Alumina fiber three-dimensional fabric containing lanthanum phosphate coating and preparation method and application thereof
By forming a uniform lanthanum phosphate coating on the alumina fiber three-dimensional fabric, the problem of uniformity of interface modification in high-temperature environments is solved, the toughness and high-temperature oxidation resistance of the composite material are improved, and it is suitable for aerospace thermal structures.
Patent Information
- Application Number
- CN202211413723.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-11
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-11-11
AI Technical Summary
In high-temperature environments, it is difficult to achieve uniformity in the interface modification of alumina fiber three-dimensional fabrics, resulting in insufficient toughness of the material under high-temperature conditions, making it difficult to meet the high-temperature mechanical load-bearing requirements in aerospace and other fields.
The alumina fiber is pretreated with an organic cationic polymer flocculant to form a positive surface charge, and then a negatively charged lanthanum phosphate precursor solution is used for vacuum impregnation and temperature heating to form a uniform lanthanum phosphate coating to ensure the fiber interface modified.
Through the use of lanthanum phosphate coating, the toughness and high-temperature oxidation resistance of the composite material are improved, ensuring a high strength retention rate after long-term high-temperature treatment, and is suitable for the field of aerospace thermal structures.
Smart Images

Figure CN115787285B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, and in particular to a three-dimensional fabric of aluminum oxide fibers containing a lanthanum phosphate coating, and a preparation method and application thereof. Background Art
[0002] Continuous ceramic fiber reinforced ceramic matrix composites (CFRCMCs) have the advantages of high temperature resistance, high strength, high hardness, low density, wear resistance, and good toughness. They are the main candidate materials for high-temperature components of aircraft engines and have broad application backgrounds in aerospace and other fields. At present, the most widely used CFRCMCs are silicon carbide (SiC)-based composites, mainly using carbon fiber and silicon carbide fiber as reinforcements, namely C / SiC and SiC / SiC composites. Both have broad application prospects in aerospace and other fields as high-temperature structural materials, but these materials have poor performance stability in high-temperature aerobic environments, especially in water-oxygen atmospheres, and cannot be reused for a long time.
[0003] Compared with non-oxide composite materials, continuous oxide fiber reinforced oxide-based composite materials have the characteristics of low cost and oxidation resistance. They can serve for a long time in high-temperature aerobic environments and ensure the stability of mechanical properties. Among them, quartz fiber reinforced ceramic-based composite materials have good oxidation resistance, but the use temperature of this material does not exceed 1000℃, the high-temperature mechanical properties are insufficient, and it is difficult to meet the needs of high-temperature mechanical bearing in the hot end. Alumina fiber reinforced alumina (Al2O3 / Al2O3) ceramic-based composite materials are important alternative materials for high-temperature components such as aircraft engines due to their oxidation resistance, high temperature resistance, heat shock resistance, water and oxygen corrosion resistance, and high mechanical strength.
[0004] In order to avoid the brittle fracture of the Al2O3 / Al2O3 composite material caused by the excessively strong bonding force between the fiber and the matrix at high temperature, it is necessary to introduce an interface phase between the fiber and the matrix to achieve a weak interface bond, deflect the cracks, and improve the toughness of the composite material. Currently, the interface phases used in Al2O3 / Al2O3 composite materials include weak interface phases, porous interface phases, and interstitial interface phases. Among them, rare earth-phosphate materials (ABO4) such as LaPO4 (monazite) have low mechanical properties, can withstand up to 2000℃, and have good physical and chemical compatibility with alumina fibers. They are widely used oxide interface materials.
[0005] In the process of modifying the alumina fiber surface with lanthanum phosphate, in order to avoid damage to the interface during fiber weaving, it is necessary to directly modify the alumina fiber three-dimensional fabric. The difficulty lies in that due to the obstruction of the fibers outside the fabric, the microscopic environment of the fibers inside the fabric is different, and the uniformity of the fiber interface preparation inside the fabric is difficult to ensure. Therefore, it is very necessary to provide a method for achieving uniform interface modification of alumina fiber three-dimensional fabric. Summary of the invention
[0006] The present invention provides a method for preparing a three-dimensional fabric of aluminum oxide fibers containing a lanthanum phosphate coating, and can provide a three-dimensional fabric of aluminum oxide fibers with a uniform lanthanum phosphate coating. The method of the present invention uses an organic cationic polymer flocculant to pretreat the aluminum oxide fibers so that the fiber surface is positively charged, and then a negatively charged lanthanum phosphate precursor solution is prepared, and the electrostatic attraction between the positive and negative charges is used to uniformly coat the aluminum oxide fibers with a lanthanum phosphate interface layer, thereby effectively ensuring the effect of modifying the fiber interface inside the fabric. The aluminum oxide fiber reinforced aluminum oxide composite material prepared by using the three-dimensional fabric of aluminum oxide fibers containing a lanthanum phosphate interface layer can improve the toughness of the composite material by virtue of the high melting point and high-temperature oxidation resistance of the lanthanum phosphate coating.
[0007] In order to achieve the above object, the present invention provides a method for preparing a three-dimensional fabric of alumina fibers containing a lanthanum phosphate coating in a first aspect, the method comprising the following steps:
[0008] (1) treating the continuous alumina fiber three-dimensional fabric to remove the wetting agent on the surface of the continuous alumina fiber;
[0009] (2) treating the surface of the alumina fiber three-dimensional fabric with an organic cationic polymer flocculant to obtain an alumina fiber fabric with a positive charge on the surface;
[0010] (3) preparing a negatively charged lanthanum phosphate precursor solution;
[0011] (4) vacuum impregnating the three-dimensional alumina fiber fabric with positive charges on the surface with the lanthanum phosphate precursor solution;
[0012] (5) The vacuum impregnated alumina fiber three-dimensional fabric is subjected to a heating treatment, and then subjected to the steps of washing, drying, and high-temperature treatment to obtain a continuous alumina fiber three-dimensional fabric with a lanthanum phosphate coating.
[0013] Preferably, step (3) prepares a lanthanum phosphate precursor solution at a temperature not greater than 5° C.;
[0014] Preferably, in step (4), the lanthanum phosphate precursor solution is used to vacuum impregnate the three-dimensional alumina fiber fabric with positive charges on the fiber surface under vacuum and at a temperature not greater than 10° C.;
[0015] Preferably, in step (5), the three-dimensional alumina fiber fabric after vacuum impregnation is heated and then sequentially subjected to the steps of washing, drying, and high-temperature treatment, and the process is repeated multiple times to obtain the continuous three-dimensional alumina fiber fabric with a lanthanum phosphate coating.
[0016] Preferably, the organic cationic polymer flocculant is at least one selected from polydimethyldiallylammonium chloride (PADAMA) and polyethyleneimine (PEI).
[0017] Preferably, the mass concentration of the organic cationic polymer flocculant solution is 0.5-5wt%; and / or the pH of the organic cationic polymer flocculant solution is 6-8.
[0018] Preferably, the preparation of the lanthanum phosphate precursor solution comprises the following steps:
[0019] (a) preparing an aqueous solution containing lanthanum ions at a temperature not greater than 5° C., then adding a reaction rate regulator, citric acid, to the aqueous solution containing lanthanum ions, and then adjusting the pH of the aqueous solution containing lanthanum ions to 6 to 8 to obtain a lanthanum ion solution;
[0020] (b) preparing an aqueous solution containing phosphate ions at a temperature not greater than 5° C., and adjusting the pH value of the aqueous solution containing phosphate ions to 6 to 8 to obtain a phosphate ion solution;
[0021] (c) mixing the lanthanum ion solution and the phosphate ion solution in a molar ratio of lanthanum to phosphorus of 1:1 to obtain the lanthanum phosphate precursor solution.
[0022] Preferably, the aqueous solution containing lanthanum ions is prepared using lanthanum chloride, lanthanum nitrate, lanthanum hydroxide, lanthanum carbonate, lanthanum oxide or other lanthanum salts that are easily soluble in water.
[0023] Preferably, the concentration of lanthanum ions in the mixed solution obtained by mixing is 0.4 to 1 mol / L.
[0024] Preferably, the molar ratio of the lanthanum ions contained in the lanthanum ion-containing aqueous solution to the citric acid is 1:(1-5).
[0025] Preferably, the aqueous solution containing phosphate is prepared by using phosphoric acid, phosphorus pentoxide, trimethylphosphoric acid, ammonium dihydrogen phosphate, water-soluble hydrogen phosphate, dihydrogen phosphate or phosphate.
[0026] Preferably, the concentration of phosphate ions in the mixed solution obtained by mixing is 0.4 to 1 mol / L.
[0027] Preferably, the pH of the lanthanum ion-containing aqueous solution and / or the phosphate aqueous solution is adjusted using ammonia water, urea, hydrochloric acid, nitric acid or sodium hydroxide; and / or the pH of the lanthanum ion-containing aqueous solution and / or the phosphate aqueous solution is adjusted to 6-8.
[0028] Preferably, the concentration of lanthanum ions in the lanthanum ion-containing aqueous solution and / or the concentration of phosphate ions in the phosphate ion solution is not less than 0.4 mol / L.
[0029] Preferably, the vacuum impregnation time is not less than 2 hours; and / or the heating temperature is not higher than 40°C, preferably 15-40°C, and the treatment time is 1-2 hours; preferably, the heating temperature is 25°C, and the heating time is 1.5 hours. The high temperature treatment temperature is 800-1000°C, and the insulation time is 1-2 hours; preferably, the high temperature treatment temperature is 900°C, and the high temperature treatment time is 1 hour.
[0030] In a second aspect, the present invention provides a modified alumina fiber three-dimensional fabric obtained by interfacial modification using the method described in the first aspect of the present invention.
[0031] In a third aspect, the application of the modified alumina fiber three-dimensional fabric with lanthanum phosphate coating obtained according to the second aspect includes preparing an oxide ceramic-based composite material using the alumina fiber three-dimensional fabric with lanthanum phosphate coating to obtain an oxide ceramic-based composite material with excellent toughness and high-temperature oxidation resistance.
[0032] Compared with the prior art, the present invention has at least the following beneficial effects:
[0033] (1) The preparation method of the three-dimensional fabric of alumina fiber with lanthanum phosphate coating provided by the present invention is simple, low-cost, green and environmentally friendly, and has low energy consumption. Water is directly used as a solvent, the reaction conditions are mild, and no complicated equipment and reagents are required during the preparation process. The raw materials used in the present invention are common industrial raw materials such as commonly used inorganic salts and inorganic acids and alkalis, which have a wide range of sources and are low-cost.
[0034] (2) The present invention combines an organic cationic polymer flocculant solution to pre-treat the alumina fiber, so that the surface of the fabric fiber adsorbs positive charges, and then vacuum impregnates the negatively charged lanthanum phosphate precursor solution to promote the subsequent interface layer to grow uniformly on the fiber surface inside the fabric. Through the process steps of vacuum impregnation and temperature rise, the uniformity of the interface modification of the fiber surface inside the fabric is effectively guaranteed.
[0035] (3) The lanthanum phosphate coating interface prepared by the present invention can protect the fiber from damage during the matrix densification and heat treatment process of the oxide ceramic-based composite material. At the same time, lanthanum phosphate has a monazite structure and does not react with alumina, etc. It has good high-temperature stability and can form a weak interface between the fiber and the matrix, thereby improving the toughness of the composite material.
[0036] (4) The lanthanum phosphate interface layer used in the present invention has excellent high-temperature oxidation resistance, and the alumina fiber reinforced alumina-based composite material prepared by the interface-modified alumina fiber three-dimensional fabric still has a high strength retention rate after long-term high-temperature treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the drawings without paying creative work.
[0038] Figure 1 It is a preparation flow chart of the present invention.
[0039] Figure 2 It is a preparation flow chart in a specific embodiment of the present invention.
[0040] Figure 3 This is a physical picture of the continuous oxide fiber three-dimensional fabric with a lanthanum phosphate interface layer prepared in Example 1 of the present invention.
[0041] Figure 4 The electron microscope images of the continuous oxide fiber three-dimensional fabric with a lanthanum phosphate interface layer prepared in Example 1 of the present invention at magnifications of 2000 and 5000; wherein (a) is a 2000-fold magnification image, and (b) is a 5000-fold magnification image.
[0042] Figure 5 This is the EDS element distribution diagram of the continuous oxide fiber three-dimensional fabric with a lanthanum phosphate interface layer prepared in Example 1 of the present invention.
[0043] Figure 6 The figures are electron microscope images of the continuous oxide fiber fabric with a lanthanum phosphate interface layer prepared in Example 2 of the present invention at magnifications of 2000 and 5000; wherein (a) is a magnified image at 2000 times, and (b) is a magnified image at 5000 times.
[0044] Figure 7 , Figure 8 This is an element distribution diagram of the continuous oxide fiber fabric with a lanthanum phosphate interface layer prepared in Example 2 of the present invention.
[0045] Fig. 9 The continuous oxide fiber fabric with a lanthanum phosphate interface layer prepared in Example 3 of the present invention is an electron microscope image at 3000 and 5000 magnifications; wherein (a) is a 3000-fold magnification image, and (b) is a 5000-fold magnification image. DETAILED DESCRIPTION
[0046] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0047] The present invention provides a method for preparing a continuous alumina fiber three-dimensional fabric with a lanthanum phosphate coating. The preparation method has an overall process as follows: Figure 1 The specific process is as shown in Figure 2 As shown, the following steps are included:
[0048] (1) pretreating the alumina fiber three-dimensional fabric to remove the wetting agent on the surface of the alumina fiber fabric;
[0049] (2) preparing an organic cationic polymer flocculant solution with a mass concentration of 0.5 to 5 wt%; and / or the pH of the organic cationic polymer flocculant solution is 6 to 8.
[0050] (3) Immersing the pretreated alumina fiber three-dimensional fabric in an organic cationic polymer flocculant solution and keeping the solution warm for 30 minutes to 2 hours.
[0051] (4) preparing a lanthanum phosphate precursor solution having a temperature not greater than 5° C.; in the present invention, the temperature of the lanthanum phosphate precursor solution before impregnation is maintained below 5° C., and the pH value may be between 6 and 8, preferably between 6 and 7.
[0052] (5) Under vacuum conditions and a temperature not exceeding 10°C, the lanthanum phosphate precursor solution is used to perform low-temperature vacuum impregnation on the alumina fiber three-dimensional fabric; in the present invention, the alumina three-dimensional fabric can be placed in a vacuum container with a feed port, and after the container is evacuated, the prepared lanthanum phosphate precursor solution is injected into the vacuum container using a pressure difference, so that the precursor solution completely infiltrates the alumina fiber three-dimensional fabric, and the vacuum impregnation is performed by keeping the temperature for 4 hours.
[0053] (6) The vacuum impregnated alumina fiber three-dimensional fabric is kept at 15 to 40°C (e.g., 20°C, 30°C or 40°C) for 1 to 2 hours (e.g., 1 hour, 1.5 hours or 2 hours), and then sequentially subjected to the steps of washing, drying and high-temperature treatment, thereby completing the interface modification of the alumina three-dimensional fabric; finally, the fabric is treated at 800 to 1000°C for 1 to 2 hours, and steps (5) and (6) are repeated to complete the preparation of the lanthanum phosphate interface on the fiber surface in the alumina fiber three-dimensional fabric.
[0054] The present invention proposes a simple method for interface modification of alumina fiber three-dimensional fabrics, which has low requirements on the required equipment, does not require complex equipment, does not require atmosphere protection, can be completed in an air atmosphere, and has a short preparation cycle, uses raw materials from a wide range of sources, has low cost, is simple to operate, and is safe and easy.
[0055] The present invention proposes a method for uniformly modifying the fiber interface of a three-dimensional alumina fiber fabric. Since the three-dimensional alumina fiber fabric has a certain thickness, when the lanthanum phosphate precursor solution diffuses to the vicinity of the fibers inside the fabric, it is affected by the steric hindrance of the surface fibers, making it easier for the surface fibers to generate an interface layer. Once the lanthanum phosphate precursor around the internal fibers is consumed, it is more difficult to replenish, so the interface of the fiber surface inside the fabric is more difficult to generate. The present invention first pre-treats the three-dimensional alumina fiber fabric with an organic cationic polymer flocculant, so that the surface of the fabric fiber adsorbs part of the organic cationic polymer flocculant and carries a positive charge, and then immerses the lanthanum phosphate precursor solution, and adjusts the pH value of the solution to make the precursor solution negatively charged. The lanthanum phosphate precursor solution can overcome the steric hindrance of the surface fibers through the attraction of positive and negative charges, so that there is a higher concentration of lanthanum ions around the fibers inside the fabric, thereby easily forming an interface layer of a certain thickness, effectively ensuring the uniformity of the interface modification of the fibers inside the fabric.
[0056] In the present invention, the lanthanum phosphate precursor solution is vacuum impregnated, and the temperature of the lanthanum phosphate precursor solution is controlled to be no more than 5°C, which can effectively ensure that the lanthanum phosphate precursor solution can still maintain a low viscosity for a long time and has good fluidity, which is conducive to the lanthanum phosphate precursor solution fully impregnating the pre-alumina three-dimensional fiber fabric under vacuum conditions. After high-temperature treatment, the lanthanum phosphate coating on the fiber surface can further remove crystal water and achieve better bonding with the fiber.
[0057] The lanthanum phosphate interface layer prepared by the present invention has good high-temperature oxidation resistance, and at the same time has good physical and chemical compatibility with alumina fibers, does not react with alumina fibers at high temperatures, and uses lanthanum phosphate for the interface phase of the oxide composite material, which can produce a weak bond between the alumina fibers and the matrix, thereby preventing the continuous oxide fiber fabric from brittle fracture along with the matrix. Therefore, the alumina fiber reinforced alumina composite material prepared by using alumina fiber three-dimensional fabric after lanthanum phosphate interface modification has the advantages of high temperature resistance, oxidation resistance, high strength and good toughness, and still has a high strength retention rate after long-term high-temperature treatment.
[0058] According to some preferred embodiments, the organic cationic polymer flocculant is at least one selected from polydimethyldiallylammonium chloride (PADAMA) and polyethyleneimine (PEI).
[0059] According to some preferred embodiments, the mass concentration of the organic cationic polymer flocculant solution (e.g., organic cationic polymer flocculant aqueous solution) is 0.5-5wt% (e.g., 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%). In the present invention, the mass concentration of the organic cationic polymer flocculant solution refers to the mass fraction of the organic cationic polymer flocculant contained in the organic cationic polymer flocculant solution; and / or the pH of the organic cationic polymer flocculant solution is 6-8. In the present invention, the mass concentration of the organic cationic polymer flocculant is preferably 2-4wt%, because at this concentration, the viscosity of the polymer solution is relatively small, which is conducive to the diffusion of the organic cationic polymer flocculant solution in the fabric. At the same time, the concentration of the organic cationic polymer flocculant is moderate, which can ensure that the fiber surface polymer modification is relatively sufficient.
[0060] According to some preferred embodiments, the preparation of the lanthanum phosphate precursor solution comprises the following steps:
[0061] (a) preparing a lanthanum ion aqueous solution at a temperature not greater than 5° C., then adding citric acid or ethylenediaminetetraacetic acid (EDTA) to the lanthanum ion aqueous solution, and adjusting the pH of the lanthanum ion aqueous solution to 6-8 after complete dissolution, to obtain a lanthanum ion solution (lanthanum ion low-temperature solution) at a temperature not greater than 5° C.; in the present invention, the addition of citric acid or EDTA can effectively prevent the solution from reacting too quickly to form a macroscopic precipitate of lanthanum phosphate; in the present invention, the pH of the lanthanum ion aqueous solution can be adjusted with an inorganic acid or an inorganic base;
[0062] (b) preparing a phosphate-containing aqueous solution at a temperature not greater than 5° C., and adjusting the pH of the phosphate-containing aqueous solution to 6-8, to obtain a phosphate ion solution (phosphate ion low-temperature solution) at a temperature not greater than 5° C.; in the present invention, the pH of the phosphate-containing aqueous solution may be adjusted with an inorganic acid or alkali;
[0063] (c) mixing the lanthanum ion solution and the phosphate ion solution in a molar ratio of lanthanum (La) to phosphorus (P) of 1:1 to obtain the lanthanum phosphate precursor solution (LaPO4 precursor solution).
[0064] According to some preferred embodiments, the lanthanum ion-containing aqueous solution is prepared using lanthanum nitrate, lanthanum chloride or other lanthanum salts that are easily soluble in water.
[0065] According to some preferred embodiments, the phosphate-containing aqueous solution is prepared using phosphoric acid, water-soluble hydrogen phosphate, water-soluble dihydrogen phosphate or water-soluble phosphate.
[0066] According to some preferred embodiments, the pH of the lanthanum ion-containing aqueous solution and / or the phosphate-containing aqueous solution is adjusted using common inorganic acids or bases such as ammonia water, hydrochloric acid, nitric acid or sodium hydroxide; and / or the pH of the lanthanum ion-containing aqueous solution and / or the phosphate-containing aqueous solution is adjusted to about 6 to 8.
[0067] According to some preferred embodiments, the molar ratio of the lanthanum ions contained in the lanthanum ion-containing aqueous solution to the citric acid is 1:(1-2); and / or the lanthanum ion concentration contained in the lanthanum ion solution and / or the phosphate ion concentration contained in the phosphate ion solution is not less than 0.4 mol / L. In the present invention, it is preferred that the lanthanum ion concentration contained in the lanthanum ion solution and / or the phosphate ion concentration contained in the phosphate ion solution is not less than 0.4 mol / L, so as to reduce the number of times the fiber fabric is impregnated.
[0068] According to some preferred embodiments, the structural form of the alumina fiber three-dimensional fabric includes but is not limited to a three-dimensional orthogonal structure, a needle-punched structure, a stitched structure and a 2.5D structure, and the volume fraction of the contained fibers is 20% to 50%.
[0069] According to some preferred embodiments, in step (1), the method for pretreating the alumina fiber is: washing the fabric with acetone at least three times; or the method for high-temperature sintering is: sintering the fabric at a temperature of 500-1000°C for 1-3h, and after removing the wetting agent, the wetting agent content of the fabric is less than 1%.
[0070] According to some preferred embodiments, in step (2), the organic cationic polymer flocculant solution uses polydimethyldiallylammonium chloride (PADAMA) with a mass concentration of 1-5% and a pH of 6-7.
[0071] According to some preferred embodiments, in step (5), the vacuum impregnation is carried out under vacuum and at a temperature of 0 to 10°C, and the time for the vacuum impregnation is not less than 2 hours, preferably 2 to 4 hours (e.g. 2, 3 or 4 hours); of course, in the present invention, vacuum impregnation can also be carried out under vacuum and below 0°C, but additional low-temperature equipment is required to maintain it.
[0072] According to some preferred embodiments, in step (6), the insulation temperature of the vacuum impregnated alumina fiber three-dimensional fabric is 20-40°C, and the insulation time is 1-2 hours; finally, the fabric is treated at 800-1000°C for 1-2 hours, preferably, the temperature of the high temperature treatment is 900°C, and the insulation time is 1 hour.
[0073] According to some specific embodiments, the method for preparing the lanthanum phosphate interface of the alumina fiber three-dimensional fabric of the present invention can be achieved by the following steps:
[0074] In the first step, the alumina fiber three-dimensional fabric is pretreated to remove the wetting agent on the surface of the alumina fiber fabric.
[0075] The fabric is cleaned three times with acetone at room temperature; or the fabric is sintered at high temperature for 1 hour at 500-600°C.
[0076] In the second step, the alumina fiber three-dimensional fabric is pretreated using an organic cationic polymer flocculant.
[0077] A polydimethyldiallylammonium chloride (PADAMA) aqueous solution with a mass fraction of 2-4 wt% is prepared, and the pretreated continuous alumina fiber fabric is immersed in the mixed solution, and is placed at room temperature for 30 minutes to 2 hours and then dried.
[0078] The third step is to prepare a low-temperature lanthanum phosphate precursor solution.
[0079] The lanthanum phosphate precursor solution is prepared by mixing lanthanum ions and phosphate ions at a low temperature below 5° C. The pH value of the lanthanum ion and phosphate ion solution before mixing is 6 to 8, and the molar ratio of lanthanum element to phosphorus element during mixing is preferably 1:1.
[0080] The aqueous solution containing lanthanum ions is prepared by using lanthanum nitrate, lanthanum chloride or other lanthanum salts that are easily soluble in water, and the concentration of the solution is preferably above 0.4 mol / L. The molar ratio of lanthanum ions to citric acid is 1:(1-2), and the pH of the solution is adjusted by using common inorganic acids or bases such as ammonia, hydrochloric acid, nitric acid or sodium hydroxide, and the final value is 6-8.
[0081] The aqueous solution containing phosphate ions is prepared using phosphoric acid, water-soluble hydrogen phosphate, dihydrogen phosphate or phosphate. The pH of the solution is adjusted using common inorganic acids or bases such as ammonia water, hydrochloric acid, nitric acid or sodium hydroxide, and the final value is 6 to 8. The concentration of phosphorus is preferably above 0.4 mol / L, and the mixing temperature of the two is below 5°C.
[0082] In the fourth step, the lanthanum phosphate precursor solution is vacuum impregnated into the alumina fiber three-dimensional fabric.
[0083] The alumina fiber three-dimensional fabric is placed in a vacuum container, and the lanthanum phosphate precursor solution is filled into the vacuum container under vacuum conditions to ensure that the fiber bundle inside the fiber can be fully impregnated by the solution, and the impregnation temperature is kept below 5°C for 2 to 4 hours. The fabric is then taken out, kept warm at 20 to 40°C for 1 to 2 hours, soaked and cleaned with a large amount of clean water, and dried at 80 to 100°C for 1 to 2 hours.
[0084] The fifth step is to high-temperature treat the impregnated alumina fiber three-dimensional fabric, and repeat the vacuum impregnation and high-temperature treatment process to obtain the alumina fiber three-dimensional fabric containing lanthanum phosphate coating.
[0085] The alumina fiber three-dimensional fabric impregnated with the lanthanum superphosphate precursor solution was treated at 900-1000° C. for 1 hour in an air atmosphere.
[0086] In a second aspect, the present invention provides a continuous alumina fiber three-dimensional fabric with a lanthanum phosphate layer, and the continuous alumina fiber three-dimensional fabric with a lanthanum phosphate coating is obtained by the preparation method provided by the present invention.
[0087] In a third aspect, the present invention provides an application of a continuous alumina fiber three-dimensional fabric with a lanthanum phosphate coating, including using the continuous oxide fiber fabric with a lanthanum phosphate coating to prepare an oxide ceramic-based composite material, a high-strength oxide ceramic-based composite material with excellent high-temperature oxidation resistance and toughness, and can be applied to the field of aerospace thermal structures.
[0088] The technical solutions in the present invention are clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0089] Embodiment 1:
[0090] (1) placing a continuous alumina fiber three-dimensional fabric (fiber volume fraction 30%) in a methane fluorine furnace at 600° C. for 1 h to remove the surface sizing agent and set aside;
[0091] (2) preparing a polydimethyldiallyl ammonium chloride (PADAMA) aqueous solution with a mass fraction of 3% and a pH of 6, and then immersing 5 g of the pretreated continuous alumina fiber three-dimensional fabric in the mixed solution at room temperature (25° C.) for 1 hour to obtain a polydimethyldiallyl ammonium chloride pretreated alumina fiber three-dimensional fabric;
[0092] (3) preparing a lanthanum nitrate hexahydrate solution at a concentration of 0.4 mol / L, a citric acid concentration of 0.8 mol / L, adjusting the pH value of the solution to 6 with concentrated ammonia water, placing the solution in an ice-water mixture, and maintaining the temperature below 5° C. to obtain a lanthanum ion solution; preparing an aqueous solution of phosphoric acid at a concentration of 0.4 mol / L, adjusting the pH value of the solution to 6 with concentrated ammonia water, placing the solution in an ice-water mixture, and maintaining the temperature below 5° C. to obtain a phosphate ion solution; mixing the above solutions containing lanthanum ions and phosphate ions in equal volumes at below 5° C. to obtain a lanthanum phosphate precursor solution;
[0093] (4) placing the alumina fiber three-dimensional fabric pretreated with polydimethyldiallylammonium chloride in a vacuum container, maintaining the temperature below 5°C, and quickly injecting the lanthanum phosphate precursor solution into the container after vacuuming until the container is filled, and vacuum impregnating for 2 hours;
[0094] (5) taking the impregnated alumina fiber three-dimensional fabric out of the vacuum container, keeping it at 30°C for 1.5 hours, then soaking and washing it with a large amount of clean water for more than 5 times, and drying it at 80°C for 1 hour;
[0095] (6) The dried alumina fiber three-dimensional fabric is subjected to high temperature treatment at 900°C in an air atmosphere for 1 hour to obtain an alumina fiber three-dimensional fabric containing a lanthanum phosphate interface.
[0096] (7) Repeat steps (4)-(6) three times to obtain a three-dimensional fabric of alumina fibers containing a lanthanum phosphate interface.
[0097] Figure 3 is a physical picture of a continuous oxide fiber three-dimensional fabric with a lanthanum phosphate interface layer prepared in Example 1 of the present invention;
[0098] Figure 4 are electron microscope images of the continuous oxide fiber three-dimensional fabric with a lanthanum phosphate interface layer prepared in Example 1 of the present invention at magnifications of 2000 and 5000;
[0099] Figure 5 This is an element distribution diagram of the continuous oxide fiber three-dimensional fabric with a lanthanum phosphate interface layer prepared in Example 1 of the present invention.
[0100] Embodiment 2:
[0101] (1) The continuous alumina fiber three-dimensional fabric (fiber volume fraction 30%) was washed with acetone three times at room temperature (25°C) to remove the surface sizing agent;
[0102] (2) preparing a polyethyleneimine (PEI) aqueous solution with a mass fraction of 5% and a pH of 6.5, and then immersing 5 g of the pretreated continuous alumina fiber three-dimensional fabric in the mixed solution at room temperature (25° C.) for 1.5 h to obtain a polyethyleneimine pretreated alumina fiber three-dimensional fabric;
[0103] (3) preparing a lanthanum nitrate hexahydrate solution at a concentration of 0.4 mol / L, a citric acid concentration of 0.6 mol / L, adjusting the pH value of the solution to 6.5 with concentrated ammonia water, placing the solution in an ice-water mixture, and maintaining the temperature at about 1° C. to obtain a lanthanum ion solution; preparing an aqueous solution of phosphoric acid at a concentration of 0.4 mol / L, adjusting the pH value of the solution to 6.5 with concentrated ammonia water, placing the solution in an ice-water mixture, and maintaining the temperature at about 1° C. to obtain a phosphate ion solution; mixing the above solutions containing lanthanum ions and phosphate ions at equal volumes at 1° C. to obtain a lanthanum phosphate precursor solution;
[0104] (4) placing the three-dimensional alumina fiber fabric pretreated with polyethyleneimine in a vacuum container, maintaining the temperature at 1°C, and quickly injecting the lanthanum phosphate precursor solution into the container after vacuuming until the container is filled, and vacuum impregnating for 3 hours;
[0105] (5) taking the impregnated alumina fiber three-dimensional fabric out of the vacuum container, keeping it at 25°C for 2 hours, then soaking and washing it with a large amount of clean water for more than 5 times, and drying it at 80°C for 2 hours;
[0106] (6) The dried alumina fiber three-dimensional fabric was subjected to high temperature treatment at 950°C in an air atmosphere for 1.5 h.
[0107] (7) Repeat steps (4)-(6) three times to obtain a three-dimensional fabric of alumina fibers containing a lanthanum phosphate interface layer.
[0108] Figure 6 are electron microscope images of the continuous oxide fiber fabric with a lanthanum phosphate interface layer prepared in Example 2 of the present invention at magnifications of 2000 and 5000;
[0109] Figure 7 , Figure 8 This is an element distribution diagram of the continuous oxide fiber fabric with a lanthanum phosphate interface layer prepared in Example 2 of the present invention.
[0110] Depend on Figure 7 It can be seen that a large amount of Al, Si, La, P, O and other related elements can be detected on the surface of the fiber sample after the LaPO4 interface is deposited, and each element is evenly distributed on the fiber surface without any element enrichment phenomenon. This also proves that the LaPO4 coating has good coverage on the fiber surface and is continuously and evenly distributed.
[0111] Table 1. EDS element distribution table of continuous oxide fiber fabric with lanthanum phosphate interface layer prepared in Example 2 of the present invention
[0112] element Wt% At% O 32.03 64.65 Al 11.09 13.26 Si 10.23 1.18 P 9.80 10.21 La 46.06 10.70 Total amount: 100.00 100.00
[0113] In order to investigate whether there are LaPO4 related elements on the fiber surface, EDS energy spectrum analysis was performed. Figure 8 The element distribution results in Table 1 are consistent with the composition of alumina fibers: Al2O3 and SiO2, and the element composition of the interface layer LaPO4, and the element content is roughly consistent with the chemical element dosage ratio of lanthanum phosphate, which further confirms the presence of LaPO4 on the fiber surface.
[0114] Embodiment 3:
[0115] (1) The continuous alumina fiber three-dimensional fabric (fiber volume fraction 30%) was treated at 500°C for 1 h to remove the surface sizing agent;
[0116] (2) preparing a polyethyleneimine (PEI) aqueous solution with a mass fraction of 3% and a pH of 7.5, and then immersing 5 g of the pretreated continuous alumina fiber three-dimensional fabric in the mixed solution at room temperature (25° C.) for 2.5 hours to obtain a polyethyleneimine pretreated alumina fiber three-dimensional fabric;
[0117] (3) preparing a lanthanum nitrate hexahydrate solution at a concentration of 0.6 mol / L, a citric acid concentration of 0.6 mol / L, adjusting the pH value of the solution to 7.5 with concentrated ammonia water, placing the solution in an ice-water mixture, and maintaining the temperature at about 3° C. to obtain a lanthanum ion solution; preparing an aqueous solution of phosphoric acid at a concentration of 0.6 mol / L, adjusting the pH value of the solution to 7.5 with concentrated ammonia water, placing the solution in an ice-water mixture, and maintaining the temperature at about 3° C. to obtain a phosphate ion solution; mixing the above solutions containing lanthanum ions and phosphate ions at equal volumes at 3° C. to obtain a lanthanum phosphate precursor solution;
[0118] (4) placing the three-dimensional alumina fiber fabric pretreated with polyethyleneimine in a vacuum container, maintaining the temperature at 3°C, and quickly injecting the lanthanum phosphate precursor solution into the container after vacuuming until the container is filled, and vacuum impregnating for 3 hours;
[0119] (5) taking the impregnated alumina fiber three-dimensional fabric out of the vacuum container, keeping it at 30°C for 2.5 hours, then soaking and washing it with a large amount of clean water for more than 5 times, and drying it at 100°C for 2 hours;
[0120] (6) The dried alumina fiber three-dimensional fabric is subjected to high temperature treatment at 1000° C. in an air atmosphere for 1 h to obtain an alumina fiber three-dimensional fabric containing a lanthanum phosphate interface.
[0121] (7) Repeat steps (4)-(6) three times to obtain a three-dimensional fabric of alumina fibers containing a lanthanum phosphate interface.
[0122] Fig. 9 It is an electron microscope picture of the continuous oxide fiber fabric with a lanthanum phosphate interface layer prepared in Example 3 of the present invention at magnifications of 3000 and 5000.
[0123] Finally, it is noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, it should be understood by those skilled in the art that the technical solutions described in the embodiments may still be modified, or some of the technical features therein may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a three-dimensional fabric of alumina fibers containing a lanthanum phosphate coating, characterized in that: The preparation method comprises the following steps: Treating the continuous alumina fiber three-dimensional fabric to remove the wetting agent on the surface of the continuous alumina fiber; The surface of the aluminum oxide fiber three-dimensional fabric is treated with an organic cationic polymer flocculant to obtain an aluminum oxide fiber three-dimensional fabric with a positive charge on the surface; the mass concentration of the organic cationic polymer flocculant is 2-4wt%; the pH of the organic cationic polymer flocculant solution is 6-8; preparing a negatively charged lanthanum phosphate precursor solution; The negatively charged lanthanum phosphate precursor solution is used to vacuum impregnate the three-dimensional alumina fiber fabric with positive charges on the surface, so that the lanthanum phosphate precursor solution overcomes the steric hindrance of the surface fibers through the attraction of positive and negative charges, so that an interface layer of a certain thickness is formed around the fibers inside the fabric; The vacuum impregnated alumina fiber three-dimensional fabric is subjected to a heating treatment, and then subjected to the steps of washing, drying, and high-temperature treatment to obtain a continuous alumina fiber three-dimensional fabric with a lanthanum phosphate coating; The preparation of the negatively charged lanthanum phosphate precursor solution comprises the following steps: An aqueous solution containing lanthanum ions is prepared, and then a reaction rate regulator citric acid is added to the aqueous solution containing lanthanum ions, and then the pH of the aqueous solution containing lanthanum ions is adjusted to 6 to 8 to obtain a lanthanum ion solution; the molar ratio of the lanthanum ions contained in the aqueous solution containing lanthanum ions to the citric acid is 1:(1 to 5); preparing an aqueous solution containing phosphate ions, and then adjusting the pH of the aqueous solution containing phosphate ions to 6 to 8 to obtain a phosphate ion solution; The temperature of the lanthanum ion solution and the phosphate ion solution is lowered to no greater than 5° C., and then mixed in a molar ratio of lanthanum to phosphorus of 1:1 to obtain the negatively charged lanthanum phosphate precursor solution; The organic cationic polymer flocculant contained in the organic cationic polymer flocculant solution is at least one selected from polydimethyldiallylammonium chloride and polyethyleneimine; Under the conditions of vacuum and temperature of 0-10°C, the vacuum impregnation is carried out for no less than 2 hours; and / or the temperature of the heating treatment is not higher than 40°C and the time is 1 hour to 2 hours; and / or the temperature of the high temperature treatment is 800-1000°C and the insulation time is 1 to 2 hours.
2. The method according to claim 1, characterized in that: The steps of vacuum impregnation, heating treatment at elevated temperature, cleaning, drying and high temperature treatment are repeated multiple times to obtain a lanthanum phosphate coating with a certain thickness.
3. The method according to claim 1, characterized in that: The aqueous solution containing lanthanum ions is prepared by using at least one of lanthanum nitrate, lanthanum carbonate, lanthanum chloride, lanthanum hydroxide, and lanthanum oxide, and the concentration of lanthanum ions in the mixed solution obtained by mixing is 0.4 to 1 mol / L; the aqueous solution containing phosphate ions is at least one of phosphoric acid, a water-soluble hydrogen phosphate solution, a water-soluble dihydrogen phosphate solution, or a water-soluble phosphate solution, and the concentration of phosphate ions in the mixed solution obtained by mixing is 0.4 to 1 mol / L.
4. The method according to claim 1, characterized in that: The pH of the lanthanum ion-containing aqueous solution and / or the phosphate-containing aqueous solution is adjusted using ammonia water, urea, hydrochloric acid, nitric acid or sodium hydroxide.
5. A three-dimensional fabric of alumina fibers containing a lanthanum phosphate coating, characterized in that: The method according to any one of claims 1 to 4 is used to prepare the present invention.
6. The use of the three-dimensional alumina fiber fabric containing a lanthanum phosphate coating according to claim 5, characterized in that: The three-dimensional alumina fiber fabric with lanthanum phosphate coating is used to prepare oxide ceramic-based composite materials.
Citation Information
Cited By
Preparation method and application of flexible high-emissivity coating on surface of continuous alumina fiber fabric