Polyimide film having excellent filler dispersibility and display device including the same
By uniformly dispersing the filler in the polyimide film and controlling the density ratio and particle volume concentration, the problem of insufficient dispersion of the polyimide film filler is solved, excellent mechanical and optical properties are achieved, and it is suitable for display devices Cover windows.
Patent Information
- Application Number
- CN202180048975.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-07-10
- Filing Date
- 2021-07-09
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-07-09
AI Technical Summary
Existing polyimide films have poor mechanical and optical properties due to insufficient filler dispersion, making it difficult to meet the needs of display device cover windows.
By uniformly dispersing the filler in the polyimide film, controlling the density ratio (DR) to 1.10 or less, the particle volume concentration (PVC) to 5% to 38%, and using a composite method of solution-solution mixing and solution-powder mixing. Preparation, ensuring uniform dispersion of fillers and excellent mechanical and optical properties.
It achieves excellent filler dispersion of polyimide films, improves its mechanical properties such as Young's modulus, elongation and indentation hardness, and improves optical properties such as light transmittance and visibility, making it suitable for display devices. Cover windows.
Smart Images

Figure CN115803385B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a polyimide-based film having excellent filler dispersibility, and to a display device including the polyimide-based film. Background Art
[0002] Polyimide (PI) resins are used as automotive materials, aviation materials, spacecraft materials, insulating coatings, insulating films, protective films, etc. due to their excellent insolubility, chemical resistance, heat resistance, radiation resistance, low temperature characteristics, etc.
[0003] Recently, for the purpose of reducing the thickness and weight of display devices and increasing flexibility, it has been considered to use polyimide films instead of glass as cover windows of display devices. In order to use polyimide films as cover windows of display devices, the polyimide films need to have excellent physical properties such as hardness, wear resistance and flexibility, as well as optical properties such as visibility and light transmittance. In order to give the polyimide films desired properties, fillers can be added to the polyimide films. Summary of the invention
[0004] Technical issues
[0005] Therefore, the present disclosure has been made in view of the above problems, and an object of the present disclosure is to provide a polyimide-based film including a filler uniformly dispersed in a polyimide-based resin.
[0006] Another object of the present disclosure is to provide a polyimide-based film having a density ratio (DR, defined as the ratio of true density to density of a density gradient tube) of 1.10 or less.
[0007] Another object of the present disclosure is to provide a polyimide-based film having a particle volume concentration (PVC) of 5% to 38%.
[0008] Technical Solution
[0009] According to the present disclosure, the above and other objects can be achieved by providing a polyimide film comprising a polyimide matrix and a filler dispersed in the polyimide matrix, wherein the polyimide film has a density ratio (DR, defined as the ratio of true density to density gradient tube density) of 1.10 or less,
[0010] The density ratio of the true density to the density of the density gradient tube is calculated according to the following formula 1:
[0011] <Formula 1>
[0012] Density ratio (DR) = true density / density gradient tube density
[0013] The particle volume concentration (PVC) of the polyimide film may be 5% to 38%.
[0014] The particle volume concentration (PVC) can be calculated according to the following formula 2:
[0015] <Formula 2>
[0016] PVC (%) = [V1 / (V1+V2)] * 100
[0017] Where V1 is the volume of the filler and V2 is the volume of the matrix.
[0018] The filler may include silicon dioxide (SiO2).
[0019] At least a portion of silicon dioxide (SiO 2 ) may be surface-treated with an organic compound having an alkoxy group.
[0020] The filler may have an average particle size of 5 nm to 50 nm.
[0021] The filler may be present in an amount of 5 wt % to 50 wt % based on the total weight of the polyimide-based film.
[0022] The polyimide-based film may have a Young's modulus of 5.0 GPa or more.
[0023] The polyimide-based film may have an elongation of 15% or more.
[0024] The polyimide-based film may have an indentation hardness of 45 or more.
[0025] The polyimide-based film may have a yellowness (yellowness index, YI) of 3 or less.
[0026] The polyimide-based film may have a haze of 1% or less.
[0027] The polyimide-based film may have a light transmittance of more than 85%.
[0028] According to another aspect of the present disclosure, a display device is provided, including a display panel and a polyimide-based film disposed on the display panel.
[0029] Beneficial Effects
[0030] According to one embodiment of the present disclosure, a polyimide-based film having excellent filler dispersibility may be prepared.
[0031] Generally, when fillers are dispersed in a polyimide film, the haze of the polyimide film increases. In contrast, according to an embodiment of the present disclosure, due to the excellent filler dispersibility of the polyimide film, the polyimide film can be given a density ratio of true density to density gradient tube density of less than 1.10. As a result, the polyimide film according to an embodiment of the present disclosure can exhibit excellent optical and mechanical properties.
[0032] The polyimide-based film according to one embodiment of the present disclosure may exhibit excellent optical and mechanical properties, and thus may effectively protect a display surface of a display device when used as a cover window of the display device. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 is a schematic diagram showing a polyimide-based film according to one embodiment of the present invention;
[0034] Figure 2 shows the difference in pores inside a polyimide-based film according to the density ratio (DR, defined as the ratio of true density to density of a density gradient tube);
[0035] Figure 3 The difference in pores inside a polyimide film according to the particle volume concentration (PVC) of the polyimide film is shown;
[0036] Figure 4 is a schematic diagram showing a state in which a filler is dispersed in a polyimide-based film according to an embodiment of the present invention;
[0037] Figure 5 is a cross-sectional view showing a portion of a display device according to another embodiment of the present invention;
[0038] Figure 6 It is shown Figure 5 An enlarged cross-sectional view of the "P" portion of the PCB. DETAILED DESCRIPTION
[0039] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. However, the following embodiments are exemplarily provided only for clear understanding of the present disclosure, rather than limiting the scope of the present disclosure.
[0040] The shapes, sizes, proportions, angles and numbers disclosed in the drawings used to describe the embodiments of the present disclosure are examples only, and the present disclosure is not limited to the details shown in the drawings. Throughout this specification, similar reference numerals represent similar elements. In the following description, when the detailed description of the relevant known functions or configurations is determined to be unnecessary to obscure the main points of the present disclosure, the detailed description will be omitted.
[0041] In the case where terms such as "include", "have" or "include" are used in this specification, other parts may also exist unless "only" is used. Unless otherwise specified, terms in the singular form may include plural meanings. In addition, when explaining an element, even if it is not explicitly described, the element is understood to include a range of errors.
[0042] When describing a positional relationship, for example, when the positional relationship is described as “on,” “over,” “under,” or “next,” a case where there is no contact between them may be included unless “just” or “directly” is used.
[0043] Spatially related terms such as "under," "below," "lower," "above," and "upper" may be used herein to describe the relationship of a device or element as shown in the figures to another device or another element. It should be understood that, in addition to the orientations described in the figures, spatially related terms are intended to include different orientations of the device during use or operation of the device. For example, if a device in a figure is inverted, an element described as being "under" or "below" other elements will be located "above" the other elements. Therefore, the exemplary terms "under" or "below" may include the meanings of both "under" or "above." In the same manner, the exemplary terms "above" or "upper" may include the meanings of both "above" and "under."
[0044] When describing a time relationship, for example, when "after", "subsequently", "next", or "before" is used to describe a time order, the case of a non-continuous relationship may be included unless "just" or "directly" is used.
[0045] It will be understood that although the terms "first", "second", etc. may be used herein to describe various elements, these elements should not be limited by these terms. These terms are only used to distinguish one element from another element. Therefore, within the technical concept of the present disclosure, the first element may be referred to as the second element.
[0046] It should be understood that the term "at least one" includes all combinations related to any one item. For example, "at least one of a first element, a second element, and a third element" may include all combinations of two or more elements selected from the first, second, and third elements, as well as each of the first, second, and third elements.
[0047] The features of the various embodiments of the present disclosure may be partially or completely combined or combined with each other, and may be technically interoperable and driven in various ways, as will be readily understood by those skilled in the art. The embodiments of the present disclosure may be performed independently of each other, or may be performed together in an interrelated manner.
[0048] Figure 1is a diagram illustrating a polyimide-based film 100 according to an embodiment of the present disclosure.
[0049] like Figure 1 As shown in , the polyimide-based film 100 according to one embodiment of the present disclosure includes a polyimide-based matrix 110 and a filler 120 dispersed in the polyimide-based matrix 110 .
[0050] The ratio of the true density, referred to as "density ratio" (DR), of the polyimide-based film according to one embodiment of the present disclosure to the density of the density gradient tube is 1.10 or less.
[0051] The density ratio (DR, defined as the ratio of true density to density gradient tube density) can be calculated according to the following formula 1:
[0052] <Formula 1>
[0053] Density ratio (DR) = true density / density gradient tube density
[0054] The term "true density" refers to solid density, which means the density of a portion completely filled with a material, excluding pores between particles. According to one embodiment of the present disclosure, the true density refers to the density of a portion filled with a polyimide-based matrix 110 and a filler 120, excluding pores.
[0055] During the measurement process, the true density may vary according to the size of the sample of the film 100 to be measured. Therefore, according to one embodiment of the present disclosure, the true density of the film 100 may be obtained by powderization analysis.
[0056] Specifically, a sample (10×10 cm 2 ) is finely cut into 1×1em size 2 The following fragments are placed in a sample holder together with iron beads (crusher). A cryogenic crusher (Japan Analytical Industry, JFC-300) is filled more than 2 / 3 with liquid nitrogen, and the sample holder containing the cut samples is mounted on the cryogenic crusher, and then the chamber is closed. After precooling for 15 minutes, the sample is crushed using a cryogenic crusher with a running time of more than 15 minutes. The true density of the powder sample of the film 100 is measured seven times using an AccuPyc1340 densimeter (using helium) produced by Micromeritics Co., Ltd. The average value of the true density values remaining after removing the highest and lowest values from the measured true density of the powder film 100 corresponds to the true density of the film 100 in the present disclosure.
[0057] The term "density gradient tube density" refers to the density measured using a density gradient tube. The density gradient tube is a device used to measure density.
[0058] According to one embodiment of the present disclosure, the density gradient tube density of the film 100 may be obtained using a density gradient tube that complies with the ASTM D1505 standard.
[0059] Specifically, the density gradient tube has a density gradient generated between a liquid with a large specific gravity disposed at the lower part of the glass column and another liquid with a small specific gravity disposed at the upper part thereof. When a sample of the film 100 is placed in such a density gradient tube, it is suspended and suspended at a position corresponding to its density, and the density gradient tube density of the sample of the film 100 can be determined based on the density corresponding to the position. The gradient of the density of the density gradient tube is determined by: a method of placing a spherical glass float with a known specific gravity; a method including measuring the specific gravity of zinc chloride aqueous solutions of various concentrations in advance and then fixing them in the density gradient tube; or by a colorimetric method using a dye dissolved in only one of the multiple liquids with different specific gravities of the density gradient tube.
[0060] In the following, reference will be made to Figure 2 The density ratio (DR) of the true density of the film 100 to the density of the density gradient tube is described in detail. Figure 2 The difference in pores inside the film 100 according to the density ratio (DR) of the true density of the film 100 to the density of the density gradient tube is shown.
[0061] Based on the ratio of the true density of the film 100 to the density of the density gradient tube, the density ratio (DR) of the true density of the film 100 to the density of the density gradient tube indicates the amount of pores present in the film 100 (in other words, its porosity). The true density refers to the density of the matrix 110 and the filler 120 excluding the pores in the film 100, the density gradient tube density indicates the density of the film 100 including the pores, and the porosity of the film 100 can be expressed by the ratio of the true density to the density gradient tube density.
[0062] like Figure 2 As shown in , as the density ratio (DR) of the true density of the film 100 to the density of the density gradient tube increases, the pores in the film 100 increase. Conversely, as the density ratio (DR) of the true density to the density gradient tube decreases, the pores in the film 100 decrease.
[0063] In general, when the film 100 includes the filler 120, a difference may occur in the pores in the film 100 depending on the degree of dispersion of the filler 120. When particles of the filler 120 are aggregated due to low dispersion of the filler 120, the space between the filler particles cannot be sufficiently filled by the matrix 110, and thus, pores may be formed therein. On the contrary, when particles of the filler 120 are well dispersed, in a state where the matrix 110 and the filler 120 are sufficiently well mixed, the matrix 110 may sufficiently fill the space between the particles of the filler 120, and thus, the pores are reduced.
[0064] As the pores in the film 100 are reduced, the tensile strength, Young's modulus, elongation, indentation hardness and light transmittance of the film 100 are increased, and the yellowness (yellowness index, YI) and haze are reduced. As a result, the mechanical properties of the film 100 such as abrasion resistance and flexibility and the optical properties of the film 100 such as light transmittance and visibility are excellent.
[0065] According to one embodiment of the present disclosure, the density ratio (DR) of the true density of the film 100 to the density of the density gradient tube is 1.10 or less.
[0066] When the density ratio (DR) of the true density to the density gradient tube density is greater than 1.10, the filler 120 has a reduced effect of filling the film 100 and a reduced effect of improving the hardness and Young's modulus of the film 100. In addition, the increase in porosity in the film 100 due to the aggregation of the filler 120 disadvantageously causes a decrease in the elongation and indentation hardness of the film 100. In addition, the aggregation of the filler 120 causes the haze of the film 100 to increase.
[0067] The polyimide-based film 100 according to one embodiment of the present disclosure has a particle volume concentration (PVC) of 5% to 38%.
[0068] The particle volume concentration (PVC) can be calculated according to the following formula 2:
[0069] <Formula 2>
[0070] PVC (%) = [V1 / (V1+V2)] * 100
[0071] Where V1 is the volume of the filler and V2 is the volume of the matrix.
[0072] In the following, reference will be made to Figure 3 Describe the particle volume concentration (PVC) in detail. Figure 3 The difference in pores inside the film 100 according to the particle volume concentration (PVC) of the film 100 is shown.
[0073] The particle volume concentration (PVC) indicates the ratio of the volume occupied by the filler 120 to the total volume of the matrix 110 and the filler 120 in the film 100 as a percentage (%).
[0074] like Figure 3 As shown in , when the particle volume concentration (PVC) of the film 100 decreases, the pores of the film 100 decrease, and when the particle volume concentration (PVC) increases, the pores of the film 100 increase.
[0075] As the particle volume concentration (PVC) of the film 100 increases, the volume occupied by the filler 120 in the film 100 increases and the average distance between the filler particles decreases. When the average distance between the filler particles decreases, it is difficult for the matrix 110 to fill the space between the filler particles, and thus, the pores increase.
[0076] The volume (V1) of the filler can be calculated by dividing the mass of the filler by the density. Specifically, the volume (V1) of the filler can be calculated by measuring the mass and density of the filler included in the film 100. For example, the mass of the filler can be determined by measuring the weight of the filler added when preparing the film 100. The density of the filler can be measured using a method of measuring true density or a method of measuring density gradient tube density.
[0077] The volume (V2) of the matrix can be calculated by dividing the mass of the matrix by its density. Specifically, the volume (V2) of the matrix can be calculated by measuring the mass and density of the matrix included in the film 100. For example, the mass of the matrix can be determined by measuring the weight of the matrix added when preparing the film 100. The density of the matrix can be measured using a method for measuring true density or a method for measuring density gradient tube density.
[0078] According to one embodiment of the present disclosure, the particle volume concentration (PVC) of the film 100 is 5% to 38%.
[0079] When the particle volume concentration (PVC) is less than 5%, the effect of improving the mechanical properties of the film 100 by the filler 120 is insufficient. In addition, when the particle volume concentration (PVC) is greater than 38%, discontinuity occurs between the contact surfaces of the filler 120 and the matrix 110, and thus, the elongation and the indentation hardness decrease.
[0080] According to one embodiment of the present disclosure, the polyimide-based matrix 110 is light-transmissive. In addition, the polyimide-based matrix 110 is flexible. For example, the polyimide-based matrix 110 may be bendable, foldable, and rollable.
[0081] The polyimide-based matrix 110 includes a polyimide-based resin. For example, the polyimide-based matrix 110 may include a polyimide-based resin.
[0082] The polyimide-based matrix 110 according to one embodiment of the present disclosure may be prepared from a monomer component including a dianhydride and a diamine.
[0083] More specifically, the polyimide-based matrix 110 according to one embodiment of the present disclosure may have an imide repeating unit formed of dianhydride and diamine.
[0084] However, the polyimide-based matrix 110 according to one embodiment of the present disclosure is not limited thereto. In addition, the polyimide-based matrix 110 according to one embodiment of the present disclosure may be prepared from a monomer component including a dicarbonyl compound in addition to a dianhydride and a diamine. Therefore, the polyimide-based matrix 110 according to one embodiment of the present disclosure may have an imide repeating unit and an amide repeating unit. For example, the polyimide-based matrix 110 having an imide repeating unit and an amide repeating unit is a polyamide-imide resin.
[0085] Therefore, the polyimide-based matrix 110 according to one embodiment of the present disclosure may include a polyimide resin or a polyamide-imide resin.
[0086] According to one embodiment of the present disclosure, the polyimide-based resin used as the polyimide-based matrix 110 may have excellent mechanical and optical properties.
[0087] The polyimide-based matrix 110 may have a thickness that enables the polyimide-based film 100 to protect the display panel. For example, the polyimide-based matrix 110 may have a thickness of 10 μm to 100 μm.
[0088] The polyimide-based matrix 110 may have an average light transmittance of 85% or more measured using a UV spectrophotometer based on a thickness of 10 μm to 100 μm, and may have a yellowness (yellowness index, YI) of 5 or less in a visible light region.
[0089] According to one embodiment of the present disclosure, the filler 120 may be an inorganic material or an organic material. The filler 120 may have a particle shape. According to one embodiment of the present disclosure, for example, an inorganic filler may be used.
[0090] According to one embodiment of the present disclosure, the filler 120 may include at least one of silica (SiO 2 ), zirconium oxide (ZrO 2 ), aluminum oxide (Al 2 O 3 ), titanium dioxide (TiO 2 ), styrene, or acrylic acid. For example, inorganic silica (SiO 2 ) particles may be used as the filler 120 .
[0091] According to one embodiment of the present disclosure, at least a portion of the silicon dioxide (SiO 2 ) used as the filler 120 may be surface-treated. More specifically, surface-treated silicon dioxide (SiO 2 ) particles may be used as the filler 120 .
[0092] According to one embodiment of the present disclosure, at least a portion of the silica (SiO 2 ) used as the filler 120 may be surface-treated with an organic compound having an alkoxy group. For example, silica (SiO 2 ) particles surface-treated with at least one of a substituted or unsubstituted alkylalkoxysilane or a phenylalkoxysilane may be used as the filler 120.
[0093] Specifically, silica (SiO2) particles surface-treated with methylalkoxysilane, ethylalkoxysilane or phenylalkoxysilane may be used as the filler 120. More specifically, silica (SiO2) particles surface-treated with trimethoxy(methyl)silane and phenyltrimethoxysilane may be used as the filler 120.
[0094] According to one embodiment of the present disclosure, the filler 120 may have a unit structure represented by the following Chemical Formula 1 to Chemical Formula 6:
[0095] [Chemical formula 1]
[0096]
[0097] [Chemical formula 2]
[0098]
[0099] [Chemical formula 3]
[0100]
[0101] [Chemical formula 4]
[0102]
[0103] [Chemical formula 5]
[0104]
[0105] [Chemical formula 6]
[0106]
[0107] wherein each R is independently at least one of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, or a phenyl group having 6 to 18 carbon atoms.
[0108] The polyimide-based film 100 according to one embodiment of the present disclosure has excellent mechanical and optical properties.
[0109] Regarding optical properties, the polyimide-based film 100 according to one embodiment of the present disclosure may have a yellowness (yellow index, YI) of 3 or less. In addition, the polyimide-based film 100 according to one embodiment of the present disclosure may have a haze of 1% or less. The polyimide-based film 100 according to one embodiment of the present disclosure may have a light transmittance of 85% or more.
[0110] In addition, regarding mechanical properties, the polyimide film 100 according to an embodiment of the present disclosure may have a Young's modulus of 5.0 GPa or more. In addition, the polyimide film 100 according to an embodiment of the present disclosure may have an elongation of 15% or more. In addition, the polyimide film 100 according to an embodiment of the present disclosure may have an indentation hardness of 45 or more.
[0111] According to one embodiment of the present disclosure, in order to make the polyimide-based film 100 have excellent optical and mechanical properties, the particle size of the filler 120 , the content of the filler 120 , and the interparticle distance of the filler 120 may be controlled.
[0112] Furthermore, in order to uniformly mix the filler 120 in the polyimide-based matrix 110 so that the polyimide-based film 100 exhibits excellent optical and mechanical properties, one embodiment of the present disclosure provides a new method of mixing the polyimide-based polymer constituting the polyimide-based matrix 110 with the filler 120 .
[0113] According to one embodiment of the present disclosure, the filler 120 may have an average particle size of 5 nm to 50 nm. When the average particle size of the filler 120 is less than 5 nm, the dispersibility of the filler 120 may deteriorate and the particles of the filler 120 may aggregate. On the other hand, when the average particle size of the filler 120 is greater than 50 nm, the optical properties of the polyimide-based film 100 including the filler 120 may deteriorate. For example, when the filler 120 having an average particle size greater than 50 nm is excessively included, the haze of the polyimide-based film 100 may increase.
[0114] In addition, when the average particle size of the filler 120 is less than 5 nm, the mechanical strength of the polyimide film 100 is deteriorated in the portion where the filler 120 is aggregated due to the aggregation of the filler 120, and thus the tensile strength, Young's modulus and indentation hardness of the polyimide film 100 are deteriorated. When the average particle size of the filler 120 is greater than 50 nm, the elongation of the polyimide film 100 may be less than 15%.
[0115] In addition, when the average particle size of the filler 120 is less than 5 nm, the dispersibility of the filler 120 is reduced, and when the average particle size of the filler 120 is greater than 50 nm, sufficient space cannot be ensured between particles of the filler 120. Therefore, the density ratio (DR) of the true density to the density gradient tube density is higher than 1.10.
[0116] According to another embodiment of the present disclosure, the filler 120 may have an average particle diameter of 10 nm to 20 nm, or may have an average particle diameter of 10 nm to 15 nm.
[0117] When the polyimide-based film 100 includes the filler 120 having a nano-scale particle size, optical properties of the polyimide-based film 100 may be improved by light scattering of the filler 120. In addition, when the polyimide-based film 100 includes the filler 120, mechanical properties of the polyimide-based film 100 may be improved.
[0118] According to one embodiment of the present disclosure, the content of the filler 120 may be in a range of 5 wt % to 50 wt % based on the total weight of the polyimide-based film 100 .
[0119] When the content of the filler 120 is less than 5 wt % based on the total weight of the polyimide-based film 100, the light scattering effect based on the filler 120 is insufficient, and the light transmittance improvement effect of the polyimide-based film 100 is almost not obtained. In addition, when the content of the filler 120 is less than 5 wt % based on the total weight of the polyimide-based film 100, the effect of improving the tensile strength, Young's modulus, elongation, and hardness of the polyimide-based film 100 may be insufficient.
[0120] On the other hand, when the content of the filler 120 is higher than 50 wt % based on the total weight of the polyimide film 100, the dispersibility of the filler 120 is deteriorated and the haze of the polyimide film 100 is aggravated, whereby the excess filler 120 blocks light, and thus, the light transmittance of the polyimide film 100 is deteriorated.
[0121] Figure 4 is a diagram showing a state in which a filler 120 is dispersed in a polyimide-based film 100 according to an embodiment of the present disclosure.
[0122] like Figure 4 As shown in , some particles of filler 120 are spaced apart from each other and dispersed, while the rest form aggregates. Figure 4 In the above, "Group A" indicates particles of filler 120 that form aggregates. Particles of filler 120 other than the particles of filler present in "Group A" are not aggregated but are dispersed (parts other than Group A). Figure 4The number of aggregated particles of the filler 120 in the “A group” is reduced, and the uniformity of the particles of the filler 120 dispersed in the polyimide-based film 100 is increased.
[0123] When aggregates are formed, such as Figure 4 When the amount of filler 120 of "Group A" is small, the density ratio (DR) of true density to density gradient tube density is 1.10 or less, and thus, the polyimide-based film 100 can exhibit excellent tensile strength, Young's modulus, elongation, and indentation hardness. In addition, when the amount of filler 120 forming aggregates such as "Group A" is small, the particle volume concentration (PVC) is in the range of 5% to 38%, and the polyimide-based film 100 can exhibit excellent tensile strength and Young's modulus.
[0124] Generally, in the case of including the filler 120, when the filler 120 is not sufficiently uniformly dispersed, the mechanical properties and optical properties of the polyimide film 100 are deteriorated; for example, the tensile strength, Young's modulus, elongation, indentation hardness and transmittance of the polyimide film 100 are deteriorated, and the yellowness (yellowness index, YI) and haze increase. However, according to one embodiment of the present disclosure, by adjusting the density ratio (DR) of the true density to the density gradient tube density to less than 1.10, the tensile strength, Young's modulus, elongation and indentation hardness of the polyimide film 100 can be prevented from deteriorating, and the increase of yellowness (yellowness index, YI) and haze can be prevented.
[0125] In addition, according to one embodiment of the present disclosure, by adjusting the particle volume concentration (PVC) to 5% to 38%, the deterioration of the tensile strength and the Young's modulus of the polyimide-based film 100 may be prevented.
[0126] According to one embodiment of the present disclosure, by adjusting the density ratio (DR) of the true density of the polyimide-based film 100 to the density of the density gradient tube to 1.10 or less, a Young's modulus of 5.0 GPa or more may be imparted to the polyimide-based film 100.
[0127] In addition, according to one embodiment of the present disclosure, the polyimide-based film 100 may have an elongation of 15% or more.
[0128] In addition, according to one embodiment of the present disclosure, the polyimide-based film 100 may have an indentation hardness of 45 or more.
[0129] In addition, according to one embodiment of the present disclosure, the polyimide-based film 100 may have a light transmittance of 85% or more.
[0130] In addition, according to one embodiment of the present disclosure, the polyimide-based film 100 may have a haze of 1% or less.
[0131] In addition, according to an embodiment of the present disclosure, the polyimide-based film 100 may have a yellowness (yellowness index, YI) of 3.0 or less.
[0132] Figure 5 is a cross-sectional view showing a portion of a display device 200 according to another embodiment, and Figure 6 yes Figure 5 An enlarged cross-sectional view of the "P" portion of FIG.
[0133] Reference Figure 5 , a display device 200 according to another embodiment of the present disclosure includes a display panel 501 and a polyimide-based film 100 on the display panel 501 .
[0134] Reference Figure 5 and Figure 6 The display panel 501 includes a substrate 510, a thin film transistor TFT on the substrate 510, and an organic light emitting device 570 connected to the thin film transistor TFT. The organic light emitting device 570 includes a first electrode 571, an organic light emitting layer 572 on the first electrode 571, and a second electrode 573 on the organic light emitting layer 572. Figure 5 and Figure 6 The display device 200 shown in FIG. 2 is an organic light emitting display device.
[0135] The substrate 510 may be formed of glass or plastic. Specifically, the substrate 510 may be formed of plastic such as a polyimide resin or a polyimide film. Although not shown, a buffer layer may be provided on the substrate 510.
[0136] The thin film transistor TFT is disposed on the substrate 510. The thin film transistor TFT includes a semiconductor layer 520, a gate electrode 530 insulated from the semiconductor layer 520 and overlapping at least a portion of the semiconductor layer 520, a source electrode 541 connected to the semiconductor layer 520, and a drain electrode 542 spaced apart from the source electrode 541 and connected to the semiconductor layer 520.
[0137] Reference Figure 6 The gate insulating layer 535 is disposed between the gate electrode 530 and the semiconductor layer 520. The interlayer insulating layer 551 may be disposed on the gate electrode 530, and the source electrode 541 and the drain electrode 542 may be disposed on the interlayer insulating layer 551.
[0138] The planarization layer 552 is disposed on the thin film transistor TFT to planarize the top of the thin film transistor TFT.
[0139] The first electrode 571 is disposed on the planarization layer 552. The first electrode 571 is connected to the thin film transistor TFT through a contact hole disposed in the planarization layer 552.
[0140] The bank layer 580 is disposed on the planarization layer 552 in a portion of the first electrode 571 to define a pixel region or a light emitting region. For example, the bank layer 580 is disposed at a boundary between a plurality of pixels in a matrix form to define each pixel region.
[0141] The organic light emitting layer 572 is disposed on the first electrode 571. The organic light emitting layer 572 may also be disposed on the bank layer 580. The organic light emitting layer 572 may include one light emitting layer or two light emitting layers stacked in a vertical direction. Light of any one color of red, green, and blue may be emitted from the organic light emitting layer 572, and white light may be emitted therefrom.
[0142] The second electrode 573 is disposed on the organic light emitting layer 572 .
[0143] The first electrode 571 , the organic light emitting layer 572 , and the second electrode 573 may be stacked to constitute the organic light emitting device 570 .
[0144] Although not shown, when the organic light emitting layer 572 emits white light, each pixel may include a color filter that filters the white light emitted from the organic light emitting layer 572 based on a specific wavelength. The color filter is formed in a light path.
[0145] The thin film encapsulation layer 590 may be disposed on the second electrode 573. The thin film encapsulation layer 590 may include at least one organic layer and at least one inorganic layer, and the at least one organic layer and the at least one inorganic layer may be alternately disposed.
[0146] The polyimide-based film 100 is disposed on the display panel 501 having the above stacked structure. The polyimide-based film 100 includes a polyimide-based matrix 110 and a filler 120 dispersed in the polyimide-based matrix 110.
[0147] The polyimide-based film 100 according to one embodiment of the present disclosure may be prepared by a composite mixing method using a combination of solution-solution mixing and solution-powder mixing.
[0148] According to one embodiment of the present invention, a method for preparing a polyimide film 100 includes: preparing a polyimide resin powder; dissolving a first amount of the polyimide resin powder in a first solvent to prepare a polyimide resin solution; dispersing a filler in a second solvent to prepare a filler dispersion; mixing the filler dispersion with the polyimide resin solution to prepare a first mixed solution; and adding a second amount of the polyimide resin powder to the first mixed solution and then dissolving it to prepare a second mixed solution.
[0149] According to one embodiment of the present disclosure, the polyimide-based resin powder is divided into at least two equal parts and mixed with the filler dispersion.
[0150] Specifically, a first amount of polyimide-based resin powder is dissolved in a first solvent and mixed with a filler dispersion in the form of a polyimide-based resin solution. The first amount may be 0.5% to 10% by weight of the filler, preferably 1% to 5% thereof.
[0151] In addition, a second amount of polyimide-based resin powder is added in the form of powder. Specifically, the second amount of polyimide-based resin powder may be added in the form of powder to the first mixed solution prepared by mixing the filler dispersion with the polyimide-based resin solution.
[0152] The second amount of the polyimide-based resin powder may be 10 to 200 times the first amount. More specifically, the second amount of the polyimide-based resin powder may be 60 to 200 times the first amount.
[0153] According to one embodiment of the present disclosure, before adding the second amount of polyimide resin powder to the first mixed solution, the method may further include adding a third solvent to the first mixed solution. The third solvent may be the same as or different from the first solvent. According to one embodiment of the present disclosure, the third solvent may be the same as the first solvent.
[0154] DMAc (N, N-dimethylacetamide) can be used as the first solvent. DMAc (N, N-dimethylacetamide) or methyl ethyl ketone (MEK) can be used as the second solvent. DMAc (N, N-dimethylacetamide) can be used as the third solvent. However, the embodiments of the present disclosure are not limited thereto, and other known solvents can be used as the first solvent, the second solvent, and the third solvent.
[0155] According to one embodiment of the present disclosure, first, a portion (first amount) of the polyimide-based resin powder is dissolved in a solvent and then mixed with a filler dispersion. As a result, the dispersibility of the filler is improved.
[0156] For reference, when polyimide resin powder is directly injected into a filler dispersion in which a filler is dispersed, the solvent immediately penetrates from the surface of the powder to the inside of the powder, and the concentration around the surface of the powder immediately increases, whereby filler particles aggregate.
[0157] On the other hand, according to one embodiment of the present disclosure, by first adding a polyimide resin solution prepared by dissolving a polyimide resin powder into a filler dispersion containing a solvent, the polymer chains of the polyimide resin dispersed between the filler particles can prevent the aggregation of the filler particles. Then, even if a second amount of polyimide resin powder is also added, no aggregation occurs between the filler particles. As a result, the aggregation of the filler can be prevented, and the dispersibility of the filler can be improved.
[0158] According to one embodiment of the present disclosure, the polyimide-based film 100 including the filler 120 uniformly dispersed therein may be prepared using a composite mixing method in which solution-solution mixing and solution-powder mixing are combined.
[0159] According to one embodiment of the present disclosure, the filler 120 and the light-transmitting resin can be kept at a high degree of freedom, and thus, an environment conducive to dispersion can be created. As a result, the filler 120 can be combined with the light-transmitting resin with a high degree of freedom, and a polyimide-based film 100 in which the filler 120 is uniformly dispersed in the matrix 110 formed by the light-transmitting resin can be prepared.
[0160] According to one embodiment of the present disclosure, silica particles may be used as the filler 120. For example, the silica particles may be prepared from tetraethyltriethoxysilane.
[0161] Specifically, silica particles (SiO2) having an average particle size of 20 nm can be prepared by injecting ethanol and tetraethyltriethoxysilane (TEOS, Si(OC2H5)4) into a reactor, stirring the components at room temperature, adding NH4OH thereto, stirring the components, filtering the obtained reaction product, washing the filtrate with ethanol, and drying the residue under reduced pressure.
[0162] A silica dispersion may be used as the dispersion of the filler 120. The silica dispersion may be prepared, for example, by injecting dimethylacetamide (DMAc) and silica particles into a reactor, followed by stirring.
[0163] Hereinafter, the present disclosure will be described in more detail with reference to Preparation Examples and Examples. However, the Preparation Examples and Examples should not be construed as limiting the scope of the present disclosure.
[0164] <Preparation Example 1: Preparation of Polyimide Polymer Solid>
[0165] 776.655 g of N, N-dimethylacetamide (DMAc) was charged into a 1 L reactor equipped with a stirrer, a nitrogen injector, a dropping funnel, a temperature controller and a cooler, while nitrogen was passed through the reactor. The temperature of the reactor was adjusted to 25°C, 54.439 g (0.17 mol) of TFDB was dissolved therein, and the resulting solution was maintained at 25°C. 15.005 g (0.051 mol) of BPDA was added thereto, followed by stirring for 3 hours to completely dissolve BPDA, and then 22.657 g (0.051 mol) of 6FDA was added thereto to completely dissolve it. The temperature of the reactor was lowered to 10°C, 13.805 g (0.068 mol) of TPC was added thereto, and the reaction was carried out at 25°C for 12 hours to obtain a polymer solution with a solid concentration of 12% by weight.
[0166] 17.75 g of pyridine and 22.92 g of acetic anhydride were added to the obtained polymer solution, followed by stirring for 30 minutes, and then further stirred at 70° C. for 1 hour. The resultant was cooled to room temperature, 20 L of methanol was added to the obtained polymer solution to precipitate a solid, and the precipitated solid was filtered, pulverized, washed again with 2 L of methanol, and then dried at 100° C. in a vacuum for 6 hours to obtain a powdered polyimide polymer solid. The polyimide polymer solid prepared here is a polyamide-imide polymer solid.
[0167] <Example 1>
[0168] 35.42 parts by weight of N,N-dimethylacetamide (DMAc) (first solvent) was added to a 1 L reactor, followed by stirring for a predetermined time while maintaining the temperature of the reactor at 10° C. Then, 0.36 parts by weight (first amount) of the polyamide-imide prepared in Preparation Example 1 as a solid powder (polyimide-based resin powder) was added thereto, followed by stirring for 1 hour, and then heated to 25° C. to prepare a polyimide-based resin solution as a liquid.
[0169] 23.85 parts by weight of silica dispersion A (SSD-330T, Ranco) in which silica particles having an average particle size of 10 nm were dispersed in a DMAc (N,N-dimethylacetamide) solution (second solvent) in an amount of 30% by weight was charged into another 1 L reactor, and the prepared liquid polyimide resin solution was slowly injected for 1 hour using a cylindrical pump while maintaining the temperature of the reactor at 25° C. to prepare a first mixed solution in which the silica dispersion was mixed with the polyimide resin solution.
[0170] 348.23 parts by weight of DMAc as the third solvent was added to the first mixed solution, followed by stirring. Then, 64.04 parts by weight (second amount) of the polyamide-imide prepared in Preparation Example 1 as a solid powder (polyimide resin powder) was added thereto, followed by stirring to prepare a second mixed solution. The second mixed solution was a polyimide resin solution in which silica particles were dispersed.
[0171] The obtained second mixed solution is cast. A casting substrate is used for casting. There is no particular restriction on the type of the casting substrate. The casting substrate can be a glass substrate, a stainless steel (SUS) substrate, a Teflon substrate, etc. According to one embodiment of the present disclosure, the casting substrate can be, for example, a glass substrate.
[0172] Specifically, the obtained second mixed liquid was coated on a glass substrate, cast, and dried with hot air at 120° C. for 30 minutes to prepare a thin film, and then the prepared thin film was peeled off from the glass substrate and fixed on a frame with pins.
[0173] The frame with the film fixed thereon was placed in a vacuum oven, slowly heated from 100° C. to 280° C. for 2 hours, slowly cooled, and then separated from the frame to obtain a polyimide film. The polyimide film was further heat treated at 250° C. for 5 minutes.
[0174] As a result, the preparation of the polyimide-based film 100 having a thickness of 50 μm and including the polyimide-based matrix 110 and the silica-based filler 120 dispersed in the polyimide-based matrix 110 is completed.
[0175] <Example 2 to Example 7>
[0176] Polyimide-based films of Examples 2 to 7 were prepared in the same manner as Example 1 by changing only the type and total amount of the silica dispersion, the first and second amounts of the polyamide-imide, the first and third solvent amounts.
[0177] The details of the silica dispersions of Examples 1 to 7, the total amount, the first amount and the second amount of the polyamide-imide, the amount of the first solvent, and the amount of the third solvent are shown in Table 1 below.
[0178] <Comparative Example 1>
[0179] The polyimide-based film 100 was prepared in the same manner as Example 1 by changing only the type and total amount of the silica dispersion, the first and second amounts of the polyamide-imide, the amount of the first solvent, and the amount of the third solvent.
[0180] The details of the silica dispersion of Comparative Example 1, the total amount, the first amount and the second amount of the polyamide-imide, the amount of the first solvent, and the amount of the third solvent are shown in Table 1 below.
[0181] <Comparative Example 2>
[0182] 35.80 parts by weight of silica dispersion C (50nmSP-AD1, Admatechs) in which silica particles having an average particle diameter of 50 nm are dispersed in a DMAc (NlN-dimethylacetamide) solution (second solvent) in an amount of 20% by weight is loaded into another 1L reactor, 371.73 parts by weight of DMAc (third solvent) are added thereto, followed by stirring. Then, 64.40 parts by weight (second amount) of polyamide-imide (polyimide resin powder) prepared in Preparation Example 1 as a solid powder are added to the stirred solution, followed by further stirring to prepare a mixed solution in which the silica dispersion is mixed with a polyimide resin. The mixed solution is a polyimide resin solution in which silica particles are dispersed.
[0183] The obtained mixed solution was casted. The casting and subsequent processes were performed in the same manner as in Example 1 to prepare a polyimide-based film 100 .
[0184] <Comparative Example 3>
[0185] 35.80 parts by weight of silica dispersion D (DMAc-ST-ZL, Nissan) in which silica particles having an average particle diameter of 70 nm were dispersed in a DMAc (N, N-dimethylacetamide) solution (second solvent) in an amount of 20% by weight was loaded into another 1L reactor, 371.06 parts by weight of DMAc (third solvent) was added thereto, followed by stirring. Then, 64.40 parts by weight (second amount) of polyamide-imide (polyimide resin powder) prepared in Preparation Example 1 as a solid powder was added to the stirred solution, followed by further stirring to prepare a mixed solution in which the silica dispersion was mixed with a polyimide resin. The mixed solution is a polyimide resin solution in which silica particles are dispersed.
[0186] The obtained mixed solution was casted. The casting and subsequent processes were performed in the same manner as in Example 1 to prepare a polyimide-based film 100 .
[0187] <Comparative Examples 4 to 7>
[0188] The polyimide-based films 100 of Comparative Examples 4 to 7 were prepared in the same manner as Example 1 by changing only the type and total amount of the silica dispersion, the first and second amounts of the polyamide-imide, the first and third solvent amounts.
[0189] The details of the silica dispersions of Comparative Examples 4 to 7, the total amount, the first amount and the second amount of the polyamide-imide, the amount of the first solvent, and the amount of the third solvent are shown in Table 1 below.
[0190] [Table 1]
[0191]
[0192]
[0193]
[0194] <Measurement Example>
[0195] The following measurements were performed on the polyimide-based films prepared in Examples 1 to 7 and Comparative Examples 1 to 7.
[0196] 1) Measurement of density ratio (DR) between true density and density gradient tube density
[0197] The true density and density gradient tube density of the polyimide-based film are measured as follows, and the density ratio (DR) of the true density to the density gradient tube density is calculated according to the following formula using the measured true density and density gradient tube density.
[0198] <Formula 1>
[0199] DR = true density / density of density gradient tube
[0200] (1) Measurement of true density
[0201] Specifically, a sample (10×10 cm 2 ) Finely cut into 1×1cm 2 The following fragments are placed in a sample holder together with iron beads (crushing agent). A low-temperature crusher (Japan Analytical Industry, JFC-300) is filled with liquid nitrogen to more than 2 / 3, the sample holder containing the cut sample is mounted on the low-temperature crusher, and then the chamber is closed. After precooling for 15 minutes, the sample is crushed using a low-temperature crusher with a running time of more than 15 minutes. The true density of the powdered sample of film 100 is measured seven times using an AccuPyc 1340 densimeter (using helium) produced by Micromeritics Co., Ltd. The average value of the true density values remaining after removing the highest and lowest values from the measured true density of the powdered film 100 is taken as the true density of film 100.
[0202] (2) Measurement of density gradient tube density
[0203] The density gradient tube density of the polyimide-based film 100 may be obtained by using a density gradient tube according to ASTM D1505 standard.
[0204] 2) Measurement of particle volume concentration (PVC)
[0205] The volume of the filler (V1) and the volume of the matrix (V2) of the polyimide film, as well as the particle volume concentration (PVC) of the polyimide film are calculated according to the following formula 2:
[0206] <Formula 2>
[0207] PVC (%) = [V1 / (V1+V2)] * 100
[0208] Where V1 is the volume of the filler and V2 is the volume of the matrix.
[0209] The volume (V1) of the filler can be calculated by dividing the mass of the filler by its density. Specifically, the volume (V1) of the filler can be calculated by measuring the mass and density of the filler included in the film 100. For example, the mass of the filler can be determined by measuring the weight of the filler added when preparing the film 100. The density of the filler can be measured using a method for measuring true density or a method for measuring density gradient tube density.
[0210] The volume (V2) of the matrix can be calculated by dividing the mass of the matrix by its density. Specifically, the volume (V2) of the matrix can be calculated by measuring the mass and density of the matrix included in the film 100. For example, the mass of the matrix can be determined by measuring the weight of the matrix added when preparing the film 100. The density of the matrix can be measured using a method for measuring true density or a method for measuring density gradient tube density.
[0211] 3) Young's modulus and elongation: The Young's modulus and elongation of the polyimide film were measured using a universal tensile testing machine produced by Instron according to ASTM D885.
[0212] 4) Indentation hardness: The prepared polyimide film was cut into pieces with a size of 2 cm×10 cm, and its HV value was measured using HM2000Fischerscope (Helmut Fischer) (measurement conditions: F=12.000mN / 12 seconds, C=5.0 seconds). The HV value was measured 7 times in total, and the average value of the remaining HV values after excluding the highest and lowest values from the 7 HV values was calculated to obtain the indentation hardness of the polyimide film.
[0213] 5) Light transmittance (%): According to ASTM E313, the average light transmittance at a wavelength of 360 nm to 740 nm was measured using a spectrophotometer (CM-3700D, KONICAMINOLTA).
[0214] 6) Yellowness (yellowness index, YI): Yellowness (yellowness index, YI) was measured using a spectrophotometer (CM-3700D, KONICA MINOLTA) according to ASTM E313.
[0215] 7) Haze: The prepared polyimide-based film was cut into pieces of 50 mm×50 mm, and measured five times using a haze meter (model name: HM-150) produced by Murakami Color Research Laboratory according to ASTM D1003, and the average value thereof was taken as the haze.
[0216] The measurement results are shown in Tables 2 and 3 below.
[0217] [Table 2]
[0218]
[0219]
[0220] [Table 3]
[0221]
[0222] It can be seen from the measurement results shown in Tables 2 and 3 that the density ratio (DR) of the true density of the polyimide film 100 according to the embodiment of the present disclosure to the density gradient tube density is less than 1.10, thereby exhibiting excellent mechanical properties such as Young's modulus, elongation and indentation hardness, and excellent optical properties such as excellent light transmittance, low yellowness (yellowness index, YI) and low haze.
[0223] However, according to comparison example 1 in which the amount of filler is higher than 50 weight % based on the total weight of the polyimide film, the density ratio (DR) of the true density to the density of the density gradient tube is greater than 1.10, the particle volume concentration (PVC) is greater than 38%, the Young's modulus is less than 5.0 GPa, the elongation is less than 15%, the indentation hardness is less than 45%, and the yellowness (yellowness index, YI) is greater than 3.0.
[0224] According to comparison example 2, in which the polyimide resin powder is mixed with a filler dispersion without separating the polyimide resin powder into a first amount and a second amount, the density ratio (DR) of the true density to the density gradient tube density of the polyimide film 100 is greater than 1.10, the Young's modulus is less than 5.0 GPa, the elongation is less than 15%, the indentation hardness is less than 45%, and the yellowness (yellowness index, YI) is greater than 3.0.
[0225] According to comparison example 3, in which the polyimide resin powder is mixed with the filler dispersion without separating the polyimide resin powder into the first amount and the second amount and the average particle size of the filler is greater than 50 nm, the density ratio (DR) of the true density to the density of the density gradient tube is greater than 1.10, the Young's modulus is less than 5.0 GPa, the elongation is less than 15%, the indentation hardness is less than 45%, the yellowness (yellowness index, YI) is greater than 3.0, and the haze is greater than 1%.
[0226] According to comparison example 4 in which the average particle size of the filler is greater than 50 nm, the density ratio (DR) of the true density of the polyimide film 100 to the density of the density gradient tube is greater than 1.10, the Young's modulus is less than 5.0 GPa, the elongation is less than 15%, the indentation hardness is less than 45%, the yellowness (yellowness index, YI) is greater than 3.0, and the haze is greater than 1%.
[0227] According to comparison example 5, in which the first amount of polyimide resin powder based on the weight of the filler is less than 0.5%, the density ratio (DR) of the true density to the density of the density gradient tube is greater than 1.10, the Young's modulus is less than 5.0 GPa, the elongation is less than 15%, the indentation hardness is less than 45%, and the yellowness (yellowness index, YI) is greater than 3.0.
[0228] According to Comparative Example 6, in which the first amount of polyimide resin powder based on the weight of the filler is higher than 10%, the density ratio (DR) of the true density to the density of the density gradient tube is greater than 1.10, the Young's modulus is less than 5.0 GPa, the elongation is less than 15%, the indentation hardness is less than 45%, and the yellowness (yellowness index, YI) is greater than 3.0.
[0229] According to Comparative Example 7, in which the amount of filler is less than 5 weight % based on the total weight of the polyimide film, the density ratio (DR) of the true density to the density of the density gradient tube is greater than 1.10, the Young's modulus is less than 5.0 GPa, the elongation is less than 15%, the indentation hardness is less than 45%, and the yellowness (yellowness index, YI) is greater than 3.0.
[0230] [Explanation of Reference Numerals]
[0231] 100: Polyimide film
[0232] 110: Polyimide matrix
[0233] 120: Filler
[0234] 200: Display device
[0235] 501: Display panel
Claims
1. A polyimide film comprising: Polyimide matrix; and A filler dispersed in the polyimide matrix, Wherein, the density ratio (DR) of the true density of the polyimide film to the density of the density gradient tube is less than 1.10, Wherein, the density ratio is calculated according to the following formula 1: <Formula 1> Density ratio (DR) = true density / density gradient tube density, The particle volume concentration of the polyimide film, i.e., PVC, is 5% to 38%. The particle volume concentration, i.e., PVC, is calculated according to the following formula 2: <Formula 2> PVC (%) = [V1 / (V1+V2)] * 100 Wherein, V1 is the volume of the filler, and V2 is the volume of the matrix.
2. The polyimide film according to claim 1, wherein The filler includes silicon dioxide (SiO2).
3. The polyimide film according to claim 2, wherein: At least a portion of the silicon dioxide (SiO2) is surface-treated with an organic compound having an alkoxy group.
4. The polyimide film according to claim 2, wherein: The average particle size of the filler is 5 nm to 50 nm.
5. The polyimide film according to claim 1, wherein The filler is present in an amount of 5 wt % to 50 wt % based on the total weight of the polyimide-based film.
6. The polyimide film according to claim 1, wherein: The Young's modulus of the polyimide film is 5.0 GPa or more.
7. The polyimide film according to claim 1, wherein: The elongation of the polyimide film is greater than 15%.
8. The polyimide film according to claim 1, wherein The indentation hardness of the polyimide film is 45 or more.
9. The polyimide film according to claim 1, wherein: The yellowness of the polyimide film, that is, the yellowness index YI, is 3 or less.
10. The polyimide film according to claim 1, wherein The haze of the polyimide film is less than 1%.
11. The polyimide film according to claim 1, wherein: The light transmittance of the polyimide film is above 85%.
12. A display device, comprising: Display panel; and The polyimide film according to any one of claims 1 to 11 is disposed on the display panel.