A method for preparing a water-based binder for a lithium iron phosphate positive electrode

Through the composite method of solution glue and emulsion glue, a water-based lithium iron phosphate binder with both mechanical and bonding properties is prepared, which solves the problem of difficulty in balancing the performance of water-based binders in the existing technology and achieves environmentally friendly, high-efficiency Battery performance.

CN115832313BActive Publication Date: 2024-10-18SHAANXI COAL & CHEM TECH INST
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211739785.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-10-18
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

It is difficult for existing water-based binders to balance mechanical properties and bonding properties when used in lithium iron phosphate cathodes, and there are common problems of brittleness and difficulty in homogenization. In addition, the use of toxic organic solvents in traditional binders leads to environmental pollution.

Method used

Using the physical compounding method of solution glue and emulsion glue, the water-based adhesive is formed by polymerizing monomers such as acrylonitrile, acrylamide, β-acryloyloxypropionic acid and vinyl acetate, combining non-polar and polar monomers , emulsifier and initiator, adjust the pH value, and prepare a lithium iron phosphate water-based binder with both flexibility and bonding properties.

Benefits of technology

It achieves both pole piece processing performance and electrochemical performance in an aqueous system, reduces environmental costs, avoids pollution from organic solvents, and improves battery cycle and rate performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004031950740000011
    Figure HDA0004031950740000011
  • Figure HDA0004031950740000012
    Figure HDA0004031950740000012
Patent Text Reader

Abstract

The present invention discloses a method for preparing a water-based binder for lithium iron phosphate positive electrode, which is a method for improving the performance of water-based binder by physical compounding of emulsion-solution, wherein two or more of acrylonitrile, acrylamide, β-acryloxypropionic acid and vinyl acetate are mixed with acrylic acid, part of the carboxyl groups are neutralized, added to water, and neutralized to neutrality after polymerization reaction to obtain solution glue; non-polar monomer, polar monomer, emulsifier and initiator are added to water, and pH is adjusted to 6-8 after polymerization reaction to obtain emulsion glue; solution glue is mixed with emulsion glue, and pH is adjusted to 5-9. The present invention adopts a two-phase mixture of solution glue and emulsion glue, which can ensure the flexibility and bonding force of the pole piece while ensuring that the material has good cycle rate performance. The binder of the present invention is an aqueous homogenization system, which fundamentally eliminates the discharge of organic pollutants, greatly reduces environmental costs, and takes into account both processing performance and electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the fields of lithium battery materials and adhesives, and in particular to a method for preparing a water-based binder for a lithium iron phosphate positive electrode. Background Art

[0002] With the rapid development of the lithium battery industry, lithium iron phosphate positive electrodes have been increasingly used in lithium-ion batteries. The binder used in traditional lithium iron phosphate is mainly PVDF, which has a high cost and requires the use of toxic organic solvent NMP as a solvent, which causes great environmental pollution and is highly toxic. As an electrode bonding material, the binder has a great impact on the processing performance of the electrode, battery cycle, rate, capacity and other properties. How to replace PVDF with water while ensuring the processing performance and electrochemical performance of the binder is a major problem that needs to be solved urgently in the new energy industry.

[0003] In the prior art, water-based adhesives are currently basically used alone as solution adhesives or emulsion adhesives, which makes it difficult to achieve both mechanical properties and bonding properties, and there are common problems of brittle flakes and difficulty in homogenizing. Summary of the invention

[0004] In order to overcome the common problems of brittle flakes and difficulty in homogenization when aqueous binders are used in positive electrodes in the prior art, the purpose of the present invention is to provide a method for preparing an aqueous binder for lithium iron phosphate positive electrode, wherein the water-washable adhesive prepared by the method has both mechanical properties and bonding properties.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] A method for preparing a lithium iron phosphate positive electrode using an aqueous binder comprises the following steps:

[0007] Mixing two or more of acrylonitrile, acrylamide, β-acryloxypropionic acid and vinyl acetate with acrylic acid to obtain a mixture, then neutralizing 10% to 50% of the total amount of carboxyl groups in the mixture to obtain a neutralized monomer; adding the neutralized monomer and an initiator to water to obtain a pre-reaction liquid, subjecting the pre-reaction liquid to a polymerization reaction under nitrogen protection and then neutralizing it to neutrality to obtain a solution glue;

[0008] Adding a non-polar monomer, a polar monomer, an emulsifier and an initiator into water to obtain a reaction system, emulsifying the reaction system to obtain a pre-emulsion; adding the pre-emulsion into an emulsifier solution, and then performing a polymerization reaction under nitrogen protection, adjusting the pH to 6-8, and obtaining an emulsion glue;

[0009] The solution glue and the latex glue are mixed and the pH is adjusted to 5 to 9 to obtain a water-based binder for lithium iron phosphate.

[0010] Furthermore, the mass percentage of acrylic acid in the mixture is 40% to 90%.

[0011] Furthermore, the mass concentration of the neutralized monomer in the pre-reaction liquid is 15-30%, and the mass concentration of the initiator in the pre-reaction liquid is 0.1%-0.6%.

[0012] Furthermore, the non-polar monomer is one or two of butyl acrylate, isooctyl acrylate, styrene and vinyl acetate.

[0013] Furthermore, the polar monomer is one or two of acrylic acid, acrylonitrile, acrylamide and β-acryloxypropionic acid.

[0014] Furthermore, the polymerization reaction temperature was 70-85°C and the time was 2.5-3h.

[0015] Furthermore, the initiators are ammonium persulfate or potassium persulfate.

[0016] Furthermore, in the reaction system, the non-polar monomer accounts for 70% to 98% of the total mass of the non-polar monomer and the polar monomer, the polar monomer accounts for 2% to 30% of the total mass of the non-polar monomer and the polar monomer, the emulsifier accounts for 1% to 4% of the total mass of the non-polar monomer and the polar monomer, and the initiator accounts for 0.1% to 0.6% of the total mass of the non-polar monomer and the polar monomer.

[0017] Furthermore, the mass concentration of the emulsifier solution is 0.2%, and the amount used is 50% of the total mass of the non-polar monomer and the polar monomer.

[0018] Furthermore, the emulsifier is a reactive emulsifier.

[0019] Furthermore, the reactive emulsifier is one or more of DNS-86, JS-20, SR-10, SR-20 and SR-30.

[0020] Furthermore, the mass ratio of the solution glue to the latex glue is 1:1-2.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] In the present invention, solution glue and latex glue are prepared, and then the solution glue and latex glue are polymerized in two phases, and non-polar monomers and polar monomers are mixed in a certain ratio. The non-polar monomer has a low Tg value, which can well ensure the flexibility of the colloid. At the same time, a small amount of carboxyl groups on the polar monomers form hydrogen bonds, taking into account good bonding performance; the solution glue has a main monomer and a functional monomer, the main monomer is polypropylene, and the functional monomer is acrylonitrile, acrylamide, β-acryloxy propionic acid and vinyl acetate. The main monomer contains rich carboxyl groups and cyano groups, which well ensure the bonding of the colloid. At the same time, these groups coordinate with lithium ions, which can improve the ion conductivity to a certain extent. All monomers belong to polar polymers and are resistant to swelling of electrolytes, so that the obtained colloid has a large viscosity, and the stability of the water-based adhesive is guaranteed. The present invention adopts a two-phase mixture of solution glue and latex glue, which can ensure the flexibility and bonding force of the pole piece while ensuring that the material has good cycle rate performance. The adhesive of the present invention does not contain organic solvents and is an aqueous homogenization system, which fundamentally eliminates the discharge (or recycling) of organic pollutants and greatly reduces environmental costs. The water-based adhesive of the present invention takes into account both processing performance and electrochemical performance in an aqueous system and reduces environmental costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a performance comparison chart of Example 1 solution glue and PVDF, the mainstream positive electrode binder on the market. Among them, a is the capacity retention rate, b is the capacity utilization; c is the constant current charging ratio; d is 1C cycle.

[0024] Figure 2 This is a performance comparison chart of the latex glue in Example 2 and the mainstream positive electrode binder PVDF on the market. Among them, a is the capacity retention rate, b is the capacity utilization; c is the constant current charging ratio; d is 1C cycle. DETAILED DESCRIPTION

[0025] The present invention will be described in detail below through specific embodiments in conjunction with the accompanying drawings.

[0026] As a common binder, polyacrylic acid and its ester binders are used in many fields due to their excellent physical and chemical properties. Based on their excellent electrochemical stability and bonding performance, they are introduced into lithium-ion batteries.

[0027] The present invention proposes a method for improving the performance of water-based binders by physical compounding of emulsions and solutions, wherein the solution glue obtained by solution polymerization and the emulsion glue obtained by emulsion polymerization are compounded in a certain ratio (both are water-based), thereby obtaining a water-based binder for lithium iron phosphate. When the binder obtained by the method is used, it has excellent electrode processing performance, and the battery cycle and rate performance are good, and the capacity is normal.

[0028] A method for preparing a lithium iron phosphate positive electrode using an aqueous binder comprises the following steps:

[0029] 1) Preparation of solution glue: two or more of acrylonitrile, acrylamide, β-acryloxypropionic acid and vinyl acetate are mixed with acrylic acid to obtain a mixture, wherein the mass percentage of acrylic acid in the mixture is 40% to 90%, and then sodium hydroxide or lithium hydroxide solution is added to neutralize 10% to 50% of the total amount of carboxyl groups to obtain a neutralized monomer;

[0030] The neutralized monomer and initiator are added to a solvent to obtain a pre-reaction liquid, wherein the mass concentration of the neutralized monomer is 15-30%, and the mass concentration of the initiator is 0.1%-0.6%. The pre-reaction liquid is polymerized under nitrogen protection at a reaction temperature of 70-85°C. After reacting for 2.5-3 hours, it is cooled to room temperature and neutralized to neutrality with a sodium hydroxide or lithium hydroxide aqueous solution to obtain a solution glue having a molecular weight of 3000000-2000000.

[0031] The solvent is water, and the initiator is ammonium persulfate or potassium persulfate.

[0032] 2) Preparation of emulsion glue: using one or two of butyl acrylate, 2-ethylhexyl acrylate, styrene and vinyl acetate as non-polar monomers, and one or two of acrylic acid, acrylonitrile, acrylamide and β-acryloxypropionic acid as polar monomers;

[0033] Adding a non-polar monomer, a polar monomer, an emulsifier and an initiator into deionized water to obtain a reaction system, and emulsifying the reaction system to obtain a pre-emulsion;

[0034] A DNS-86 emulsifier solution with a mass concentration of 0.2% is prepared as a base liquid; the amount of the base liquid is 50% of the total mass of the non-polar monomer and the polar monomer, and then transferred to a reaction kettle, the pre-emulsion is added dropwise to the emulsifier solution at 70°C to 85°C, and then an emulsion polymerization reaction is carried out at 70°C to 85°C under nitrogen protection for 2-3 hours, and sodium hydroxide solution or potassium hydroxide solution is added dropwise to neutralize to pH 6 to 8 to obtain an emulsion glue.

[0035] Among them, the non-polar monomer accounts for 70% to 98% of the total mass of the non-polar monomer and the polar monomer, the polar monomer accounts for 2% to 30% of the total mass of the non-polar monomer and the polar monomer, the emulsifier accounts for 1% to 4% of the total mass of the non-polar monomer and the polar monomer, and the initiator accounts for 0.1% to 0.6% of the total mass of the non-polar monomer and the polar monomer.

[0036] The emulsifier is a reactive emulsifier, and the reactive emulsifier refers to one or more of DNS-86, JS-20, SR-10, SR-20 and SR-30.

[0037] The initiator is ammonium persulfate or potassium persulfate.

[0038] 3) Compounding of solution glue and latex glue: Mix the solution glue and the latex glue in a mass ratio of 1:1-2, stir evenly, and then neutralize with sodium hydroxide or lithium hydroxide aqueous solution to a pH of 5-9 to obtain an aqueous binder for lithium iron phosphate.

[0039] The lithium battery binder prepared by this method can be used for lithium iron phosphate positive electrode, taking into account both processing performance and electrochemical performance, and is suitable for large-scale production.

[0040] The present invention is further described in detail with reference to the following examples, but the present invention is not limited to these examples.

[0041] Example 1

[0042] (1) Solution glue: 74% acrylic acid, 20% acrylonitrile and 6% β-acryloxypropionic acid are mixed by mass percentage to obtain a mixture, and then sodium hydroxide or lithium hydroxide solution is added to the mixture to neutralize 20% of the total amount of carboxyl groups to obtain a neutralized monomer;

[0043] The neutralized monomer and initiator are added to the solvent to obtain a pre-reaction liquid, wherein the mass concentration of the neutralized monomer is 22%, and the mass concentration of the initiator is 0.3%. The pre-reaction liquid is polymerized under nitrogen protection at a reaction temperature of 75°C. After reacting for 3 hours, it is cooled to room temperature, neutralized with sodium hydroxide solution to neutrality, and diluted with deionized water to a mass concentration of 10% to obtain a solution glue for standby use (30 g of acrylic acid, acrylonitrile and β-acryloxypropionic acid in total, 500 mL reaction bottle).

[0044] The solvent is water and the initiator is potassium persulfate.

[0045] (2) Emulsion glue: butyl acrylate and styrene are non-polar monomers, and β-acryloxypropionic acid is a polar monomer;

[0046] By mass percentage, butyl acrylate accounts for 65%, styrene accounts for 30%, and beta-acryloxypropionic acid accounts for 5%.

[0047] Butyl acrylate, styrene, β-acryloxypropionic acid, DNS-86 emulsifier and potassium persulfate are added to deionized water (the mass of deionized water is equal to the total mass of butyl acrylate, styrene and β-acryloxypropionic acid) to obtain a reaction system, and the reaction system is emulsified to obtain a pre-emulsion; the DNS-86 emulsifier accounts for 3% of the total mass of butyl acrylate, styrene and β-acryloxypropionic acid, and the potassium persulfate accounts for 0.4% of the total mass of butyl acrylate, styrene and β-acryloxypropionic acid.

[0048] A DNS-86 emulsifier solution with a mass concentration of 0.2% was prepared as a base liquid; the amount of the base liquid was 50% of the total mass of butyl acrylate, styrene and β-acryloxypropionic acid, and was added into a 500 mL reaction bottle for later use.

[0049] Under nitrogen protection, at 75°C, the pre-emulsion was added dropwise to the bottom liquid for 1 hour. After the addition was completed, the reaction was continued at 75°C for 2 hours, and sodium hydroxide solution was added dropwise to neutralize to pH 6-8 to obtain an emulsion glue. (The total mass of butyl acrylate, styrene and β-acryloxypropionic acid was 50g, 500mL reaction bottle).

[0050] (3) The above solution glue and latex glue are mixed in a mass ratio of 1:2, stirred evenly, and a water-based binder for lithium iron phosphate is obtained for later use.

[0051] (4) Slurry was homogenized in a ratio of lithium iron phosphate: SP: binder = 95:5:5. The slurry had no granular feeling and good fluidity. Figure 1 After coating, the electrode has good flexibility, and the 180° peeling is ≥25N / m before and after rolling. It is made into a button-type half-cell. Compared with the PVDF binder with the same formula, it has advantages in rate and cycle. Figure 1 a, b, c and d. It can be seen that the single solution glue and the mainstream positive electrode binder product PVDF on the market have advantages in capacity retention rate, capacity play, constant current charging ratio, 1C cycle and other performances.

[0052] Example 2

[0053] (1) Solution glue: 70% acrylic acid, 15% acrylonitrile, 5% β-acryloxypropionic acid, and 10% vinyl acetate are mixed by mass percentage to obtain a mixture, and then sodium hydroxide or lithium hydroxide solution is added to the mixture to neutralize 20% of the total amount of carboxyl groups to obtain a neutralized monomer;

[0054] The neutralized monomer and initiator are added to the solvent to obtain a pre-reaction liquid, wherein the mass concentration of the neutralized monomer is 22%, and the mass concentration of the initiator is 0.3%. The pre-reaction liquid is polymerized under nitrogen protection at a reaction temperature of 75°C. After reacting for 3 hours, it is cooled to room temperature, neutralized with sodium hydroxide solution to neutrality, and diluted with deionized water to a mass concentration of 10% to obtain a solution glue for standby use (acrylic acid, acrylonitrile, β-acryloxypropionic acid and vinyl acetate, a total of 30 g, 500 mL reaction bottle).

[0055] The solvent is water and the initiator is potassium persulfate.

[0056] (2) Emulsion glue: 2-ethylhexyl acrylate is used as the non-polar monomer;

[0057] Acrylic acid, acrylonitrile and β-acryloxypropionic acid are used as polar monomers;

[0058] In terms of mass percentage, the content of isooctyl acrylate is 40%, the content of acrylic acid is 42%, the content of acrylonitrile is 12%, and the content of β-acryloxypropionic acid is 6%.

[0059] Adding isooctyl acrylate, acrylic acid, acrylonitrile, β-acryloxy propionic acid, JS-20 emulsifier and potassium persulfate into deionized water (the mass of the deionized water is the same as the total mass of isooctyl acrylate, acrylic acid, acrylonitrile and β-acryloxy propionic acid) to obtain a reaction system, and emulsifying the reaction system to obtain a pre-emulsion;

[0060] A DNS-86 emulsifier solution with a mass concentration of 0.2% was prepared as a base liquid; the amount of the base liquid was 50% of the total mass of isooctyl acrylate, acrylic acid, acrylonitrile and β-acryloxypropionic acid;

[0061] Under nitrogen protection, at 75°C, the pre-emulsion was added dropwise to the bottom liquid for 1 hour. After the addition was completed, the reaction was continued at a reaction temperature of 75°C for 3 hours, and sodium hydroxide solution was added dropwise to neutralize to pH 6-8 to obtain an emulsion glue. (The total mass of isooctyl acrylate, acrylic acid, acrylonitrile and β-acryloxypropionic acid was 50g, 500mL reaction bottle).

[0062] Among them, JS-20 emulsifier accounts for 3% of the total mass of isooctyl acrylate, acrylic acid, acrylonitrile and β-acryloxy propionic acid, and potassium persulfate accounts for 0.4% of the total mass of isooctyl acrylate, acrylic acid, acrylonitrile and β-acryloxy propionic acid.

[0063] (3) The above solution glue and latex glue are mixed in a mass ratio of 1:1, stirred evenly, and a water-based binder for lithium iron phosphate is obtained for later use.

[0064] (4) Slurry was homogenized in a ratio of lithium iron phosphate: SP: binder = 95:5:5. The slurry had no granular feeling and good fluidity. Figure 1 After coating, the electrode sheet has good flexibility, and the 180° peeling is ≥25N / m before and after rolling. It is made into a button-type half-cell. Compared with the PVDF binder with the same formula, it has advantages in rate and cycle. Figure 2 a, b, c and d. It can be seen that the latex alone and the mainstream positive electrode binder product PVDF on the market have advantages in terms of capacity retention, capacity play, constant current charging ratio, 1C cycle and other performances.

[0065] Example 3

[0066] (1) Solution glue: 40% acrylic acid, 40% acrylonitrile and 20% acrylamide are mixed by mass percentage to obtain a mixture, and then sodium hydroxide solution is added to the mixture to neutralize 20% of the total amount of carboxyl groups to obtain a neutralized monomer;

[0067] The neutralized monomer and potassium persulfate are added into water to obtain a pre-reaction liquid, wherein the mass concentration of the neutralized monomer is 25%, and the mass concentration of potassium persulfate is 0.6%. The pre-reaction liquid is polymerized under nitrogen protection at a reaction temperature of 70°C. After reacting for 3 hours, it is cooled to room temperature, neutralized to neutrality with a sodium hydroxide solution, and diluted to a mass concentration of 10% with deionized water to obtain a solution glue for standby use (30 g of acrylic acid, acrylonitrile and acrylamide in a 500 mL reaction bottle).

[0068] (2) Emulsion glue: butyl acrylate is used as the non-polar monomer;

[0069] Acrylic acid is used as the polar monomer;

[0070] By mass percentage, butyl acrylate is 98% and acrylic acid is 2%.

[0071] Add butyl acrylate, acrylic acid, SR-10 emulsifier and ammonium persulfate to deionized water (the mass of deionized water is the same as the total mass of butyl acrylate and acrylic acid) to obtain a reaction system, wherein the SR-10 emulsifier accounts for 1% of the total mass of butyl acrylate and acrylic acid, and the ammonium persulfate accounts for 0.2% of the total mass of butyl acrylate and acrylic acid. Emulsify the reaction system to obtain a pre-emulsion;

[0072] A DNS-86 emulsifier solution with a mass concentration of 0.2% was prepared as a base liquid; the amount of the base liquid was 50% of the total mass of butyl acrylate and acrylic acid;

[0073] Under nitrogen protection, at 80°C, the pre-emulsion was added dropwise to the bottom liquid for 1 hour. After the addition was completed, the reaction was continued at 80°C for 3 hours, and sodium hydroxide solution was added dropwise to neutralize to pH 8 to obtain an emulsion glue. (The total mass of butyl acrylate and acrylic acid was 50g, 500mL reaction bottle).

[0074] (3) The above solution glue and latex glue are mixed in a mass ratio of 1:1, stirred evenly, and a water-based binder for lithium iron phosphate is obtained for later use.

[0075] Example 4

[0076] (1) Solution glue: 90% acrylic acid, 3% acrylonitrile, 2% vinyl acetate and 5% β-acryloxypropionic acid are mixed by mass percentage to obtain a mixture, and then a lithium hydroxide solution is added to the mixture to neutralize 50% of the total amount of carboxyl groups to obtain a neutralized monomer;

[0077] The neutralized monomer and potassium persulfate are added into water to obtain a pre-reaction liquid, wherein the mass concentration of the neutralized monomer is 30%, and the mass concentration of potassium persulfate is 0.4%. The pre-reaction liquid is polymerized under nitrogen protection at a reaction temperature of 85°C. After reacting for 2 hours, it is cooled to room temperature, neutralized to neutrality with a sodium hydroxide solution, and diluted to a mass concentration of 10% with deionized water to obtain a solution glue for standby use (30 g of acrylic acid, acrylonitrile, vinyl acetate and β-acryloxypropionic acid in total, in a 500 mL reaction bottle).

[0078] (2) Emulsion glue: propylene glycol and styrene are non-polar monomers;

[0079] Acrylonitrile and acrylamide are used as polar monomers;

[0080] Calculated by mass percentage, the content of isooctyl propylene is 30%, the content of styrene is 40%, the content of acrylonitrile is 10%, and the content of acrylamide is 20%.

[0081] Isooctyl propylene, styrene, acrylonitrile, acrylamide, SR-30 emulsifier and potassium persulfate are added to deionized water (the mass of deionized water is the same as the total mass of isooctyl propylene, styrene, acrylonitrile and acrylamide) to obtain a reaction system, in which the SR-30 emulsifier accounts for 4% of the total mass of isooctyl propylene, styrene, acrylonitrile and acrylamide, and the potassium persulfate accounts for 0.1% of the total mass of isooctyl propylene, styrene, acrylonitrile and acrylamide.

[0082] emulsifying the reaction system to obtain a pre-emulsion;

[0083] A DNS-86 emulsifier solution with a mass concentration of 0.2% was prepared as a base liquid; the amount of the base liquid was 50% of the total mass of 2-ethylhexyl propylene, styrene, acrylonitrile and acrylamide;

[0084] Under nitrogen protection, at 85°C, the pre-emulsion was added dropwise to the bottom liquid for 1 hour. After the addition was completed, the reaction was continued at 85°C for 2 hours, and sodium hydroxide solution was added dropwise to neutralize to pH 7 to obtain an emulsion glue. (The total mass of propylene octyl ester, styrene, acrylonitrile and acrylamide was 50g, 500mL reaction bottle).

[0085] (3) The above solution glue and latex glue are mixed in a mass ratio of 1:2, stirred evenly, and a water-based binder for lithium iron phosphate is obtained for later use.

[0086] Example 5

[0087] (1) Solution glue: 63% acrylic acid, 30% acrylamide and 7% vinyl acetate are mixed by mass percentage to obtain a mixture, and then sodium hydroxide solution is added to the mixture to neutralize 35% of the total amount of carboxyl groups to obtain a neutralized monomer;

[0088] The neutralized monomer and ammonium persulfate are added into water to obtain a pre-reaction liquid, wherein the mass concentration of the neutralized monomer is 15%, and the mass concentration of ammonium persulfate is 0.1%. The pre-reaction liquid is polymerized under nitrogen protection at a reaction temperature of 80°C. After reacting for 3 hours, it is cooled to room temperature, neutralized to neutrality with a sodium hydroxide solution, and diluted to a mass concentration of 10% with deionized water to obtain a solution glue for standby use (30 g of acrylic acid, acrylonitrile and β-acryloxypropionic acid in total, in a 500 mL reaction bottle).

[0089] (2) Emulsion glue: styrene and vinyl acetate are non-polar monomers;

[0090] Acrylamide and β-acryloxypropionic acid are used as polar monomers;

[0091] In terms of mass percentage, styrene accounts for 20%, vinyl acetate accounts for 60%, acrylamide accounts for 5%, and beta-acryloxypropionic acid accounts for 15%.

[0092] Add styrene, vinyl acetate, acrylamide, β-acryloxypropionic acid, SR-20 emulsifier and potassium persulfate to deionized water (the mass of deionized water is the same as the total mass of styrene, vinyl acetate, acrylamide and β-acryloxypropionic acid) to obtain a reaction system, wherein the SR-20 emulsifier accounts for 1% of the total mass of styrene, vinyl acetate, acrylamide and β-acryloxypropionic acid, and the potassium persulfate accounts for 0.6% of the total mass of styrene, vinyl acetate, acrylamide and β-acryloxypropionic acid. Emulsify the reaction system to obtain a pre-emulsion;

[0093] A DNS-86 emulsifier solution with a mass concentration of 0.2% was prepared as a base liquid; the amount of the base liquid was 50% of the total mass of styrene, vinyl acetate, acrylamide and β-acryloxypropionic acid;

[0094] Under nitrogen protection, at 70°C, the pre-emulsion was added dropwise to the bottom liquid for 1 hour. After the addition was completed, the reaction was continued at 70°C for 3 hours, and sodium hydroxide solution was added dropwise to neutralize to pH 6 to obtain an emulsion glue. (The total mass of styrene, vinyl acetate, acrylamide and β-acryloxypropionic acid was 50g, and the reaction bottle was 500mL).

[0095] (3) The above solution glue and latex glue are mixed in a mass ratio of 1:1.5, stirred evenly, and a water-based binder for lithium iron phosphate is obtained for later use.

Claims

1. A method for preparing a lithium iron phosphate positive electrode using an aqueous binder, characterized in that: The following steps are involved: Mixing two or more of acrylonitrile, acrylamide, β-acryloxypropionic acid and vinyl acetate with acrylic acid to obtain a mixture, then neutralizing 10% to 50% of the total amount of carboxyl groups in the mixture to obtain a neutralized monomer; adding the neutralized monomer and an initiator to water to obtain a pre-reaction liquid, subjecting the pre-reaction liquid to a polymerization reaction under nitrogen protection and then neutralizing it to neutrality to obtain a solution glue; Adding a non-polar monomer, a polar monomer, an emulsifier and an initiator into water to obtain a reaction system, and emulsifying the reaction system to obtain a pre-emulsion; The pre-emulsion is added to the emulsifier solution, and then a polymerization reaction is carried out under nitrogen protection, and the pH is adjusted to 6-8 to obtain an emulsion glue; The solution glue and the latex glue are mixed and the pH is adjusted to 5 to 9 to obtain a water-based binder for lithium iron phosphate.

2. The method for preparing a lithium iron phosphate positive electrode using an aqueous binder according to claim 1, characterized in that: The mass percentage of acrylic acid in the mixture is 40% to 90%.

3. The method for preparing a lithium iron phosphate positive electrode using an aqueous binder according to claim 1, characterized in that: The mass concentration of the neutralized monomer in the preliminary reaction liquid is 15-30%, and the mass concentration of the initiator in the preliminary reaction liquid is 0.1%-0.6%.

4. The method for preparing a lithium iron phosphate positive electrode using an aqueous binder according to claim 1, characterized in that: The non-polar monomer is one or two of butyl acrylate, isooctyl acrylate, styrene and vinyl acetate.

5. The method for preparing a lithium iron phosphate positive electrode using an aqueous binder according to claim 1, characterized in that: The polar monomer is one or two of acrylic acid, acrylonitrile, acrylamide and β-acryloxypropionic acid.

6. The method for preparing a lithium iron phosphate positive electrode using an aqueous binder according to claim 1, characterized in that: The polymerization reaction temperature was 70-85°C and the reaction time was 2-3h.

7. The method for preparing a lithium iron phosphate positive electrode using an aqueous binder according to claim 1, characterized in that: The initiators are all ammonium persulfate or potassium persulfate.

8. The method for preparing a lithium iron phosphate positive electrode using an aqueous binder according to claim 1, characterized in that: In the reaction system, the non-polar monomer accounts for 70-98% of the total mass of the non-polar monomer and the polar monomer, the polar monomer accounts for 2%-30% of the total mass of the non-polar monomer and the polar monomer, the emulsifier accounts for 1%-4% of the total mass of the non-polar monomer and the polar monomer, and the initiator accounts for 0.1%-0.6% of the total mass of the non-polar monomer and the polar monomer.

9. The method for preparing a lithium iron phosphate positive electrode using an aqueous binder according to claim 1, characterized in that: The mass concentration of the emulsifier solution is 0.2%, and the amount used is 50% of the total mass of the non-polar monomer and the polar monomer.

10. The method for preparing a lithium iron phosphate positive electrode using an aqueous binder according to claim 1, characterized in that: The mass ratio of solution glue to latex glue is 1:1-2.

Citation Information

Patent Citations

  • Water-based binder as well as preparation method and application thereof

    CN108276937A

  • Three-dimensional network water-based composite binder and application thereof in lithium ion battery

    CN111180733A

  • Aqueous solution type lithium iron phosphate positive electrode adhesive and preparation method and application thereof

    CN112467142A

  • Aqueous binder, manufacturing method of positive pole piece and lithium ion battery

    CN115093520A