Optical film with antifouling layer
By using a combined structure of transparent substrate, hard coating, inorganic oxide substrate and high-hardness anti-fouling layer in optical films, the problem of deterioration of anti-fouling layer after repeated wiping is solved, and high peel resistance is achieved Optical films that are both resistant and antifouling.
Patent Information
- Application Number
- CN202180049236.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-11-16
- Filing Date
- 2021-07-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-07-13
AI Technical Summary
When using an optical film with an anti-fouling layer, repeated wiping operations will lead to a reduction in the anti-fouling property of the anti-fouling layer and peeling, affecting its anti-fouling function.
A combined structure of a transparent substrate, a hard coating layer, an inorganic oxide base layer and an antifouling layer is adopted. The antifouling layer is arranged on the inorganic oxide base layer by a dry coating film, with a surface hardness of 1.05GPa or above, and is passed The elastic recovery rate and hardness product measured by the nano-indentation method are above 0.8 to improve the peel resistance and stain resistance of the anti-fouling layer.
It effectively improves the peel resistance and stain resistance of the anti-fouling layer, prevents the anti-fouling layer from decreasing after wiping operation, and maintains the anti-fouling function of the optical film.
Smart Images

Figure CN115835957B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an optical film with an antifouling layer. Background Art
[0002] From the viewpoint of antifouling property, an optical film with an antifouling layer is attached to the outer surface of the image display side of a display such as a touch panel display. The optical film with an antifouling layer includes a transparent substrate and an antifouling layer, and the antifouling layer is arranged on the outermost surface of one side of the transparent substrate. The antifouling layer is used to suppress the adhesion of pollutants such as hand grease to the display surface, and the attached pollutants are easily removed. The related technology of such an optical film with an antifouling layer is described in, for example, the following patent document 1.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2020-52221 Summary of the invention
[0006] Problem that the invention aims to solve
[0007] When using an optical film with an antifouling layer, contaminants attached to the antifouling layer are removed by, for example, wiping operation. However, repeated wiping operation of the antifouling layer may cause the antifouling property of the antifouling layer to decrease, and may also cause the antifouling layer to peel off. From the viewpoint of the antifouling function of the optical film with an antifouling layer, the antifouling property of the antifouling layer to decrease and peel off are not preferred.
[0008] The present invention provides an optical film with an antifouling layer which is suitable for ensuring the peeling resistance in the antifouling layer and suppressing the reduction of the antifouling property.
[0009] Solutions for solving problems
[0010] The present invention [1] includes an optical film with an antifouling layer, which comprises a transparent substrate, a hard coating layer, an inorganic oxide base layer and an antifouling layer in sequence, wherein the antifouling layer is a dry coating film arranged on the inorganic oxide base layer, and the hardness of the surface of the antifouling layer on the opposite side to the inorganic oxide base layer at 25°C measured by nanoindentation method is greater than 1.05 GPa.
[0011] The present invention [2] includes the optical film with an antifouling layer according to the above [1], wherein the product of the elastic recovery rate at 25° C. measured by nanoindentation method and the hardness (GPa) of the surface of the antifouling layer is 0.8 or more.
[0012] The present invention [3] comprises the optical film with an antifouling layer according to [1] or [2], wherein the elastic recovery rate of the surface of the antifouling layer at 25° C. measured by a nanoindentation method is 0.76 or more.
[0013] The present invention [4] comprises the optical film with an antifouling layer according to any one of [1] to [3] above, wherein the antifouling layer has a thickness of 1 nm to 25 nm.
[0014] The present invention [5] comprises the optical film with an antifouling layer according to any one of [1] to [4] above, wherein the inorganic oxide underlayer comprises silicon dioxide.
[0015] The present invention [6] includes the optical film with an antifouling layer according to any one of [1] to [5] above, wherein the inorganic oxide underlayer has a thickness of 50 nm or more.
[0016] The present invention [7] includes the optical film with an antifouling layer according to any one of [1] to [6], wherein the hard coat layer has a thickness of 1 μm or more and 50 μm or less.
[0017] Effects of the Invention
[0018] As described above, the optical film with an antifouling layer of the present invention is a dry coating film disposed on an inorganic oxide base layer. This configuration is suitable for ensuring high bonding strength of the antifouling layer in the optical film with an antifouling layer, and therefore suitable for ensuring peeling resistance of the antifouling layer. In addition, the hardness of the surface of the antifouling layer of the optical film with an antifouling layer on the opposite side of the inorganic oxide base layer measured by the nanoindentation method at 25° C. is 1.05 GPa. This configuration is suitable for withstanding the wiping operation performed on the antifouling layer and suppressing the reduction of the antifouling property of the antifouling layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic cross-sectional view of one embodiment of the optical film of the present invention.
[0020] Figure 2 It is a schematic cross-sectional view of a modification of the optical film of the present invention (in this modification, the optical film includes an antireflection layer).
[0021] Figure 3 This is a graph in which the surface hardness H (horizontal axis) measured for each optical film of Examples 1 to 9 and Comparative Example 1 and the measurement results of the water contact angle θ2 after the second rubber sliding test (vertical axis) are plotted. DETAILED DESCRIPTION
[0022] An optical film F as one embodiment of the optical film with an antifouling layer of the present invention is as follows Figure 1As shown in FIG. 1 , the transparent substrate 11, the hard coating layer 12, the inorganic oxide underlayer 13 and the antifouling layer 14 are sequentially provided on one side in the thickness direction T. In the present embodiment, the optical film F sequentially includes the transparent substrate 11, the hard coating layer 12, the adhesion layer 15, the inorganic oxide underlayer 13 and the antifouling layer 14 on one side in the thickness direction T. In addition, the optical film F has a shape extending in a direction (surface direction) perpendicular to the thickness direction T.
[0023] The transparent substrate 11 is a transparent resin film with flexibility. As the material of the transparent substrate 11, for example, polyester resin, polyolefin resin, polystyrene resin, acrylic resin, polycarbonate resin, polyethersulfone resin, polysulfone resin, polyamide resin, polyimide resin, cellulose resin, norbornene resin, polyarylate resin and polyvinyl alcohol resin can be listed. As polyester resin, for example, polyethylene terephthalate (PET), polybutylene terephthalate and polyethylene naphthalate can be listed. As polyolefin resin, for example, polyethylene, polypropylene and cycloolefin polymer (COP) can be listed. As cellulose resin, for example, cellulose triacetate (TAC) can be listed. These materials can be used alone or in combination of two or more. As the material of the transparent substrate 11, from the viewpoint of transparency and strength, one selected from the group consisting of polyester resin, polyolefin resin and cellulose resin can be used, and one selected from the group consisting of PET, COP and TAC can be more preferably used.
[0024] The surface of the hard coat layer 12 side of the transparent substrate 11 may be subjected to a surface modification treatment. Examples of the surface modification treatment include corona treatment, plasma treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment.
[0025] From the viewpoint of strength, the thickness of the transparent substrate 11 is preferably 5 μm or more, more preferably 10 μm or more, and further preferably 20 μm or more. From the viewpoint of handleability, the thickness of the transparent substrate 11 is preferably 300 μm or less, and more preferably 200 μm or less.
[0026] The total light transmittance (JIS K 7375-2008) of the transparent substrate 11 is preferably 80% or more, more preferably 90% or more, and further preferably 95% or more. This configuration is suitable for ensuring the transparency required for the optical film F when the surface of a display such as a touch panel display is provided with the optical film F. The total light transmittance of the transparent substrate 11 is, for example, 100% or less.
[0027] The hard coating layer 12 is disposed on one side of the transparent substrate 11 in the thickness direction T. The hard coating layer 12 is used to make the exposed surface of the optical film F (in Figure 1 The upper surface in the middle is a layer that is not easily scratched.
[0028] The hard coat layer 12 is a cured product of a curable resin composition. As the curable resin contained in the curable resin composition, for example, polyester resins, acrylic resins, carbamate resins, acrylic carbamate resins, amide resins, silicone resins, epoxy resins and melamine resins can be listed. These curable resins can be used alone or in combination of two or more. From the viewpoint of ensuring the high hardness of the hard coat layer 12, acrylic carbamate resins are preferably used as the curable resin.
[0029] In addition, as a curable resin composition, for example, a UV-curable resin composition and a thermosetting resin composition can be listed. From the viewpoint that it can be cured without high-temperature heating, thereby contributing to improving the manufacturing efficiency of the optical film F, as a curable resin composition, a UV-curable resin composition is preferably used. The UV-curable resin composition includes at least one selected from the group consisting of a UV-curable monomer, a UV-curable oligomer, and a UV-curable polymer. As a specific example of a UV-curable resin composition, a hard coat forming composition described in Japanese Patent Publication No. 2016-179686 can be listed.
[0030] The curable resin composition may contain microparticles. The mixing of microparticles with the curable resin composition helps to adjust the hardness of the hard coat layer 12, adjust the surface roughness, adjust the refractive index, and impart anti-glare properties. As microparticles, for example, metal oxide particles, glass particles, and organic particles can be listed. As materials for metal oxide particles, for example, silicon dioxide, aluminum oxide, titanium oxide, zirconium oxide, calcium oxide, tin oxide, indium oxide, cadmium oxide, and antimony oxide can be listed. As materials for organic particles, for example, polymethyl methacrylate, polystyrene, polyurethane, acrylic-styrene copolymer, benzoguanamine, melamine, and polycarbonate can be listed.
[0031] From the viewpoint of ensuring the hardness of the surface of the antifouling layer 14 by ensuring the hardness of the hard coating layer 12, the thickness of the hard coating layer 12 is preferably 1 μm or more, more preferably 3 μm or more, and further preferably 5 μm or more. From the viewpoint of ensuring the flexibility of the optical film F, the thickness of the hard coating layer 12 is preferably 50 μm or less, more preferably 40 μm or less, further preferably 35 μm or less, and particularly preferably 30 μm or less.
[0032] The surface of the adhesive layer 15 side of the hard coating layer 12 may be subjected to surface modification treatment. Examples of surface modification treatments include plasma treatment, corona treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment. From the perspective of ensuring high adhesion between the hard coating layer 12 and the adhesive layer 15, the surface of the adhesive layer 15 side of the hard coating layer 12 is preferably subjected to plasma treatment.
[0033] The adhesion layer 15 is a layer for ensuring the adhesion of the inorganic oxide layer (in the present embodiment, the inorganic oxide base layer 13) to the transparent substrate 11. The adhesion layer 15 is arranged on one side of the thickness direction T of the hard coating layer 12. As the material of the adhesion layer 15, metals such as silicon, indium, nickel, chromium, aluminum, tin, gold, silver, platinum, zinc, titanium, tungsten, zirconium, palladium, etc.; alloys of two or more of these metals; and oxides of these metals can be listed. From the viewpoint of taking into account the adhesion to both the organic layer (specifically the hard coating layer 12) and the inorganic oxide layer (specifically the inorganic oxide base layer 13 in the present embodiment) and the transparency of the adhesion layer 15, indium tin oxide (ITO) or silicon oxide (SiOx) is preferably used as the material of the adhesion layer 15. When silicon oxide is used as the material of the adhesion layer 15, it is preferred to use SiOx with less oxygen content than the stoichiometric composition, and more preferably to use SiOx with x being 1.2 or more and 1.9 or less.
[0034] From the viewpoint of ensuring the adhesion between the hard coat layer 12 and the inorganic oxide underlayer 13 and the transparency of the adhesion layer 15 , the thickness of the adhesion layer 15 is preferably 1 nm or more and 10 nm or less.
[0035] The inorganic oxide underlayer 13 is a layer for ensuring the peeling resistance of the antifouling layer 14. Examples of the material of the inorganic oxide underlayer 13 include silicon dioxide (SiO2) and magnesium fluoride, and silicon dioxide is preferably used.
[0036] The thickness of the inorganic oxide underlayer 13 is preferably 50 nm or more, more preferably 65 nm or more, further preferably 80 nm or more, and particularly preferably 90 nm or more from the viewpoint of ensuring the peeling resistance of the antifouling layer 14. The thickness of the inorganic oxide underlayer 13 is, for example, 300 nm or less.
[0037] The antifouling layer 14 is a layer having an antifouling function. The antifouling layer 14 is disposed on one side of the inorganic oxide base layer 13 in the thickness direction T. The antifouling layer 14 has a surface 14a (outer surface) on one side in the thickness direction T. The antifouling function of the antifouling layer 14 includes: a function of inhibiting the adhesion of pollutants such as hand grease to the exposed surface of the film when the optical film F is used, and a function of making the attached pollutants easy to remove.
[0038] As the material of the antifouling layer 14, for example, an organic compound containing a fluorine group can be cited. As the organic compound containing a fluorine group, an alkoxysilane compound having a perfluoropolyether group is preferably used. As the alkoxysilane compound having a perfluoropolyether group, for example, a compound represented by the following general formula (1) can be cited.
[0039] R 1 -R 2 -X-(CH2)m -Si(OR 3 )3(1)
[0040] In the general formula (1), R 1 It represents a linear fluoroalkyl group or a branched fluoroalkyl group (having, for example, 1 to 20 carbon atoms) in which one or more hydrogen atoms in the alkyl group are substituted with fluorine atoms, and preferably represents a perfluoroalkyl group in which all hydrogen atoms in the alkyl group are substituted with fluorine atoms.
[0041] R 2 The structure of the repeating structure including at least one perfluoropolyether (PFPE) group is preferably a structure of the repeating structure including two PFPE groups. Examples of the repeating structure of the PFPE group include a repeating structure of a linear PFPE group and a repeating structure of a branched PFPE group. Examples of the repeating structure of the linear PFPE group include -(OC n F 2n ) p - (n represents an integer of 1 to 20, and p represents an integer of 1 to 50. The same shall apply to the following). Examples of the repeating structure of the branched PFPE group include -(OC(CF3)2) p -Structure shown and -(OCF2CF(CF3)CF2) p As the repeating structure of the PFPE group, a repeating structure of a linear PFPE group can be preferably listed, and -(OCF2) can be more preferably listed. p -and-(OC2F4) p -.
[0042] R 3 It represents an alkyl group having 1 to 4 carbon atoms, and preferably represents a methyl group.
[0043] X represents an ether group, a carbonyl group, an amino group or an amide group, and preferably represents an ether group.
[0044] m represents an integer of 1 or more. In addition, m preferably represents an integer of 20 or less, more preferably 10 or less, and even more preferably 5 or less.
[0045] Among such alkoxysilane compounds having a perfluoropolyether group, the compound represented by the following general formula (2) is preferably used.
[0046] CF3-(OCF2) q -(OC2F4) r -O-(CH2)3-Si(OCH3)3(2)
[0047] In the general formula (2), q represents an integer of 1 to 50, and r represents an integer of 1 to 50.
[0048] The alkoxysilane compound having a perfluoropolyether group may be used alone or in combination of two or more.
[0049] The antifouling layer 14 is a film formed by a dry coating method (dry coating film). Examples of dry coating methods include sputtering, vacuum deposition, and CVD. The antifouling layer 14 is preferably a film formed by a vacuum deposition method (vacuum deposition film).
[0050] The material of the antifouling layer 14 includes an alkoxysilane compound having a perfluoropolyether group and the antifouling layer 14 is a dry coating film (preferably a vacuum-deposited film), which is suitable for ensuring high bonding strength of the antifouling layer 14 to the inorganic oxide base layer 13, and therefore, suitable for ensuring the peeling resistance of the antifouling layer 14. High peeling resistance of the antifouling layer 14 contributes to maintaining the antifouling function of the antifouling layer 14.
[0051] The hardness (surface hardness H) of the surface 14a of the antifouling layer 14 at 25°C measured by the nanoindentation method is 1.05 GPa or more, preferably 1.1 GPa or more, more preferably 1.15 GPa or more, further preferably 1.2 GPa or more, further preferably 1.25 GPa or more, and particularly preferably 1.3 GPa or more. This structure is suitable for withstanding the wiping operation performed on the antifouling layer 14 and suppressing the reduction in the antifouling property of the antifouling layer 14. The hardness (surface hardness H) of the surface 14a of the antifouling layer 14 at 25°C measured by the nanoindentation method is preferably 30 GPa or less, more preferably 20 GPa or less, and further preferably 15 GPa or less. This structure is suitable for ensuring the flexibility of the antifouling layer 14, and therefore, is suitable for ensuring the flexibility of the optical film F.
[0052] Nanoindentation refers to a technique for measuring the physical properties of a sample at a nanometer scale. In the present embodiment, the nanoindentation method is implemented in accordance with ISO14577. In the nanoindentation method, a process of pressing a head on a sample placed on a base (a load application process) is implemented, and thereafter a process of removing the head from the sample (a load removal process) is implemented. In a series of processes, the load acting between the head and the sample and the relative displacement of the head to the sample (load-displacement measurement) are measured. A load-displacement curve can thus be obtained. According to the load-displacement curve, physical properties such as hardness and elastic modulus based on nanometer-sized measurement can be obtained for the measured sample. In the load-displacement measurement of the surface of the anti-fouling layer based on the nanoindentation method, for example, a nanoindenter (trade name "Triboindenter", manufactured by Hysitron) can be used. In this measurement, the measurement mode is set to single indentation measurement, the measurement temperature is set to 25°C, the indenter is set to a Berkovich (triangular pyramid) type diamond indenter, the maximum indentation depth (maximum displacement H1) of the indenter on the measurement sample during the load application process is set to 200nm, the indentation speed of the indenter is set to 20nm / second, and the speed of removing the indenter from the measurement sample during the unloading process is set to 20nm / second. Based on the load-displacement curve obtained by this measurement, the maximum load Pmax (the load acting on the indenter at the maximum displacement H1), the contact projection area Ap (the projection area of the contact area between the indenter and the sample at the maximum load) and the plastic deformation H2 of the sample surface after the unloading process (the depth of the concave portion maintained on the sample surface after the indenter leaves the sample surface) can be obtained. Then, based on the maximum load Pmax and the contact projection area Ap, the hardness of the antifouling layer surface can be calculated (=Pmax / Ap). Furthermore, the elastic recovery rate (=(H1-H2) / H1) of the antifouling layer surface after the load is applied and then released can be calculated from the maximum displacement H1 and the plastic deformation H2.
[0053] Examples of methods for adjusting the surface hardness H of the antifouling layer 14 include adjusting the hardness and thickness of the hard coat layer 12 and adjusting the hardness and thickness of the underlayer for the antifouling layer 14 .
[0054] The elastic recovery rate (elastic recovery rate R) at 25°C of the surface 14a of the antifouling layer 14 measured by the nanoindentation method is preferably 0.76 or more, more preferably 0.80 or more, further preferably 0.815 or more, and particularly preferably 0.85 or more. This structure is suitable for withstanding the wiping operation performed on the antifouling layer 14 and suppressing the reduction in the antifouling property of the antifouling layer 14. The elastic recovery rate (elastic recovery rate R) at 25°C of the surface 14a of the antifouling layer 14 measured by the nanoindentation method is preferably 1.0 or less, more preferably 0.95 or less. This structure is suitable for ensuring the bendability of the antifouling layer 14, and therefore, is suitable for ensuring the bendability of the optical film F. As a method for adjusting the elastic recovery rate R of the antifouling layer 14, for example, hardness adjustment and elastic modulus adjustment of the hard coat layer 12, and hardness adjustment and elastic modulus adjustment of the base layer for the antifouling layer 14 can be listed.
[0055] The product of the surface hardness H (GPa) and the elastic recovery rate R of the antifouling layer 14 is preferably 0.8 or more, more preferably 0.9 or more, further preferably 1.0 or more, and particularly preferably 1.1 or more. This structure is suitable for withstanding the wiping operation of the antifouling layer 14 and suppressing the reduction of the antifouling property of the antifouling layer 14. The product of the surface hardness H (GPa) and the elastic recovery rate R of the antifouling layer 14 is preferably 2.0 or less, more preferably 1.7 or less, and further preferably 1.5 or less. This structure is suitable for ensuring the bendability of the antifouling layer 14, and therefore, is suitable for ensuring the bendability of the optical film F.
[0056] The water contact angle (pure water contact angle) of the surface 14a of the antifouling layer 14 is preferably 110° or more, preferably 111° or more, more preferably 112° or more, further preferably 113° or more, and particularly preferably 114° or more. The configuration in which the water contact angle of the surface 14a is as high as this degree is suitable for achieving high antifouling properties in the antifouling layer 14. The water contact angle is, for example, 130° or less. The water contact angle is obtained by forming water droplets (pure water droplets) with a diameter of less than 2 mm on the surface 14a (exposed surface) of the antifouling layer 14 and measuring the contact angle of the water droplets relative to the surface 14a. The water contact angle of the surface 14a can be adjusted by, for example, adjusting the composition of the antifouling layer 14, the roughness of the surface 14a, the composition of the hard coating layer 12, and the roughness of the surface of the hard coating layer 12 on the antifouling layer 14 side.
[0057] The thickness of the antifouling layer 14 is preferably 1 nm or more, more preferably 3 nm or more, further preferably 5 nm or more, and particularly preferably 7 nm or more. This configuration is suitable for achieving the above-mentioned surface hardness in the antifouling layer 14. The thickness of the antifouling layer 14 is preferably 25 nm or less, more preferably 20 nm or less, and further preferably 18 nm or less. This configuration is suitable for achieving the above-mentioned water contact angle in the antifouling layer 14.
[0058] The optical film F can be produced by preparing a transparent substrate 11 and then sequentially forming a hard coat layer 12, an adhesion layer 15, and an antifouling layer 14 on the transparent substrate 11, for example, by a roll-to-roll method.
[0059] The hard coat layer 12 can be formed by, for example, applying a curable resin composition on the transparent substrate 11 to form a coating film, and then curing the coating film. When the curable resin composition contains an ultraviolet curable resin, the coating film is cured by ultraviolet irradiation. When the curable resin composition contains a thermosetting resin, the coating film is cured by heating.
[0060] The exposed surface of the hard coating layer 12 formed on the transparent substrate 11 may be subjected to surface modification treatment as required. When plasma treatment is performed as the surface modification treatment, argon gas, for example, is used as an inert gas. In addition, the discharge power in the plasma treatment is, for example, 10 W or more, and, for example, 10000 W or less.
[0061] The inorganic oxide underlayer 13 is formed by forming a material into a film by dry coating. Examples of the dry coating method include sputtering, vacuum deposition, and CVD, and sputtering is preferably used.
[0062] In the sputtering method, gas is introduced into the sputtering chamber under vacuum conditions, and a negative voltage is applied to the target arranged on the cathode. Thus, a glow discharge is generated to ionize the gas atoms, so that the gas ions hit the target surface at high speed, and the target material is ejected from the target surface, and the ejected target material is deposited on a specified surface. From the viewpoint of film formation speed, reactive sputtering is preferably used as a sputtering method. In reactive sputtering, a metal target is used as a target, and as the above-mentioned gas, a mixed gas of an inert gas such as argon and oxygen (reactive gas) is used. By adjusting the flow ratio (sccm) of the inert gas to the oxygen, the proportion of oxygen contained in the inorganic oxide formed can be adjusted.
[0063] As power sources for implementing the sputtering method, for example, a DC power supply, an AC power supply, an RF power supply, and an MFAC power supply (an AC power supply with a frequency band of several kHz to several MHz) can be listed. The discharge voltage in the sputtering method is, for example, 200V or more, and, for example, 1000V or less. In addition, the film-forming gas pressure in the sputtering chamber for implementing the sputtering method is preferably 0.01Pa or more, more preferably 0.05Pa or more, and further preferably 0.1Pa or more. This structure is preferred from the viewpoint of forming an anti-fouling layer 14 in which the material is densely deposited. In addition, from the viewpoint of discharge stability, the film-forming gas pressure is, for example, 2Pa or less.
[0064] The antifouling layer 14 is formed by dry coating a film of, for example, an organic compound containing a fluorine group on the inorganic oxide underlayer 13. Examples of the dry coating method include vacuum deposition, sputtering, and CVD, and vacuum deposition is preferably used.
[0065] For example, the optical film F can be manufactured as described above. The transparent substrate 11 side of the optical film F is bonded to an adherend via an adhesive, for example. Examples of the adherend include a transparent cover disposed on the image display side of a display such as a touch panel display.
[0066] As described above, the antifouling layer 14 of the optical film F is a dry coating film disposed on the inorganic oxide base layer 13. This configuration is suitable for ensuring high bonding strength of the antifouling layer 14 of the optical film F, and therefore suitable for ensuring the peeling resistance of the antifouling layer 14. The high peeling resistance of the antifouling layer 14 contributes to maintaining the antifouling function of the antifouling layer 14.
[0067] In the optical film F, as described above, the surface 14a of the antifouling layer 14 (the surface of the antifouling layer 14 on the opposite side to the inorganic oxide base layer 13) has a surface hardness H at 25° C. measured by nanoindentation method of 1.05 GPa or more, preferably 1.1 GPa or more, more preferably 1.15 GPa or more, further preferably 1.2 GPa or more, further preferably 1.25 GPa or more, and particularly preferably 1.3 GPa or more. This configuration is suitable for withstanding the wiping operation of the antifouling layer 14 and suppressing the reduction of the antifouling property of the antifouling layer 14.
[0068] Furthermore, in the optical film F, as described above, the elastic recovery rate R at 25° C. measured by the nanoindentation method of the surface 14a of the antifouling layer 14 is preferably 0.76 or more, more preferably 0.80 or more, further preferably 0.815 or more, and particularly preferably 0.85 or more. This configuration is suitable for withstanding the wiping operation of the antifouling layer 14 and suppressing the reduction of the antifouling property of the antifouling layer 14.
[0069] Furthermore, in the optical film F, as described above, the product of the surface hardness H and the elastic recovery rate R of the antifouling layer 14 is preferably 0.8 or more, more preferably 0.9 or more, further preferably 1.0 or more, and particularly preferably 1.1 or more. This configuration is suitable for withstanding the wiping operation performed on the antifouling layer 14 and suppressing the reduction of the antifouling property of the antifouling layer 14.
[0070] As described above, the optical film F is suitable for ensuring the peeling resistance in the antifouling layer 14 and suppressing the reduction of the antifouling property.
[0071] The optical film F may include a layer having a predetermined optical function (optical functional layer). When the optical functional layer includes a plurality of layers, the layer on the antifouling layer 14 side surface of the optical functional layer preferably also serves as the inorganic oxide underlayer 13 .
[0072] Figure 2 The optical function layer 20 is shown in the embodiment of the optical film F between the adhesion layer 15 and the antifouling layer 14. As described later, the optical function layer 20 has a layer also serving as the inorganic oxide underlayer 13 on the antifouling layer 14 side surface.
[0073] The optical function layer 20 is disposed on one surface of the adhesion layer 15 in the thickness direction T. In this modification, the optical function layer 20 is an antireflection layer for suppressing the reflection intensity of external light. That is, the optical film F in this modification is an antireflection film with an antifouling layer.
[0074] The optical functional layer 20 (anti-reflection layer) alternately has a high refractive index layer with a relatively large refractive index and a low refractive index layer with a relatively small refractive index in the thickness direction. In the anti-reflection layer, the actual reflected light intensity is attenuated by the interference between the reflected light at multiple interfaces of the multiple thin layers (high refractive index layer, low refractive index layer) contained in the layer. In addition, in the anti-reflection layer, by adjusting the optical film thickness (the product of the refractive index and the thickness) of each thin layer, it is possible to exhibit an interference effect that attenuates the reflected light intensity. In the present embodiment, specifically, the optical functional layer 20 as the anti-reflection layer has a first high refractive index layer 21, a first low refractive index layer 22, a second high refractive index layer 23, and a second low refractive index layer 24 that also serves as the above-mentioned inorganic oxide base layer 13 in sequence toward one side of the thickness direction T.
[0075] The first high refractive index layer 21 and the second high refractive index layer 23 are respectively formed of a high refractive index material having a refractive index of preferably 1.9 or more at a wavelength of 550 nm. From the viewpoint of taking both high refractive index and low absorption of visible light into account, as high refractive index materials, for example, niobium oxide (Nb2O5), titanium oxide, zirconium oxide, tin-doped indium oxide (ITO) and antimony-doped tin oxide (ATO) can be cited, and niobium oxide is preferably used.
[0076] The optical thickness (product of refractive index and thickness) of the first high refractive index layer 21 is, for example, not less than 20 nm, and not more than 55 nm. The optical thickness of the second high refractive index layer 23 is, for example, not less than 60 nm, and not more than 330 nm.
[0077] The first low-refractive index layer 22 and the second low-refractive index layer 24 are respectively formed by a low-refractive index material having a refractive index of preferably less than 1.6 at a wavelength of 550nm. From the viewpoint of taking into account both the low refractive index and the low absorptivity of visible light, as low-refractive index materials, for example silicon dioxide (SiO2) and magnesium fluoride can be listed, preferably silicon dioxide. As mentioned above, SiO2 and magnesium fluoride are also preferably used as materials for the inorganic oxide base layer 13.
[0078] The optical film thickness of the first low refractive index layer 22 is, for example, not less than 15 nm, and, for example, not more than 70 nm. The optical film thickness of the second low refractive index layer 24 is, for example, not less than 100 nm, and, for example, not more than 160 nm.
[0079] The first high refractive index layer 21, the first low refractive index layer 22 and the second high refractive index layer 23 can be formed by forming a material into a film using a dry coating method. The second low refractive index layer 24, which also serves as the inorganic oxide base layer 13, is formed by forming a material into a film using a dry coating method. As dry coating methods, sputtering, vacuum evaporation and CVD can be listed, and sputtering is preferably used. As sputtering, from the viewpoint of film formation speed, reactive sputtering is preferably used. The conditions of the sputtering method are the same as the conditions of the sputtering method related to the formation of the inorganic oxide base layer 13 in the above-described conditions.
[0080] exist Figure 2 In the optical film F shown, the antifouling layer 14 is a dry coating film disposed on the second low refractive index layer 24 (inorganic oxide base layer 13). Figure 2 In the optical film F shown, the hardness (surface hardness H) of the surface 14a of the antifouling layer 14 at 25°C measured by the nanoindentation method is 1.05 GPa or more, preferably 1.1 GPa or more, more preferably 1.15 GPa or more, further preferably 1.2 GPa or more, further preferably 1.25 GPa or more, and particularly preferably 1.3 GPa or more. Figure 2 In the optical film F shown, the elastic recovery rate (elastic recovery rate R) of the surface 14a of the antifouling layer 14 at 25°C measured by the nanoindentation method is preferably 0.76 or more, more preferably 0.80 or more, further preferably 0.815 or more, and particularly preferably 0.85 or more. Figure 2 In the optical film F shown, the product of the surface hardness H (GPa) and the elastic recovery rate R of the antifouling layer 14 is preferably 0.8 or more, more preferably 0.9 or more, further preferably 1.0 or more, and particularly preferably 1.1 or more. This optical film F is suitable for ensuring peeling resistance in the antifouling layer 14 and suppressing the reduction of antifouling properties.
[0081] Example
[0082] The present invention is specifically described below with reference to the following embodiments. The present invention is not limited to the embodiments. In addition, the specific numerical values of the compounding amount (content), physical property values, parameters, etc. described below can replace the upper limit (a numerical value defined in the form of "below" or "less than") or the lower limit (a numerical value defined in the form of "above" or "exceeding") of the corresponding compounding amount (content), physical property values, parameters, etc. described in the above-mentioned "Specific Implementation Methods".
[0083] [Example 1]
[0084] First, a hard coating layer is formed on one side of a polyethylene terephthalate (PET) film (trade name "50U48", thickness 50 μm, manufactured by Toray Industries) as a transparent substrate (hard coating layer forming process). Specifically, 100 parts by mass (solid content conversion) of a butyl acetate solution (trade name "UNIDIC17-806", solid content concentration of 80% by mass, manufactured by DIC) of a mixture of ultraviolet-curable monomers and oligomers (containing urethane acrylate as the main component), 5 parts by mass of a photopolymerization initiator (trade name "IRGACURE906", manufactured by BASF) and 0.01 parts by mass of a leveling agent (trade name "GRANDICPC4100", manufactured by DIC) are mixed to obtain a mixed solution. Next, a mixed solvent of cyclopentanone (CPN) and propylene glycol monomethyl ether (PGM) (the mass ratio of CPN to PGM is 45:55) is added to adjust the solid content concentration of the mixed solution to 36%. Thus, an ultraviolet curable resin composition (varnish) is prepared. Next, the resin composition is applied to one side of the above-mentioned PET film to form a coating film. Next, the coating film is dried by heating it, and then cured by ultraviolet irradiation. The heating temperature is set to 90°C, and the heating time is set to 60 seconds. In the ultraviolet irradiation, a high-pressure mercury lamp is used as the light source, ultraviolet rays with a wavelength of 365nm are used, and the cumulative irradiation light amount is set to 300mJ / cm 2 Thus, a hard coating layer (HC) having a thickness of 5 μm was formed on the PET film.
[0085] Next, the HC layer surface of the HC layer-attached PET film was subjected to plasma treatment using a roll-to-roll plasma treatment apparatus in a vacuum atmosphere of 1.0 Pa. In the plasma treatment, argon gas was used as an inert gas, and the discharge power was set to 780 W.
[0086] Next, a bonding layer and an inorganic oxide underlayer were sequentially formed on the HC layer of the plasma-treated PET film with the HC layer (sputtering film forming process). Specifically, a 2.0 nm thick indium tin oxide (ITO) layer as a bonding layer and a 165 nm thick SiO2 layer as an inorganic oxide underlayer were sequentially formed on the HC layer of the PET film with the HC layer using a roll-to-roll sputtering film forming device. In the formation of the bonding layer, an ITO target was used, and argon as an inert gas and 10 parts by volume of oxygen as a reactive gas relative to 100 parts by volume of argon were used, the discharge voltage was set to 350 V, the gas pressure in the film forming chamber (film forming gas pressure) was set to 0.4 Pa, and the ITO layer was formed by MFAC sputtering. In the formation of the inorganic oxide underlayer, a Si target was used, 100 parts by volume of argon and 30 parts by volume of oxygen were used, the discharge voltage was set to 350 V, the film forming gas pressure was set to 0.3 Pa, and the SiO2 layer was formed by MFAC sputtering.
[0087] Next, an antifouling layer is formed (antifouling layer forming step). Specifically, an antifouling layer with a thickness of 12 nm is formed on the inorganic oxide base layer by a vacuum evaporation method using an alkoxysilane compound containing a perfluoropolyether group as an evaporation source. The evaporation source is a solid component obtained by drying "KY1903-1" (an alkoxysilane compound containing a perfluoropolyether group, with a solid content concentration of 20% by mass) manufactured by Shin-Etsu Chemical Co., Ltd. In addition, the heating temperature of the evaporation source in the vacuum evaporation method is set to 260°C.
[0088] As described above, an optical film of Example 1 was produced. The optical film of Example 1 includes a transparent substrate (resin film), a hard coat layer, an adhesion layer, an inorganic oxide underlayer, and an antifouling layer in this order toward one side in the thickness direction.
[0089] [Example 2]
[0090] An optical film of Example 2 was produced in the same manner as in Example 1 except that the thickness of the HC layer was set to 10 μm instead of 5 μm.
[0091] [Example 3]
[0092] An optical film of Example 3 was produced in the same manner as in Example 1, except that the thickness of the HC layer was 10 μm instead of 5 μm and the thickness of the inorganic oxide underlayer was 100 nm instead of 165 nm.
[0093] [Example 4]
[0094] An optical film of Example 4 was produced in the same manner as in Example 1 except that the film-forming gas pressure during formation of the inorganic oxide underlayer was 0.1 Pa instead of 0.3 Pa.
[0095] [Example 5]
[0096] An optical film of Example 5 was produced in the same manner as in Example 1 except that the thickness of the HC layer was set to 10 μm instead of 5 μm and the film-forming gas pressure during formation of the inorganic oxide underlayer was set to 0.1 Pa instead of 0.3 Pa.
[0097] [Example 6]
[0098] An optical film of Example 6 was produced in the same manner as in Example 1 except that the thickness of the antifouling layer was set to 8 nm instead of 12 nm.
[0099] [Example 7]
[0100] An optical film of Example 7 was produced in the same manner as in Example 1 except that the thickness of the antifouling layer was set to 6 nm instead of 12 nm.
[0101] [Example 8]
[0102] An optical film of Example 8 was produced in the same manner as in Example 1 except that the thickness of the antifouling layer was set to 16 nm instead of 12 nm.
[0103] [Example 9]
[0104] First, a hard coating layer is formed on one side of a PET film (trade name "50U48", thickness 50 μm, manufactured by Toray Industries) as a transparent substrate. Specifically, 100 parts by mass (solid content conversion) of a UV-curable multifunctional acrylate resin (trade name "Z-850-50H-D", solid content concentration of 44%, manufactured by Aica Kogyo), 4 parts by mass of a photopolymerization initiator (trade name "OMNIRAD2959", manufactured by BASF) and 0.05 parts by mass of a leveling agent (trade name "LE-303", manufactured by Kyoeisha Chemical Co., Ltd.) are mixed to obtain a mixed solution. Then, methyl isobutyl ketone is added to the mixed solution to adjust the solid content concentration of the mixed solution to 40%. Thus, a UV-curable resin composition (varnish) is prepared. Next, the resin composition is applied to one side of the above-mentioned PET film to form a coating film. Next, the coating film is dried by heating it and then cured by ultraviolet irradiation. The heating temperature is set to 80°C and the heating time is set to 60 seconds. In the ultraviolet irradiation, a high-pressure mercury lamp was used as the light source, and ultraviolet rays with a wavelength of 365 nm were used, and the cumulative irradiation light amount was set to 300 mJ / cm 2 Thus, a hard coating layer (HC) having a thickness of 5 μm was formed on the PET film.
[0105] Next, the surface of the HC layer of the PET film with HC layer was subjected to plasma treatment using a roll-to-roll plasma treatment apparatus in a vacuum atmosphere of 1.0 Pa. In the plasma treatment, argon gas was used as an inert gas, and the discharge power was set to 150W.
[0106] Next, a bonding layer and an antireflection layer were sequentially formed on the HC layer of the plasma-treated PET film with an HC layer. Specifically, a 1.5 nm thick indium tin oxide (ITO) layer as a bonding layer, a 12 nm thick Nb2O5 layer as a first high refractive index layer, a 28 nm thick SiO2 layer as a first low refractive index layer, a 100 nm thick Nb2O5 layer as a second high refractive index layer, and a 85 nm thick SiO2 layer as a second low refractive index layer were sequentially formed on the HC layer of the plasma-treated PET film with an HC layer using a roll-to-roll sputtering film forming apparatus. In the formation of the bonding layer, an ITO target was used, and argon gas as an inert gas and oxygen gas as a reactive gas in an amount of 10 parts by volume relative to 100 parts by volume of argon gas were used, the discharge voltage was set to 400 V, the gas pressure in the film forming chamber (film forming gas pressure) was set to 0.2 Pa, and the ITO layer was formed by MFAC sputtering. In the formation of the first high refractive index layer, a Nb target was used, and 100 parts by volume of argon and 5 parts by volume of oxygen were used, the discharge voltage was set to 415V, and the film forming gas pressure was set to 0.7Pa, and the Nb2O5 layer was formed by MFAC sputtering. In the formation of the first low refractive index layer, a Si target was used, and 100 parts by volume of argon and 30 parts by volume of oxygen were used, the discharge voltage was set to 350V, and the film forming gas pressure was set to 0.7Pa, and the SiO2 layer was formed by MFAC sputtering. In the formation of the second high refractive index layer, a Nb target was used, and 100 parts by volume of argon and 13 parts by volume of oxygen were used, the discharge voltage was set to 460V, and the film forming gas pressure was set to 0.7Pa, and the Nb2O5 layer was formed by MFAC sputtering. In the formation of the second low refractive index layer, a Si target was used, and 100 parts by volume of argon gas and 30 parts by volume of oxygen were used, the discharge voltage was set to 340V, and the film forming pressure was set to 0.7 Pa, and the SiO2 layer was formed by MFAC sputtering. As described above, an anti-reflection layer (first high refractive index layer, first low refractive index layer, second high refractive index layer, second low refractive index layer) was stacked on the HC layer of the PET film with the HC layer through the adhesion layer. In this embodiment, the second low refractive index layer is an inorganic oxide base layer for the antifouling layer.
[0107] Next, an antifouling layer is formed on the formed antireflection layer (ie, on the second low refractive index layer).
[0108] As described above, an optical film of Example 9 was prepared. The optical film of Example 9 comprises, in order toward one side in the thickness direction, a transparent substrate (resin film), a hard coat layer, an adhesion layer, an antireflection layer (including a second low refractive index layer as an inorganic oxide underlayer), and an antifouling layer.
[0109] [Comparative Example 1]
[0110] An optical film of Comparative Example 1 was produced in the same manner as in Example 1 except that the thickness of the HC layer was 10 μm instead of 5 μm and the thickness of the inorganic oxide underlayer was 30 nm instead of 165 nm.
[0111] 〈Hardness and elastic recovery rate of antifouling layer surface〉
[0112] The load-displacement measurement was performed on the antifouling layer surface of each optical film of Examples 1 to 9 and Comparative Example 1 using the nanoindentation method. Specifically, first, a measurement sample (5 mm × 5 mm) was cut out from the optical film. Next, a nanoindenter (trade name "Triboindenter", manufactured by Hysitron) was used to perform a load-displacement measurement on the antifouling layer surface in the measurement sample in accordance with ISO14577 to obtain a load-displacement curve. In this measurement, the measurement mode was set to a single indentation measurement, the measurement temperature was set to 25°C, the indenter used was a Berkovich (triangular pyramid) type diamond indenter, the maximum indentation depth (maximum displacement H1) of the indenter to the measurement sample during the load application process was set to 200 nm, the indentation speed of the indenter was set to 20 nm / sec, and the speed of removing the indenter from the measurement sample during the unloading process was set to 20 nm / sec. According to the obtained load-displacement curve, the maximum load Pmax (the load acting on the indenter at the maximum displacement H1), the contact projection area Ap (the projection area of the contact area between the indenter and the sample at the maximum load) and the plastic deformation H2 of the sample surface after the unloading process (the depth of the concave portion maintained on the sample surface after the indenter leaves the sample surface) are obtained. Then, the surface hardness of the anti-fouling layer is calculated based on the maximum load Pmax and the contact projection area Ap (= Pmax / Ap). In addition, based on the maximum displacement H1 and the plastic deformation H2, the elastic recovery rate of the surface of the anti-fouling layer after the load is applied and then unloaded is calculated (= (H1-H2) / H1). These surface hardnesses (GPa) and elastic recovery rates (%) are shown in Table 1.
[0113] 〈Water contact angle〉
[0114] The water contact angle on the surface of the antifouling layer of each optical film of Examples 1 to 9 and Comparative Example 1 was investigated. First, about 1 μL of pure water was dripped onto the surface of the antifouling layer of the optical film to form a water droplet. Next, the angle between the surface of the water droplet on the surface of the antifouling layer and the surface of the antifouling layer was measured. A contact angle meter (trade name "DMo-501", manufactured by Kyowa Interface Science Co., Ltd.) was used in the measurement. The measurement results are shown in Table 1 as the initial water contact angle θ0.
[0115] Rubber sliding test
[0116] The degree of reduction in the antifouling property of the antifouling layer surface caused by the rubber sliding test was investigated for each optical film of Examples 1 to 9 and Comparative Example 1. Specifically, a sliding test (first rubber sliding test) was first performed in which a rubber was slid back and forth relative to the antifouling layer surface of the optical film. In this test, a rubber (Φ6 mm) manufactured by Minoan was used, the load of the rubber on the antifouling layer surface was set to 1 kg / 6 mmΦ, the sliding distance of the rubber on the antifouling layer surface (one way in the back and forth movement) was set to 20 mm, the sliding speed of the rubber was set to 40 rpm, and the number of back and forth movements of the rubber relative to the antifouling layer surface was set to 3000. Next, the water contact angle of the rubber sliding portion of the antifouling layer surface of the optical film was measured using the same method as the method for measuring the initial water contact angle θ0. The measurement results are shown in Table 1 as the water contact angle θ1 after the first rubber sliding test.
[0117] Next, a sliding test (second rubber sliding test) was performed in which the rubber was further slid back and forth relative to the antifouling layer surface of the optical film. The sliding conditions were the same as those of the first rubber sliding test (the number of times the rubber was moved back and forth in the first rubber sliding test and the subsequent second rubber sliding test was 6000 times in total). Next, the water contact angle of the rubber sliding portion of the antifouling layer surface of the optical film was measured by the same method as the method for measuring the initial water contact angle θ0. The measurement results are shown in Table 1 as the water contact angle θ2 after the second rubber sliding test. Figure 3 This is a graph in which the surface hardness H and the water contact angle θ2 of each optical film of Examples 1 to 9 and Comparative Example 1 are plotted. Figure 3 In the figure, the horizontal axis represents the surface hardness H (GPa), and the vertical axis represents the water contact angle θ2 (°). Figure 3 In the figure, marks E1 to E9 represent the measurement results of Examples 1 to 9, and mark C1 represents the measurement result of Comparative Example 1.
[0118] <evaluate>
[0119] In each of the optical films of Examples 1 to 9, compared with the optical film of Comparative Example 1, the degree of decrease in the water contact angle on the surface of the antifouling layer due to the rubber sliding test (the first rubber sliding test, the second rubber sliding test) is significantly smaller, and therefore, the decrease in antifouling properties is significantly smaller (on the surface of the antifouling layer, the smaller the decrease in the water contact angle, the smaller the decrease in antifouling properties).
[0120] [Table 1]
[0121]
[0122] The above-mentioned embodiments are examples of the present invention, and the present invention is not to be interpreted as being limitative of the embodiments. Modifications of the present invention that are obvious to those skilled in the art are included in the scope of protection of the claims.
[0123] Industrial Applicability
[0124] The optical film with an antifouling layer of the present invention can be applied to, for example, an antireflection film with an antifouling layer, a transparent conductive film with an antifouling layer, and an electromagnetic wave shielding film with an antifouling layer.
[0125] Description of Reference Numerals
[0126] F optical film (optical film with antifouling layer)
[0127] 11Transparent substrate
[0128] 12 Hard coating
[0129] 13Inorganic oxide base layer
[0130] 14 Antifouling layer
[0131] 14a Surface
[0132] 15 Sealing layer
[0133] 20 optical functional layer
[0134] 21 first high refractive index layer
[0135] 22 first low refractive index layer
[0136] 23 Second high refractive index layer
[0137] 24 Second low refractive index layer
Claims
1. An optical film with an antifouling layer, which comprises a transparent substrate, a hard coating layer, an inorganic oxide base layer and an antifouling layer in this order, The antifouling layer is a dry coating film disposed on the inorganic oxide base layer. The antifouling layer uses an alkoxysilane compound having a perfluoropolyether group represented by the following general formula (1): R 1 -R 2 -X-(CH2) m -Si(OR 3 )3(1) In the general formula (1), R 1 represents a perfluoroalkyl group, R 2 Indicates inclusion - (OCF2) p -and-(OC2F4) p -a perfluoropolyether group repeating structure, p represents an integer of 1 to 50, R 3 represents an alkyl group having 1 to 4 carbon atoms, X represents an ether group, a carbonyl group, an amino group or an amide group, and m represents an integer greater than 1. The hardness of the surface of the antifouling layer opposite to the inorganic oxide underlayer at 25° C. measured by a nanoindentation method is 1.05 GPa or more, The product of the elastic recovery rate at 25° C. measured by the nanoindentation method and the hardness (GPa) of the surface of the antifouling layer is 0.8 or more, Nanoindentation: The measurement mode was set to single indentation measurement, the measurement temperature was set to 25°C, the indenter used was a Berkovich triangular pyramid-shaped diamond indenter, the maximum indentation depth of the indenter on the measurement sample during the load application process, i.e., the maximum displacement H1, was set to 200 nm, the indentation speed of the indenter was set to 20 nm / sec, and the speed of removing the indenter from the measurement sample during the unloading process was set to 20 nm / sec. Based on the load-displacement curve obtained by this measurement, the maximum load Pmax, i.e., the load acting on the indenter at the maximum displacement H1, the contact projection area Ap, i.e., the projection area of the contact area between the indenter and the sample at the maximum load, and the plastic deformation amount H2 of the sample surface after the unloading process, i.e., the depth of the concave portion maintained on the sample surface after the indenter leaves the sample surface, were obtained. Based on the maximum load Pmax and the contact projection area Ap, the hardness of the antifouling layer surface was calculated as Pmax / Ap, and based on the maximum displacement H1 and the plastic deformation amount H2, the elastic recovery rate of the antifouling layer surface after the load application and subsequent unloading was calculated as (H1-H2) / H1.
2. The optical film with an antifouling layer according to claim 1, wherein: The surface of the antifouling layer has an elastic recovery rate at 25° C. measured by a nanoindentation method of 0.76 or more.
3. The optical film with an antifouling layer according to claim 1 or 2, wherein: The antifouling layer has a thickness of 1 nm or more and 25 nm or less.
4. The optical film with an antifouling layer according to claim 1 or 2, wherein: The inorganic oxide base layer includes silicon dioxide.
5. The optical film with an antifouling layer according to claim 1 or 2, wherein: The hard coating layer has a thickness of 1 μm or more and 50 μm or less.