Ultra-high early strength ultra-high performance concrete and preparation method thereof
Through the combination of silicate and sulfaluminate cement composite system and fiber materials, ultra-high performance concrete with ultra-high strength and later strength improvement at room temperature is achieved, and the poor constructionability and high energy consumption in the existing technology are solved. Problem, suitable for rapid emergency repair projects.
Patent Information
- Application Number
- CN202211596372.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-12
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-12-12
AI Technical Summary
It is difficult for existing ultra-high performance concrete to achieve ultra-high early strength and controllable settling time at room temperature, and it has both steady improvement in later strength and crack resistance, and has poor construction properties, which are difficult to quickly thermal maintenance with high energy consumption.
Adopt silicate and sulfaluminate cement composite system, combined with premature strength agents and fiber materials with specific ratios, combined with silica fume, volcanic rock micro powder, quartz sand, steel fiber, polymer fiber and nano iron trioxide, through normal temperature The curing achieves rapid condensation and later strength improvement, and improves compactness through specific ratios of quartz sand and defoaming agents.
Achieve ultra-high early strength at room temperature (24h compressive strength ≥100MPa), and the later strength is steadily improved (28d compressive strength ≥180MPa), with excellent toughness and crack resistance, and the process is simple and efficient, suitable for rapid emergency repair projects.
Smart Images

Figure CN115819052B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of civil engineering materials, and more specifically, to an ultra-high early strength ultra-high performance concrete and a preparation method thereof. Background Art
[0002] Ultra-high performance concrete (UHPC) is the most innovative cement-based material developed in the 1990s, with excellent mechanical properties, toughness and durability. Therefore, UHPC shows great potential in application projects with special requirements, such as rapid repair and construction projects, protective projects, long-span bridges, ports and docks, nuclear power plants and offshore platforms.
[0003] With the development of economy and technology, some modern rapid repair projects require concrete to show ultra-high mechanical strength in the shortest possible construction time, and the setting time can be controlled to ensure construction performance. In addition, concrete must have excellent late strength, no strength shrinkage, and good toughness, crack resistance and durability.
[0004] In response to the above requirements, the special cements currently on the market often cannot meet the dual requirements of ultra-high early strength and adjustable setting time. In order to meet the excessively high early strength, too high an amount of early strength components are often added, which makes the newly mixed concrete unworkable, that is, it starts to harden and loses workability 10 to 20 minutes after forming, and it is impossible to reserve suitable construction time for the project site. Excessive early strength components will cause damage to the later strength of the silicate cement system. In addition, the large-scale use of rapid heat curing methods such as steam curing to maintain ultra-high performance concrete on construction sites also has the disadvantages of high difficulty and high energy consumption.
[0005] In view of the above, there is an urgent need to invent an ultra-high performance concrete that has ultra-high early strength, controllable setting time, steadily increasing strength in the later stage, no shrinkage, and excellent toughness and crack resistance under room temperature curing. Summary of the invention
[0006] Based on the above-mentioned technical problems existing in the prior art, the present invention provides an ultra-high performance concrete with ultra-high early strength, which has the characteristics of rapid coagulation and hardening, ultra-high early strength, steadily increasing later strength, no shrinkage, and excellent toughness, and can realize the construction and reinforcement of special engineering projects for emergency repair and construction.
[0007] In order to achieve the above object, the technical solution of the present invention is as follows:
[0008] An ultra-high early strength ultra-high performance concrete, wherein each cubic meter of the ultra-high performance concrete comprises the following components:
[0009]
[0010] In some embodiments, the silicate cement is at least one of P·II 42.5, P·II 52.5, P·II 42.5R, and P·II 52.5R.
[0011] In some embodiments, the specific surface area of the sulphoaluminate cement is ≥350 m 2 / kg,Al 2 O 3 Content>30%, SiO 2 Content <10.5%.
[0012] In some embodiments, the SiO 2 Content ≥93wt%, specific surface area ≥16000m 2 / kg.
[0013] In some embodiments, the volcanic rock powder has an average particle size of ≤10 μm and a specific surface area of ≥600 m 2 / kg,SiO 2 +Al 2 O 3 ≥65%.
[0014] In some embodiments, the quartz sand is graded in three ways: 26-40 mesh, 40-70 mesh, and 150-200 mesh, with a mass ratio of 0.50-0.53: 0.22-0.25: 0.25-0.28. The use of a specific ratio of continuously graded quartz sand can make the initial packing density of aggregate particles higher, and the use of a defoaming agent can eliminate the disadvantages of ultra-high performance concrete that the viscosity is too high and the internal bubbles cannot be vibrated out, which is beneficial to improving the compactness of the material microstructure and further improving the later mechanical strength of the concrete.
[0015] In some embodiments, the steel fiber is a straight copper-plated fine steel fiber with a diameter of 0.18 to 0.20 mm and a length of 8 to 13 mm.
[0016] In some embodiments, the polymer fiber is an ultra-high molecular weight polyethylene fiber, the weight average molecular weight of the polyethylene is 1 million to 3 million, the diameter of the polyethylene fiber is 20 to 70 μm, and the length is 18 to 24 mm.
[0017] In some embodiments, the early strength agent is a composite of CSH seed crystals and triethanolamine, and the mass ratio of the CSH seed crystals to the triethanolamine is 20 to 30: 1 to 5. The silicate and sulphoaluminate cement composite system, matched with the composite early strength agent, can not only accelerate the early strength development of concrete, but also adjust the dosage of sulphoaluminate cement, CSH seed crystals and triethanolamine composite early strength agent to achieve the control of the setting time of the system.
[0018] In some embodiments, the water reducing agent is a powdered polycarboxylic acid superplasticizer.
[0019] In some embodiments, the defoaming agent is a polyether high-performance powder defoaming agent.
[0020] In some embodiments, the ultra-high performance concrete further comprises CaSO 4 Whiskers, the CaSO 4 Whiskers are columnar fibers, with CaSO 4 The content is ≥95wt%, the diameter is 1-15μm, and the length is 10-300μm.
[0021] In some embodiments, the ultra-high performance concrete further comprises nano-ferric oxide, wherein the average particle size of the nano-ferric oxide is 35±5 nm, which can further promote hydration and achieve a reinforcing effect.
[0022] The present invention also provides a method for preparing ultra-high early strength ultra-high performance concrete according to any of the above embodiments, the method comprising the following steps:
[0023] S1, mixing the raw materials according to the ratio, mixing the silicate cement, sulphoaluminate cement, silica fume, volcanic rock powder and quartz sand, and then adding the CaSO 4 whiskers, polymer fibers, steel fibers and nano-iron oxide are mixed to obtain a dry material mixture;
[0024] S2, adding the early strength agent, water reducing agent, defoaming agent and water to the dry material mixture and mixing to form a slurry;
[0025] S3, molding, vibrating and plastering the slurry, and curing at room temperature (20±1° C.) to obtain the ultra-high early strength ultra-high performance concrete.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1) The present invention adopts a composite system of silicate and sulphoaluminate cement, and matches a specific amount of an early strength agent of the composite system, which can accelerate the early setting speed of concrete. Without the aid of rapid thermal curing means, the synergistic early strength effect of aluminate cement and early strength agent enables the ultra-high performance concrete to have ultra-high early strength (24h compressive strength ≥ 100MPa) under normal temperature (20±1°C) curing;
[0028] 2) The addition of solid waste resources such as silica fume and volcanic rock powder, and the replacement of some silicate cement with sulphoaluminate cement (the CO2 emitted by producing the same quality of sulphoaluminate cement is 2.5 times that of silicate cement). 2 The amount of silicate cement used can be reduced effectively, thereby improving the greenness of the ultra-high performance concrete of the present invention, and the low-energy consumption room temperature curing method is adopted, so that the ultra-high performance concrete of the present invention has the characteristics of being green, low-carbon and environmentally friendly;
[0029] 3) The addition of quartz sand as aggregate particles and defoaming agent eliminates the disadvantages of ultra-high performance concrete that the viscosity is too high and the internal bubbles cannot be vibrated out, which is beneficial to improve the compactness of the material microstructure, thereby improving the later mechanical strength of ultra-high performance concrete (28d compressive strength ≥ 180MPa);
[0030] 4) The composite use of steel fiber, polymer fiber and whisker, combined with highly chemically active nano-iron oxide, is conducive to the multi-scale reinforcement and toughening effect of fiber / particles from the main hydration product CSH gel (micro-nano) to the cement matrix (macro), thereby achieving ultra-high toughness of ultra-high performance concrete (3, 5.5 and 10.5 times the initial crack (peak) deflection flexural toughness index I 5 ≥5, I 10 ≥10 and I 20 ≥20);
[0031] 5) The method for preparing ultra-high performance concrete with ultra-high early strength provided by the present invention is simple, efficient, and operable, and has on-site constructability, which is conducive to the promotion and application of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The flexural and compressive failure morphology diagram of the ultra-high performance concrete prepared in Example 1;
[0033] Figure 2 The flexural and compressive failure morphology diagram of the ultra-high performance concrete prepared in Example 2;
[0034] Figure 3 The flexural and compressive failure morphology diagrams of the ultra-high performance concrete prepared in Example 3;
[0035] Figure 4This is a microscopic scanning electron microscope image of the ultra-high performance concrete prepared in Example 1;
[0036] Figure 5 This is a microscopic scanning electron microscope image of the ultra-high performance concrete prepared in Example 2;
[0037] Figure 6 This is a microscopic scanning electron microscope image of the ultra-high performance concrete prepared in Example 3. DETAILED DESCRIPTION
[0038] Many specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar modifications without violating the connotation of the present invention, so the present invention is not limited to the specific implementation disclosed below.
[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0040] In the following examples and comparative examples, the silicate cement used is P·II 52.5 cement; the sulphoaluminate cement is fast-hardening (low alkalinity) sulphoaluminate cement (SAC); the silica fume is Aiken 940 grade microsilica fume; and the CaSO 4 The whiskers are NP-S02-PI type calcium sulfate whiskers; the nano-iron oxide is grade I (particle size 35±5nm) nano-Fe 2 O 3 The early strength agent is a complex of VIVID-300 CSH seed and triethanolamine, with a mass ratio of 20:1; the water reducer is SD-600P-S polycarboxylic acid superdispersant; and the defoamer is CQ-406 high-performance defoamer.
[0041] Examples 1 to 3
[0042] The raw material proportions per cubic meter of the ultra-high performance concrete of Examples 1 to 3 are shown in Table 1 below.
[0043] Table 1 Raw material ratio per cubic meter of ultra-high performance concrete of Examples 1 to 3 (kg / m 3 )
[0044]
[0045] The preparation method of the ultra-high performance concrete of Examples 1 to 3 comprises the following steps:
[0046] S1. Weighing of raw materials: weigh the corresponding raw materials according to the raw material ratio in Table 1;
[0047] S2. Dry mixing of powders: Put silicate cement P·II 52.5, sulphoaluminate cement SAC, silica fume, volcanic rock powder and quartz sand into a stirring pot for dry mixing, and add fiber / particle reinforcement materials polymer fiber and steel fiber (Example 1) in sequence; or add polymer fiber, steel fiber and CaSO 4 Whiskers (Example 2); or adding polymer fibers, steel fibers, CaSO 4 Whiskers and nano-Fe 2 O 3 (Example 3), dry-mixing to obtain a dry material mixture;
[0048] S3, preparation of fresh concrete: adding water, early strength agent, water reducing agent and defoaming agent into the mixing pot, and mixing them with the dry material mixture to form slurry;
[0049] S4, concrete molding: the slurry obtained in step S3 is loaded into a 40 mm × 40 mm × 160 mm mold, followed by vibration and plastering, and the molded surface is covered with a film and cured at room temperature (20 ± 1 ° C) to obtain ultra-high early strength ultra-high performance concrete.
[0050] Comparative Example 1
[0051] The raw material proportion per cubic meter of the concrete of Comparative Example 1 is shown in Table 2 below.
[0052] Table 2 Raw material ratio per cubic meter of concrete of comparative example 1 (kg / m 3 )
[0053]
[0054] The preparation method of the concrete of Comparative Example 1 comprises the following steps:
[0055] S1. Weighing of raw materials: weigh the corresponding raw materials according to the raw material ratio described in Table 2;
[0056] S2. Dry mixing of powders: Put silicate cement P·II 52.5, silica fume, volcanic rock powder and quartz sand into a stirring pot for dry mixing, and add fiber-reinforced polymer fiber and steel fiber in sequence, dry mix evenly, and obtain a dry material mixture;
[0057] S3, preparation of fresh concrete: adding water, water reducing agent and defoaming agent into the mixing pot, and mixing with the dry material mixture to form slurry;
[0058] S4, concrete molding: the slurry obtained in step S3 is loaded into a 40 mm × 40 mm × 160 mm mold, followed by vibration and plastering, and the molded surface is covered with a plastic film and placed at room temperature (20 ± 1 ° C) for curing to obtain ordinary ultra-high performance concrete.
[0059] The concrete obtained in Examples 1 to 3 and Comparative Example 1 was tested for mechanical strength and flexural toughness. The test results are shown in Table 3.
[0060] Table 3 Mechanical strength and flexural toughness test results of concrete obtained from Examples 1 to 3 and Comparative Example 1
[0061]
[0062] It can be seen from Table 3 that the ultra-high performance concrete with ultra-high early strength of Examples 1 to 3 of the present invention has flexural and compressive strengths greater than 5MPa and 20MPa respectively when cured at room temperature for 6 hours, and greater than 25MPa and 100MPa respectively at 24 hours. This shows that the ultra-high performance concrete with ultra-high early strength of the present invention has ultra-high mechanical strength at a curing age of 1d, and has a fast setting speed (hardening in about 2 to 3 hours), and has a reasonable construction time. However, Comparative Example 1 has not hardened to form strength at 6 hours, and cannot meet the requirements of rapid repair projects with high strength in a short time. In addition, at 24 hours, the flexural and compressive strengths of Comparative Example 1 are relatively low, only about 70% of the flexural and compressive strengths of Examples 1 to 3. In general, the ultra-high performance concrete of the present invention has good workability, a reasonably controllable setting time, ultra-high strength in the early stage (compressive strength ≥ 100 MPa after 1 day of standard curing at 20°C), and the strength steadily increases within 28 days, achieving excellent late mechanical strength performance (28d compressive strength ≥ 180 MPa), without strength shrinkage, and ultra-high bending toughness (I 5 ≥5, I 10 ≥10 and I 20 ≥20).
[0063] In addition, the instruction manual Figures 1 to 3 It can be seen intuitively that after the bending and compression tests of Examples 1 to 3, the test pieces did not break into two pieces and still had good integrity; Figures 4 to 6 It can be observed that the cement matrix of Examples 1 to 3 is very dense, and the matrix and the aggregate are tightly bonded, which further illustrates the ultra-high strength and ultra-high toughness of the specimens of Examples 1 to 3.
[0064] In summary, the ultra-high early strength ultra-high performance concrete described in the present invention can provide a feasible technical solution for the construction and building of high-grade / high-requirement rapid emergency repair projects.
[0065] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0066] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An ultra-high early strength ultra-high performance concrete, characterized in that: Each cubic meter of the ultra-high performance concrete includes the following components: Portland cement 600~800kg / m 3 Sulphoaluminate cement 50~150 kg / m 3 Silica fume 150~250 kg / m 3 Volcanic rock powder 100~200 kg / m 3 Quartz sand 1000~1200 kg / m 3 Steel fiber 156~234 kg / m 3 Polymer fiber 3~6kg / m 3 Early strength agent 4~10 kg / m 3 Water reducing agent 6~18 kg / m 3 Defoaming agent 1~2 kg / m 3 Water 155~180 kg / m 3 ; The specific surface area of the sulphoaluminate cement is ≥350m 2 / kg, Al2O3 content>30%, SiO2 content<10%; The quartz sand adopts three gradations of 26-40 mesh, 40-70 mesh and 150-200 mesh, and the mass ratio is 0.50-0.53:0.22-0.25:0.25-0.28; The ultra-high performance concrete also includes 20-30 kg / m CaSO4 whiskers 3 and nano-iron oxide 3~6 kg / m 3 The CaSO4 whiskers are columnar fibers with a CaSO4 content of ≥95wt%, a diameter of 1-15μm, and a length of 10-300μm; the average particle size of the nano-iron oxide is 35±5nm; The silica fume has a SiO2 content of ≥93wt% and a specific surface area of ≥16000 m 2 / kg; The average particle size of the volcanic rock powder is ≤10μm, and the specific surface area is ≥600 m 2 / kg, SiO2+Al2O3≥65%; The steel fiber is a straight copper-plated fine steel fiber with a diameter of 0.18-0.20 mm and a length of 8-13 mm; and / or the polymer fiber is an ultra-high molecular weight polyethylene fiber with a weight average molecular weight of 1 million to 3 million; the polyethylene fiber has a diameter of 20-70 μm and a length of 18-24 mm; The early strength agent is a compound of CSH seed crystals and triethanolamine, and the mass ratio of the CSH seed crystals to the triethanolamine is 20-30:1-5.
2. The ultra-high early strength ultra-high performance concrete according to claim 1, characterized in that: The silicate cement is at least one of P·II 42.5, P·II 52.5, P·II 42.5R, and P·II 52.5R.
3. The ultra-high early strength ultra-high performance concrete according to claim 1, characterized in that: The water reducing agent is a powdered polycarboxylic acid superplasticizer; and / or the defoaming agent is a polyether high-performance powdered defoaming agent.
4. The method for preparing ultra-high performance concrete with ultra-high early strength according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1. Mix the silicate cement, sulphoaluminate cement, silica fume, volcanic rock powder and quartz sand according to the raw material ratio, then add the polymer fiber, steel fiber, CaSO4 whisker and nano-iron trioxide, mix well and obtain a dry material mixture; S2, adding the early strength agent, water reducing agent, defoaming agent and water to the dry material mixture and mixing to form a slurry; S3, molding, vibrating and plastering the slurry, and curing at room temperature to obtain the ultra-high early strength ultra-high performance concrete.