A polyurethane modified silicone softener and its preparation method and application

Through the preparation method of polyurethane modified silicone softener, the problem of intimate bonding of silicone softener and fabric is solved. Through block copolymerization technology and high-temperature baking, the softness, hydrophilicity and water-resistant performance of cotton fabrics are improved. , achieving better mechanical properties.

CN115787301BActive Publication Date: 2024-11-19HANGZHOU TRANSFAR FINE CHEM CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211446589.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-18
Publication Date
2024-11-19
Estimated Expiration
2042-11-18

AI Technical Summary

Technical Problem

The existing silicone softeners do not bind closely to the fabric and lack groups that continue to react with the active groups on the fabric, resulting in poor washing resistance and insufficient mechanical properties.

Method used

The preparation method of polyurethane modified silicone softener is adopted. The polymerization of isophorone diisocyanate with N-methyldiethanolamine is made by adding the blocking agent and reacting with end epoxy silicone oil and polyetheramine to form a block copolymer and combine it. Emulsifier emulsifies to produce polyurethane modified silicone softener, and is applied to cotton fabrics through a padding process, and bakes at high temperatures to enhance bonding.

Benefits of technology

It improves the bonding density between softener and fabric, enhances the softness, hydrophilicity, water-resistant and resilience of the fabric, and has better performance than original fabrics and commercially available softener.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115787301B_ABST
    Figure CN115787301B_ABST
Patent Text Reader

Abstract

The present invention provides a polyurethane modified silicone softener and a preparation method and application thereof, belonging to the field of textile printing and dyeing finishing, and the preparation method comprises the following steps: isophorone diisocyanate and N-methyldiethanolamine are subjected to polymerization reaction in a first organic solvent, and then a sealing agent is added to seal the remaining active isocyanate to obtain a polyurethane prepolymer; under the action of an acidic catalyst, the obtained polyurethane prepolymer and terminal epoxy silicone oil are subjected to polymerization reaction in a second organic solvent to obtain a polyurethane silicone oil component; the terminal epoxy silicone oil and polyether amine are reacted in a second organic solvent to obtain a block silicone oil component; the obtained polyurethane silicone oil component and the block silicone oil component are compounded according to a preset ratio, and then an emulsifier is added for emulsification, and finally a polyurethane modified silicone softener is obtained. The polyurethane modified silicone softener prepared by the method provided by the present invention can further increase the polymer molecular weight and combine the softener and the fabric more closely.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of textile printing and dyeing finishing, and more specifically, relates to a polyurethane modified organic silicon softener and a preparation method and application thereof. Background Art

[0002] Silicone softener is one of the most popular softeners in the field of textile printing and dyeing finishing. It can make the fabric have a silky or cotton-like feel after finishing. How to further improve the performance of silicone softener has always been the focus of attention of technicians in the printing and dyeing industry.

[0003] After in-depth research on silicone polymers by researchers in recent years, the preparation technology of ternary block silicone oil has become highly mature. Ternary block silicone oil softener introduces polyether segments and amino groups into the silicone structure at the same time. Among them, the polyether segment gives the silicone oil emulsion excellent stability, adapts to various processing procedures, and adheres to the surface of the fabric after finishing, giving the fabric good hydrophilicity; the amino group has weak cationicity after acidification, and can form directional adsorption on the surface of the fabric, giving the fabric a good feel. However, there are also some shortcomings, such as the combination of softener and fabric only relies on electrostatic adsorption, resulting in poor washability; silicone itself is relatively soft and has poor mechanical properties, resulting in poor resilience and smoothness of the fabric. Polyurethane has many special properties, such as good mechanical properties, strong flexibility, good weather resistance and strong adhesion. More and more researchers have begun to introduce polyurethane into silicone to synthesize polyurethane-silicone block copolymers with various properties.

[0004] Regarding polyurethane modified silicone softener, CN111171267B discloses a highly elastic resin modified silicone oil and a preparation method thereof. The technical scheme specifically comprises the following steps: firstly preparing a polyurethane resin capable of reacting with epoxy silicone oil, and then continuing to perform ring-opening polymerization with epoxy silicone oil to prepare a highly elastic resin modified silicone oil, which is then applied to fabrics to improve the resilience and smoothness of the fabrics. However, the molecular chain contains only quaternary ammonium groups and carbamate groups, and does not contain other active groups. Directional adsorption can only be produced on the fabrics through the electrostatic adsorption of quaternary ammonium salts and the hydrogen bonding effect formed by carbamates, and the softener cannot be more closely bonded to the fabrics. CN110527052A discloses a polyurethane modified silicone copolymer containing quaternary ammonium salt. The technical scheme is as follows: first, epoxy silicone oil reacts with a tertiary amine compound to prepare silicone oil with a quaternary ammonium structure, then diisocyanate is added to continue to react with the silicone oil, and finally the remaining isocyanate is blocked with polyether or the like to obtain a copolymer, which is then applied to fabric to give the fabric good hydrophilicity and hand feel. However, the copolymer does not contain a group that can continue to react with an active group on the fabric, and still cannot meet the market demand for cotton fabric finishing. Summary of the invention

[0005] In view of the defects of the prior art, the purpose of the present invention is to provide a polyurethane modified silicone softener and a preparation method and application thereof, aiming to solve the problem that the existing softener is not tightly combined with the fabric and does not contain groups that continue to react with the active groups on the fabric.

[0006] To achieve the above object, the present invention provides a method for preparing a polyurethane modified silicone softener, the preparation method comprising the following steps:

[0007] S1: polymerizing isophorone diisocyanate and N-methyldiethanolamine in a first organic solvent, and then adding a blocking agent to block the remaining active isocyanate to obtain a polyurethane prepolymer;

[0008] S2, polymerizing the polyurethane prepolymer obtained in step S1 with the epoxy-terminated silicone oil in a second organic solvent under the action of an acidic catalyst to obtain a polyurethane silicone oil component;

[0009] S3 reacting the terminal epoxy silicone oil with the polyether amine in a second organic solvent to obtain a block silicone oil component;

[0010] S4: compounding the polyurethane silicone oil component obtained in step S2 and the block silicone oil component obtained in step S3 according to a preset ratio, then adding an emulsifier for emulsification, and finally obtaining the polyurethane modified silicone softener.

[0011] As further preferred, step S1 includes the following sub-steps:

[0012] S11: adding isophorone diisocyanate and N-methyldiethanolamine into a first organic solvent in a molar ratio of 3:2 or 2:1, wherein the N-methyldiethanolamine is added dropwise for 15 to 180 minutes, and the mass of the first organic solvent is 10% to 80% of the total mass of the isophorone diisocyanate and the N-methyldiethanolamine;

[0013] S12 is stirred at 30-70°C for 2-8h to allow polymerization to occur;

[0014] S13 After the polymerization reaction is completed, the reaction temperature is maintained at 40 to 80° C., and a blocking agent is added to block the remaining active isocyanate, wherein the molar ratio of the blocking agent to the remaining active isocyanate is 1.05:1 to 1.2:1;

[0015] S14 continues to react for 2 to 6 hours. After infrared detection shows no isocyanate peak, the first organic solvent is removed by vacuum distillation and then a second organic solvent is added for dilution to obtain a polyurethane prepolymer.

[0016] As further preferred, step S2 includes the following sub-steps:

[0017] S21: adding a polyurethane prepolymer and an epoxy-terminated silicone oil into a second organic solvent at a molar ratio of epoxy value to amine value of 1:1 to 1:2, and simultaneously adding an acidic catalyst having a molar number of 100% to 200% of the amine value in the polyurethane prepolymer;

[0018] S22 is stirred and reacted at a temperature of 60 to 120° C. for 4 to 24 hours, and then the second organic solvent is removed by vacuum to obtain the polyurethane silicone oil component.

[0019] As further preferred, step S3 includes the following sub-steps:

[0020] S31: adding the terminal epoxy silicone oil and the polyether amine into a second organic solvent at a molar ratio of epoxy value to amine value of 1:1 to 1:2;

[0021] S32 is stirred to react at a temperature of 60 to 120° C. for 6 to 24 hours, and then the second organic solvent is removed by vacuum to obtain the block silicone oil component.

[0022] As further preferred, in step S1, the blocking agent is one or more of butanone oxime, phenol, sodium bisulfite, caprolactam, acetylacetone and diethyl malonate; in step S2, the acidic catalyst is one or more of formic acid, acetic acid, dilute hydrochloric acid, lauric acid and citric acid; in step S3, the polyetheramine is one or more of polyetheramine ED600, polyetheramine ED900, polyetheramine ED2003 and polyetheramine T403.

[0023] As further preferred, in step S4, the polyurethane silicone oil component and the block silicone oil component are compounded in a mass ratio of 2:1 to 1:1.

[0024] As further preferred, the first organic solvent is one or more of acetone, butanone and tetrahydrofuran, and the second organic solvent is one or more of diethylene glycol butyl ether, ethylene glycol butyl ether, dipropylene glycol butyl ether, dipropylene glycol, propylene glycol acetate and isopropanol.

[0025] As further preferred, the emulsifier is a compound of isomeric tridecanol polyoxyethylene ethers with different EO addition numbers, and its HLB value is 4-18.

[0026] According to another aspect of the present invention, a polyurethane-modified silicone softener prepared by the above method is provided.

[0027] According to another aspect of the present invention, there is provided an application of the above-mentioned polyurethane modified silicone softener in cotton fabrics, specifically: applying the polyurethane modified organic solvent to the cotton fabric, using a dipping and padding process, and then pre-baking at 90 to 110° C. for 30 to 90 seconds, and finally baking at 160 to 170° C. for 30 to 120 seconds.

[0028] In general, the above technical solution conceived by the present invention has the following beneficial effects compared with the prior art:

[0029] 1. The polyurethane modified silicone softener provided by the present invention is composed of a polyurethane silicone oil component and a block silicone oil component, both of which are synthesized by block copolymerization technology, so there are no problems such as poor compatibility between polyurethane and silicone and phase separation. Among them, the molecular structure of the polyurethane silicone oil component is regular and controllable, and can be freely controlled by the molar ratio of the polyurethane prepolymer and the terminal epoxy silicone oil. Its molecular chain contains not only carbamate groups and quaternary ammonium salt groups, but also blocked active isocyanate groups on the sides of the molecular chain; the block silicone oil component is mainly composed of amino, polyether and siloxane segments, and the molecular chain contains A large number of active amino groups can be prepared into linear or network block silicone oil according to the polyetheramine structure; when the polyurethane modified silicone softener is applied to cotton fabric by padding, the quaternary ammonium salt group in the polyurethane silicone oil component provides cationicity and hydrophilicity, and the carbamate group provides the characteristics of polyurethane, which produces microphase separation with the silicone segment. After the active isocyanate group blocked on the side chain is unblocked by high-temperature baking, it can undergo in-situ cross-linking reaction with the amino group in the block silicone oil component and the hydroxyl group on the cotton fabric and other active hydrogen-containing groups, further increasing the polymer molecular weight and combining the softener and the fabric more closely;

[0030] 2. At the same time, the present invention optimizes the molar ratio of isophorone diisocyanate to N-methyldiethanolamine, thereby ensuring that the reaction of the polyurethane prepolymer and epoxy silicone oil is controllable and the structure is regular, thereby avoiding the generation of gel in the subsequent polymerization process;

[0031] 3. In addition, the present invention also optimizes the molar ratio of the polyurethane prepolymer to the epoxy-terminated silicone oil, which can avoid the free polyurethane prepolymer in the polyurethane silicone oil component and prevent the polyurethane silicone oil component from being terminated with epoxy groups, which is not conducive to the compounding stability with the block silicone oil component in the next step;

[0032] 4. The polyurethane modified silicone softener prepared by the present invention is applied to cotton fabrics, which can give the fabrics functions such as softness, good hydrophilicity, water resistance and good resilience, and the application performance is better than that of the original fabric and commercially available softeners. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a flow chart of the preparation of a polyurethane modified silicone softener provided by a preferred embodiment of the present invention;

[0034] Figure 2 is the infrared spectrum of the polyurethane prepolymer prepared in Example 1 of the present invention;

[0035] Figure 3 This is the infrared spectrum of the polyurethane silicone oil component prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0037] like Figure 1 As shown, the present invention provides a method for preparing a polyurethane modified silicone softener, the preparation method comprising the following steps:

[0038] S1: polymerizing isophorone diisocyanate and N-methyldiethanolamine in a first organic solvent, and then adding a blocking agent to block the remaining active isocyanate to obtain a polyurethane prepolymer that can react with epoxy;

[0039] S2, polymerizing the polyurethane prepolymer prepared in step S1 with the epoxy-terminated silicone oil in a second organic solvent under the action of an acidic catalyst to obtain a polyurethane silicone oil component;

[0040] S3 reacting the terminal epoxy silicone oil with the polyether amine in a second organic solvent to obtain a block silicone oil component;

[0041] S4: compounding the polyurethane silicone oil component obtained in step S2 and the block silicone oil component obtained in step S3 according to a preset ratio, and then adding an emulsifier for emulsification to finally obtain a polyurethane modified silicone softener.

[0042] The synthetic route of the polyurethane modified silicone softener provided by the present invention is as follows:

[0043] (1) Synthesis of polyurethane prepolymer:

[0044]

[0045] Isophorone diisocyanate and N-methyldiethanolamine are added in a molar ratio of 3:2 or 2:1 in a first organic solvent for polymerization reaction, and then a blocking agent is added to block the remaining active isocyanate, and after infrared detection shows no characteristic peak of isocyanate, the first organic solvent is removed by vacuum distillation, and then an appropriate amount of a second organic solvent is added for dilution to obtain a polyurethane prepolymer;

[0046] (2) Synthetic polyurethane silicone oil component:

[0047]

[0048] The polyurethane prepolymer is acidified by an acid catalyst, and then polymerized with the terminal epoxy silicone oil in a second organic solvent. After the reaction is completed, the second organic solvent is removed by distillation under reduced pressure to obtain a polyurethane silicone oil component.

[0049] (3) Synthetic block silicone oil component:

[0050]

[0051]

[0052] The terminal epoxy silicone oil and the polyetheramine are polymerized in a second organic solvent in a molar ratio of 1:1 to 1:2, and after the reaction is completed, the second organic solvent is removed by vacuum distillation to obtain a block silicone oil component, i.e., block silicone oil;

[0053] (4) The polyurethane silicone oil component and the block silicone oil component are compounded in a mass ratio of 2:1 to 1:1, and then an emulsifier is added for emulsification to obtain a polyurethane modified silicone softener.

[0054] Further, step S1 includes the following sub-steps:

[0055] S11: adding isophorone diisocyanate and N-methyldiethanolamine in a molar ratio of 3:2 or 2:1 into a first organic solvent to ensure that the polyurethane prepolymer contains two or one tertiary amine groups that can react with epoxy, so that the reaction with epoxy silicone oil is controllable and the structure is regular, thereby avoiding the generation of gel in the subsequent polymerization process. At the same time, N-methyldiethanolamine is added dropwise for 15 to 180 minutes, thereby effectively controlling the polymerization reaction rate and avoiding too fast reaction and reaction failure caused by large amount of heat release. The mass of the first organic solvent is 10% to 80% of the total mass of isophorone diisocyanate and N-methyldiethanolamine.

[0056] S12 is stirred at 30-70°C for 2-8h to allow polymerization to occur;

[0057] S13 After the polymerization reaction is completed, the reaction temperature is maintained at 40-80° C., and a blocking agent is added to block the remaining active isocyanate. The molar ratio of the blocking agent to the remaining active isocyanate is 1.05:1-1.2:1, so as to prevent the isocyanate from reacting with other substances containing active hydrogen too early and ensure that the isocyanate is unblocked during the finishing process of the fabric sample. The blocking agent is one or more of butanone oxime, phenol, sodium bisulfite, caprolactam, acetylacetone and diethyl malonate;

[0058] S14 continues to react for 2 to 6 hours. After infrared detection shows no isocyanate peak, the first organic solvent is removed by vacuum distillation and then an appropriate amount of a second organic solvent is added for dilution to obtain a polyurethane prepolymer.

[0059] Further, step S2 includes the following sub-steps:

[0060] S21: adding the polyurethane prepolymer and the terminal epoxy silicone oil into the second organic solvent at a molar ratio of epoxy value to amine value of 1:1 to 1:2, so as to avoid the free polyurethane prepolymer that has not reacted with the terminal epoxy silicone oil in the polyurethane silicone oil component, and at the same time avoid the polyurethane silicone oil component being epoxy group-terminated, because the epoxy group will slowly react with the amine group at room temperature, which is not conducive to the compounding stability with the block silicone oil component in the next step, and at the same time adding an acid catalyst with a molar number of 100% to 200% of the amine value in the polyurethane prepolymer, the acid catalyst is one or more of formic acid, acetic acid, dilute hydrochloric acid, lauric acid and citric acid, the terminal epoxy silicone oil structure can be free of polyether segments and contain polyether segments, and the chemical structure of the terminal epoxy silicone oil without polyether segments is:

[0061]

[0062] Where n is a natural number between 30 and 200.

[0063] The chemical structure of the epoxy-terminated silicone oil containing polyether chain segments is:

[0064]

[0065] Wherein, n is a natural number from 30 to 200, p is a natural number from 3 to 25, and q is a natural number from 0 to 10;

[0066] S22 is stirred and reacted at a temperature of 60 to 120° C. for 4 to 24 hours, and then the second organic solvent is removed by vacuum to obtain a polyurethane silicone oil component.

[0067] Further, step S3 includes the following sub-steps:

[0068] S31: adding the terminal epoxy silicone oil and the polyetheramine into the second organic solvent at a molar ratio of epoxy value to amine value of 1:1 to 1:2, wherein the polyetheramine is one or more of polyetheramine ED600, polyetheramine ED900, polyetheramine ED2003 and polyetheramine T403;

[0069] S32 is stirred and reacted at a temperature of 60 to 120° C. for 6 to 24 hours, and then the second organic solvent is removed by vacuum to obtain a block silicone oil component.

[0070] Furthermore, the first organic solvent is one or more of acetone, butanone and tetrahydrofuran; the second organic solvent is one or more of diethylene glycol butyl ether, ethylene glycol butyl ether, dipropylene glycol butyl ether, dipropylene glycol, propylene glycol acetate and isopropanol.

[0071] According to another aspect of the present invention, a polyurethane modified silicone softener prepared by the above method is provided, which includes a polyurethane silicone oil component and a block silicone oil component. Both components are synthesized by block copolymerization technology, so there is no problem of poor compatibility between polyurethane and silicone, such as phase separation. Among them, the block silicone oil component is mainly composed of amino, polyether segment and siloxane segment. The cationic amino group in the molecular chain not only provides a soft feel to the fabric by directional adsorption on the surface of the fabric, but also continues to react with the unblocked active isocyanate in the polyurethane silicone oil component. The polyurea group formed by the reaction with the amino group also belongs to the hard segment, which not only provides the fabric with smoothness on the surface of the fabric, but also can generate hydrogen bond crosslinking with groups such as carbamate. Polyurethane silicone oil is mainly composed of polyurethane segments and silicone segments. The carbamate group in the polyurethane segment belongs to the hard segment, which can not only form hydrogen bonds with hydroxyl groups, but also give cotton fabric flexibility when covered on it. The blocked isocyanate on the side chain can be unblocked by high-temperature baking and can react chemically with the hydroxyl groups on the surface of the cotton fabric, the amino and hydroxyl groups in the block silicone oil molecular chain, the hydroxyl groups at the ends of the emulsifier molecules and other active hydrogen-containing groups, and continue to undergo in-situ polymerization on the surface of the cotton fabric to form a polymer on the fiber surface, and the four components of block silicone oil, polyurethane silicone oil, emulsifier and cotton fiber are tightly combined through chemical bonds, further improving the application performance of the cotton fabric.

[0072] According to another aspect of the present invention, there is provided an application of the above-mentioned polyurethane modified silicone softener in cotton fabrics, specifically: applying a polyurethane modified organic solvent to the cotton fabric, using a dipping and padding process, and then pre-baking at 90 to 110° C. for 30 to 90 seconds, and finally baking at 160 to 170° C. for 30 to 120 seconds.

[0073] The present invention will be further described below with reference to specific embodiments.

[0074] Example 1

[0075] Step 1: Synthesize polyurethane prepolymer

[0076] Weigh 100g of isophorone diisocyanate and 55g of acetone into a four-necked flask, heat to 40-45°C, then drop 35.74g of N-methyldiethanolamine in 30min, keep warm for 4h, heat to 55-60°C for 2h, then drop 27.50g of butanone oxime in 60min, keep warm for 3h at 60°C, no characteristic peak of isocyanate is detected by infrared detection, remove acetone by vacuum distillation, then add 107g of dipropylene glycol butyl ether to dilute, cool to room temperature and discharge to obtain a light yellow transparent polyurethane prepolymer with a solid content of 59-63%;

[0077] The infrared spectrum of polyurethane prepolymer is as follows Figure 1 As shown, from Figure 1It can be seen that 3327cm -1 and 1510cm -1 The absorption peaks at 1713 cm are the stretching vibration peaks and deformation vibration peaks of NH in carbamate. -1 It is the stretching vibration peak of the carbonyl group in carbamate, 2260cm -1 There is no isocyanate characteristic peak nearby, indicating that the blocking agent has been capped. The above characteristic peaks indicate that the structure of the polyurethane prepolymer is consistent with the design;

[0078] Step 2: Prepare polyurethane silicone oil

[0079] Weigh 30g of the prepared polyurethane prepolymer and add it to a four-necked flask, add 100g of terminal epoxy silicone oil (without polyether segment) with a molecular weight of 8000, add 2.50g of glacial acetic acid, add 100g of isopropanol, heat to 83-86°C, keep warm for 12h, after the reaction is completed, remove the solvent by vacuum distillation, add 20g of dipropylene glycol butyl ether, and obtain light yellow transparent viscous polyurethane silicone oil with a solid content of 78%-83%;

[0080] The infrared spectrum of polyurethane silicone oil is as follows Figure 2 As shown, from Figure 2 It can be seen that 3324cm -1 and 1545cm -1 The absorption peaks at 2961cm are the stretching vibration peaks and deformation vibration peaks of NH in carbamate; -1 is the stretching vibration peak of methyl group; 1700cm -1 It is the stretching vibration peak of the carbonyl group in carbamate; 1257cm -1 is the bending vibration peak of Si-CH3; 1020cm -1 and 1082cm -1 It is the characteristic peak of Si-O-Si and COC; 789cm -1 It is the bending vibration peak of Si-C; 2260cm -1 There is no isocyanate characteristic peak nearby, and the above characteristic peaks indicate that the structure and design of polyurethane silicone oil are consistent;

[0081] Step 3: Preparation of block silicone oil

[0082] Weigh 100 g of terminal epoxy silicone oil (without polyether segment) with a molecular weight of 8000, add 7.80 g of polyetheramine T403, add 100 g of isopropanol, raise the temperature to 80-85°C, keep the temperature for 8 hours, remove the organic solvent by vacuum distillation, add 26 g of diethylene glycol butyl ether to adjust the viscosity, and obtain a light yellow transparent three-dimensional network block silicone oil with a solid content of 78-83%;

[0083] Step 4: Preparation of polyurethane modified silicone softener

[0084] The polyurethane silicone oil combination and the block silicone oil component were evenly mixed in a mass ratio of 2:1 to obtain 250 g of polyurethane modified silicone softener crude oil, 30 g of isomeric tridecanol polyoxyethylene ether 1303 (EO addition number is 3), 30 g of isomeric tridecanol polyoxyethylene ether 1312 (EO addition number is 12) and 3.50 g of glacial acetic acid were added, and the mixture was stirred at a high speed, and 550 g of deionized water was added step by step to obtain a polyurethane modified silicone softener emulsion.

[0085] Example 2

[0086] Step 1: Synthesize polyurethane prepolymer

[0087] Weigh 100g of isophorone diisocyanate and 65g of acetone into a four-necked flask, heat to 55-60°C, then drop 26.80g of N-methyldiethanolamine in 150min, keep warm for 2h, drop 42g of butanone oxime in 2h, heat to 65°C, keep warm for 1.5h, no characteristic peak of isocyanate is detected by infrared detection, remove acetone by vacuum distillation, continue to add 84g of isopropanol to dilute, cool to room temperature and discharge to obtain a light yellow transparent polyurethane prepolymer with a solid content of 66%-72%;

[0088] Step 2: Prepare polyurethane silicone oil

[0089] Weigh 57.50g of the prepared polyurethane prepolymer, add 100g of terminal epoxy silicone oil (without polyether segment) with a molecular weight of 4000, add 3.40g of glacial acetic acid, add 60g of isopropanol, heat to 80-83°C, and keep warm for 6h. After the reaction is completed, remove the solvent by vacuum distillation, add 36g of dipropylene glycol butyl ether, and obtain light yellow transparent polyurethane silicone oil with a solid content of 79%-83%;

[0090] Step 3: Preparation of block silicone oil

[0091] Weigh 100 g of terminal epoxy silicone oil (containing polyether segments) with a molecular weight of 10,000, add 5.40 g of polyetheramine T403, add 80 g of isopropanol, heat to 80-82°C, keep warm for 12 hours, remove the organic solvent by vacuum distillation, add 28 g of dipropylene glycol butyl ether to adjust the viscosity, and obtain a light yellow transparent three-dimensional network block silicone oil with a solid content of 79%-83%;

[0092] Step 4: Preparation of polyurethane modified silicone softener

[0093] The polyurethane silicone oil combination and the block silicone oil component were uniformly mixed in a mass ratio of 3:2 to obtain 260 g of polyurethane modified silicone softener crude oil, 40 g of isomeric tridecanol polyoxyethylene ether 1306 (EO addition number is 6), 20 g of isomeric tridecanol polyoxyethylene ether 1309 (EO addition number is 9) and 4.50 g of glacial acetic acid were added, and the mixture was stirred at a high speed, and 550 g of deionized water was added step by step to obtain a polyurethane modified silicone softener emulsion;

[0094] Example 3

[0095] In step 2 of Example 1, 30 g of polyurethane prepolymer is replaced by 27 g of polyurethane prepolymer, 100 g of terminal epoxy silicone oil (without polyether segment) with a molecular weight of 8000 is replaced by 133 g of terminal epoxy silicone oil (with polyether segment) with a molecular weight of 10000, 2.50 g of glacial acetic acid is replaced by 2.00 g, 100 g of isopropanol is replaced by 118 g, heating to 83-86° C. for reaction for 12 h is replaced by heating to 85° C. for reaction for 8 h, 20 g of dipropylene glycol butyl ether is replaced by 27 g of diethylene glycol butyl ether, and the rest is the same as in Example 1, to obtain light yellow, transparent and viscous polyurethane silicone oil with a solid content of 78% to 83%.

[0096] Example 4

[0097] In step 3 of Example 1, 7.80 g of polyetheramine T403 is replaced by 32.40 g of polyetheramine ED2003, 100 g of isopropanol is replaced by 170 g, the temperature is raised to 81° C. instead of 80-85° C., the reaction is kept warm for 16 h instead of 8 h, the organic solvent is removed by distillation under reduced pressure, 27 g of diethylene glycol butyl ether is added for adjustment instead of adding 34 g of dipropylene glycol, and the rest is the same as in Example 1 to obtain a light yellow transparent block silicone oil with a solid content of 78% to 82%.

[0098] Example 5

[0099] In step 1 of Example 2, 65 g of acetone was replaced by 90 g of butanone, the temperature was increased to 55-60° C. instead of 55° C., the dropping time of N-methyldiethanolamine was changed from 150 min to 180 min, the dropping of 42 g of butanone oxime was changed to the dropping of 44.50 g of phenol, the dropping within 2 h was changed to the dropping within 1.5 h, the temperature was increased to 65° C. for insulation reaction for 1.5 h was changed to the temperature increased to 70° C. for insulation reaction for 4 h, and after removing butanone by distillation under reduced pressure, 81 g of isopropanol was added to dissolve the prepolymer, and finally a polyurethane prepolymer with a solid content of 68% was obtained. The rest was the same as in Example 2.

[0100] Example 6

[0101] In step 1 of Example 2, 65 g of acetone was replaced by 57 g of tetrahydrofuran, the temperature was increased from 55 to 60° C. to 60° C., the dropping time of N-methyldiethanolamine was changed from 150 min to 90 min, the temperature was increased to 72° C. after the dropping was completed, 42 g of butanone oxime was added dropwise, 54 g of caprolactam was added in batches, the dropping was completed within 2 h, the addition was completed within 1.5 h, the temperature was increased to 65° C. and the reaction was kept warm for 1.5 h, and the reaction was continued at 72° C. for 3.5 h. After the tetrahydrofuran was removed by distillation under reduced pressure, 74 g of isopropanol was added to dilute the mixture, and finally a polyurethane prepolymer with a solid content of 71% was obtained. The rest was the same as in Example 2.

[0102] The samples prepared in Examples 1 and 2 and two commercially available softeners were applied to cotton knitted fabrics at a dosage of 20 g / L and a rolling rate of 85%. The evaluation results are shown in Tables 1 and 2.

[0103] The application process is: liquid preparation → one dip and one rolling → pre-baking (105℃×70s) → baking (165℃×90s) → moisture regain → evaluation.

[0104] Application performance testing:

[0105] 1) Hand feel rating: The product is evaluated by touching with hands, with a score of 1 to 5, 1 being the worst and 5 being the best. Five people evaluate the product at the same time and the average value is taken. The evaluation includes: softness and smoothness.

[0106] 2) The hydrophilicity is evaluated by the water drop method: use a dropper to drop water at a height of 2 cm from the fabric, start timing, and observe that the water drop completely wets the fabric surface. When there is no mirror reflection, the timing ends.

[0107] 3) Tensile elastic recovery rate test: Use a universal material testing machine to test according to the "Textile Woven Fabric Tensile Elasticity Test Method" FZ / T-01034-2008. The fabric sample is not flat after washing, so only the elasticity before washing is tested.

[0108] 4) Fabric washing procedure: Fabric washing was carried out according to AATCC 135-2018t standard, and tumble dried after washing 10 times.

[0109] 5) Silicon content test: The silicon content of the fabric is obtained by EDS test.

[0110] Table 1 Performance evaluation table of different softeners before washing

[0111]

[0112] Table 2 Performance evaluation of different softeners after 10 washes

[0113]

[0114]

[0115] It can be seen from Table 1 and Table 2 that the cotton knitted fabric treated with the polyurethane modified silicone softener provided by the present invention has better application performance than the original fabric and the commercial softener before washing and after washing 10 times.

[0116] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a polyurethane modified silicone softener, It is characterized in that The preparation method comprises the following steps: S1: adding isophorone diisocyanate and N-methyldiethanolamine in a molar ratio of 3:2 or 2:1 into a first organic solvent for polymerization reaction, wherein the N-methyldiethanolamine is added dropwise, and then a blocking agent is added to block the remaining active isocyanate to obtain a polyurethane prepolymer; S2, polymerizing the polyurethane prepolymer obtained in step S1 with the epoxy-terminated silicone oil in a second organic solvent under the action of an acidic catalyst to obtain a polyurethane silicone oil component; S3 reacting the terminal epoxy silicone oil with the polyether amine in a second organic solvent to obtain a block silicone oil component; S4: compounding the polyurethane silicone oil component obtained in step S2 and the block silicone oil component obtained in step S3 according to a preset ratio, then adding an emulsifier for emulsification, and finally obtaining the polyurethane modified silicone softener.

2. The method for preparing the polyurethane modified silicone softener according to claim 1, It is characterized in that Step S1 includes the following sub-steps: S11: adding isophorone diisocyanate and N-methyldiethanolamine into a first organic solvent in a molar ratio of 3:2 or 2:1, wherein the N-methyldiethanolamine is added dropwise for 15 to 180 minutes, and the mass of the first organic solvent is 10% to 80% of the total mass of the isophorone diisocyanate and the N-methyldiethanolamine; S12 is stirred at 30-70°C for 2-8h to allow polymerization to occur; S13 After the polymerization reaction is completed, the reaction temperature is maintained at 40 to 80° C., and a blocking agent is added to block the remaining active isocyanate, wherein the molar ratio of the blocking agent to the remaining active isocyanate is 1.05:1 to 1.2:1; S14 continues to react for 2 to 6 hours. After infrared detection shows no isocyanate peak, the first organic solvent is removed by vacuum distillation and then a second organic solvent is added for dilution to obtain a polyurethane prepolymer.

3. The method for preparing the polyurethane modified silicone softener according to claim 1, It is characterized in that Step S2 includes the following sub-steps: S21: adding a polyurethane prepolymer and an epoxy-terminated silicone oil into a second organic solvent at a molar ratio of epoxy value to amine value of 1:1 to 1:2, and simultaneously adding an acidic catalyst having a molar number of 100% to 200% of the amine value in the polyurethane prepolymer; S22 is stirred and reacted at a temperature of 60 to 120° C. for 4 to 24 hours, and then the second organic solvent is removed by vacuum to obtain the polyurethane silicone oil component.

4. The method for preparing the polyurethane modified silicone softener according to claim 1, It is characterized in that Step S3 includes the following sub-steps: S31: adding the terminal epoxy silicone oil and the polyether amine into a second organic solvent at a molar ratio of epoxy value to amine value of 1:1 to 1:2; S32 is stirred to react at a temperature of 60 to 120° C. for 6 to 24 hours, and then the second organic solvent is removed by vacuum to obtain the block silicone oil component.

5. The method for preparing the polyurethane modified silicone softener according to claim 1, It is characterized in that In step S1, the blocking agent is one or more of butanone oxime, phenol, sodium bisulfite, caprolactam, acetylacetone and diethyl malonate; in step S2, the acidic catalyst is one or more of formic acid, acetic acid, dilute hydrochloric acid, lauric acid and citric acid; in step S3, the polyetheramine is one or more of polyetheramine ED600, polyetheramine ED900, polyetheramine ED2003 and polyetheramine T403.

6. The method for preparing the polyurethane modified silicone softener according to claim 1, It is characterized in that In step S4, the polyurethane silicone oil component and the block silicone oil component are compounded in a mass ratio of 2:1 to 1:

1.

7. The method for preparing the polyurethane modified silicone softener according to claim 1, It is characterized in that The first organic solvent is one or more of acetone, butanone and tetrahydrofuran, and the second organic solvent is one or more of diethylene glycol butyl ether, ethylene glycol butyl ether, dipropylene glycol butyl ether, dipropylene glycol, propylene glycol acetate and isopropanol.

8. A method for preparing a polyurethane modified silicone softener according to any one of claims 1 to 7, It is characterized in that The emulsifier is obtained by compounding isomeric tridecanol polyoxyethylene ethers with different EO addition numbers, and its HLB value is 4-18.

9. A polyurethane modified silicone softener prepared by the method according to any one of claims 1 to 8.

10. Use of the polyurethane modified silicone softener according to claim 9 in cotton fabrics, It is characterized in that The specific application method is: applying the polyurethane modified organic solvent to cotton fabric, using a dipping and padding process, and then pre-baking at 90-110° C. for 30-90 seconds, and finally baking at 160-170° C. for 30-120 seconds.