A separator, a method for preparing the same, and a secondary battery and an electric device containing the same

By using a porous isolation film in a lithium-ion battery to control its porosity gradient, the problem of lithium precipitation in the center of the pole piece is solved, and the safety and cycle performance of the battery are improved.

CN115810874BActive Publication Date: 2024-10-11CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202210810267.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-11
Publication Date
2024-10-11
Estimated Expiration
2042-07-11

AI Technical Summary

Technical Problem

During the cycling process of lithium-ion batteries, lithium precipitation is prone to occur in the center of the pole piece, which affects the cycle capacity retention rate and safety performance of the battery.

Method used

A porous isolation membrane is used, which has the characteristic of decreasing porosity gradient from the center to the edge in the direction perpendicular to the thickness. The porosity gradient is controlled through the stretching process to enhance the extrusion and reflux efficiency of the electrolyte and prevent the pole pieces from Lithium is extracted in the center.

Benefits of technology

Significantly reduce the risk of lithium precipitation in the center of the pole piece, improve the safety performance and cycle performance of the battery core, and extend the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115810874B_ABST
    Figure CN115810874B_ABST
Patent Text Reader

Abstract

The present invention relates to a separator, a preparation method thereof, a secondary battery and an electric device containing the separator, wherein the separator is a porous separator; in a direction perpendicular to the thickness of the separator, the porosity gradient of the separator decreases along the center to the edge of the separator. After the separator is assembled into a secondary battery cell, the electrolyte extrusion and reflux efficiency in the central area can be increased, thereby enhancing the wettability of the electrolyte to the pores of the pole piece, while preventing the problem of lithium deposition in the center of the pole piece caused by poor electrolyte infiltration due to insufficient standing time between battery charge and discharge processes, thereby improving the safety performance and cycle performance of the battery cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary batteries, and in particular to an isolation film, a preparation method thereof, and a secondary battery and an electric device comprising the isolation film. Background Art

[0002] Non-aqueous secondary batteries represented by lithium-ion batteries have the advantages of high energy density and high operating voltage, and have been widely used in portable electronic devices (mobile phones, computers, cameras) and power battery vehicles.

[0003] Currently, common single-cell lithium-ion batteries are assembled from bare cells, and the production methods of bare cells mainly include stacking and winding. In the wound bare cell, the two sides with larger side areas are called large sides, and the other two sides are called narrow sides. During the battery cycle, it can be found that lithium deposition is prone to occur in the center of the large-surface electrode, which affects the battery's cycle capacity retention rate. In stacked or other types of bare cells, similar phenomena also exist in the center of the electrode. Summary of the invention

[0004] The object of the present invention is to provide an isolation membrane, a preparation method thereof, a secondary battery and an electrical device comprising the same. When the isolation membrane is used in a secondary battery, the risk of lithium plating in the center of the electrode can be significantly reduced, and the safety performance and cycle performance of the battery cell can be improved.

[0005] To this end, in a first aspect, the present invention provides an isolation membrane, which is a porous isolation membrane; in a thickness direction perpendicular to the isolation membrane, along the center to the edge of the isolation membrane, the porosity gradient of the isolation membrane decreases.

[0006] According to the technical solution of the present invention, the central area of ​​the isolation membrane has better electrolyte extrusion and reflux efficiency than the edge area, thereby enhancing the wettability of the electrolyte to the pores in the central area of ​​the electrode, preventing lithium deposition in the center of the electrode caused by poor electrolyte wetting during battery charging and discharging, and improving the safety and cycle performance of the battery cell.

[0007] In some embodiments, the thickness direction perpendicular to the isolation membrane includes a length direction and a width direction. In the length direction and / or the width direction of the isolation membrane, the porosity gradient of the isolation membrane decreases from the center to the edge of the isolation membrane.

[0008] In some embodiments, in the width direction of the isolation membrane, the porosity gradient of the isolation membrane decreases from the center to the edge of the isolation membrane.

[0009] In some embodiments, in the length direction of the isolation membrane, the porosity gradient of the isolation membrane decreases from the center to the edge of the isolation membrane.

[0010] In some embodiments, in the width direction and the length direction of the isolation membrane, the porosity gradient of the isolation membrane decreases from the center to the edge of the isolation membrane.

[0011] In some embodiments, in the width direction and / or length direction of the isolation membrane, the isolation membrane is divided into n regions in sequence from the center to the edge, where n is a positive integer greater than or equal to 2; for any two regions, the region closer to the center of the isolation membrane has a larger porosity than the region farther from the center of the isolation membrane.

[0012] In some embodiments, in the width direction and / or length direction of the isolation membrane, the isolation membrane is divided into n regions in sequence from the center to the edge, where n is a positive integer greater than or equal to 2; the region closest to the center of the isolation membrane is the first region, and the region farthest from the center of the isolation membrane is the nth region; the difference between the porosity of the first region and the porosity of the nth region is 2% to 20%.

[0013] In some embodiments, the porosity of the first region is 30% to 60%, and the porosity of the nth region is 20% to 50%.

[0014] In some embodiments, the distance from the center to the edge of the isolation membrane is W, and the isolation membrane is divided into two regions along the direction from the center to the edge. The range of 0 to 1 / 3W from the center of the isolation membrane is the first region, and the porosity of the first region is 30% to 60%; the range of 1 / 3W to W from the center of the isolation membrane is the second region, and the porosity of the second region is 20% to 50%.

[0015] In some embodiments, the isolation film has a thickness of 5 to 60 μm.

[0016] In some embodiments, the isolation membrane is a single-layer membrane or a composite membrane with two or more layers.

[0017] In some embodiments, the material of the isolation membrane includes one or a combination of two or more selected from the following group: glass fiber, non-woven fabric, polyvinylidene fluoride, polyolefin (such as polyethylene, polypropylene).

[0018] In some embodiments, the isolation membrane is made of a combination of polyethylene and polypropylene.

[0019] In some embodiments, the isolation membrane is made of polyolefin with a molecular weight of 800,000 to 1.6 million.

[0020] The second aspect of the present invention provides a method for preparing the isolation membrane described in the first aspect of the present invention, which comprises: weighing raw materials for preparing the isolation membrane, wherein the raw materials include a substrate, a pore-forming agent and an antioxidant; after mixing the raw materials evenly, sequentially performing extrusion, stretching, extraction and shaping; wherein the stretching step comprises: stretching in a direction perpendicular to the thickness of the isolation membrane, and the stretching ratio gradient decreases from the center to the edge of the isolation membrane to reduce the porosity gradient.

[0021] According to the technical solution of the present invention, a separator with a gradient porosity can be prepared by applying different stretching ratios during the stretching process. The preparation method can be carried out using existing separator production equipment and has the advantages of simple operation, no increase in cost, good stability, etc.

[0022] In some embodiments, the stretching step comprises: stretching along the width direction of the separator, and the stretching ratio gradient decreases from the center to the edge of the separator to reduce the porosity gradient; and / or,

[0023] The separator is stretched along the length direction, and the stretching ratio decreases gradually from the center to the edge of the separator to reduce the porosity gradient.

[0024] In some embodiments, the stretching step includes: stretching along the width direction of the isolation membrane, reducing the stretching ratio gradient from the center to the edge of the isolation membrane to reduce the porosity gradient; and uniformly stretching along the length direction of the isolation membrane.

[0025] In some embodiments, the stretching step includes: stretching along the length direction of the isolation membrane, with the stretching ratio gradient decreasing from the center to the edge of the isolation membrane to reduce the porosity gradient; and uniformly stretching along the width direction of the isolation membrane.

[0026] In some embodiments, the isolation membrane is stretched along the width direction and / or length direction, and is divided into n regions in sequence from the center to the edge of the isolation membrane, where n is a positive integer greater than or equal to 2; for any two regions, a larger stretching ratio is applied to the region closer to the center of the isolation membrane than to the region farther from the center of the isolation membrane.

[0027] In some embodiments, the distance from the center to the edge of the isolation membrane is W, and the range of 0 to 1 / 3W from the center of the isolation membrane is the first region, and the first region is stretched by 4 to 8 times in the stretching step; the range of 1 / 3W to W from the center of the isolation membrane is the second region, and the second region is stretched by 2 to 4 times in the stretching step.

[0028] In some embodiments, the raw materials include, by weight: 30 to 65 parts of a base material, 10 to 40 parts of a pore former, and 5 to 10 parts of an antioxidant.

[0029] In some embodiments, the substrate includes one or a combination of two or more selected from the following group: glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride.

[0030] In some embodiments, the pore former is an organic pore former and / or an inorganic pore former.

[0031] In some embodiments, the antioxidant includes one or a combination of two or more selected from the following groups: 4,4-thiobis(6-tert-butyl-m-cresol), dibutylhydroxytoluene, phosphite, tert-butylhydroquinone, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid octadecanoate, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 2-tert-butyl-6-methylphenol, N,N'-di-β-naphthyl-p-phenylenediamine, dilauryl thiodipropionate, tris(nonylphenyl) phosphite, and triphenyl phosphite.

[0032] A third aspect of the present invention provides a secondary battery, which includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator between the positive electrode sheet and the negative electrode sheet, wherein the separator is the separator described in the first aspect of the present invention.

[0033] In some embodiments, the secondary battery is one of a lithium ion battery, a sodium ion battery, or a potassium ion battery.

[0034] A fourth aspect of the present invention provides a battery module, which includes the secondary battery described in the third aspect of the present invention.

[0035] A fifth aspect of the present invention provides a battery pack, which includes the battery module described in the fourth aspect of the present invention.

[0036] A sixth aspect of the present invention provides an electrical device comprising at least one of the secondary battery described in the third aspect of the present invention, the battery module described in the fourth aspect of the present invention, or the battery pack provided in the fifth aspect of the present invention.

[0037] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0038] The separator provided by the present invention has a gradient porosity distribution in the length direction and / or width direction, and the porosity decreases from the center to the edge direction. After being assembled into a battery cell, the electrolyte extrusion and reflux efficiency in the central area can be increased, thereby enhancing the electrolyte's wettability to the pole piece pores, while preventing the problem of lithium deposition in the pole piece center caused by poor electrolyte infiltration due to insufficient standing time between battery charging and discharging processes, thereby improving the safety performance and cycle performance of the battery cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. Moreover, the same reference symbols are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:

[0040] Figure 1 is a schematic diagram of an isolation membrane according to one embodiment of the present invention;

[0041] Figure 2 is a schematic diagram of a secondary battery according to one embodiment of the present invention;

[0042] Figure 3 yes Figure 2 An exploded view of a secondary battery according to an embodiment of the present invention is shown;

[0043] Figure 4 is a schematic diagram of a battery module according to an embodiment of the present invention;

[0044] Figure 5 is a schematic diagram of a battery pack according to an embodiment of the present invention;

[0045] Figure 6 yes Figure 5 An exploded view of a battery pack according to an embodiment of the present invention is shown;

[0046] Figure 7 is a schematic diagram of an electrical device using a secondary battery according to an embodiment of the present invention as a power source;

[0047] Description of reference numerals:

[0048] 1 battery pack; 2 upper box; 3 lower box; 4 battery module; 5 lithium-ion battery; 51 shell; 52 electrode assembly; 53 top cover assembly; 6 isolation membrane; 61 first area; 62 second area. DETAILED DESCRIPTION

[0049] The exemplary embodiments of the present disclosure will be described in more detail below with reference to the accompanying drawings. Although the exemplary embodiments of the present disclosure are shown in the accompanying drawings, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present disclosure and to fully convey the scope of the present disclosure to those skilled in the art.

[0050] The "range" disclosed in the present invention is defined in the form of a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way is inclusive and can be combined arbitrarily, that is, any lower limit can be combined with any upper limit to form a range.

[0051] If not otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form a new technical solution.

[0052] Unless otherwise specified, all technical features and optional technical features of the present invention can be combined with each other to form a new technical solution.

[0053] If not specifically stated, all steps of the present invention may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially.

[0054] In the prior art, regarding secondary batteries - lithium-ion batteries as an example - common single-cell lithium-ion batteries are assembled from bare cells, and the production methods of bare cells mainly include stacking and winding. In the wound bare cell, the two sides with larger side areas are called large sides, and the other two sides are called narrow sides. During the battery cycle, it can be found that lithium deposition is prone to occur in the center of the large-surface electrode, and it affects the battery's cycle capacity retention rate. In stacked or other types of bare cells, a similar phenomenon also exists in the center of the electrode.

[0055] In order to solve the above problems, the present invention first explores and analyzes the causes of the above defects. The pole piece of a lithium-ion battery has a porous structure. Solid materials such as active materials, conductive agents and binders constitute the skeleton of the porous structure, and the pores are filled with electrolyte. During the charge and discharge cycle of the lithium-ion battery, the active materials on the positive and negative pole pieces release lithium, which will cause the pole piece volume to shrink or expand. Since the lithium-ion battery is subjected to a certain preload in the module or battery pack, the expansion of the pole piece volume is subject to a certain restriction. Therefore, the expansion of the solid material on the pole piece will cause the volume of the pole piece pores to shrink, thereby squeezing the electrolyte inside the pole piece pores into the space outside the pole piece. Based on a similar principle, when the pole piece shrinks, the pole piece pore volume increases, and the electrolyte in the space outside the pole piece will be sucked into the pole piece pores. During the cycle of the lithium-ion battery, the shrinkage and expansion of the pole piece accompanied by the extrusion and absorption of the electrolyte has been occurring.

[0056] Taking a wound cell as an example, during the battery cycle, the volume change of the center area of ​​the large-surface electrode sheet is greater than the volume change of the edge area on the side of the large-surface electrode sheet with the pole ear and the opposite side, so the amount of electrolyte squeezed out or absorbed by the center area of ​​the large-surface electrode sheet is also higher than the edge areas on both sides. If the battery cell is left stationary for too short a time during the charge and discharge cycle, the squeezed electrolyte will not be absorbed into the pores of the electrode sheet, resulting in poor electrolyte infiltration, which will affect the cycle capacity retention rate at the least, and cause lithium deposition in the center of the large surface of the battery cell at the worst.

[0057] In addition, a similar situation exists for stacked battery cells. The volume change in the center area of ​​the electrode is greater than the volume change in the edge area on the side of the electrode with the electrode ear and the opposite side, which can easily cause poor electrolyte infiltration in the center area of ​​the electrode, affecting the cycle capacity retention rate and causing lithium plating.

[0058] Based on this, the present invention proposes the following technical solutions and specific implementation methods.

[0059] In some embodiments, a separator is provided, which is a porous separator; in a direction perpendicular to the thickness of the separator and along a direction from the center to the edge of the separator, the porosity gradient of the separator decreases.

[0060] The following terms are defined and / or explained to better understand the present invention:

[0061] "Width direction" is also called transverse direction, TD for short; "length direction" is also called machine direction, MD for short. For a thin film isolation membrane with a three-dimensional (XYZ) structure, which has a structure in which the Z dimension is significantly smaller than its X and Y dimensions, the X dimension is defined as the thickness direction, the X dimension is defined as the length direction, and the Y dimension is defined as the width direction, Z<Y≤X. It should be pointed out that for the isolation membrane, since it is usually used to prepare folded or wound battery cells, it has the characteristic of Y<X, that is, in some embodiments, the length of the isolation membrane described in the present invention is greater than its width; in addition, according to the technical solution of the present invention, when the isolation membrane is used to prepare other types of battery cells, it may also have the characteristic of Y=X, that is, in some embodiments, the length of the isolation membrane described in the present invention is equal to its width.

[0062] Therefore, the porosity distribution characteristics of the isolation membrane can be described from the length direction, width direction and thickness direction respectively. According to the technical solution of the present invention, the porosity distribution of the isolation membrane is limited along the thickness direction perpendicular to the isolation membrane (i.e., the length direction and / or width direction); no limitation is made in the thickness direction of the isolation membrane, and the isolation membrane of the present invention can have uniform porosity along the thickness direction.

[0063] The term "center" refers to a point along a selected dimension of the separator that is equidistant from the two edges of the separator.

[0064] Since the porosity of the central area of ​​the isolation membrane is higher than that of the edge area, it can facilitate the extrusion and backflow of the electrolyte and enhance the wettability of the electrolyte to the pores in the central area of ​​the electrode, thereby preventing lithium deposition in the center of the large-surface electrode caused by poor electrolyte wetting during the cycle.

[0065] In some embodiments, the porosity gradient of the separator decreases along the center to the edge of the separator in the width direction and / or the length direction of the separator.

[0066] In some embodiments, in the width direction of the separator, the porosity gradient of the separator decreases from the center to the edge of the separator.

[0067] In some embodiments, in the width direction of the isolation membrane, the porosity gradient of the isolation membrane decreases from the center to the edge of the isolation membrane; and the isolation membrane has uniform porosity along its length direction.

[0068] Those skilled in the art know that, whether for wound cells or laminated cells, they are assembled using an isolating membrane whose length is greater than the width. In the wound cell, the positive electrode sheet, the isolating membrane, and the negative electrode sheet are stacked in sequence, then wound, and the tabs are set; this allows the two edges of the isolating membrane along the width direction to be arranged opposite to the side of the large-surface electrode sheet with the tabs and its opposite edge. When the isolating membrane has a porosity that decreases gradually from the center to the edge in the width direction, since the porosity of the central area of ​​the isolating membrane is larger than that of the edge area, it can help the extrusion and reflux of the electrolyte, and enhance the wettability of the electrolyte to the pores in the central area of ​​the large-surface electrode sheet, thereby preventing the problem of lithium precipitation in the center of the large-surface electrode sheet caused by poor electrolyte infiltration during the cycle.

[0069] In the laminated battery cell, the positive and negative electrode sheets are alternately placed on the Z-shaped folded separator and stacked, and the pole ears are arranged; this makes the two edges of the separator along the width direction opposite to the side of the pole piece with the pole ears and the opposite side edge. When the separator has a porosity that decreases from the center to the edge in the width direction, since the porosity of the central area of ​​the separator is larger than that of the edge area, it can help the extrusion and reflux of the electrolyte, and enhance the wettability of the electrolyte to the pores in the central area of ​​the pole piece, thereby preventing the problem of lithium precipitation in the center of the pole piece caused by poor electrolyte infiltration during the cycle.

[0070] In some embodiments, the porosity gradient of the separator decreases along the center to the edge of the separator in the width direction and the length direction of the separator.

[0071] There are other types of battery cells in the art, such as battery cells assembled by stacking a positive electrode monolith, a separator monolith, and a negative electrode monolith in sequence and setting a tab. When the separator has a porosity that decreases gradually from the center to the edge in the width and length directions, since the porosity of the center area of ​​the separator is larger than that of the edge area, it can help the extrusion and reflux of the electrolyte, enhance the wettability of the electrolyte to the pores in the center area of ​​the pole piece, thereby preventing the problem of lithium deposition in the center of the pole piece caused by poor electrolyte infiltration during the cycle.

[0072] In some embodiments, the porosity gradient of the separator decreases along the length direction of the separator from the center to the edge of the separator. When the separator is applied to the above-mentioned battery cell, it can also enhance the wettability of the electrolyte to the pores in the central area of ​​the pole piece to a certain extent, thereby preventing the problem of lithium deposition in the center of the pole piece caused by poor electrolyte infiltration during the cycle.

[0073] In some embodiments, in the width direction of the isolation membrane, the isolation membrane is divided into n regions in sequence from the center to the edge, where n is a positive integer greater than or equal to 2; the region closest to the center of the isolation membrane is the first region, and the region farthest from the center of the isolation membrane is the nth region; for any two regions, the region closer to the center of the isolation membrane has a greater porosity than the region farther from the center of the isolation membrane. Wherein, n can be 2, 3, 4, 5, etc., and is preferably 2 or 3 for ease of processing.

[0074] In some embodiments, in the length direction of the isolation membrane, the isolation membrane is divided into n regions in sequence from the center to the edge, where n is a positive integer greater than or equal to 2; the region closest to the center of the isolation membrane is the first region, and the region farthest from the center of the isolation membrane is the nth region; for any two regions, the region closer to the center of the isolation membrane has a greater porosity than the region farther from the center of the isolation membrane. Wherein, n can be 2, 3, 4, 5, etc., and is preferably 2 or 3 for ease of processing.

[0075] In some embodiments, the isolation membrane is divided into n regions in the width direction and the length direction along the center to the edge direction of the isolation membrane, where n is a positive integer greater than or equal to 2; the region closest to the center of the isolation membrane is the first region, and the region farthest from the center of the isolation membrane is the nth region; for any two regions, the region closer to the center of the isolation membrane has a greater porosity than the region farther from the center of the isolation membrane. Wherein, n can be 2, 3, 4, 5, etc.

[0076] In some embodiments, the difference between the porosity of the first region and the porosity of the nth region is 2% to 20%; for example, 2%, 4%, 5%, 8%, 10%, 12%, 15%, 17%, 20%, etc.

[0077] According to the technical solution of the present invention, for the difference in porosity between the first region and the nth region, if the difference is too small, the difference in ion penetration in the electrolyte through the central region and the edge region of the isolation membrane cannot be reflected; if the difference is too large, it will cause the concentration difference of electrolyte ions in the pores of the central region and the edge region of the isolation membrane to be too large, resulting in a large difference in polarization, and then leading to uneven lithium insertion.

[0078] In some embodiments, the porosity of the first region is 30% to 60%, for example 30%, 35%, 40%, 45%, 50%, 55%, 60%, etc.; the porosity of the nth region is 20% to 50%, for example 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc.

[0079] According to the technical solution of the present invention, the porosity of the first region is 30% to 60%; the porosity of the nth region is 20% to 50%. During charging, due to the slow kinetics of lithium insertion in the negative electrode, if the porosity is too large (for example, greater than 60%), the lithium ion concentration on the negative electrode surface will be too high, and lithium deposition will easily occur; if the porosity is too small (for example, less than 20%), the resistance of lithium ions passing through the isolation membrane will be too large, and the liquid phase polarization will be large, which will cause the voltage to reach the cut-off voltage earlier, resulting in a decrease in the actual capacity, but the risk of lithium deposition in the negative electrode during charging will be reduced.

[0080] Figure 1 6 is an example of a separator. Figure 1 In the width direction of the isolation membrane 6, the distance from the center to the edge of the isolation membrane 6 is W, the range of 0 to 1 / 3W from the center of the isolation membrane is the first region 61, and the porosity of the first region 61 is 30% to 60%; the range of 1 / 3W to W from the center of the isolation membrane 6 is the second region 62, and the porosity of the second region 62 is 20% to 50%.

[0081] In some embodiments, the isolation film has a thickness of 5 to 60 μm, for example, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, etc.

[0082] According to the technical solution of the present invention, if the thickness of the isolation membrane is too thin and the mechanical strength is low, it is very easy to pierce the isolation membrane when lithium deposition occurs, causing a short circuit in the battery cell, thereby causing thermal runaway; if the thickness of the isolation membrane is too thick, the volume energy density of the battery cell will decrease.

[0083] In some embodiments, the isolation membrane is a single-layer membrane or a composite membrane of two or more layers.

[0084] In some embodiments, the material of the isolation membrane includes one or a combination of two or more selected from the following group: glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride.

[0085] In some embodiments, a method for preparing the isolation membrane of the present invention is provided, comprising: weighing raw materials for preparing the isolation membrane, the raw materials comprising a substrate, a pore-forming agent and an antioxidant; after mixing the above raw materials evenly, sequentially performing extrusion, stretching, extraction and shaping; wherein the stretching step comprises: stretching in a direction perpendicular to the thickness of the isolation membrane, and the stretching ratio gradient decreases from the center to the edge of the isolation membrane to reduce the porosity gradient.

[0086] By applying different stretching ratios during the stretching process, an isolation membrane with a gradient porosity can be prepared. The preparation method can be carried out using existing isolation membrane production equipment and has the advantages of simple operation, no increase in cost, good stability, etc.

[0087] In some embodiments, the stretching step includes: stretching along the width direction of the separator, and the stretching ratio gradient decreases from the center to the edge of the separator to reduce the porosity gradient; and,

[0088] The separator is stretched along the length direction, and the stretching ratio decreases gradually from the center to the edge of the separator to reduce the porosity gradient.

[0089] In some embodiments, the stretching step includes: stretching along the width direction of the separator, and the stretching ratio gradient decreases from the center to the edge of the separator to reduce the porosity gradient; and,

[0090] The separator is stretched uniformly along the length direction.

[0091] In some embodiments, the stretching step includes: stretching along the length direction of the separator, with the stretching ratio gradually decreasing from the center to the edge of the separator to reduce the porosity gradient; and uniformly stretching along the width direction of the separator.

[0092] In some embodiments, along the width direction of the isolation membrane, it is divided into n regions in sequence from the center to the edge of the isolation membrane, where n is a positive integer greater than or equal to 2; the region closest to the center of the isolation membrane is the first region, and the region farthest from the center of the isolation membrane is the nth region; stretching is performed along the width direction of the isolation membrane, and for any two regions, a larger stretching ratio is applied to the region closer to the center of the isolation membrane than to the region farther from the center of the isolation membrane.

[0093] In some embodiments, along the length direction of the isolation membrane, the isolation membrane is divided into n regions in sequence from the center to the edge, where n is a positive integer greater than or equal to 2; the region closest to the center of the isolation membrane is the first region, and the region farthest from the center of the isolation membrane is the nth region; the isolation membrane is stretched along the length direction, and for any two regions, a larger stretching ratio is applied to the region closer to the center of the isolation membrane than to the region farther from the center of the isolation membrane.

[0094] In some embodiments, in the width direction and the length direction of the isolation membrane, the isolation membrane is divided into n regions in sequence from the center to the edge direction, where n is a positive integer greater than or equal to 2; the region closest to the center of the isolation membrane is the first region, and the region farthest from the center of the isolation membrane is the nth region; the isolation membrane is stretched along the width direction and the length direction, and for any two regions, a larger stretching ratio is applied to the region closer to the center of the isolation membrane than to the region farther from the center of the isolation membrane.

[0095] In some embodiments, the first region is stretched by 4 to 8 times in the stretching step, for example, 4 times, 5 times, 6 times, 7 times, 8 times, etc.; the nth region is stretched by 2 to 4 times in the stretching step, for example, 2 times, 2.5 times, 3 times, 3.5 times, 4 times, etc.

[0096] In some embodiments, in the width direction of the isolation membrane, the distance from the center to the edge of the isolation membrane is W, and the range of 0 to 1 / 3W from the center of the isolation membrane is the first region, and the first region is stretched by 4 to 8 times in the stretching step; the range of 1 / 3W to W from the center of the isolation membrane is the second region, and the second region is stretched by 2 to 4 times in the stretching step.

[0097] In some embodiments, the raw materials include, by weight: 30 to 65 parts of substrate, 10 to 40 parts of pore formers, and 5 to 10 parts of antioxidants. For example, the weight of the substrate can be selected from 30 parts, 40 parts, 50 parts, 60 parts, 65 parts, etc.; the weight of the pore former can be selected from 10 parts, 20 parts, 30 parts, 40 parts, etc.; the weight of the antioxidant can be selected from 5 parts, 6 parts, 8 parts, 10 parts, etc.

[0098] In some embodiments, the substrate includes one or a combination of two or more selected from the following group: glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride.

[0099] In some embodiments, the pore former is an organic pore former and / or an inorganic pore former. For example, the organic pore former may include one or a combination of two or more selected from the group consisting of white oil, paraffin oil, kerosene, or dioctyl phthalate (DOP). For example, the inorganic pore former may include one or a combination of two or more selected from the group consisting of sodium carbonate, potassium carbonate, lithium carbonate, cobalt carbonate, ammonium bicarbonate, ammonium chloride, and ammonium nitrate.

[0100] In some embodiments, the antioxidant includes one or a combination of two or more selected from the following groups: 4,4-thiobis(6-tert-butyl-m-cresol), dibutylhydroxytoluene, phosphite, tert-butylhydroquinone, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid octadecanoate, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 2-tert-butyl-6-methylphenol, N,N'-di-β-naphthyl-p-phenylenediamine, dilauryl thiodipropionate, tris(nonylphenyl) phosphite, and triphenyl phosphite.

[0101] In some embodiments, a method for preparing the isolation membrane of the present invention is provided, comprising:

[0102] 1) Feeding: Weigh the raw materials including substrate, pore-forming agent and antioxidant, mix the raw materials evenly and then convey them to the extrusion system.

[0103] 2) Extrusion: The raw materials in step 1) are passed through a twin-screw extruder at a temperature of 160°C to 200°C to obtain a high-temperature melt, which is then accurately metered by a melt pump and fed into a die head, extruded from the slit of the die head, and the extruded high-temperature melt is treated with a chilled roller to obtain an extruded cast sheet.

[0104] 3) Stretching: feeding the extruded cast sheet obtained in step 2) into a synchronous stretching machine or an asynchronous stretching machine, and stretching the film synchronously or asynchronously in the length direction (MD) and the width direction (TD) to obtain a film containing a pore-forming agent;

[0105] 4) Extraction: Soak the film containing the pore-forming agent obtained in step 3) in an organic solvent for 10 to 20 minutes to fully remove the pore-forming agent in the film, and then evaporate the organic solvent by drying to form a film containing micropores. The drying temperature is 35° C. to 45° C.

[0106] 5) Shaping: The microporous film obtained in step 4) is subjected to a temperature of 120° C. to 150° C. to fully eliminate internal stress and to obtain a separator through shaping.

[0107] In some embodiments, after step 5), the method further includes step 6) cutting: cutting the isolation film prepared in step 5) into finished films according to the specifications of the battery cell.

[0108] In some embodiments, a secondary battery is provided, comprising a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator according to the present invention; wherein the separator is located between the positive electrode sheet and the negative electrode sheet. The secondary battery may be, for example, a lithium ion battery, a sodium ion battery, or a potassium ion battery.

[0109] [Positive electrode]

[0110] The positive electrode sheet includes a positive electrode current collector and a positive electrode material disposed on at least one surface of the positive electrode current collector, wherein the positive electrode material includes a positive electrode active material.

[0111] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0112] In some embodiments, when the secondary battery is a lithium-ion battery, the positive electrode active material may adopt a positive electrode active material for lithium-ion batteries that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide, and their respective modified compounds. However, the present invention is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3Mn 1 / 3 O2 (also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds, etc. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0113] In some embodiments, when the secondary battery is a sodium ion battery, the positive electrode active material may be a positive electrode active material for a sodium ion battery known in the art. As an example, the positive electrode active material may be used alone or in combination of two or more. Among them, the positive electrode active material may be selected from sodium iron composite oxide (NaFeO2), sodium cobalt composite oxide (NaCoO2), sodium chromium composite oxide (NaCrO2), sodium manganese composite oxide (NaMnO2), sodium nickel composite oxide (NaNiO2), sodium nickel titanium composite oxide (NaNi 1 / 2 Ti 1 / 2 O2), sodium nickel manganese composite oxide (NaNi 1 / 2 Mn 1 / 2 O2), sodium iron manganese composite oxide (Na 2 / 3 Fe 1 / 3 Mn 2 / 3 O2), sodium nickel cobalt manganese composite oxide (NaNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2), sodium iron phosphate (NaFePO4), sodium manganese phosphate (NaMn P O4), sodium cobalt phosphate compounds (NaCoPO4), Prussian blue materials, polyanion materials (phosphates, fluorophosphates, pyrophosphates, sulfates), etc., but the present invention is not limited to these materials. The present invention can also use other traditionally known materials that can be used as positive electrode active materials for sodium ion batteries.

[0114] In some embodiments, the cathode material may further include a binder. For example, the binder may include one or a combination of two or more selected from the group consisting of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.

[0115] In some embodiments, the cathode material may further include a conductive agent. For example, the conductive agent may include one or a combination of two or more selected from the group consisting of Super P, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0116] In some embodiments, the positive electrode sheet can be prepared in the following manner: the above-mentioned positive electrode materials, such as positive electrode active materials, conductive agents, binders and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0117] [Negative electrode]

[0118] The negative electrode sheet includes a negative electrode current collector and a negative electrode material disposed on at least one surface of the negative electrode current collector, wherein the negative electrode material includes a negative electrode active material.

[0119] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0120] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery known in the art. For example, the negative electrode active material includes one or a combination of two or more selected from the following groups: natural graphite, artificial graphite, mesophase microcarbon beads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composite, Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, TiO2-Li4Ti5O 12 , Li-Al alloy. However, the present invention is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for lithium-ion batteries can also be used. These negative electrode active materials can be used alone or in combination of two or more.

[0121] In some embodiments, the negative electrode material may further include a binder. For example, the binder may include one or a combination of two or more selected from the group consisting of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0122] In some embodiments, the negative electrode material may further include a conductive agent. For example, the conductive agent may include one or a combination of two or more selected from the group consisting of Super P, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0123] In some embodiments, the negative electrode material may further include other auxiliary agents, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0124] In some embodiments, the negative electrode sheet can be prepared by the following method: the above-mentioned negative electrode materials, such as negative electrode active materials, conductive agents, binders and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0125] [Electrolyte]

[0126] The electrolyte plays a role in conducting ions between the positive electrode plate and the negative electrode plate. The electrolyte includes electrolyte salt and solvent.

[0127] In some embodiments, the electrolyte salt can be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0128] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0129] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.

[0130] [Isolation film]

[0131] The isolation film of the present invention is used.

[0132] [Preparation of Secondary Battery]

[0133] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.

[0134] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.

[0135] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0136] The present invention has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 2 The secondary battery 5 is a square structure as an example.

[0137] In some embodiments, reference Figure 3 , the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0138] In some embodiments, secondary batteries may be assembled into a battery module. The number of secondary batteries contained in the battery module may be one or more, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery module.

[0139] Figure 4 4 is an example of a battery module. Figure 4 In the battery module 4, the plurality of secondary batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 5 may be fixed by fasteners.

[0140] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0141] In some embodiments, the battery modules 4 may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.

[0142] Figure 5 and Figure 6 1 is a battery pack 1 as an example. Figure 5 and Figure 6The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.

[0143] In addition, the present invention further provides an electric device, the electric device includes the secondary battery provided by the present invention. In some embodiments, the electric device includes at least one of the battery module or battery pack provided by the present invention. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0144] As the electrical device, a secondary battery, a battery module or a battery pack may be selected according to its usage requirements.

[0145] Figure 7 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the secondary battery, a battery pack or a battery module can be used.

[0146] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a secondary battery may be used as a power source.

[0147] Example 1

[0148] (1) Weigh the following raw materials in parts by weight and mix them evenly: 62 parts of polyethylene with an average molecular weight of 1.2 million, 30 parts of paraffin oil, and 8 parts of phosphite.

[0149] (2) the raw materials mixed uniformly in step (1) are passed through a twin-screw extruder at 180° C. to obtain a high-temperature melt, the high-temperature melt is accurately metered by a melt pump and fed into a die head, the high-temperature melt fed into the die head flows out from the slit of the die head, and the high-temperature melt flowing out from the slit of the die head passes through a chilled roller to obtain an extruded cast sheet;

[0150] (3) placing the extruded cast sheet into a biaxial asynchronous stretching machine and stretching it 3 times in the longitudinal direction (MD); stretching it in different regions in the width direction (TD), with the region near the center being stretched 1.6 times and the region near the edge being stretched 1.5 times, to obtain a film containing a pore-forming agent; in the width direction (TD), the distance between the center and the edge of the film containing the pore-forming agent is W, the region 0 to 1 / 3W away from the center is stretched 1.6 times in the width direction, and the region 1 / 3W to W away from the center is stretched 1.5 times in the width direction;

[0151] (4) soaking the film containing the pore-forming agent obtained in step (3) in dichloromethane for 20 minutes, removing the pore-forming agent, and then drying at 40° C. to volatilize the organic solvent, thereby preparing a microporous film;

[0152] (5) The microporous isolation membrane obtained in step (4) was kept in a high-temperature shaping device at 130° C. for 6 hours to fully remove the membrane stress, thereby preparing an isolation membrane I-1 with a thickness of 20 μm. The prepared isolation membrane was cut into finished membranes according to the specifications of the battery cell.

[0153] Example 2

[0154] A separator I-2 was prepared in the same manner as in Example 1 except for the following parameters.

[0155] In step (3), the distance between the center and the edge of the film containing the pore-forming agent in the width direction (TD) is W, the area 0 to 1 / 3W away from the center is stretched 5.9 times in the width direction, and the area 1 / 3W to W away from the center is stretched 5.3 times in the width direction.

[0156] Example 3

[0157] A separator I-3 was prepared in the same manner as in Example 1 except for the following parameters.

[0158] In step (3), the distance between the center and the edge of the film containing the pore-forming agent in the width direction (TD) is W, the area 0 to 1 / 3W away from the center is stretched 2.5 times in the width direction, and the area 1 / 3W to W away from the center is stretched 2 times in the width direction.

[0159] Example 4

[0160] A separator I-4 was prepared in the same manner as in Example 1 except for the following parameters.

[0161] In step (3), the distance between the center and the edge of the film containing the pore-forming agent in the width direction (TD) is W, the area 0 to 1 / 3W away from the center is stretched 3.6 times in the width direction, and the area 1 / 3W to W away from the center is stretched 2.4 times in the width direction.

[0162] Example 5

[0163] A separator I-5 was prepared in the same manner as in Example 1 except for the following parameters.

[0164] In step (3), the distance between the center and the edge of the film containing the pore-forming agent in the width direction (TD) is W, the area 0 to 1 / 3W away from the center is stretched 4.2 times in the width direction, and the area 1 / 3W to W away from the center is stretched 2.9 times in the width direction.

[0165] Example 6

[0166] A separator I-6 was prepared in the same manner as in Example 1 except for the following parameters.

[0167] In step (3), the distance between the center and the edge of the film containing the pore-forming agent in the width direction (TD) is W, the area 0 to 1 / 3W away from the center is stretched 4.2 times in the width direction, and the area 1 / 3W to W away from the center is stretched 2.4 times in the width direction.

[0168] Example 7

[0169] A separator I-7 was prepared in the same manner as in Example 1 except for the following parameters.

[0170] In step (3), the distance between the center and the edge of the film containing the pore-forming agent in the width direction (TD) is W, the area 0 to 1 / 3W away from the center is stretched 4.8 times in the width direction, and the area 1 / 3W to W away from the center is stretched 2.9 times in the width direction.

[0171] Example 8

[0172] A separator I-8 was prepared in the same manner as in Example 1 except for the following parameters.

[0173] In step (3), the distance between the center and the edge of the film containing the pore-forming agent in the width direction (TD) is W, the area 0 to 1 / 3W away from the center is stretched 7 times in the width direction, and the area 1 / 3W to W away from the center is stretched 5.3 times in the width direction.

[0174] Example 9

[0175] A separator I-9 was prepared in the same manner as in Example 1 except for the following parameters.

[0176] In step (3), the distance between the center and the edge of the film containing the pore-forming agent in the width direction (TD) is W, the area 0 to 1 / 3W away from the center is stretched 5.9 times in the width direction, and the area 1 / 3W to W away from the center is stretched 3.5 times in the width direction.

[0177] Example 10

[0178] A separator I-10 was prepared in the same manner as in Example 1 except for the following parameters.

[0179] In step (3), the distance between the center and the edge of the film containing the pore-forming agent in the width direction (TD) is W, the area 0 to 1 / 3W away from the center is stretched 5.3 times in the width direction, and the area 1 / 3W to W away from the center is stretched 2.9 times in the width direction.

[0180] Embodiment 11

[0181] A separator I-7 was prepared in the same manner as in Example 1 except for the following parameters.

[0182] In step (3), the distance between the center and the edge of the film containing the pore-forming agent in the width direction (TD) is W, the area 0 to 1 / 3W away from the center is stretched 7 times in the width direction, and the area 1 / 3W to W away from the center is stretched 4.1 times in the width direction.

[0183] Comparative Example 1

[0184] A separator II-1 was prepared in the same manner as in Example 1 except for the following parameters.

[0185] In step (3), the distance between the center and the edge of the film containing the pore-forming agent in the width direction (TD) is W, the area 0 to 1 / 3W away from the center is stretched 1.6 times in the width direction, and the area 1 / 3W to W away from the center is stretched 1.7 times in the width direction.

[0186] Comparative Example 2

[0187] A separator II-2 was prepared in the same manner as in Example 1 except for the following parameters.

[0188] In step (3), the distance between the center and the edge of the film containing the pore-forming agent in the width direction (TD) is W, the area 0 to 1 / 3W away from the center is stretched 2.5 times in the width direction, and the area 1 / 3W to W away from the center is stretched 2.4 times in the width direction.

[0189] Comparative Example 3

[0190] A separator II-3 was prepared in the same manner as in Example 1 except for the following parameters.

[0191] In step (3), the distance between the center and the edge of the film containing the pore-forming agent in the width direction (TD) is W, the area 0 to 1 / 3W away from the center is stretched 3.6 times in the width direction, and the area 1 / 3W to W away from the center is stretched 3.5 times in the width direction.

[0192] Comparative Example 4

[0193] A separator II-4 was prepared in the same manner as in Example 1 except for the following parameters.

[0194] In step (3), the distance between the center and the edge of the film containing the pore-forming agent in the width direction (TD) is W, the area 0 to 1 / 3W away from the center is stretched 3.6 times in the width direction, and the area 1 / 3W to W away from the center is stretched 4.7 times in the width direction.

[0195] Comparative Example 5

[0196] A separator II-5 was prepared in the same manner as in Example 1 except for the following parameters.

[0197] In step (3), the distance between the center and the edge of the film containing the pore-forming agent in the width direction (TD) is W, the area 0 to 1 / 3W away from the center is stretched 3.6 times in the width direction, and the area 1 / 3W to W away from the center is stretched 5.3 times in the width direction.

[0198] Comparative Example 6

[0199] A separator II-6 was prepared in the same manner as in Example 1 except for the following parameters.

[0200] In step (3), the distance between the center and the edge of the film containing the pore-forming agent in the width direction (TD) is W, the area 0 to 1 / 3W away from the center is stretched 4.8 times in the width direction, and the area 1 / 3W to W away from the center is stretched 4.7 times in the width direction.

[0201] Comparative Example 7

[0202] A separator II-7 was prepared in the same manner as in Example 1 except for the following parameters.

[0203] In step (3), the distance between the center and the edge of the film containing the pore-forming agent in the width direction (TD) is W, the area 0 to 1 / 3W away from the center is stretched 6.5 times in the width direction, and the area 1 / 3W to W away from the center is stretched 6.6 times in the width direction.

[0204] Experimental example

[0205] The isolation films prepared in Examples 1 to 11 and Comparative Examples 1 to 7 were tested.

[0206] Test (1):

[0207] The porosity of the isolation membrane is tested in the following way: Knead the isolation membrane into a ball and put it into the sample cup, then place the sample cup with the isolation membrane in the true density tester; close the test system, introduce helium according to the program, test the pressure of the gas in the sample chamber and the expansion chamber, and then calculate the real volume according to Bohr's law (PV=nRT), so as to obtain the porosity of the isolation membrane sample to be tested. Sample cup volume: 3.5cm 3 , Analysis gas: helium. The test results are shown in Table 1, where the area 0 to 1 / 3W from the center along the width direction (TD) of the isolation film is referred to as the "first area", and the area 1 / 3W to W from the center along the width direction of the isolation film is referred to as the "second area".

[0208] Table 1 Stretching ratio and porosity of separator

[0209]

[0210] Test (2):

[0211] Three parallel samples were selected from the isolation membranes of Examples 1 to 11 and Comparative Examples 1 to 7, and they were assembled into small soft-pack batteries, as follows: NCM523 positive electrode sheets, isolation membranes, and graphite negative electrode sheets were stacked in sequence, so that the isolation membrane was located between the positive and negative electrode sheets to isolate the positive and negative electrodes, and bare cells were wound, and the tabs were welded, and the bare cells were placed in an outer package; the electrolyte was injected into the dried cells, and lithium-ion batteries were prepared through packaging, standing, formation, and shaping.

[0212] The prepared lithium-ion battery was subjected to a constant current 1C charge / 1C discharge cycle in a 25°C constant temperature box for 600 cls. The battery was then disassembled, and the anode large-surface electrode sheet (in a wound battery cell, the surface with a larger side area is called the large surface) was taken. The Li element content of the central area of ​​the large surface and the area near the edge of the pole ear was measured by an ICP (Inductive Coupled Plasma Emission Spectrometer) inductively coupled plasma spectrometer, and the difference between the Li content of the large surface center and the Li content of the large surface edge was calculated. The test results are shown in Table 2.

[0213] Table 2 Analysis results of Li element content in large anode electrode

[0214] sample Li content in the center of the large surface - Li content at the edge of the large surface wt.% Example 1 0.45 Example 2 0.37 Example 3 0.32 Example 4 0.19 Example 5 0.06 Example 6 0.13 Example 7 0.34 Example 8 0.58 Example 9 0.46 Example 10 0.4 Embodiment 11 0.83 Comparative Example 1 0.62 Comparative Example 2 0.54 Comparative Example 3 0.41 Comparative Example 4 0.23 Comparative Example 5 0.03 Comparative Example 6 0.56 Comparative Example 7 0.87

[0215] Test (3):

[0216] A lithium-ion battery was prepared according to the method in test (2) and its cycle performance was tested. The method for determining the cycle capacity is as follows: the battery cell is fully charged at a constant current of 1 / 3C and a constant voltage of 4.35V until the current is less than 0.05C, and then discharged at a constant current of 1 / 3C to 2.5V after standing for 30 minutes. The measured capacity is the actual capacity of the current cycle. The capacity retention rate of the nth cycle = the actual discharge capacity of the nth week / the actual discharge capacity of the first week × 100%. The test results are shown in Table 3.

[0217] Table 3

[0218]

[0219]

[0220] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A separator, characterized in that the separator is a porous separator; in a direction perpendicular to the thickness of the separator, the porosity gradient of the separator decreases from the center to the edge of the separator, The material of the isolation membrane includes one or a combination of two or more selected from the following group: glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride.

2. The isolation membrane as claimed in claim 1, characterized in that the isolation membrane includes a length direction and a width direction in a direction perpendicular to the thickness of the isolation membrane; in the width direction of the isolation membrane, the porosity gradient of the isolation membrane decreases from the center to the edge of the isolation membrane.

3. The isolation membrane as described in claim 1 or 2 is characterized in that the isolation membrane is divided into n regions in sequence from the center to the edge, where n is a positive integer greater than or equal to 2; for any two regions, the region closer to the center of the isolation membrane has a larger porosity than the region farther from the center of the isolation membrane.

4. The isolation film according to claim 3, It is characterized in that The area closest to the center of the isolation membrane is the first area, and the area farthest from the center of the isolation membrane is the nth area; the difference between the porosity of the first area and the porosity of the nth area is 2% to 20%.

5. The isolation film according to claim 4, It is characterized in that The porosity of the first region is 30% to 60%, and the porosity of the nth region is 20% to 50%.

6. The isolation film according to claim 4, It is characterized in that The distance from the center to the edge of the isolation membrane is W, and the isolation membrane is divided into two regions along the direction from the center to the edge. The range of 0~1 / 3W from the center of the isolation membrane is the first region, and the porosity of the first region is 30%~60%; the range of 1 / 3W~W from the center of the isolation membrane is the second region, and the porosity of the second region is 20%~50%.

7. The isolation film according to claim 1 or 2, It is characterized in that The thickness of the isolation film is 5-60 μm.

8. The isolation film according to claim 1 or 2, It is characterized in that The isolation film is a single-layer film or a composite film with two or more layers.

9. The method for preparing the isolation film according to any one of claims 1 to 8, It is characterized in that The method comprises: weighing raw materials for preparing the isolation membrane, wherein the raw materials include a substrate, a pore-forming agent and an antioxidant; after the raw materials are evenly mixed, extrusion, stretching, extraction and shaping are performed in sequence; wherein the stretching step comprises: stretching in a direction perpendicular to the thickness of the isolation membrane, and the stretching ratio gradient decreases from the center to the edge of the isolation membrane so as to reduce the porosity gradient, The substrate includes one or a combination of two or more selected from the following group: glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride.

10. The preparation method according to claim 9, It is characterized in that The stretching step includes: stretching along the width direction of the separator, and the stretching ratio gradient decreases from the center to the edge of the separator to reduce the porosity gradient; and / or, The separator is stretched along the length direction, and the stretching ratio decreases gradually from the center to the edge of the separator to reduce the porosity gradient.

11. The preparation method according to claim 9 or 10, It is characterized in that The isolation film is divided into n regions in sequence from the center to the edge, where n is a positive integer greater than or equal to 2; for any two regions, a larger stretching ratio is applied to the region closer to the center of the isolation film than to the region farther from the center of the isolation film.

12. The preparation method according to claim 11, It is characterized in that The distance from the center to the edge of the isolation film is W, and the range of 0~1 / 3W from the center of the isolation film is the first region, and the first region is stretched by 4~8 times in the stretching step; the range of 1 / 3W~W from the center of the isolation film is the second region, and the second region is stretched by 2~4 times in the stretching step.

13. The preparation method according to claim 9 or 10, It is characterized in that The raw materials include, by weight: 30-65 parts of base material, 10-40 parts of pore former and 5-10 parts of antioxidant.

14. The preparation method according to claim 13, It is characterized in that The pore former is an organic pore former and / or an inorganic pore former.

15. The preparation method according to claim 13, It is characterized in that The antioxidant includes one or a combination of two or more selected from the following groups: 4,4-thiobis(6-tert-butyl-m-cresol), dibutylhydroxytoluene, phosphite, tert-butylhydroquinone, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid octadecanoate, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 2-tert-butyl-6-methylphenol, N,N'-di-β-naphthyl-p-phenylenediamine, dilauryl thiodipropionate, tris(nonylphenyl) phosphite, and triphenyl phosphite.

16. A secondary battery comprising a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator between the positive electrode sheet and the negative electrode sheet, It is characterized in that The isolation membrane is the isolation membrane according to any one of claims 1 to 8.

17. The secondary battery according to claim 16, It is characterized in that The secondary battery is a lithium ion battery, a sodium ion battery or a potassium ion battery.

18. A battery module comprising the secondary battery according to claim 16 or 17.

19. A battery pack comprising the battery module according to claim 18.

20. An electrical device comprising at least one of the secondary battery according to claim 16 or 17, the battery module according to claim 18, or the battery pack according to claim 19.

Citation Information

Patent Citations

  • Lithium ion battery and isolating film

    CN101510597A

  • Lithium ion battery

    CN102368562A

  • Battery insulating film, battery core, lithium ion battery and preparation method

    CN109686908A

  • Composite isolation membrane and preparation method thereof and electrochemical device adopting composite isolation membrane

    CN109994688A

  • Composite current collector, composite electrode sheet comprising composite current collector and electrochemical device

    CN109994740A