Laser welding method, laser welding equipment and laser welding assembly
Through the dual-beam concentric laser welding technology, the combination of the central beam and the annular beam is used to control the delayed reduction of the annular arc closing power of the annular beam, which solves the crack problem caused by the too fast cooling rate of the welding seam during the welding process, and improves the welding stability and Quality, suitable for welding dissimilar metal materials.
Patent Information
- Application Number
- CN202210825284.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-07-14
AI Technical Summary
In the existing technology, the weld seam cools too fast during the laser welding process of metal materials, which can easily lead to defects such as cracks and pores. Especially when welding dissimilar metal materials (such as steel and copper), the difference in expansion coefficient causes the weld seam to be in different locations. Cracks are prone to occur under stress.
The dual-beam concentric laser welding method is used. Through the combination of the central beam and the annular beam, the annular arc power of the annular beam is controlled to decrease with delay, slowing down the cooling speed of the weld, reducing shrinkage stress, and ensuring the stability of the welding process. Specific measures include gradually reducing the central arc power of the central beam during the arc closing stage of the welding and maintaining it between 50% and 70% of the initial working power. The annular arc power of the annular beam is reduced to zero with delay, or the central arc power is reduced simultaneously. and the closing arc power of the annular beam to reduce the cooling rate of the weld seam.
It effectively reduces the formation of cracks in metal material welds during the cooling process, especially when welding dissimilar metal materials, improves welding stability and quality, and is suitable for different base materials and joint types.
Smart Images

Figure CN115815798B_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application relate to the field of welding technology, and specifically to a laser welding method, laser welding equipment, and laser welding assembly. Background Art
[0002] In the prior art, laser welding of metal materials is a process of rapid heating and cooling. For deep penetration welding of the same metal materials and dissimilar metal materials, if the keyhole stability in the weld pool is too poor, defects such as cracks and pores are likely to occur. Especially for laser welding of dissimilar metal materials (such as steel and copper), due to the differences in physical and chemical properties such as the expansion coefficient of the two metals, it is easy for the weld to crack under different stresses. Summary of the invention
[0003] In view of the above problems, the embodiments of the present application provide a laser welding method, a laser welding device and a laser welding assembly. The laser welding method uses a dual-beam concentric laser for welding, and the delayed reduction of the annular arc power of the annular beam can slow down the cooling rate of the weld, thereby solving the technical problem that crack defects are easily formed in metal materials during the cooling process of the weld.
[0004] A first aspect of the present application provides a laser welding method, which includes: in the welding arc ending stage, using a double-beam concentric laser formed by a central beam and an annular beam to perform laser welding; controlling the annular arc ending power of the annular beam to decrease with a delay compared to the central arc ending power of the central beam in the welding arc ending stage.
[0005] The laser welding method provided in this embodiment uses a dual-beam concentric laser consisting of a central beam and an annular beam for welding. The delayed reduction of the annular arc closing power of the annular beam can further slow down the cooling rate of the weld, thereby solving the technical problem that crack defects are easily formed in metal materials during the cooling process of the weld.
[0006] Specifically, the high-intensity laser of the central beam of the dual-beam concentric laser can melt the welding base material, and the annular beam of the dual-beam concentric laser is distributed around the central beam. The weak-intensity laser of the annular beam can not only preheat the welding base material, but also slow down the cooling rate of the weld, thereby reducing the formation of crack defects in metal materials during the cooling process of laser welding, especially reducing the phenomenon of crack defects in welds of dissimilar metal materials (such as steel and copper) during the cooling process.
[0007] In some embodiments, controlling the annular arc-ending power of the annular beam to decrease in a delayed manner compared to the central arc-ending power of the central beam during the arc-ending stage of welding specifically includes: dividing the arc-ending stage of welding into the front arc-ending stage and the back arc-ending stage of welding; controlling the central arc-ending power of the central beam to gradually decrease during the front arc-ending stage of welding, and controlling the annular arc-ending power of the annular beam to maintain at the initial working power during the front arc-ending stage of welding. By slowly reducing the central arc-ending power of the central beam during the arc-ending stage of welding, the deep fusion welding process is gradually transformed into a thermal conduction welding process, the depth of the molten pool is reduced, and the shrinkage stress is reduced. The cooling rate of the weld is slowed down by delaying the reduction of the annular arc-ending power of the annular beam, the shrinkage strain rate is reduced, and the thermal stress is further reduced to ensure the stability of the welding process, and the phenomenon of arc-ending cracks in the weld during the arc-ending stage of welding is reduced.
[0008] In some embodiments, controlling the central arc-ending power of the central beam to gradually decrease in the front section of welding arc-ending specifically includes: controlling the central arc-ending power of the central beam to continuously decrease in the front section of welding arc-ending, and reducing it to 50% to 70% of the initial working power at the boundary point between the front section of welding arc-ending and the rear section of welding arc-ending. The central arc-ending power of the central beam is decreased by more than 50% in order to reduce heat input by reducing power, so as to ensure that the deep fusion welding process can be gradually transitioned to the thermal conduction welding process, and the central arc-ending power of the central beam is decreased by less than 70% in order to avoid the central arc-ending power of the central beam from decreasing too quickly and generating a large shrinkage stress.
[0009] In some embodiments, dividing the arc closure stage into the front arc closure stage and the rear arc closure stage further includes: controlling the central arc closure power of the central light beam to be reduced to zero before the annular arc closure power of the annular light beam in the rear arc closure stage. By delaying the reduction of the annular arc closure power of the annular light beam to zero, the cooling rate of the weld can be further slowed down, solving the technical problem that crack defects are easily formed in the metal material during the cooling process of the weld.
[0010] In some embodiments, dividing the arc closure stage into the front arc closure stage and the rear arc closure stage further includes: controlling the central arc closure power of the central beam and the annular arc closure power of the annular beam to be reduced to zero at the same time in the rear arc closure stage. By reducing the central arc closure power of the central beam and the annular arc closure power of the annular beam to zero at the same time, the control difficulty of the dual-beam concentric laser formed by the central beam and the annular beam can be reduced on the basis of delaying the cooling speed of the weld.
[0011] In some embodiments, the arc closure stage of welding is divided into the front section of arc closure and the rear section of arc closure, specifically including: obtaining the disappearance position of the welding keyhole in the arc closure stage of welding; generating the boundary point between the front section of arc closure and the rear section of arc closure according to the disappearance position of the welding keyhole. When the keyhole disappears, the laser welding transitions from the deep fusion welding process to the thermal conduction welding process. At this time, the annular arc closure power of the annular beam begins to decrease. As the central arc closure power and the annular arc closure power decrease at the same time, the depth of the molten pool continues to decrease, thereby reducing the shrinkage stress and avoiding the generation of welding cracks.
[0012] In some embodiments, controlling the annular arc-ending power of the annular beam to decrease in a delayed manner compared to the central arc-ending power of the central beam during the arc-ending stage of welding further includes: determining that the ratio of P and p satisfies 1≤P / p≤4 based on the central arc-ending power of the central beam being p and the annular arc-ending power of the annular beam being P. P / p≥1 is based on the consideration that the minimum spot diameter of the annular beam is twice the spot diameter of the central beam. If the energy (power) of the annular beam is too low, the effects of preheating, slow cooling and cleaning the surface are not significant; P / p≤4 is to avoid excessive heat input of the annular beam, which may cause burning and evaporation of low-melting-point alloy elements.
[0013] In some embodiments, controlling the annular arc-ending power of the annular beam to decrease in a delayed manner compared to the central arc-ending power of the central beam at the welding arc-ending stage also includes: determining that the ratio of D to d satisfies 3≤D / d≤8 based on the spot diameter of the central beam at the welding arc-ending stage being d and the spot diameter of the annular beam at the welding arc-ending stage being D. D / d≥3 can ensure that the spot diameter of the annular beam exceeds the spot diameter of the central beam by at least 2 times, and the portion of the annular beam diameter exceeding the central beam can play a role in preheating and slow cooling, as well as the effect of cleaning the weld surface; D / d≤8 is to avoid the phenomenon that the heat-affected zone is too large due to the excessive spot diameter of the annular beam, resulting in the coarsening of the grains in the welding area of the welding base material and affecting the performance of the base material.
[0014] In some embodiments, controlling the annular arc-ending power of the annular beam to decrease in a delayed manner compared to the central arc-ending power of the central beam during the arc-ending stage of welding also includes: controlling the central beam to be emitted in a modulated pulse wave manner, the central arc-ending power being the pulse power of the modulated pulse wave during the arc-ending stage of welding, and / or controlling the annular beam to be emitted in a continuous wave manner, the annular arc-ending power being the arc-ending power of the continuous wave during the arc-ending stage of welding. Setting the central beam to a modulated pulse laser can reduce the heat input of the central beam, reduce the burning and evaporation of low-melting-point alloy elements; continuous preheating of the annular beam can increase the absorption rate of the welding base material to the laser, improve welding stability, and clean the surface of the welding base material, volatilize low-melting-point pollutants, and reduce spatter caused by low-melting-point pollutants. Continuous preheating of the annular beam can also slow down the cooling rate of the weld, reduce the local thermal stress of the weld, and avoid the generation of weld cracks.
[0015] A second aspect of the present application provides a laser welding device, which includes a laser transmitter, and the laser transmitter is used to implement the laser welding method of the first aspect of the present application.
[0016] The laser welding equipment provided in this embodiment uses a dual-beam concentric laser consisting of a central beam and an annular beam for welding. The delayed reduction of the annular arc closing power of the annular beam can further slow down the cooling rate of the weld, thereby solving the technical problem that crack defects are easily formed in metal materials during the cooling process of the weld.
[0017] Specifically, the high-intensity laser of the central beam of the dual-beam concentric laser can melt the welding base material, and the annular beam of the dual-beam concentric laser is distributed around the central beam. The weak-intensity laser of the annular beam can not only preheat the welding base material, but also slow down the cooling rate of the weld, thereby reducing the formation of crack defects in metal materials during the cooling process of laser welding, especially reducing the phenomenon of crack defects in welds of dissimilar metal materials (such as steel and copper) during the cooling process.
[0018] In some embodiments, the laser welding equipment also includes a controller, which is provided with a computer-readable storage medium and a control device, and the control device includes: a control module, which is used to perform laser welding using a double-beam concentric laser formed by a central beam and an annular beam during the arc ending stage of welding; and a control module which is used to control the annular arc ending power of the annular beam to decrease with a delay compared to the central arc ending power of the central beam during the arc ending stage of welding.
[0019] A third aspect of the present application provides a laser welding assembly, which is welded by the laser welding device according to the second aspect of the present application.
[0020] In some embodiments, the laser welded assembly includes an aluminum alloy welded assembly.
[0021] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present application. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the drawings:
[0023] Figure 1A flow chart of a laser welding method according to some embodiments of the present application;
[0024] Figure 2 An axonometric diagram of a dual-beam concentric laser according to some embodiments of the present application;
[0025] Figure 3 for Figure 2 A front view of the dual beam concentric laser shown;
[0026] Figure 4 for Figure 2 The schematic diagram of the application of dual-beam concentric laser is shown;
[0027] Figure 5 for Figure 4 The schematic diagram of the double-beam concentric laser in the arc closing stage of welding is shown;
[0028] Figure 6 For the first embodiment of this application Figure 5 Schematic diagram of power variation of double-beam concentric laser shown;
[0029] Figure 7 For the second embodiment of this application Figure 5 Schematic diagram of power variation of double-beam concentric laser shown;
[0030] Figure 8 for Figure 2 Schematic diagram of the central beam of the dual-beam concentric laser shown;
[0031] Fig. 9 for Figure 2 Schematic diagram of annular beams of dual-beam concentric lasers shown;
[0032] Fig.10 is a schematic diagram of a central light beam of the first embodiment of the present application;
[0033] Fig.11 is a schematic diagram of a central light beam of a second embodiment of the present application;
[0034] Fig.12 is a schematic diagram of a central light beam of a third embodiment of the present application;
[0035] Fig.13 is a schematic diagram of a central light beam of a fourth embodiment of the present application;
[0036] Fig.14 is a schematic diagram of a central light beam of a fifth embodiment of the present application;
[0037] Fig.15 A schematic diagram of an annular light beam according to a first embodiment of the present application;
[0038] Fig.16A schematic diagram of an annular light beam according to a second embodiment of the present application;
[0039] Fig.17 A schematic diagram of a ring-shaped light beam according to a third embodiment of the present application;
[0040] Fig.18 A schematic diagram of a ring-shaped light beam according to a fourth embodiment of the present application;
[0041] Fig.19 A schematic diagram of a ring-shaped light beam according to a fifth embodiment of the present application;
[0042] Fig. 20 A schematic diagram of a ring-shaped light beam according to a sixth embodiment of the present application;
[0043] Fig.21 A structural block diagram of a controller according to an embodiment of the present application;
[0044] Fig. 22 This is the appearance diagram of the weld arc closure of the first embodiment of the present application;
[0045] Fig.23 This is the appearance diagram of the arc closure of the weld in the prior art;
[0046] Fig.24 This is an appearance diagram of the weld arc closure of the second embodiment of the present application.
[0047] Some of the reference numerals in the specific implementation manner are as follows:
[0048] 100 double beam concentric laser; 10 central beam; 20 annular beam, 21 inner wall surface, 22 outer wall surface;
[0049] 200 welding base material, 201 molten pool, 202 keyhole, 210 first aluminum alloy plate, 220 second aluminum alloy plate;
[0050] 300 is a controller, 310 is a computer-readable storage medium, 320 is a control device, and 321 is a control module. DETAILED DESCRIPTION
[0051] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0052] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0053] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0054] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0055] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0056] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0057] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "perpendicular", "parallel", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.
[0058] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.
[0059] The existing arc synchronous preheating assisted laser welding process uses the arc as the preheating heat source to alleviate the cracks that occur in the welding base material during the welding process, effectively improve the shortcomings of the welding base material's low laser absorption rate and high energy consumption during the welding process, and improve the laser utilization rate. However, in addition to controlling the laser welding process parameters, this welding process also requires coordinated control of the arc current, shielding gas flow, welding gun inclination angle, and the distance between the arc center and the laser spot center, and there are many control parameters. Moreover, this welding process can only preheat the workpiece, and cannot play a slow cooling role to slow down the cooling rate of the weld. This welding process is also only suitable for V-groove joints, and requires filling powder to use the newly formed material to connect the welding base material. It is not suitable for overlapped joints where the workpiece is distributed up and down.
[0060] In order to solve the technical problem that the existing laser welding method cannot play a slow cooling effect to slow down the cooling rate of the weld, especially cannot play a slow cooling effect to slow down the cooling rate of the weld in the arc closing stage of welding, the laser welding method of the present application can play a slow cooling effect to slow down the cooling rate of the weld, thereby reducing the risk of cracks in the weld.
[0061] The laser welding method of the present application is applicable to the welding of steel-copper alloy components and aluminum alloy components but is not limited to the welding of steel-copper alloy components and aluminum alloy components. The laser welding method of the present application is applicable to the welding of other workpieces of the same parent material and workpieces of different parent materials, and can also be applicable to the welding of V-groove joints and overlapped joints with upper and lower distributions of the welding parent material.
[0062] In some embodiments of the present application, Figures 1 to 3 As shown, a laser welding method is provided, the laser welding method comprising: in the arc ending stage of welding, using a double-beam concentric laser 100 formed by a central light beam 10 and an annular light beam 20 to perform laser welding; controlling the central arc ending power of the central light beam 10 to decrease before the annular arc ending power of the annular light beam 20 in the arc ending stage of welding.
[0063] In this embodiment, the arc closing stage of welding refers to the welding closing stage, which will produce arc pits, and often have looseness, cracks, pores, slag inclusions and other phenomena. In order to overcome the arc pit defects, the embodiment of the present application adjusts the weld morphology by controlling the power of the dual-beam concentric laser 100. Specifically, the laser welding method provided in this embodiment uses a dual-beam concentric laser 100 composed of a central beam 10 and an annular beam 20 for welding. The cooling rate of the weld can be further delayed by delaying the reduction of the annular arc closing power of the annular beam 20, which solves the technical problem that crack defects are easily formed in metal materials during the cooling process of the weld.
[0064] like Figure 4As shown, the laser welding method provided in this embodiment uses a double-beam concentric laser 100 composed of a central beam 10 and an annular beam 20 for welding. The high-intensity laser of the central beam 10 can melt the welding base material 200, and the annular beam 20 is distributed around the central beam 10. The weak-intensity laser of the annular beam 20 can not only preheat the welding base material 200, but also slow down the cooling rate of the weld, thereby reducing the formation of crack defects in metal materials during the cooling process of laser welding, especially reducing the formation of crack defects in the welds of dissimilar metal materials (such as steel and copper) and overlapped joints during the cooling process of welding arc closing stage.
[0065] Furthermore, since the central light beam 10 and the annular light beam 20 disclosed in the present application are arranged to be concentrically distributed, there is no need to coordinately adjust the defocus amount, arc starting point, arc ending point, arc incident angle and the distance between the central light beam 10 and the annular light beam 20 in the arc ending stage of welding, thereby reducing the control parameters of the dual-beam concentric laser 100. Compared with the prior art, the synchronous action of the central light beam 10 and the annular light beam 20 can not only play a slow cooling role to delay the cooling rate of the weld, but also can be applicable to V-groove joints and overlapped joints with the welding base material 200 distributed up and down.
[0066] In addition, the weld type also includes the material of the welding base material 200 and the structure of the weld. Different welding base materials have different physical and chemical properties such as expansion coefficients. According to the physical and chemical properties such as the expansion coefficient of the welding base material, a matching dual-beam concentric laser 100 is selected. For example, the effective welding area of the dual-beam concentric laser 100 and the welding arc ending power in the welding arc ending stage are selected to reduce the phenomenon of cracks in the weld of the welding base material 200 under stress.
[0067] Different weld structures also require matching dual-beam concentric lasers 100 of different sizes and powers. For example, V-groove joints and overlapped joints of the welding base material 200 distributed up and down require the selection of the effective welding area of the dual-beam concentric laser 100 and the welding arc ending power in the welding arc ending stage, which can reduce the phenomenon of cracks in the weld of the welding base material 200 under stress.
[0068] like Figure 6 and Figure 7 As shown, in some embodiments, the delayed decrease of the annular arc-ending power of the annular beam 20 in the welding arc-ending stage compared with the central arc-ending power of the central beam 10 specifically includes: controlling the welding arc-ending stage to be divided into a welding arc-ending front section and a welding arc-ending rear section; controlling the central arc-ending power of the central beam 10 to gradually decrease in the welding arc-ending front section and controlling the annular arc-ending power of the annular beam 20 to maintain at the initial working power in the welding arc-ending front section.
[0069] In this embodiment, the initial working power is the working power of the annular beam 20 when the dual-beam concentric laser 100 is in normal operation. The annular arc-ending power of the annular beam 20 is controlled to be maintained at the initial working power in the front section of welding arc-ending, that is, the annular beam 20 is still in a normal working state in the front section of welding arc-ending. Controlling the central arc-ending power of the central beam 10 to gradually decrease in the front section of welding arc-ending includes linear reduction and nonlinear reduction. The reduction mode of the central arc-ending power depends on the welding parent material 200. Different weld parent materials have different physical and chemical properties such as expansion coefficients. The present application selects a matching central arc-ending power reduction mode according to the physical and chemical properties such as the expansion coefficient of the welding parent material 200, which can reduce the phenomenon of cracks generated in the weld arc-ending stage of the welding parent material 200 under stress.
[0070] In this embodiment, the central arc-ending power of the central light beam 10 is slowly reduced in the arc-ending stage of welding, so that the deep fusion welding process is gradually transformed into a thermal conduction welding process, the depth of the molten pool 201 is reduced, and the shrinkage stress is reduced. The cooling rate of the weld is delayed by the subsequent reduction of the annular arc-ending power of the annular light beam 20, the shrinkage strain rate is reduced, and the thermal stress is further reduced to ensure the stability of the welding process. The entire welding process only needs to change the power parameters to reduce the phenomenon of arc-ending cracks in the weld in the arc-ending stage of welding.
[0071] like Figure 6 and Figure 7 As shown, in some embodiments, controlling the central arc-ending power of the central light beam 10 to gradually decrease in the front section of welding arc-ending specifically includes: controlling the central arc-ending power of the central light beam 10 to continuously decrease in the front section of welding arc-ending, and reducing it to 50% to 70% of the initial working power at the dividing point between the front section of welding arc-ending and the rear section of welding arc-ending.
[0072] In this embodiment, the initial working power of the central light beam 10 is the working power of the central light beam 10 when the dual-beam concentric laser 100 is in normal operation. The central light beam 10 can be a modulated pulse laser or a continuous laser. Taking the central light beam 10 as a modulated pulse laser as an example, the central arc closing power is reduced to 50% to 70% of the initial working power before the arc closing of welding, including the laser wave height of the modulated pulse laser being reduced to 50% to 70% of the height of the laser wave of the initial working power, and also including the pulse spacing of adjacent laser waves of the modulated pulse laser being increased to 143% to 200% of the spacing of adjacent laser waves of the initial working power.
[0073] In this embodiment, the central arc-ending power of the central light beam 10 is gradually reduced to 50% to 70% of the original initial working power in the front section of arc-ending of welding. The central arc-ending power of the central light beam 10 is reduced by more than 50% in order to reduce heat input by reducing power, thereby ensuring a gradual transition from deep fusion welding to thermal conduction welding. The central arc-ending power of the central light beam 10 is reduced by less than 70% in order to avoid a large shrinkage stress caused by a too fast reduction in the central arc-ending power of the central light beam 10.
[0074] like Figure 7 As shown, in some embodiments, dividing the welding arc extinguishing stage into the welding arc extinguishing front section and the welding arc extinguishing rear section also includes: controlling the central arc extinguishing power of the central light beam 10 to be reduced to zero before the annular arc extinguishing power of the annular light beam 20 in the welding arc extinguishing rear section.
[0075] In this embodiment, the central arc ending power and / or the annular arc ending power decrease linearly or nonlinearly. The central arc ending power and / or the annular arc ending power decrease linearly or nonlinearly, both of which can achieve good welding arc ending effect.
[0076] This embodiment can further slow down the cooling rate of the weld by delaying the annular arc-ending power of the annular light beam 20 to zero, thereby solving the technical problem that crack defects are easily formed in the weld cooling process of the metal material in the post-arc-ending stage of welding.
[0077] like Figure 6 As shown, in some embodiments, dividing the welding arc extinguishing stage into the welding arc extinguishing front section and the welding arc extinguishing rear section also includes: controlling the central arc extinguishing power of the central light beam 10 to be reduced to zero simultaneously with the annular arc extinguishing power of the annular light beam 20 in the welding arc extinguishing rear section.
[0078] In this embodiment, the central arc ending power and / or the annular arc ending power decrease linearly or nonlinearly. The central arc ending power and / or the annular arc ending power decrease linearly or nonlinearly, both of which can achieve good welding arc ending effect.
[0079] This embodiment reduces the difficulty of controlling the dual-beam concentric laser 100 formed by the central beam 10 and the annular beam 20 by reducing the central arc-ending power of the central beam 10 and the annular beam 20 to zero at the same time, thereby delaying the cooling rate of the weld. In other words, the defocusing amount, arc-ending starting point, arc-ending ending point, arc-ending incident angle of the central beam 10 and the annular beam 20 in the arc-ending stage of welding, as well as the distance between the central beam 10 and the annular beam 20 are synchronously controlled.
[0080] like Figure 5As shown, in some embodiments, dividing the welding arc closure stage into the welding arc closure front section and the welding arc closure rear section specifically includes: obtaining the disappearance position of the welding keyhole 202 in the welding arc closure stage; generating a dividing point between the welding arc closure front section and the welding arc closure rear section according to the disappearance position of the welding keyhole 202 (such as Figure 5 The arc ending point b) is shown.
[0081] In this embodiment, during the welding process, the pressure generated by the violent vaporization and expansion of the welding material ejects the molten metal to form a keyhole 202. The hole wall of the keyhole 202 is always in a highly fluctuating state, causing the oscillation of the molten pool and affecting the overflow of bubbles in the molten pool during the solidification process. Therefore, the disappearance of the keyhole 202 is the dividing point where laser welding transitions from a deep fusion welding process to a thermal conduction welding process.
[0082] The embodiment of the present application first determines the arc ending starting point a, arc ending decomposition point b and arc ending end point c of the weld in the arc ending stage of welding. When the dual-beam concentric laser 100 reaches the arc ending starting point a, as shown in FIG. Figure 5 As shown, there is a keyhole 202 in the molten pool 201, which is in the deep fusion welding process. At this time, the central arc-ending power of the central beam 10 is controlled to start to decrease, and the annular arc-ending power of the annular beam 20 is controlled to remain unchanged to delay the cooling rate of the weld and maintain the stability of the keyhole 202. When the laser reaches the arc-ending decomposition point b, the central arc-ending power of the central beam 10 has dropped to 50% to 70% of the original initial working power, the keyhole 202 disappears, and the welding process transitions from deep fusion welding to thermal conduction welding. The welding stress is relatively stable, as shown in FIG. Figure 5 As shown, at this time, the annular arc ending power of the annular beam 20 begins to decrease. When the dual-beam concentric laser 100 reaches the arc ending end point c, as the central arc ending power and the annular arc ending power decrease simultaneously, the depth of the molten pool 201 continues to decrease, thereby reducing the shrinkage stress and avoiding the generation of welding cracks.
[0083] It should be noted that for different types of aluminum alloys, the size and ramp-down speed of the central arc-ending power and the circular arc-ending power as well as the distance between the arc-ending starting point a and the arc-ending end point c need to be determined according to actual conditions, such as the structural type of the weld, the size of the weld and the ambient temperature.
[0084] In some embodiments, controlling the annular arc ending power of the annular beam 20 to decrease with a delay compared to the central arc ending power of the central beam 10 during the welding arc ending stage also includes: based on the central arc ending power of the central beam 10 being p and the annular arc ending power of the annular beam 20 being P, determining that the ratio of P to p satisfies 1≤P / p≤4.
[0085] In the present embodiment, P / p≥1 proposed in the present embodiment is based on the consideration that the minimum spot diameter of the annular beam 20 is twice the spot diameter of the central beam 10, and the beam energy distribution of a general laser is a Gaussian distribution, with high energy in the middle and low energy in the periphery. If the energy (power) of the annular beam 20 is too low, the energy of the peripheral portion of the annular beam 20 that exceeds the diameter of the central beam 10 is even lower, and the effects of preheating, slow cooling and cleaning the surface are not significant; P / p≤4 is to avoid excessive heat input of the annular beam 20, which may cause burning and evaporation of low-melting-point alloy elements.
[0086] In some embodiments, controlling the delayed decrease of the annular arc-ending power of the annular beam 20 in the welding arc-ending stage compared with the central arc-ending power of the central beam 10 also includes: based on the spot diameter of the central beam 10 in the welding arc-ending stage being d and the spot diameter of the annular beam 20 in the welding arc-ending stage being D, determining that the ratio of D to d satisfies 3≤D / d≤8.
[0087] In this embodiment, if Figure 8 As shown, the central beam 10 is set as a conical columnar beam, and the diameter of the central beam 10 gradually increases from high to low. The outer wall surface 22 of the central beam 10 can be set as an oblique line, an inner concave arc surface or an outer convex arc surface. By setting the central beam 10 as a conical columnar beam, the spot area of the central beam 10 acting on the welding parent material 200 can be increased, the local heat input of the central beam 10 acting on the welding parent material 200 can be reduced, and the burning and evaporation of low-melting-point alloy elements can be reduced. The larger size of the spot of the central beam 10 can also reduce the stirring effect of the keyhole 202 on the molten pool 201 during the welding process, avoid excessive mixing between dissimilar metals, and thus reduce cracks caused by different expansion coefficients during the cooling process of dissimilar metals.
[0088] like Fig. 9 As shown, the annular beam 20 is set as a conical cylindrical beam, and the diameter of the annular beam 20 gradually increases from high to low. The outer wall surface 22 of the annular beam 20 can be set as an oblique line, an inner concave arc surface or an outer convex arc surface. By setting the annular beam 20 to a conical cylindrical beam, the spot area of the annular beam 20 acting on the welding base material 200 can be increased, and continuous preheating can be achieved. The absorption rate of the workpiece to the laser is increased, the welding stability is improved, and the surface of the welding base material 200 can be cleaned to volatilize low-melting-point pollutants and reduce spatter caused by low-melting-point pollutants; the cooling rate of the weld can also be slowed down, thermal stress can be reduced, and the generation of cracks can be avoided.
[0089] The inner wall surface 21 and the outer wall surface 22 can increase the spot area of the annular light beam 20 projected on the welding base material 200, thereby increasing the effective action area of the annular light beam 20, improving the preheating effect and slow cooling effect of the annular light beam 20, and reducing the phenomenon of defects such as welding cracks in the welding base material 200 during the welding process.
[0090] The D / d≥3 proposed in this embodiment can ensure that the spot diameter of the annular beam 20 exceeds the spot diameter of the central beam 10 by at least 2 times. Since the central beam 10 is concentric with the annular beam 20, the portion of the annular beam 20 that exceeds the central beam 10 can play the role of preheating and slow cooling, as well as the effect of cleaning the weld surface; D / d≤8 is to avoid the phenomenon that the heat affected zone is too large due to the excessive spot diameter of the annular beam 20, which leads to the coarsening of the grains in the welding area of the welding base material 200 and affects the performance of the base material.
[0091] like Figures 10 to 20 As shown, in some embodiments, controlling the annular arc-ending power of the annular beam 20 to decrease delayedly compared with the central arc-ending power of the central beam 10 in the welding arc-ending stage also includes: controlling the central beam 10 to be emitted in a modulated pulse wave manner, the central arc-ending power is the pulse power of the modulated pulse wave in the welding arc-ending stage, and / or controlling the annular beam 20 to be emitted in a continuous wave manner, the annular arc-ending power is the arc-ending power of the continuous wave in the welding arc-ending stage.
[0092] In this embodiment, emission in a modulated pulse mode refers to emission in a pulse-width modulation (PWM) mode, which is a method of reducing the average power transmitted by the central light beam 10 by dispersing the effective central light beam 10 into discrete forms; emission in a continuous wave mode refers to the laser outputting the annular light beam 20 in a continuous manner rather than in a pulsed manner, and the annular light beam 20 is emitted by a sine wave and a continuous wave synthesized by several sinusoidal components.
[0093] like Figures 10 to 14 As shown, controlling the central light beam 10 to be emitted in a modulated pulse manner specifically includes: the pulse wave of the central light beam 10 includes at least one of a triangle, a corrugated shape, a sawtooth shape, a trapezoidal shape, and a step shape. The central arc closing power of the central light beam 10 can be set to rise to the highest point first and then decrease, because after the central arc closing power reaches the highest point and breaks through the laser power threshold required to melt the welding parent material 200 to form the keyhole 202, the absorption rate of the welding parent material 200 to the laser increases. Therefore, the power of the second half of the pulse wave of the central light beam 10 can be appropriately reduced to further reduce the heat input.
[0094] like Figures 15 to 20 As shown, controlling the annular beam 20 to be emitted in a continuous manner specifically includes: controlling the power of the annular beam 20 to gradually increase to a preset working power during the arc starting stage of welding; and / or controlling the annular arc ending power of the annular beam 20 to gradually decrease from a preset initial working power during the arc ending stage of welding.
[0095] The arc starting stage of welding refers to the starting stage of welding, and the arc ending stage of welding refers to the ending stage of welding. Arc pits will be generated in both the arc starting stage and the welding ending stage, and phenomena such as looseness, cracks, pores, and slag inclusions often occur. In order to overcome the arc pit defects, the embodiment of the present application adjusts the weld morphology by controlling the power of the annular beam 20. Specifically, in the arc starting stage of welding, the power of the annular beam 20 can be gradually increased from low to high to a preset working power, so as to avoid the "match head" morphology at the arc starting point; in the arc ending stage of welding, the power of the annular beam 20 is gradually reduced, which can reduce the energy density of the welding line, the weld molten width gradually narrows, and the deep molten small hole gradually becomes shallower during welding, thereby improving the arc pit morphology at the arc ending point of the weld. The slow rise of the annular beam 20 at the arc starting point can reduce the "match head" morphology of the weld arc starting point, and the slow descent at the arc ending stage of welding can reduce the phenomenon of arc pit depression in the weld at the arc ending stage of welding.
[0096] Controlling the annular beam 20 to emit in a continuous manner also includes: controlling the power of the annular beam 20 to form a stable working stage with a preset initial working power between the welding arc starting stage and the welding arc ending stage. The annular beam 20 can play a role of stable preheating and slow cooling in the stable working stage, thereby increasing the absorption rate of the welding base material 200 to the laser, improving the welding stability, and delaying the cooling speed of the weld, reducing the local thermal stress of the weld, and avoiding the generation of weld cracks.
[0097] In this embodiment, by setting the central light beam 10 to a modulated pulse laser, the heat input of the central light beam 10 can be reduced, and the burning and evaporation of low-melting-point alloy elements can be reduced; by continuously preheating with the annular light beam 20, the absorption rate of the welding base material 200 to the laser can be increased, the welding stability can be improved, and the surface of the welding base material 200 can be cleaned to volatilize low-melting-point pollutants and reduce spatter caused by low-melting-point pollutants. Continuous preheating with the annular light beam 20 can also slow down the cooling rate of the weld, reduce the local thermal stress of the weld, and avoid the generation of weld cracks.
[0098] A second aspect of the present application provides a laser welding device, which includes a laser transmitter, and the laser transmitter is used to implement the laser welding method of the first aspect of the present application.
[0099] The laser welding method provided in this embodiment uses a dual-beam concentric laser 100 composed of a central beam 10 and an annular beam 20 for welding. The delayed reduction of the annular arc closing power of the annular beam 20 can further slow down the cooling rate of the weld, thereby solving the technical problem that crack defects are easily formed in metal materials during the cooling process of the weld.
[0100] Specifically, the high-intensity laser of the central beam 10 of the dual-beam concentric laser 100 can melt the welding base material 200, and the annular beam 20 of the dual-beam concentric laser 100 is distributed around the central beam 10. The weak-intensity laser of the annular beam 20 can not only preheat the welding base material 200, but also slow down the cooling rate of the weld, thereby reducing the phenomenon of crack defects in metal materials during the cooling process of laser welding, especially reducing the phenomenon of crack defects in welds of dissimilar metal materials (such as steel and copper) during the cooling process.
[0101] like Fig.21 As shown, in some embodiments, the laser welding equipment also includes a controller, which is provided with a computer-readable storage medium and a control device, and the control device includes: a control module 321, which is used to perform laser welding using a double-beam concentric laser 100 formed by a central beam 10 and an annular beam 20 during the arc ending stage of welding; and is used to control the annular arc ending power of the annular beam 20 to decrease with a delay compared to the central arc ending power of the central beam 10 during the arc ending stage of welding.
[0102] It should be noted that the embodiments of the present application only describe the structures on the laser welding equipment that are related to the invention points, and do not mean that the laser welding equipment only has these structures. Other structures on the laser welding equipment will not be described one by one here.
[0103] A third aspect of the present application provides a laser welding assembly, which is welded by the laser welding device according to the second aspect of the present application.
[0104] The laser welding assembly provided in the embodiment of the present application is welded by the same metal material or dissimilar metal materials through the laser welding method of the first aspect of the present application, and the laser welding method of the first aspect of the present application can reduce the generation of defects such as cracks and pores in the weld pool 201. In particular, for laser welding of dissimilar metal materials (such as steel and copper), the laser welding assembly can adapt to the differences in physical and chemical properties such as the expansion coefficient of the two metals during the welding process, and reduce the phenomenon of cracks in the weld of the laser welding assembly under different stresses.
[0105] In some embodiments, the laser welded assembly comprises an aluminum alloy welded assembly. Figure 4 , Fig. 22 , Fig.23 and Fig.24 As shown, the technical solution of the present application is described in detail below through two embodiments.
[0106] Example 1: Stitch welding of aluminum alloy
[0107] The upper welding base material 200 is a first aluminum alloy plate 210 with a thickness of 0.8 mm, and the lower welding base material 200 is a second aluminum alloy plate 220 with a thickness of 0.4 mm. The two are penetrated and welded by a double-beam concentric laser 100. The spot diameter of the central beam 10 of the double-beam concentric laser 100 is 200 μm, the spot diameter of the annular beam 20 is 800 μm, the initial working power of the central beam 10 is 700 w to 1200 w, and the initial working power of the annular beam 20 is 800 w to 1200 w. The welding speed is 200 mm / s, the defocus amount is 3.0 mm, the shielding gas is nitrogen, and the flow rate is 15 L / min to 30 L / min. The distance between the arc starting point a and the arc end point c in the arc ending stage of welding is 10 mm. The arc ending power drop curve in the arc ending stage of welding is as shown in the figure. Figure 7 As shown in the figure, when the double-beam concentric laser 100 reaches the arc closing starting point a (0mm), the central arc closing power begins to decrease nonlinearly, and the annular arc closing power remains unchanged; when the double-beam concentric laser 100 reaches the welding arc closing decomposition point b (5mm), the central arc closing power of the central beam 10 decreases to 700w, and the annular arc closing power of the annular beam 20 remains at the initial working power of 1200w; when the double-beam concentric laser 100 reaches the arc closing length of 8mm, the central arc closing power of the central beam 10 decreases nonlinearly to 0, and when the double-beam concentric laser 100 reaches the arc closing end point c, the annular arc closing power of the annular beam 20 decreases nonlinearly to 0. The welding arc closing obtained according to this method can reduce the generation of welding cracks. The appearance of the weld arc closing obtained according to this method is as follows: Fig. 22 As shown, there is no crack, and the arc closing appearance of the weld without the ring-shaped arc closing power slow-down of the annular beam 20 is as follows Fig.23 As shown, there is an obvious crack at the end of the arc.
[0108] Example 2: Stitch welding of aluminum alloy
[0109] The upper welding base material 200 is a first aluminum alloy plate 210 with a thickness of 0.6 mm, and the lower welding base material 200 is a second aluminum alloy plate 220 with a thickness of 0.4 mm. The two are penetrated and welded by a double-beam concentric laser 100. The spot diameter of the central beam 10 of the double-beam concentric laser 100 is 200 μm, the spot diameter of the annular beam 20 is 800 μm, the initial working power of the central beam 10 is 600w~900w, and the initial working power of the annular beam 20 is 800w~1200w. The welding speed is 200mm / s, the defocus amount is 3.0mm, the shielding gas is nitrogen, and the flow rate is 15L / min~30L / min. The distance between the arc starting point a and the arc end point c in the arc ending stage of welding is 10mm. The arc ending power drop curve in the arc ending stage of welding is as shown in the figure. Figure 6As shown, when the double-beam concentric laser 100 reaches the arc-ending starting point a (0mm), the central arc-ending power of the central beam 10 begins to decrease linearly, and the annular arc-ending power of the annular beam 20 remains unchanged; when the double-beam concentric laser 100 reaches the arc-ending decomposition point b (5mm), the central arc-ending power of the central beam 10 begins to decrease linearly to 500w, and the annular arc-ending power of the annular beam 20 remains at 1000w; when the double-beam concentric laser 100 reaches the arc-ending end point c (10mm), the central arc-ending power of the central beam 10 and the annular arc-ending power of the annular beam 20 decrease linearly to 0. The arc-ending obtained according to this method can also reduce the generation of welding cracks. The appearance of the weld arc-ending obtained according to this method is as follows: Fig.24 As shown, there are no cracks.
[0110] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application is described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A laser welding method, characterized in that: The laser welding method comprises: In the arc closing stage of welding, a double-beam concentric laser formed by a central beam and an annular beam is used for laser welding; Control the annular arc ending power of the annular light beam to decrease with a delay compared with the central arc ending power of the central light beam during the arc ending stage of welding; The controlling of the annular arc ending power of the annular light beam to decrease with a delay compared with the central arc ending power of the central light beam during the arc ending stage of welding specifically includes: The welding arc closure stage is divided into a welding arc closure front section and a welding arc closure rear section; The central arc ending power of the central light beam is controlled to gradually decrease in the front section of the welding arc ending, and the annular arc ending power of the annular light beam is controlled to maintain at the initial working power in the front section of the welding arc ending.
2. The laser welding method according to claim 1, characterized in that: The step of controlling the central arc-ending power of the central light beam to gradually decrease in the front section of the welding arc-ending includes: The central arc-ending power of the central light beam is controlled to continuously decrease in the front section of the welding arc-ending, and is reduced to 50% to 70% of the initial working power at the dividing point between the front section of the welding arc-ending and the rear section of the welding arc-ending.
3. The laser welding method according to claim 1, characterized in that: The step of dividing the arc closure stage of welding into the front arc closure stage of welding and the rear arc closure stage of welding further comprises: The central arc ending power of the central light beam is controlled to be reduced to zero before the annular arc ending power of the annular light beam in the later stage of arc ending of welding.
4. The laser welding method according to claim 1, characterized in that: The step of dividing the arc closure stage of welding into the front arc closure stage of welding and the rear arc closure stage of welding further comprises: The central arc-ending power of the central light beam is controlled to be reduced to zero simultaneously with the annular arc-ending power of the annular light beam in the rear stage of welding arc-ending.
5. The laser welding method according to any one of claims 1 to 4, characterized in that: The step of dividing the arc closure stage into the front section of the arc closure and the back section of the arc closure specifically includes: Obtaining the disappearance position of the welding keyhole in the arc ending stage of the welding; The dividing point between the front section of the welding arc closure and the rear section of the welding arc closure is generated according to the disappearance position of the welding keyhole.
6. The laser welding method according to claim 4, characterized in that: The controlling the annular arc ending power of the annular light beam to decrease with a delay compared with the central arc ending power of the central light beam during the welding arc ending stage also includes: According to the central arc closing power of the central light beam being p and the annular arc closing power of the annular light beam being P, it is determined that the ratio of P to p satisfies 1≤P / p≤4.
7. The laser welding method according to claim 1, characterized in that: The controlling the annular arc ending power of the annular light beam to decrease with a delay compared with the central arc ending power of the central light beam during the welding arc ending stage also includes: According to the spot diameter of the central light beam in the welding arc ending stage being d, and the spot diameter of the annular light beam in the welding arc ending stage being D, it is determined that the ratio of D to d satisfies 3≤D / d≤8.
8. A laser welding device, characterized in that: The laser welding device comprises a laser transmitter, and the laser transmitter is used to implement the laser welding method according to any one of claims 1 to 7.
9. The laser welding equipment according to claim 8, characterized in that: The laser welding device further includes a controller, wherein the controller is provided with a computer-readable storage medium and a control device, wherein the control device includes: Control module, Used for laser welding in the arc closing stage using a double-beam concentric laser formed by a central beam and an annular beam; The annular arc ending power for controlling the annular light beam decreases with a delay compared with the central arc ending power of the central light beam during the arc ending stage of welding.
10. A laser welding assembly, characterized in that: The laser welding assembly is welded by the laser welding equipment according to claim 8 or 9.
11. The laser welding assembly according to claim 10, characterized in that: The laser welding assembly includes an aluminum alloy welding assembly.
Citation Information
Patent Citations
Double beam pulse laser welding method for Ti2A1Nb-based intermetallic compound
CN104384718A
Aluminum alloy double beam laser welding method and device
CN108453374A