance of the magnesite cement. DETAILED DESCRIPTION
[0040] For ease of understanding of the present invention, the present invention will be described more fully below with reference to relevant embodiments. The following provides preferred embodiments of the present invention. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0041] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0042] In this article, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0043] Herein, when it comes to numerical ranges, unless otherwise specified, the numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0044] In this article, when referring to the unit of a data range, if there is a unit only after the right endpoint, it means that the units of the left and right endpoints are the same. For example, 750~800m 2 / kg means the units of the left endpoint "750" and the right endpoint "800" are both m 2 / kg.
[0045] Waterproof slurry is an indispensable protective material for current building decoration. It can effectively prevent accidents such as accidental water leakage that cause damage to other rooms. Waterproof slurry can generally be divided into flexible products (polymer waterproof coatings) and rigid products (polymer waterproof slurry). Among them, polymer waterproof slurry can be divided into single component (pure powder part with water added on site) and two components (powder part + liquid part), among which two-component waterproof slurry is the majority. Flexible products are more suitable for ground application due to their better flexibility and obvious advantages in crack resistance. At the same time, due to their relatively low bonding strength and high requirements for the base surface, if they are applied to walls that need to be tiled later, there will be a greater risk of bricks falling off after tiling, so they are not very suitable for wall applications; rigid products have relatively high bonding strength and are more suitable for wall applications, which can effectively reduce the risk of bricks falling off after tiling.
[0046] At present, the basic curing time of ordinary waterproof products is 24h-48h, and even under certain conditions it may be extended to more than 48h, which greatly reduces the construction efficiency. The current waterproof slurry is basically based on ordinary Portland cement as the gelling material, compounded with some fillers, additives, and polymer emulsion. Due to the limitation of the hydration rate of ordinary Portland cement itself, the strength development is relatively slow, and the required curing time is relatively long.
[0047] In the related art, quick-drying technology can be roughly divided into two categories. One is to accelerate the hydration rate of cement by greatly increasing the early hydration heat of silicate cement; therefore, the waterproof slurry has considerable safety hazards in the storage and production of raw materials. At the same time, the finished product actually produced is also prone to flash setting. The other is to compound ordinary silicate cement into a ternary system or a binary system to accelerate the hydration rate of cement. However, the waterproof slurry system is prone to stability problems in the operable time, and the operable time cannot be controlled, which affects the construction efficiency and leads to a substantial increase in construction costs.
[0048] In order to solve the above problems, the present invention provides a powder composition, which includes, by weight, 35 to 50 parts of rapid-hardening cement, 10 to 25 parts of functional materials, 35 to 60 parts of quartz sand, 0.05 to 0.2 parts of cellulose ether, 0.05 to 0.4 parts of retarder, 0.05 to 0.3 parts of early strength agent and 0.05 to 0.5 parts of water reducing agent; wherein the functional material includes modified fly ash.
[0049] In the present invention, rapid-hardening cement is used as a cementitious material, and modified fly ash is used as a modifying material of the cementitious material. Rapid-hardening cement has the same cementitious properties as cement, and at the same time has better compressive strength. Moreover, the present invention finds that the rapid-hardening cement is mixed with the functional material of the present invention to greatly improve the mechanical properties of its products such as compressive strength and flexural strength, as well as the efficiency of achieving these mechanical strengths. At the same time, during the hydration process of rapid-hardening cement, the active silicon dioxide in the modified fly ash can react with the rapid-hardening cement, such as magnesium oxide in magnesia cement, to generate a water-insoluble hydration product, magnesium silicate; at the same time, the active aluminum oxide in the modified fly ash can generate aluminum hydroxide colloid to block the capillaries of magnesia cement products and reduce the water absorption rate, thereby effectively improving the water resistance of magnesia cement products and improving the stability of mechanical properties such as compressive strength and flexural strength of magnesia cement products.
[0050] In an embodiment of the present invention, based on 35 to 50 parts of rapid hardening cement, the weight portion of the functional material in the powder composition is 10 to 25 parts; for example, 10 parts, 12 parts, 15 parts, 18 parts, 20 parts, 23 parts or 25 parts of the functional material may be included. Further, based on 35 to 50 parts of rapid hardening cement, the weight portion of the functional material in the powder composition is 15 to 25 parts.
[0051] In an embodiment of the present invention, the functional material includes modified fly ash. Further, the average particle size D50 of the modified fly ash is ≤3 μm. Furthermore, the modified fly ash is obtained by modifying fly ash with phosphoric acid and sulfate; the sulfate may include one or more of aluminum sulfate, sodium sulfate, calcium sulfate and iron sulfate.
[0052] When phosphoric acid is used to modify fly ash, phosphoric acid can increase the specific surface area by corroding the glass structure of fly ash. In addition, active metal oxides such as Al2O3 and CaO in the fly ash components are also easily dissolved by reaction with phosphoric acid; phosphoric acid also weakens the interaction between Al-O, Si-O-Si and Si-O bonds in fly ash, increases the intercrystalline spacing, and improves the adsorption efficiency, thereby improving the mechanical properties such as flexibility of the products obtained by using the above powder composition.
[0053] When fly ash is modified by sulfate, cations in the sulfate, such as Al 3+ 、Na + , Ca 2+ , Fe 3+ The cations in the solution are exchanged on the surface of the fly ash and in its pores to generate corresponding precipitates or oxides, thereby achieving the purpose of removing pollutants in the solution and improving the environmental performance of the products obtained by using the above powder composition.
[0054] In some embodiments, the rapid-hardening cement includes magnesite cement, and the mass ratio of light-burned magnesium oxide to magnesium chloride used in the preparation process of magnesite cement is 1:(0.44-0.55); for example, it can be 1:0.44, 1:0.47, 1:0.5, 1:0.52 or 1:0.55, etc.
[0055] In some embodiments, the functional material further comprises steel slag powder, and the mass ratio of the modified fly ash to the steel slag powder is (1-2):1; for example, it can be 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1 or 2:1. Further, the mass ratio of the modified fly ash to the steel slag powder is (1.5-2):1. The activity of the steel slag powder is lower than that of ordinary Portland cement, and the steel slag powder needs to be stimulated under certain excitation conditions to stimulate its later strength. Therefore, by adding steel slag powder to the powder composition, the early hydration rate of the powder composition during application can be effectively slowed down, and the flash setting of related products, such as waterproof slurry, can be better avoided; when the mass ratio of the modified fly ash to the steel slag powder is (1-2):1, the water resistance of the waterproof slurry can be further improved and the hydration rate of the waterproof slurry can be reduced.
[0056] In some embodiments, the specific surface area of the steel slag powder is 750-800 m 2 / kg; for example, it can be 750m 2 / kg, 760m 2 / kg, 770m 2 / kg, 780m 2 / kg, 790m 2 / kg or 800m 2 When the specific surface area of the steel slag powder is within the above range, the activity of the steel slag powder can be fully exerted, and as the specific surface area of the steel slag powder increases, the activity of the steel slag powder also increases. Preferably, the specific surface area of the steel slag powder is 760-800m 2 / kg; can further improve the activity of steel slag powder.
[0057] Based on 35 to 50 parts of rapid-hardening cement, the weight portion of the retarder in the powder composition is 0.05 to 0.4 parts; for example, 0.05, 0.08, 0.1, 0.13, 0.15, 0.17, 0.20, 0.22, 0.25, 0.28, 0.30, 0.33, 0.35 or 0.4 parts of the retarder may be included. Further, based on 35 to 50 parts of rapid-hardening cement, the weight portion of the retarder in the powder composition is 0.15 to 0.35 parts.
[0058] In some embodiments, the retarder includes one or more of sodium citrate and sodium gluconate; adding the retarder can reduce the hydration rate of the powder composition, increase the workability time of the powder composition product, and especially increase the workability time of the powder composition product under high temperature conditions.
[0059] In some embodiments, when the retarder is a mixture of sodium citrate and sodium gluconate, the mass ratio of sodium citrate to sodium gluconate is (1-2):1; for example, it can be 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1 or 2:1. Further, the mass ratio of sodium citrate to sodium gluconate is (1.3-2):1.
[0060] Based on 35 to 50 parts of rapid-hardening cement, the weight percentage of quartz sand in the powder composition is 35 to 60 parts; for example, quartz sand may be 35, 38.7, 40, 43.5, 45, 47, 50, 52.3, 55, 57.5 or 60 parts. Further, based on 35 to 50 parts of rapid-hardening cement, the weight percentage of quartz sand in the powder composition is 45 to 55 parts.
[0061] In some embodiments, the quartz sand includes quartz sand with a particle size of 40 to 70 mesh, quartz sand with a particle size of 70 to 100 mesh, and quartz sand with a particle size of 100 to 180 mesh in a mass ratio of (1 to 1.5): (2 to 3): (0 to 1). By adding quartz sand to the powder composition, it serves as an aggregate in the powder composition product to support the entire system, and the use of reasonable grading can make the powder composition product show a better state.
[0062] Based on 35 to 50 parts of rapid-hardening cement, the weight portion of cellulose ether in the powder composition is 0.05 to 0.2 parts; for example, it can be 0.05 parts, 0.08 parts, 0.1 parts, 0.13 parts, 0.15 parts, 0.17 parts or 0.2 parts, etc. Further, based on 35 to 50 parts of rapid-hardening cement, the weight portion of cellulose ether in the powder composition is 0.1 to 0.2 parts.
[0063] In some embodiments, the cellulose ether may include one or more of hydroxyethyl cellulose and hydroxypropyl methyl cellulose. By adding cellulose ether to the powder composition, the state of the powder composition product can be kept stable, and the risk of delamination of the powder composition product can be reduced.
[0064] Based on 35 to 50 parts of rapid-hardening cement, the weight portion of the early strength agent in the powder composition is 0.05 to 0.3 parts; for example, it can be 0.05 parts, 0.08 parts, 0.1 parts, 0.12 parts, 0.15 parts, 0.17 parts, 0.20 parts, 0.22 parts, 0.25 parts, 0.27 parts or 0.3, etc. Further, based on 35 to 50 parts of rapid-hardening cement, the weight portion of the early strength agent in the powder composition is 0.1 to 0.25 parts.
[0065] In some embodiments, the early strength agent includes a magnesite early strength agent. By adding the magnesite early strength agent to the powder composition, the curing speed of the powder composition product can be accelerated, the strength can be established more quickly, and the construction efficiency can be improved.
[0066] Based on 35 to 50 parts of rapid-hardening cement, the weight portion of the water reducer in the powder composition is 0.05 to 0.5 parts; for example, it can be 0.05 parts, 0.1 parts, 0.15 parts, 0.2 parts, 0.25 parts, 0.3 parts, 0.35 parts, 0.4 parts, 0.45 parts or 0.5 parts, etc. Further, based on 35 to 50 parts of rapid-hardening cement, the weight portion of the water reducer in the powder composition is 0.15 to 0.5 parts.
[0067] In some embodiments, the water reducer includes one or more of a polycarboxylate water reducer and a sulfonated melamine high efficiency water reducer. By adding the water reducer to the powder composition, the viscosity of the powder composition product is adjusted, so that the powder composition product has better workability.
[0068] The present invention also provides a waterproof slurry, comprising the powder composition provided above, and also comprising a liquid composition; in parts by weight, the liquid composition comprises 38 to 50 parts of a polymer emulsion, 58 to 78 parts of water, 0.1 to 0.8 parts of a hydrophobic agent, 0.1 to 0.5 parts of a bactericide and 0.1 to 0.8 parts of a defoaming agent.
[0069] In some embodiments, the polymer emulsion includes one or more of vinyl acetate-ethylene copolymer emulsion, styrene-acrylate copolymer emulsion, and butadiene-styrene copolymer emulsion.
[0070] Based on 38 to 50 parts of polymer emulsion, the weight of water in the liquid composition is 58 to 78 parts; for example, it can be 58 parts, 60 parts, 63 parts, 65 parts, 67 parts, 70 parts, 72 parts, 75 parts or 78 parts, etc. Further, based on 38 to 50 parts of polymer emulsion, the weight of water in the liquid composition is 60 to 75 parts.
[0071] Based on 38 to 50 parts of the polymer emulsion, the weight portion of the water repellent in the liquid composition is 0.1 to 0.8 parts; for example, it can be 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts or 0.8 parts, etc. Further, based on 38 to 50 parts of the polymer emulsion, the weight portion of the water repellent in the liquid composition is 0.5 to 0.8 parts.
[0072] In some embodiments, the water repellent includes an organosilicon water repellent. By adding the water repellent to the liquid composition, the waterproof performance of the product during use is further enhanced.
[0073] Based on 38 to 50 parts of the polymer emulsion, the weight portion of the fungicide in the liquid composition is 0.1 to 0.5 parts; for example, it can be 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts or 0.5 parts, etc. Further, based on 38 to 50 parts of the polymer emulsion, the weight portion of the fungicide in the liquid composition is 0.2 to 0.5 parts.
[0074] In some embodiments, the fungicide includes one or more of Kathon, BIT fungicide and composite fungicide SIG; wherein the composite fungicide SIG is a mixture of (1,2-benzisothiazolin-3-one) and 2-methyl-4-isothiazolin-3-one. By adding a fungicide to the liquid composition, the liquid can be reduced or even prevented from deteriorating or stinking due to the proliferation of fungi, bacteria and other species during storage.
[0075] Based on 38 to 50 parts of the polymer emulsion, the weight portion of the defoamer in the liquid composition is 0.1 to 0.8 parts; for example, it can be 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts or 0.8 parts, etc. Further, based on 38 to 50 parts of the polymer emulsion, the weight portion of the defoamer in the liquid composition is 0.4 to 0.8 parts.
[0076] In some embodiments, the defoaming agent may include one or more of a mineral oil defoaming agent, a silicone defoaming agent, and a polyether defoaming agent; by adding a defoaming agent to the liquid composition, bubbles introduced by the stirring head during mechanical stirring can be eliminated, making the slurry denser.
[0077] In some embodiments, the construction time of the waterproof slurry is 60 to 150 min; for example, it can be 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min or 150 min, etc.
[0078] In some embodiments, the waterproof slurry is subjected to a water-tightness test 4 to 6.5 hours after construction, and no leakage is observed after 48 hours.
[0079] In some embodiments, the anti-seepage pressure of the waterproof slurry is 0.7 to 0.8 MPa; for example, it can be 0.7 MPa, 0.71 MPa, 0.72 MPa, 0.73 MPa, 0.74 MPa, 0.75 MPa, 0.76 MPa, 0.77 MPa, 0.78 MPa, 0.79 MPa or 0.8 MPa, etc.
[0080] In some embodiments, the lateral deformation capacity of the waterproof slurry after hydration is 2.4 to 3.0 mm; for example, it can be 2.4 mm, 2.5 mm, 2.6 mm, 2.7 mm, 2.8 mm, 2.9 mm or 3.0 mm, etc.
[0081] In some embodiments, the compressive strength of the waterproof slurry after hydration is 24 to 31 MPa; for example, it can be 24 MPa, 25 MPa, 26 MPa, 27 MPa, 28 MPa, 29 MPa, 30 MPa or 31 MPa, etc.
[0082] In some embodiments, the flexural strength of the waterproof slurry after hydration is 7 to 11 MPa; for example, it can be 7 MPa, 8 MPa, 9 MPa, 10 MPa or 11 MPa, etc.
[0083] In some embodiments, the shrinkage rate of the waterproof slurry after hydration is 0.2-0.26%; for example, it can be 0.2%, 0.21%, 0.22%, 0.23%, 0.24%, 0.25% or 0.26%, etc.
[0084] In some embodiments, after the waterproof slurry is hydrated, the bonding strength in the untreated state is 1.3 to 1.8 MPa, the bonding strength on the wet base is 1.6 to 2.2 MPa, the bonding strength after alkali treatment is 1.6 to 2.2 MPa, and the bonding strength after immersion treatment is 1.7 to 2.5 MPa.
[0085] The present invention also provides a method for preparing a waterproof slurry, comprising the following steps:
[0086] Mixing rapid-hardening cement, functional materials, quartz sand, cellulose ether, retarder, early strength agent and water reducing agent to prepare a powder composition;
[0087] The polymer emulsion, the water repellent, the bactericide, the defoamer and water are mixed to prepare a liquid material composition.
[0088] The present invention also provides a method for using the waterproof slurry, comprising the following steps:
[0089] Carry out dust removal, interface agent application, watering and other treatments according to the conditions of the base layer;
[0090] The powder composition and the liquid composition are mixed in a ratio of 30-36 kg of the liquid composition per 100 kg of the powder composition, stirred for 2 minutes, and then allowed to stand for 1 minute for later use;
[0091] Use a brush or roller to dip the stirred waterproof mortar and apply it to the wall or floor to be constructed, so that the thickness reaches 0.5-0.7mm;
[0092] Depending on the wall conditions, the construction can be done 2 to 3 times. Before constructing the next waterproof layer, the surface of the previous waterproof layer must be dried.
[0093] The technical solution of the present invention is described in detail below in conjunction with specific embodiments.
[0094] It should be noted that HPMC referred to in the following examples and comparative examples represents hydroxypropyl methylcellulose, and HEC represents hydroxyethyl cellulose; the modified fly ash referred to in the following examples and comparative examples is obtained by modifying fly ash with phosphoric acid and aluminum sulfate.
[0095] The waterproof slurries prepared in the following examples and comparative examples were tested for construction time and water closure test, respectively, and tested according to the standard JC / T 2090-2011 "Polymer Cement Waterproof Slurry". The construction time test and water closure test were performed using the following method:
[0096] Construction time test: Take the waterproof slurry, let it stand, and use a brush or roller to perform construction tests at different times until construction is no longer possible. If the brush cannot brush the slurry or the roller cannot roll, it can be considered that the construction time has expired. Generally, 90 to 120 minutes is best.
[0097] Water-tightness test: Apply two coats of waterproof slurry crosswise inside the 30cm*30cm*10cm gypsum board frame. After the first coat is dry, apply the second coat. After the second coat is applied, cure for 4.5 to 24 hours, add 5 to 8 cm deep tap water into the gypsum board frame, let it stand and observe. If there is no watermark on the bottom and no obvious water absorption is found on the gypsum board, it is considered that the water-tightness test has passed.
[0098] Example 1
[0099] The powder composition includes: 350g of magnesite cement, 250g of functional material, 1g of HPMC with a viscosity of 20000mPa.s, 395g of quartz sand, 2g of retarder, 1.5g of magnesite early strength agent, and 0.5g of water reducing agent;
[0100] The mass ratio of light-burned magnesium oxide to magnesium chloride used in the preparation process of magnesite cement is 1:0.47; the functional material is modified fly ash, and the average particle size D50 of the modified fly ash is 3 μm; the retarder is sodium citrate, and the water reducer is a polycarboxylic acid water reducer; the quartz sand is a mixture of quartz sand with a particle size of 40 to 70 meshes and quartz sand with a particle size of 70 to 100 meshes, and the mass ratio of quartz sand with a particle size of 40 to 70 meshes to quartz sand with a particle size of 70 to 100 meshes is 1:3;
[0101] The liquid material composition includes: 380g of styrene-acrylate copolymer emulsion, 2g of silicone water repellent, 3g of Kathon, 4g of mineral oil defoamer and 611g of water.
[0102] Example 2
[0103] The powder composition includes: 400g of magnesite cement, 175g of functional material, 1.3g of HEC with a viscosity of 20000mPa.s, 418.4g of quartz sand, 2.5g of retarder, 2g of magnesite early strength agent, and 0.8g of water reducer;
[0104] The mass ratio of light-burned magnesium oxide to magnesium chloride used in the preparation process of magnesite cement is 1:0.49; the functional material is modified fly ash, and the average particle size D50 of the modified fly ash is 2.5 μm; the retarder is sodium gluconate, and the water reducer is sulfonated melamine high-efficiency water reducer; the quartz sand is a mixture of quartz sand with a particle size of 40-70 mesh and quartz sand with a particle size of 70-100 mesh, and the mass ratio of quartz sand with a particle size of 40-70 mesh and quartz sand with a particle size of 70-100 mesh is 1:2;
[0105] The liquid material composition includes: 450g of butadiene-styrene copolymer emulsion, 4g of organosilicon water repellent, 4g of BIT bactericide, 3g of organosilicon defoamer and 539g of water.
[0106] Example 3
[0107] The powder composition includes: 440g of magnesite cement, 135g of functional material, 1.5g of HPMC with a viscosity of 20000mPa.s, 420.1g of quartz sand, 2.0g of retarder, 0.5g of magnesite early strength agent, and 0.9g of water reducer;
[0108] The mass ratio of light-burned magnesium oxide to magnesium chloride used in the preparation process of magnesite cement is 1:0.52; the functional material is modified fly ash, and the average particle size D50 of the modified fly ash is 2 μm; the retarder is sodium citrate, and the water reducer is a polycarboxylic acid water reducer; the quartz sand is a mixture of quartz sand with a particle size of 40-70 mesh, quartz sand with a particle size of 70-100 mesh, and quartz sand with a particle size of 100-180 mesh, and the mass ratio of quartz sand with a particle size of 40-70 mesh, quartz sand with a particle size of 70-100 mesh, and quartz sand with a particle size of 100-180 mesh is 1:2:1;
[0109] The liquid material composition includes: 400g of vinyl acetate-ethylene copolymer emulsion, 8g of silicone hydrophobic agent, 2g of composite fungicide SIG, 2g of polyether defoamer and 588g of water.
[0110] Example 4
[0111] The powder composition includes: 480g of magnesite cement, 120g of functional material, 1.0g of HEC with a viscosity of 20000mPa.s, 395g of quartz sand, 0.18g of retarder, 1g of magnesite early strength agent, and 0.12g of water reducer;
[0112] The mass ratio of light-burned magnesium oxide to magnesium chloride used in the preparation of magnesite cement is 1:0.44; the functional material is a mixture of modified fly ash and steel slag powder in a mass ratio of 1:1, the average particle size D50 of the modified fly ash is 2.5 μm, and the specific surface area of the steel slag powder is 800 m 2 / kg, the grade of steel slag powder is first class; the retarder is a mixture of sodium citrate and sodium gluconate in a mass ratio of 1:1; the water reducer is a mixture of polycarboxylic acid water reducer and sulfonated melamine high-efficiency water reducer in a mass ratio of 1:1; the quartz sand is a mixture of quartz sand with a particle size of 40-70 mesh and quartz sand with a particle size of 70-100 mesh, and the mass ratio of quartz sand with a particle size of 40-70 mesh and quartz sand with a particle size of 70-100 mesh is 1.5:2;
[0113] The liquid composition includes: 450 g of styrene-acrylate copolymer emulsion, 6 g of silicone water repellent, 4 g of kason, 3.5 g of silicone defoamer and 536.5 g of water.
[0114] Example 5
[0115] The powder composition includes: 500g of magnesite cement, 115g of functional material, 0.8g of HPMC with a viscosity of 20000mPa.s, 390g of quartz sand, 3g of retarder, 0.8g of magnesite early strength agent, and 1.4g of water reducer;
[0116] The mass ratio of light-burned magnesium oxide to magnesium chloride used in the preparation of magnesite cement is 1:0.55; the functional material is a mixture of modified fly ash and steel slag powder in a mass ratio of 1:1, the average particle size D50 of the modified fly ash is 2 μm, and the specific surface area of the steel slag powder is 750 m 2 / kg, the grade of steel slag powder is first class; the retarder is a mixture of sodium citrate and sodium gluconate in a mass ratio of 2:1; the water reducer is a polycarboxylic acid water reducer; the quartz sand is a mixture of quartz sand with a particle size of 40-70 mesh and quartz sand with a particle size of 70-100 mesh, and the mass ratio of quartz sand with a particle size of 40-70 mesh and quartz sand with a particle size of 70-100 mesh is 1.5:2;
[0117] The liquid composition includes: a mixture of 500g styrene-acrylate copolymer emulsion and butadiene-styrene copolymer emulsion, 8g silicone hydrophobic agent, 4g composite bactericide SIG, 2g polyether defoamer and 486g water; wherein the mass ratio of styrene-acrylate copolymer emulsion to butadiene-styrene copolymer emulsion is 1:2.
[0118] Example 6
[0119] The difference between Example 6 and Example 4 is that the functional material in the powder composition is a mixture of modified fly ash and steel slag powder in a mass ratio of 2:1, and the rest are the same.
[0120] Example 7
[0121] The difference between Example 7 and Example 4 is that the specific surface area of the steel slag powder in the powder composition is 750 m 2 / kg, everything else is the same.
[0122] Example 8
[0123] The difference between Example 8 and Example 4 is that the specific surface area of the steel slag powder in the powder composition is 770 m 2 / kg, everything else is the same.
[0124] Example 9
[0125] The difference between Example 9 and Example 4 is that the specific surface area of the steel slag powder in the powder composition is 730 m 2 / kg, everything else is the same.
[0126] Example 10
[0127] The difference between Example 10 and Example 4 is that no steel slag powder is added to the powder composition, and the other parts are the same.
[0128] Embodiment 11
[0129] The difference between Example 11 and Example 4 is that the average particle size D50 of the modified fly ash in the powder composition is 4 μm, and the other aspects are the same.
[0130] Comparative Example 1
[0131] The powder composition includes: 550 g of ordinary Portland cement with a grade of 42.5, 0.8 g of HPMC with a viscosity of 30000 mPa.s, 445.9 g of quartz sand, 2.5 g of calcium formate, and 0.8 g of polycarboxylate water reducer;
[0132] The quartz sand is a mixture of quartz sand with a particle size of 40 to 70 meshes and quartz sand with a particle size of 70 to 100 meshes, and the mass ratio of the quartz sand with a particle size of 40 to 70 meshes to the quartz sand with a particle size of 70 to 100 meshes is 1.5:2;
[0133] The liquid composition includes: 450g of styrene-acrylate copolymer emulsion, 6g of silicone water repellent, 4g of kason, 3g of mineral oil defoamer and 537g of water.
[0134] Among them, the waterproof slurry prepared in Comparative Example 1 showed leakage in the closed water test conducted 12h and 18h after construction, and no leakage in the closed water test conducted 28h after construction.
[0135] Comparative Example 2
[0136] The powder composition includes: 370g of ordinary Portland cement with a grade of 42.5, 180g of rapid hardening cement with a grade of 42.5, 50g of anhydrous gypsum, 1.3g of HPMC with a viscosity of 30000mPa.s, 395g of quartz sand, 1.5g of sodium gluconate, 1g of lithium sulfate, and 1.2g of polycarboxylate water reducer;
[0137] The quartz sand is a mixture of quartz sand with a particle size of 40 to 70 meshes and quartz sand with a particle size of 70 to 100 meshes, and the mass ratio of the quartz sand with a particle size of 40 to 70 meshes to the quartz sand with a particle size of 70 to 100 meshes is 1.5:2;
[0138] The liquid composition includes: 450g of a mixture of styrene-acrylate copolymer emulsion and butadiene-styrene copolymer emulsion in a mass ratio of 1:2, 5g of an organosilicon water repellent, 3.5g of kason, 3.5g of a mineral oil defoamer and 518g of water.
[0139] Comparative Example 3
[0140] The powder composition includes: 480g of ordinary Portland cement with a grade of 42.5, 180g of rapid hardening cement with a grade of 42.5, 1.5g of HPMC with a viscosity of 30000mPa.s, 334.2g of quartz sand, 1.5g of sodium citrate, 1g of lithium carbonate, and 1.5g of polycarboxylate water reducer;
[0141] The quartz sand is a mixture of quartz sand with a particle size of 40 to 70 meshes and quartz sand with a particle size of 70 to 100 meshes, and the mass ratio of the quartz sand with a particle size of 40 to 70 meshes to the quartz sand with a particle size of 70 to 100 meshes is 1.5:2;
[0142] The liquid composition includes: 460g of butadiene-styrene copolymer emulsion, 4g of silicone water repellent, 3g of kason, 3g of mineral oil defoamer and 530g of water.
[0143] Comparative Example 4
[0144] The difference between Comparative Example 4 and Example 4 is that ordinary fly ash of the same mass is used to replace the modified fly ash, and the other aspects are the same.
[0145] Comparative Example 5
[0146] The difference between Comparative Example 5 and Example 4 is that no modified fly ash is added, and the other aspects are the same.
[0147] Comparative Example 6
[0148] The difference between Comparative Example 6 and Example 4 is that no retarder is added, and the other aspects are the same.
[0149] The waterproof slurries prepared in Examples 1 to 10 and Comparative Examples 1 to 6 were tested for construction time and water closure test, and were tested according to the standard JC / T 2090-2011 "Polymer Cement Waterproof Slurry". The standard of "Polymer Cement Waterproof Slurry" is shown in Table 1.
[0150] Table 1
[0151]
[0152] The performance test results of the waterproof slurry in Examples 1 to 10 and Comparative Examples 1 to 6 are shown in Table 2 below.
[0153] Table 2
[0154]
[0155]
[0156] From the results of Examples 1 to 11 and Comparative Examples 1 to 3 in Table 2, it can be seen that compared with the waterproof slurry prepared by using ordinary Portland cement, or a combination of ordinary Portland cement and rapid hardening cement, and a retarder, the waterproof slurry prepared by using the powder composition of the present invention including functional materials such as modified fly ash, rapid hardening cement and retarder can not only improve the hydration rate of the waterproof slurry, but also effectively avoid the flash setting of the waterproof slurry, extend the construction time of the waterproof slurry during use, and improve the water resistance of the waterproof slurry. On this basis, when the components in the powder composition are of different types and / or amounts, the obtained powder composition can also improve the hydration rate, water resistance, flexibility, bonding strength, compressive strength, flexural strength of the waterproof slurry when used in the waterproof slurry, and reduce the shrinkage rate of the waterproof slurry.
[0157] The main difference between Example 4 and Example 10 is that no steel slag powder is added to the powder composition of Example 10. From the results of Example 4 and Example 10, it can be seen that adding steel slag powder to the powder composition can further adjust the early hydration rate of the waterproof slurry, thereby better adjusting the construction time. The main difference between Example 4 and Examples 7 to 9 is that the specific surface area of the steel slag powder in the powder composition is different. From the results of Example 4 and Examples 7 to 9, it can be seen that when the specific surface area of the steel slag powder changes, it will affect the mechanical properties of the prepared waterproof slurry. For example, Example 9 shows relatively poor mechanical properties. This is because the specific surface area of the steel slag powder can affect the activity of the steel slag powder; and from the comparison, it can be found that when the specific surface area of the steel slag powder is 750 to 800 m 2 / kg, the activity of steel slag powder can be fully exerted, so that the steel slag powder can react with rapid-hardening cement more easily to generate water-insoluble hydration products, thereby improving the bonding performance, compressive strength, flexural strength and other properties of the resulting waterproof slurry.
[0158] The main difference between Example 4 and Example 11 is that the average particle size D50 of the modified fly ash in the powder composition is different. From the results of Example 4 and Example 11, it can be seen that when the average particle size D50 of the modified fly ash in the powder composition is ≤3μm, the water resistance, compressive strength and flexural strength of the waterproof slurry can be further improved.
[0159] The difference between Example 4 and Comparative Example 4 is that ordinary fly ash is used in Comparative Example 4; the difference between Example 4 and Comparative Example 5 is that modified fly ash is not added in Comparative Example 5; from the results of Example 4 and Comparative Examples 4-5, it can be seen that when ordinary fly ash is added or no fly ash is added, the waterproof slurry obtained cannot achieve a waterproof effect, and the base surface applied with the waterproof slurry continues to leak. It can be seen that adding modified fly ash to the powder composition and using the powder composition in the waterproof slurry can effectively improve the water resistance of the waterproof slurry.
[0160] The difference between Example 4 and Comparative Example 6 is that no retarder is added in Comparative Example 6. From the results of Example 4 and Comparative Example 6, it can be seen that by further adding a retarder to the powder composition and using the powder composition in a waterproof slurry, the construction time of the waterproof slurry during use can be further extended.
[0161] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0162] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A powder composition, characterized in that: In parts by weight, it comprises 35-50 parts of rapid hardening cement, 10-25 parts of functional materials, 35-60 parts of quartz sand, 0.05-0.2 parts of cellulose ether, 0.05-0.4 parts of retarder, 0.05-0.3 parts of early strength agent and 0.05-0.5 parts of water reducing agent; Wherein, the functional materials are modified fly ash and steel slag powder, and the rapid hardening cement is magnesite cement; The average particle size D50 of the modified fly ash is ≤3 μm, and the modified fly ash is obtained by modifying fly ash with phosphoric acid and sulfate.
2. The powder composition according to claim 1, characterized in that The sulfate includes one or more of aluminum sulfate, sodium sulfate, calcium sulfate and iron sulfate.
3. The powder composition according to any one of claims 1 to 2, characterized in that The mass ratio of the modified fly ash to the steel slag powder is (1~2):
1.
4. The powder composition according to claim 3, characterized in that The specific surface area of the steel slag powder is 750-800m 2 / kg.
5. The powder composition according to claim 1, characterized in that The retarder includes one or more of sodium citrate and sodium gluconate.
6. The powder composition according to claim 5, characterized in that When the retarder is a mixture of sodium citrate and sodium gluconate, the mass ratio of the sodium citrate to the sodium gluconate is (1-2):
1.
7. The powder composition according to claim 1, characterized in that The mass ratio of light-burned magnesium oxide to magnesium chloride used in the preparation process of the magnesite cement is 1:(0.44-0.55).
8. The powder composition according to any one of claims 1 to 2 and 4 to 7, characterized in that The quartz sand includes quartz sand with a particle size of 40-70 mesh, quartz sand with a particle size of 70-100 mesh, and quartz sand with a particle size of 100-180 mesh in a mass ratio of (1-1.5):(2-3):(0-1).
9. The powder composition according to any one of claims 1 to 2 and 4 to 7, characterized in that The cellulose ether includes one or more of hydroxyethyl cellulose and hydroxypropyl methyl cellulose; the early strength agent includes magnesia early strength agent; and the water reducer includes one or more of polycarboxylic acid water reducer and sulfonated melamine high-efficiency water reducer.
10. A waterproof slurry, characterized in that: A powder composition according to any one of claims 1 to 9, further comprising a liquid composition; In parts by weight, the liquid composition comprises 38 to 50 parts of polymer emulsion, 58 to 78 parts of water, 0.1 to 0.8 parts of water repellent, 0.1 to 0.5 parts of bactericide and 0.1 to 0.8 parts of defoaming agent.
11. The waterproof slurry according to claim 10, characterized in that: One or more of the following conditions are met: (1) The polymer emulsion includes one or more of vinyl acetate-ethylene copolymer emulsion, styrene-acrylate copolymer emulsion, and butadiene-styrene copolymer emulsion; (2) The water repellent comprises an organosilicon water repellent; (3) The defoamer includes one or more of a mineral oil defoamer, a silicone defoamer and a polyether defoamer; (4) The fungicide includes one or more of Kathon, BIT fungicide and composite fungicide SIG.
12. The waterproof slurry according to claim 11, characterized in that: The composite fungicide SIG is a mixture of (1,2-benzisothiazolin-3-one) and 2-methyl-4-isothiazolin-3-one.
13. A method for preparing a waterproof slurry according to any one of claims 10 to 12, characterized in that: The steps include: Mixing rapid-hardening cement, functional materials, quartz sand, cellulose ether, retarder, early strength agent and water reducing agent to prepare a powder composition; The polymer emulsion, the water repellent, the bactericide, the defoamer and water are mixed to prepare a liquid material composition.