Activation composition comprising an alkali metal salt and calcium carbonate and / or magnesium carbonate for activating granulated blast furnace slag powder, and a cementitious material comprising the activation composition for preparing a mortar composition or a concrete composition
By combining activated compositions of calcium carbonate particles and alkali metal salts in building materials with GGBS, the negative impact of silicate cement on the environment and health is solved, the mechanical properties and durability of building materials are improved, and the low temperature is achieved Efficient production.
Patent Information
- Application Number
- CN202080099644.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-04-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-04-08
AI Technical Summary
The production of existing silicate cement has severe negative impact on the environment and has health and safety issues during its treatment. It is necessary to develop an alternative to improve the mechanical properties and durability of building materials.
An activation composition containing at least 40% calcium carbonate particles and alkali metal salts is combined with granulated blast furnace slag powder (GGBS) for the preparation of gelled materials with early strength and long-term properties, suitable for construction mortars and concrete.
The production of building materials with excellent mechanical properties and durability at low temperatures is achieved, reducing environmental pollution and health risks, while simplifying the preparation process.
Smart Images

Figure CN115836037B_ABST
Abstract
Description
Field of the Invention
[0001] The technical field of the present invention relates to hydraulic mineral cementitious materials comprising at least one slag, such as ground granulated blast furnace slag (GGBS or slag), for use in a composition capable of setting and hardening, such as a mortar composition or a concrete composition.
[0002] More specifically, the present invention relates to cementitious materials for the construction industry and compositions capable of setting and hardening, comprising at least one slag as hydraulic cementitious material and at least one activation system.
[0003] The invention also relates to a process for the preparation of these slag-based cementitious materials, these dry or wet compositions capable of setting and hardening.
[0004] The use of the set and hardened products obtained from these compositions in construction also lies within the scope of the invention. Background Art
[0005] The production of Portland cement has a great negative impact on the environment due to the large amount of carbon dioxide emissions. During the high temperature (1450℃) calcination of raw materials in the furnace, CO2 is inevitably produced through the decarbonization of limestone (Formula (1)):
[0006] CaCO3(s)→CaO(s)+CO2(g) (Formula (1))
[0007] In addition, the burning of fossil fuels required to heat cement kilns releases carbon dioxide. Adding the additional emissions from grinding, each ton of Portland cement produces almost a ton of CO2. Overall, the cement industry accounts for about 7% to 9% of global carbon dioxide emissions.
[0008] Furthermore, handling of Portland cement can lead to health problems (e.g. allergies), particularly due to its high alkalinity (pH above 13). Furthermore, harmful elements such as hexavalent chromium (Cr(VI)) may be released during kneading, which can also be detrimental to worker health when it comes in contact with the skin. Although Cr(VI) reducing agents (e.g. ferrous sulfate) are often included in cement powder, their effectiveness is limited in time. Construction workers, particularly in the third world, are not expected to frequently check deadlines associated with such treatments.
[0009] Most current research into new cementitious materials aims to replace cement in various applications with cementitious materials that have less impact on the environment. One approach is to use resources that do not require expensive disposal, such as by-products from other industries (waste for one industry, but a major resource for others). This is the case with blast furnace slag, a by-product of the steel industry. By grinding this product into a fine powder (GGBS), a cementitious material can be obtained that can partially replace cement or, by adding some chemical activators, be used alone.
[0010] It is noteworthy that the use of GGBS is not only environmentally friendly, but also enhances several properties when used in the formulation of mortars and concretes, such as high resistance to sulfate attack, low permeability, good resistance in chemically aggressive environments, low heat of hydration (required for large structures), overall excellent durability, the possibility of curing heavy metals or radionuclides, etc.
[0011] It should be emphasized that GGBS is a hydraulic binder (in contrast to latent hydraulic binders such as fly ash or silica fume). This means that GGBS reacts with water alone. The addition of chemical activators (and / or heating) can help accelerate this reaction and improve early strength. Typically, the activator acts to raise the pH to an appropriate level to enhance the nucleophilic attack of the hydroxide ions on the glass network.
[0012] Activators accelerate the setting and / or curing and / or hardening of cementitious materials, mortar / concrete compositions.
[0013] Therefore, in order to activate GGBS, people have developed an activation system. For example, international patent application WO2017 / 198930 discloses a cementitious material comprising GGBS and an accelerating agent. The accelerating agent comprises a calcium sulfate source and a granular nucleating agent.
[0014] Although such quick-setting admixtures allow construction materials containing at least 80% by weight of GGBS to be obtained, there is still a need to develop activation systems for materials containing GGBS, in particular at low temperatures and for obtaining hardened concretes or hardened industrial mortars having better mechanical properties, in particular at an early stage, than hardened concretes and hardened industrial mortars comprising only ordinary Portland cement as binder.
[0015] In this context, the present invention aims to solve at least one of the above problems and / or needs by achieving at least one of the following objectives:
[0016] -O1- Provides a slag-based cementitious material or a mortar composition or a concrete composition comprising the slag-based cementitious material, which is an attractive alternative to ordinary Portland cement (OPC)-based compositions.
[0017] -O2- Provided is a slag-based cementitious material or a mortar composition or a concrete composition comprising the slag-based cementitious material, which is environmentally friendly.
[0018] -03- To provide a slag-based cementitious material or a mortar composition or a concrete composition comprising the slag-based cementitious material, which is more acceptable than an OPC-based composition in terms of health and safety issues.
[0019] -O4- Provide a slag-based cementitious material or a mortar composition or a concrete composition comprising the slag-based cementitious material, which produces dry mortar, dry or semi-dry prepared concrete and wet mortar and concrete formulations with appropriate capabilities manufactured by several methods such as vibro-compacting, spraying, plastering, pouring, etc.
[0020] -O5- Provide a slag-based cementitious material or a mortar composition or concrete composition comprising the slag-based cementitious material, which produces a wet preparation with appropriate rheological properties, i.e., stable rheology (good workability) within the conventional setting time (e.g., a few minutes to a few hours) required by the user of the wet preparation.
[0021] -O6- Providing a slag-based cementitious material or a mortar composition or a concrete composition comprising the slag-based cementitious material, which produces a hardened material having desired mechanical properties, especially acceptable early strength (e.g. 24 hours).
[0022] -07- Providing a slag-based cementitious material or a mortar composition or a concrete composition comprising the slag-based cementitious material, which produces a hardened material having desired durability.
[0023] -08- Providing a slag-based cementitious material or a mortar composition or a concrete composition comprising the GGBS-based cementitious material, which produces a hardened material with a generally required setting time (e.g., several minutes to several hours).
[0024] -O9- Provides a simple and inexpensive method for preparing a slag-based cementitious material or a mortar composition or concrete composition comprising the slag-based cementitious material that meets at least one of purposes -O1- to -O9-.
[0025] -O10- Provided is a simple and inexpensive method for preparing a wet slag-based cementitious material or a mortar composition or a concrete composition comprising the slag-based cementitious material.
[0026] -011-Providing a hardened product for the construction industry, which comprises slag as at least part of the cementitious material.
[0027] Advantages of the invention
[0028] One of the advantages of the present invention is the improvement of building materials, especially dry mortar compositions or dry concrete compositions, comprising GGBS, which produce hardened materials with desired mechanical properties, especially acceptable early strength (e.g. 24 hours) and long-term performance.
[0029] Another advantage is that, in embodiments of the present invention, the cementitious material composition according to the present invention can be used at low temperatures, ie, at around 5°C.
[0030] A further advantage is the universality of the activating composition, which can be included in various concretes or industrial mortars requiring various amounts of water, in particular the activating composition according to the invention can be part of a high-water content composition. Summary of the invention
[0031] The present invention relates to an activator, in particular for concrete or industrial mortar containing hydraulic cementitious materials and / or pozzolanic materials, comprising:
[0032] A. at least 40% by weight, preferably at least 50% by weight, of calcium carbonate particles and / or magnesium carbonate particles having a d80 of less than or equal to 15 μm and a d50 of less than or equal to 4 μm, and
[0033] B. At least 1.5% and at most 60% by weight of at least one alkali metal salt.
[0034] The invention also relates to a cementitious material composition comprising an activating composition according to any one of claims 1 and 2 and a component C consisting of at least one hydraulic cementitious material.
[0035] Without being bound by any theory, it is believed that the content and particle size of calcium carbonate and / or magnesium carbonate contained in the activating composition according to the invention fills the voids of the mortar / concrete to which the activating composition is intended to be added and it contributes to water retention in the product. These two phenomena, together with the alkali activation due to the presence of alkali metal salts, can enhance the early hydration of the hydraulic binder and improve the mechanical strength of the resulting concrete or industrial mortar through a better distribution of the hydrated phases.
[0036] The invention also relates to a dry concrete composition or a dry industrial mortar composition comprising at least one aggregate and the cementitious material composition.
[0037] The present invention also relates to a dry concrete composition or a dry industrial mortar composition comprising other components such as admixtures and the cementitious material composition.
[0038] Furthermore, the invention relates to a process for preparing a wet concrete composition or a wet mortar composition and to a hardened concrete composition or a hardened industrial mortar composition obtained therefrom.
[0039] definition
[0040] For the purposes of this document, the following non-limiting definitions must be considered:
[0041] - "Slag" means the stony by-product material separated from the metal during the smelting or refining of ore.
[0042] - “GGBS” or “GGBFS”: ground granulated blast furnace slag, equivalent to blast furnace slag, granulated blast furnace slag (GBFS), blast furnace slag powder and blast furnace slag fines.
[0043] - "Cement" is understood to mean a powdered substance used to make mortar or concrete. It is a mineral cementitious material which may not contain any organic compound. It means any common cement and includes slag-portland blended cements and cements based on alkali activation.
[0044] - "Cementitious material" refers to "hydraulic cementitious material", which means any material that hardens simply by adding water, such as GGBS and cement.
[0045] - "Supplementary cementitious materials" refers to materials that enhance the strength of cementitious materials through potential hydraulic or pozzolanic activity. The term herein refers to fly ash, activated clay, silica fume, basic oxygen furnace slag, natural pozzolanic materials, rice husk ash, activated recycled concrete fine aggregate or mixtures thereof.
[0046] - "Mortar" refers to a material consisting of cementitious materials, aggregates such as sand and other ingredients such as admixtures.
[0047] - "Concrete" means a material consisting of cementitious materials, aggregates such as sand and gravel, and other ingredients such as admixtures.
[0048] - "d50" gives the median size of the particle size distribution of a material (for cementitious materials, usually in micrometers). This means that 50% of the particles have a size smaller than the specified number and 50% of the particles have a size larger than the specified number. The measurement of d50 is carried out by laser diffraction analysis, also known as laser diffraction spectroscopy, and is carried out by means of a laser diffraction analyzer such as the "Mastersizer 2000" commercialized by the company Malvern, using a wet method.
[0049] - "d80" gives information on the size distribution of the particles of a material (for cementitious materials, usually in micrometers). This means that 80% of the particles have a size smaller than the specified number, while 20% have a size larger than the specified number. The measurement of d80 is carried out by laser diffraction analysis, also known as laser diffraction spectroscopy, and is carried out by means of a laser diffraction analyzer such as the "Mastersizer 2000" commercialized by the company Malvern, using a wet method. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figures 1 to 3 is a bar graph comparing the compressive strength of different industrial mortars according to the invention and outside the invention. DETAILED DESCRIPTION
[0051] Activating composition
[0052] In order to achieve the purpose of accelerating the kinetics of the hardening reaction of GGBS, especially in the early stage, and to provide a concrete or industrial mortar with an appropriate compressive strength in the early stage (24 hours) according to the final application, similar to or better than the compressive strength in the early stage (7 days) and later stage (28 days) of industrial mortar or concrete with a cementitious material made of only Portland cement, the present invention developed by the inventors, in particular, the activation composition for concrete or industrial mortar containing hydraulic cementitious materials and / or pozzolanic materials, comprises:
[0053] A. at least 40% by weight, preferably at least 50% by weight, of calcium carbonate particles and / or magnesium carbonate particles having a d80 of less than or equal to 15 μm and a d50 of less than or equal to 4 μm, and
[0054] B. At least 1.5% and at most 60% by weight of at least one alkali metal salt.
[0055] In certain embodiments, the activating compositions of the present invention are free of a calcium sulfate source.
[0056] A. Calcium carbonate / Magnesium carbonate
[0057] According to the invention, the activation composition comprises at least 40% by weight of calcium carbonate and / or magnesium carbonate. In a preferred embodiment, the activation composition comprises at least 50% by weight of calcium carbonate and / or magnesium carbonate.
[0058] According to the present invention, the calcium carbonate particles and / or magnesium carbonate particles have a d80 of less than or equal to 15 μm, preferably less than or equal to 10 μm, and a d50 of less than or equal to 4 μm.
[0059] B. Alkali metal salts
[0060] The amount of the alkali metal salt in the activating composition of the present invention is adjusted according to the concrete composition or industrial mortar composition into which the activating composition of the present invention is intended to be finally incorporated.
[0061] Thus, in one embodiment, for example for masonry mortars, the activating composition preferably comprises 1.5 to 15 wt.-%, more preferably 3 to 10 wt.-%, even more preferably 4 to 5 wt.-% of said alkali metal salt.
[0062] Thus, in another embodiment, for example for tile adhesives, the activation composition preferably comprises 25 to 60 wt. %, more preferably 35 to 55 wt. %, even more preferably 40 to 50 wt. % of said alkali metal salt.
[0063] The alkali metal salt is advantageously selected from the group consisting of sodium chloride (NaCl), sodium sulfate (Na2SO4), potassium sulfate (K2SO4), potassium chloride (KCl), sodium carbonate (Na2CO3) and potassium carbonate (K2CO3), and mixtures thereof.
[0064] Cementitious material composition
[0065] The invention also relates to a cementitious material composition comprising the activation composition and a component C consisting of at least one hydraulic cementitious material.
[0066] In one embodiment, component C consists only of ground granulated blast furnace slag.
[0067] Granulated blast furnace slag (GGBS) is a glassy granular material obtained by quenching molten slag from a blast furnace in water and then finely grinding the quenched product to increase the reactivity of GGBS. GGBS is an amorphous aluminosilicate glass, mainly composed of SiO2, CaO, MgO and Al2O3. There are many glass network cationic modifiers: Ca, Na, Mn, etc.
[0068] GGBS is preferably produced according to European Standard [NF EN 15167-1].
[0069] Therefore, the cementitious material composition according to this embodiment of the invention advantageously comprises 60 to 99 wt %, advantageously 70 to 97 wt % of ground granulated blast furnace slag.
[0070] The cementitious material composition according to this embodiment of the present invention advantageously contains 1 wt% to 40 wt%, more advantageously 3 wt% to 30 wt% of the above-mentioned activation composition. In addition, the cementitious material composition according to this embodiment of the present invention advantageously contains greater than 0.5 wt% to 10 wt%, advantageously 0.7 wt% to 7 wt% of an alkali metal salt.
[0071] In another embodiment, component C consists of a mixture of ground granulated blast furnace slag and at least one other hydraulic binder, preferably chosen from hydraulic binders according to standard EN 197-1 and cements based on alumina or calcium aluminate.
[0072] In particular, by cement we mean any common cement as described in European Standard EN 197.1, ie a hydraulic cementitious material consisting of calcium silicates (3CaOSiO2) and (2CaOSiO2) as well as Al2O3, Fe2O3 and other oxides; for example Portland cement clinker.
[0073] The hydraulic binders according to the invention also include white cement and grey cement according to standard EN 197-1, cementitious aggregates and hydraulic lime.
[0074] According to the invention, cementitious materials based on calcium sulfoaluminate clinker as described in EP-A-1306356 "Clinker sulfoalumineux sans feret sans chaux libre, son process de préparation et son utilisation dans desliants blancs" and "Calcium sulfoaluminates cements - low energy cements, special cements" JH Sharp et al., Advances in Cement Research, 1999, 11, n.1, pp.3-13. can also be used.
[0075] Calcium aluminate cements according to EN 14647 and aluminium sulphate cements and aluminoferrate cements as described in Advances in Cement Research, 1999, 11, No. 1, Jan., 15-21. may also be used.
[0076] According to the invention, super sulfated cements (SSC) as described in EN 15743 and other cements known for use under severe conditions, such as cements according to NF P 15-317 "Cements pour travaux à la mer" (PM) and NF P15-319 "Cements pour travaux en eaux à haute teneure en sulfates" (ES) can also be used.
[0077] According to the present invention, the cementitious material composition may contain one or more than one auxiliary cementitious material advantageously selected from fly ash, metakaolin, activated clay, silica fume, basic oxygen furnace slag, natural pozzolanic material, rice husk ash, active recycled concrete fine aggregate or a mixture thereof. The auxiliary cementitious material refers to a material that enhances the strength of the cementitious material through latent hydraulic activity or pozzolanic activity.
[0078] Therefore, in the cementitious material composition according to this embodiment of the present invention, component C advantageously comprises at least 30 wt %, more advantageously 40 to 90 wt %, even more advantageously 50 to 80 wt % of granulated blast furnace slag powder.
[0079] Furthermore, the cementitious material composition according to this embodiment of the invention advantageously comprises component C in an amount of 50 to 99 wt %, advantageously 60 to 97 wt %.
[0080] The cementitious material composition according to this embodiment of the invention advantageously comprises 1.5 to 35 wt %, more advantageously 2 to 28 wt %, of the above-mentioned activation composition.
[0081] Furthermore, the cementitious material composition according to this embodiment of the invention advantageously comprises greater than 0.5% to 5% by weight, advantageously 0.7% to 3.5% by weight, of an alkali metal salt.
[0082] Optional other components
[0083] The cementitious material is advantageously enriched with one or several other components, said components being ingredients of functional additives which are particularly preferably chosen from:
[0084] Water retention agent
[0085] Water retainers have the property of retaining the mixed water before setting. The water is thus trapped in the wet preparation paste, thereby improving its cohesiveness. To some extent, the absorption of water by the support is reduced.
[0086] The water retaining agent is preferably selected from: modified cellulose, modified guar gum, modified cellulose ether and / or guar gum ether and mixtures thereof, and more preferably consists of: methyl cellulose, methyl hydroxypropyl cellulose, methyl hydroxyethyl cellulose and mixtures thereof.
[0087] Rheological agent
[0088] Possible rheological agents (also called "thickeners") are preferably selected from, more preferably selected from: clays, starch ethers, cellulose ethers and / or gums (e.g. guar xanthan gum, succinoglycan), modified polysaccharides, among which modified starch ethers are preferred, polyvinyl alcohol, polyacrylamide, clay, sepiolite, bentonite and mixtures thereof, more preferably selected from clay, bentonite, montmorillonite.
[0089] Water reducing polymer
[0090] The water reducing polymer is also called a high-efficiency water reducing agent and is selected from the group consisting of lignin sulfonate polymers, melamine sulfonate polymers, naphthalene sulfonate polymers, polycarboxylate ether polymers, polyoxyethylene phosphonates, ethylene copolymers and mixtures thereof.
[0091] Defoamer / antifoaming agent
[0092] Possible defoamers are preferably selected from, more preferably selected from: polyether polyols and mixtures thereof.
[0093] Biocides
[0094] Possible biocides are preferably selected, more preferably selected, from the group consisting of mineral oxides such as zinc oxide and mixtures thereof.
[0095] Colorants
[0096] Possible colorants are preferably selected from, more preferably selected from: TiO2, iron oxide and mixtures thereof.
[0097] Flame retardant
[0098] The latent flame retardant (or fireproofing agent) makes it possible to improve the fire resistance of the composition and / or reduce the spread rate of its flame, and the flame retardant is preferably selected from, more preferably selected from:
[0099] Air entraining agent
[0100] The air entraining agent (surfactant) is advantageously selected from, more preferably selected from, natural resins, sulfated compounds or sulfonated compounds, synthetic detergents, organic fatty acids and mixtures thereof, preferably selected from, more preferably selected from, lignin sulfonates, alkaline soaps of fatty acids and mixtures thereof, more preferably selected from sulfonate olefins, sodium lauryl sulfate and mixtures thereof.
[0101] ·Retarder
[0102] The retarder is advantageously chosen, more preferably chosen, from tartaric acid and its salts: sodium or potassium, citric acid and its salts: sodium (trisodium citrate) and mixtures thereof.
[0103] In addition, other components may be:
[0104] Plasticizer
[0105] ·fiber
[0106] Dispersible powder
[0107] Wetting agent
[0108] Polymer resin
[0109] Complexing agent
[0110] Drying shrinkage reducing agents based on polyols
[0111] The total content of these optional other components in the cementitious material composition is preferably 0.001 wt % to 10 wt % based on the total weight of the cementitious material composition.
[0112] Dry concrete composition or dry industrial mortar composition
[0113] The invention also relates to dry concrete compositions or dry industrial mortar compositions, in particular tile adhesives, coatings, masonry mortars, repair mortars, plaster mortars, technical mortars and mortars for floor coverings, comprising at least one aggregate part (sand and / or gravel) of the above-mentioned cementitious material composition. The dry concrete composition or dry industrial mortar composition may eventually contain other admixtures and admixtures.
[0114] According to the present invention, a "dry" concrete composition or a "dry" industrial mortar composition refers to a composition in powder form and easily mixed with water. In other words, the dry concrete composition or dry industrial mortar composition of the present invention may contain some moisture, but it essentially contains solid components intended to be mixed with water before its application.
[0115] In a preferred embodiment, the activating composition comprises 0.1 wt % to 5 wt %, preferably 0.25 wt % to 3.5 wt % of the total dry composition comprising cementitious material, filler, sand, gravel and other components.
[0116] This embodiment is advantageous since it enables concrete and industrial mortars comprising the activating composition according to the invention to reach early strength also at low temperatures of about 5°C.
[0117] In other words, the dry concrete composition or dry industrial mortar composition comprises the cementitious material composition according to the invention as defined herein and at least one aggregate, in particular: sand and / or gravel, and / or fillers of different particle size distribution.
[0118] Aggregates include a broad class of granular materials used in construction, including sand, gravel, crushed stone, slag (ungranulated), recycled concrete and geosynthetic aggregates. They act as reinforcements to add strength to the overall composite.
[0119] The dry concrete composition or dry industrial mortar composition may also contain fillers, for example fillers based on quartz, limestone, clay and mixtures thereof, and lightweight fillers, for example perlite, diatomaceous earth, expanded mica (vermiculite) and foamed sand and mixtures thereof.
[0120] Advantageously, the dry concrete composition or dry industrial mortar composition may comprise, in addition to aggregates, one or several ingredients, in particular functional admixtures, admixtures and fibers, which may be the same as the other optional components defined above in the detailed description of the cementitious material composition.
[0121] The total content of these optional other components in the dry concrete composition or dry industrial mortar composition is preferably 0.1 wt% to 10 wt% based on the total weight of the cementitious material composition.
[0122] Wet concrete composition or wet industrial mortar composition
[0123] The invention also relates to a wet concrete composition or a wet industrial mortar composition, in particular a tile adhesive, a coating, a masonry mortar, a repair mortar, a plaster mortar, a special mortar and a mortar for floor coverings, comprising at least one aggregate and the above-described cementitious material composition.
[0124] In a particular embodiment, the wet mortar composition is a so-called "ready-to-use" mortar. "Ready-to-use" mortar is used to assemble bricks or blocks on a building site. It is obtained by mixing all the ingredients of the composition (cementitious material, aggregates and other components) directly with water in a mixing device. It includes a retarder, allowing transportation and delayed use for up to several days, while maintaining its rheological and hardening properties.
[0125] Method for preparing wet concrete composition or wet mortar composition
[0126] The invention also relates to a method for preparing the above-mentioned wet concrete composition or wet industrial mortar composition, comprising a step of mixing at least one aggregate and a cementitious material composition with water, the cementitious material composition being prepared in situ before or during the mixing step.
[0127] In other words, the wet concrete composition or the wet industrial mortar composition can be prepared by two different methods.
[0128] In the first method, the activation composition is prepared first, and then the cementitious material composition is prepared, or the cementitious material composition is directly prepared by mixing component A, component B and component C. Then at least one aggregate is mixed with the cementitious material composition to finally obtain a dry concrete composition or a dry industrial mortar composition. Then, the dry concrete composition or the dry mortar composition is mixed with water.
[0129] In the second method, a wet concrete composition or a wet industrial mortar composition is prepared by mixing each component of each composition directly in water without previously preparing the compositions separately.
[0130] According to the present disclosure, the term "mixing" has to be understood as any form of mixing.
[0131] In a preferred embodiment, a portion of the cementitious material and at least a portion of the water are mixed together prior to mixing with the aggregate.
[0132] In a preferred embodiment, the method is carried out with a water to cementitious material composition ratio of 0.2 to 2, advantageously 0.3 to 1.8.
[0133] Hardened concrete composition or hardened industrial mortar composition
[0134] The present invention also relates to a hardened concrete composition or a hardened industrial mortar composition obtained from the above concrete composition or industrial mortar composition.
[0135] Example
[0136] Example 1: Tile Adhesive
[0137] A dry tile adhesive composition (CE1) containing ordinary Portland cement (OPC) as a cementitious material and a dry tile adhesive composition (E1) containing a mixture of Portland cement and ground granulated blast furnace slag (GGBS) as a cementitious material were prepared. The content of each dry tile adhesive composition is shown in Table 1 below.
[0138]
[0139] Table 1
[0140] Each dry tile adhesive composition has been mixed with the amount of water in Table 1 to obtain the same initial mortar viscosity (measured by Brooksfield apparatus), 530 Pa*s ± 10. Both water amounts correspond to a weight ratio of water to cementitious materials (i.e. OPC and final GGBS) of 0.7 to obtain a wet tile adhesive composition. The tile adhesive formulations have been characterized according to standard EN 12004-"Tile adhesives" and the results are shown in Table 2 below.
[0141]
[0142] Table 2
[0143] From Table 2, it can be seen that the resistance of the tile adhesive (E1) of the present invention is greater than that of the tile adhesive CE1 except after 1 day. In addition, the resistance of the tile adhesive (E1) of the present invention is higher than the requirement standard of the C2E tile adhesive.
[0144] Example 2: Masonry mortar
[0145] A dry masonry mortar composition (CE2) containing ordinary Portland cement (OPC) as a cementitious material and a dry masonry mortar composition (E2) containing a mixture of Portland cement and ground granulated blast furnace slag (GGBS) as a cementitious material were prepared. The content of each dry masonry mortar composition is shown in Table 3 below.
[0146]
[0147] Table 3
[0148] Thus, the masonry mortar (E2) according to the invention comprises 15.33% by weight of a cementitious composition according to the invention, which itself comprises 20.42% by weight of an activating composition according to the invention.
[0149] Thus, each dry masonry mortar contained 12.2 wt% hydraulic binder, either OPC only (CE2) or OPC and GGBS (E2).
[0150] Each dry masonry mortar composition has been mixed with 14% by weight of water, corresponding to a weight ratio of water to cementitious material (i.e. OPC and finally GGBS) of 1.1, to obtain a wet masonry mortar composition. The compressive strength was measured after different times; the results are shown in Table 1. Figure 1 shown.
[0151] from Figure 1 It can be seen that after 1 day, 7 days and 28 days, the compressive strength of the masonry mortar E2 according to the invention is higher than the compressive strength of CE2.
[0152] Example 3: Plastering mortar
[0153] A dry plaster mortar composition (CE3) containing ordinary Portland cement (OPC) as a cementitious material and two dry plaster mortar compositions (E3 and E4) containing a mixture of Portland cement and granulated blast furnace slag powder (GGBS) as cementitious materials were prepared. The content of each dry plaster mortar composition is shown in Table 4 below.
[0154] Embodiment (plaster mortar) CE3 (Comparative Example) E3 (the present invention) E4 (the present invention) Sand (weight %) 76.8 76.8 76.8 oPC (weight %) 10.9 7.63 5.45 GGBS (weight %) 3.27 5.45 Limestone filler (wt%) 12 8.9 8.9 Cellulose ether (wt%) 0.1 0.1 0.1 Air entraining agent (weight %) 0.1 0.1 0.1 Sodium Oleate 0.1 0.1 0.1 Calcium carbonate (weight %) 0 3 3 Sodium sulfate (repolymerization %) 0 0.05 0.05 Sodium chloride (weight %) 0 0.05 0.05
[0155] Table 4
[0156] Thus, the plaster mortar compositions of Examples E3 and E4 according to the invention both contain 15.33% to 14% by weight of the cementitious material composition according to the invention, which itself contains 22.14% by weight of the activating composition according to the invention.
[0157] Thus, each dry plaster mortar contained 10.9 wt% hydraulic binder, either OPC only (CE3) or OPC and GGBS (E3 and E4).
[0158] Each dry plaster mortar composition has been mixed with 20% by weight of water, corresponding to a weight ratio of water to cementitious material (i.e. OPC and finally GGBS) of 1.8, to obtain a wet plaster mortar composition. The compressive strength was measured after different times; the measurement results are shown in Figure 2 shown.
[0159] from Figure 2 It can be seen that after 1 day, the compressive strength of the plaster mortar E3 and the plaster mortar E4 according to the present invention is lower than the compressive strength of the plaster mortar CE3. However, the compressive strength of the plaster mortar E3 and the plaster mortar E4 is sufficient to meet the application of the plaster mortar.
[0160] However, after 7 and 28 days, the compressive strength of plaster mortars E3 and E4 according to the invention is higher than that of plaster mortar CE3.
[0161] Example 4: Low temperature hardening
[0162] A dry mortar composition (CE4) containing ordinary Portland cement (OPC) as a cementitious material and two dry mortar compositions (CE5 and E5) containing a mixture of Portland cement and ground granulated blast furnace slag (GGBS) as cementitious materials were prepared. The content of each dry mortar composition is shown in Table 5 below.
[0163] Example CE4 (Comparative Example) CE5 (Comparative Example) E5 (the present invention) Sand (weight %) 75 75 70 OPC (weight %) 25 12.5 12.5 GGBS (weight %) 0 12.5 12.5 Calcium carbonate (weight %) 0 0 4.75 Sodium sulfate (weight %) 0 0 0.125 Sodium chloride (weight %) 0 0 0.125
[0164] Table 5
[0165] Thus, the mortar (E5) according to the invention comprises 30% by weight of a cementitious composition according to the invention, which itself comprises 16.66% by weight of an activating composition according to the invention.
[0166] Thus, each dry mortar contained 25 wt% hydraulic binder, either OPC only (CE4), or OPC and GGBS (CE5 and E5).
[0167] Each dry mortar composition was mixed with water at a weight ratio of 0.5 to the cementitious material (i.e., OPC and finally GGBS) to obtain a wet mortar composition that cured at a temperature of 5°C. The compressive strength was measured after different times; the measurement results are shown in Table 1. Figure 3 shown.
[0168] from Figure 3It can be seen that after 1 day, the compressive strength of mortar E5 according to the invention is equal to that of mortar CE4 (100% OPC), and after 1 and 7 days, its compressive strength is higher than that of mortar CE5 (GGBS+OPC without the activating composition of the invention).
Claims
1. An activating composition for concrete or industrial mortar containing granulated blast furnace slag powder, comprising: A. at least 40% by weight of calcium carbonate particles and / or magnesium carbonate particles having a d80 of less than or equal to 15 μm and a d50 of less than or equal to 4 μm, and B. at least 1.5 wt. % and at most 60 wt. % of at least one alkali metal salt, wherein the alkali metal salt is selected from sodium chloride (NaCl), sodium sulfate (Na2SO4), potassium sulfate (K2SO4), potassium chloride (KCl), sodium carbonate (Na2CO3) and potassium carbonate (K2CO3) and mixtures thereof.
2. The activating composition according to claim 1, wherein the activating composition comprises at least 50% by weight of calcium carbonate particles and / or magnesium carbonate particles having a d80 of less than or equal to 15 μm and a d50 of less than or equal to 4 μm.
3. The activating composition according to claim 1 or 2, wherein the activating composition comprises 1.5 to 15% by weight of the alkali metal salt.
4. The activating composition according to claim 1 or 2, wherein the activating composition comprises 3 to 10 wt% of the alkali metal salt.
5. The activating composition according to claim 1 or 2, wherein the activating composition comprises 4 to 5 wt% of the alkali metal salt.
6. The activating composition according to claim 1 or 2, wherein the activating composition comprises 25 to 60 wt% of the alkali metal salt.
7. The activating composition according to claim 1 or 2, wherein the activating composition comprises 35 to 55 wt% of the alkali metal salt.
8. The activating composition according to claim 1 or 2, wherein the activating composition comprises 40 to 50 wt% of the alkali metal salt.
9. A cementitious material composition comprising the activating composition according to any one of claims 1 to 8 and a component C consisting of at least one hydraulic cementitious material.
10. The cementitious material composition according to claim 9, wherein component C consists only of powdered granulated blast furnace slag.
11. The cementitious material composition according to claim 9, wherein component C consists of a mixture of ground granulated blast furnace slag and at least another hydraulic cementitious material.
12. A cementitious material composition according to claim 11, wherein the at least one other hydraulic cementitious material is chosen from hydraulic cementitious materials according to standard EN 197-1 and cements based on alumina or calcium aluminate and mixtures thereof.
13. The cementitious material composition according to claim 10, wherein the cementitious material composition comprises 60 wt% to 99 wt% of ground granulated blast furnace slag.
14. The cementitious material composition according to claim 10, wherein the cementitious material composition comprises 70 wt% to 97 wt% of ground granulated blast furnace slag.
15. The cementitious material composition according to any one of claims 10 and 13-14, wherein the cementitious material composition comprises 1 wt% to 40 wt% of the activating composition according to any one of claims 1 to 8.
16. The cementitious material composition according to any one of claims 10 and 13-14, wherein the cementitious material composition comprises 3 to 30 wt% of the activating composition according to any one of claims 1 to 8.
17. The cementitious material composition according to claim 15, wherein the cementitious material composition comprises greater than 0.5 wt% to 10 wt% of the alkali metal salt.
18. The cementitious material composition according to claim 15, wherein the cementitious material composition comprises 0.7 wt% to 7 wt% of the alkali metal salt.
19. The cementitious material composition according to claim 11 or 12, wherein component C comprises at least 30 wt% of ground granulated blast furnace slag.
20. The cementitious material composition according to claim 11 or 12, wherein component C comprises 40 to 90 wt% of ground granulated blast furnace slag.
21. The cementitious material composition according to claim 11 or 12, wherein component C comprises 50 to 80 wt% of ground granulated blast furnace slag.
22. The cementitious material composition according to any one of claims 11 and 12, wherein the cementitious material composition comprises 50 wt% to 99 wt% of component C.
23. The cementitious material composition according to any one of claims 11 and 12, wherein the cementitious material composition comprises 60 wt% to 97 wt% of component C.
24. The cementitious material composition according to any one of claims 11 and 12, wherein the cementitious material composition comprises 1.5 wt% to 35 wt% of the activating composition according to any one of claims 1 to 8.
25. The cementitious material composition according to any one of claims 11 and 12, wherein the cementitious material composition comprises 2 to 28 wt% of the activating composition according to any one of claims 1 to 8.
26. The cementitious material composition according to any one of claims 11 to 12, wherein the cementitious material composition comprises greater than 0.5 wt% to 5 wt% of the alkali metal salt.
27. The cementitious material composition according to any one of claims 11 to 12, wherein the cementitious material composition comprises 0.7 wt% to 3.5 wt% of the alkali metal salt.
28. A dry concrete composition or dry industrial mortar composition comprising at least one aggregate and a cementitious material composition according to any one of claims 9 to 27.
29. The dry concrete composition or dry industrial mortar composition according to claim 28, which is a tile adhesive, a coating, a masonry mortar, a repair mortar and a plaster mortar.
30. A wet concrete composition or wet industrial mortar composition comprising at least one aggregate and a cementitious material composition according to any one of claims 9 to 27 and water.
31. The wet concrete composition or wet industrial mortar composition according to claim 30, which is a tile adhesive, a coating, a masonry mortar, a repair mortar and a plaster mortar.
32. A method for preparing a wet concrete composition or a wet industrial mortar composition according to claim 30 or 31, comprising the step of mixing at least one aggregate and a cementitious material composition according to any one of claims 9 to 27 with water, the cementitious material composition being prepared from at least some of the different components of the cementitious material composition individually and / or in premixed form before the mixing step or in situ during the mixing step.
33. The method of claim 32, wherein the ratio of water to cementitious composition is from 0.2 to 2.
34. The method of claim 32, wherein the ratio of water to cementitious composition is from 0.3 to 1.
8.
35. A hardened concrete composition or hardened industrial mortar composition obtained from the wet concrete composition or wet industrial mortar composition according to claim 30 or 31.