Elastomer composition and tire
By using a combination of styrenic elastomer and temperature-responsive resin in the tire, the problem of difficulty in adjusting the performance of the tire when the temperature changes is solved, and excellent grip performance at different temperatures is achieved.
Patent Information
- Application Number
- CN202180049155.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-11-11
- Filing Date
- 2021-11-01
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-11-01
AI Technical Summary
Existing tires have trouble adjusting their performance effectively when temperatures change, and all-season tires in particular lack responsiveness when outside temperatures and road conditions change.
Adopt an elastomer composition containing a styrenic elastomer and a temperature-responsive resin that changes hydrophilicity with temperature changes to ensure that the contact angle ratio is less than 1 at two given temperatures that differ by at least 10°C, and achieve the temperature at which tire performance is achieved Responsiveness.
By changing the contact angle, the tire's grip performance on ice and dry roads is enhanced, providing excellent comprehensive performance, including improved ice grip performance and dry grip performance.
Smart Images

Figure BDA0004045587060000101 
Figure BDA0004045587060000111 
Figure BDA0004045587060000131
Abstract
Description
Technical Field
[0001] The present invention relates to an elastomeric composition and a tire. Background Art
[0002] Tires having various desired performances have been sought (see, for example, Patent Document 1).
[0003] Citation List
[0004] Patent Literature
[0005] Patent Document 1: JP 2008-214377 A Summary of the invention
[0006] [Technical problem to be solved by the invention]
[0007] For other tires, particularly all-season tires, it is desirable to change tire performance in response to large changes in outside temperature or road conditions.
[0008] However, to date, the tire industry has not paid much attention to changing tire performance in response to temperature changes. Conventional technologies have room for improvement in changing tire performance in response to temperature changes.
[0009] The present invention is directed to solving the above problems and providing an elastomer composition and a tire capable of changing tire properties in response to temperature changes.
[0010] [Methods of solving the problem]
[0011] The present invention relates to an elastomer composition, comprising: a styrene-based elastomer; and a temperature-responsive resin whose hydrophilicity changes with temperature, wherein the elastomer composition satisfies the following relationship at two given temperatures that differ by at least 10° C.:
[0012] (Contact angle at lower temperature) / (Contact angle at higher temperature)≤0.90,
[0013] The lower temperature is less than 25°C.
[0014] [Beneficial Effects of the Invention]
[0015] The elastomer composition of the present invention comprises a styrene-based elastomer and a temperature-responsive resin whose hydrophilicity changes with temperature. In addition, the elastomer composition satisfies the following relationship at two given temperatures that differ by at least 10° C.: (contact angle at the lower temperature) / (contact angle at the higher temperature)≤0.90, the lower temperature being less than 25° C. Such an elastomer composition is capable of changing tire performance in response to temperature changes. DETAILED DESCRIPTION
[0016] The elastomer composition of the present invention comprises a styrene-based elastomer and a temperature-responsive resin whose hydrophilicity changes with temperature. In addition, the elastomer composition satisfies the following relationship at two given temperatures that differ by at least 10° C.: (contact angle at the lower temperature) / (contact angle at the higher temperature)≤0.90, wherein the lower temperature is less than 25° C. Therefore, the elastomer composition is capable of changing tire performance in response to temperature changes.
[0017] The elastomer composition provides the above-mentioned effects. The reason for such beneficial effects is not entirely clear but is considered to be as follows.
[0018] The relationship: (contact angle at lower temperature) / (contact angle at higher temperature)≤0.90 means that the contact angle of the elastomeric composition at low temperature is smaller than that at high temperature (i.e., more hydrophilic at low temperature than at high temperature), and the contact angle of the elastomeric composition at high temperature is larger than that at low temperature (i.e., more hydrophobic at high temperature than at low temperature). Therefore, the elastomeric composition changes its hydrophilicity as the temperature changes, and thus can change tire performance in response to the temperature change.
[0019] The elastomer composition having such properties can be achieved by including a temperature-responsive resin that changes its hydrophilicity with temperature. Specifically, since the temperature-responsive resin changes its hydrophilicity with temperature, the resin can be added to provide an elastomer composition having the above properties.
[0020] Here, an elastomer composition that does not include a temperature-responsive resin but includes a temperature-responsive polymer as described later cannot reversibly change tire performance in response to temperature changes because the compatibility of the temperature-responsive polymer with the elastomer is low and also because the temperature-responsive polymer may be dissolved in water or otherwise flow out of the elastomer composition, for example, on rainy days. Conversely, an elastomer composition containing a temperature-responsive resin can reversibly change tire performance in response to temperature changes because the compatibility of the temperature-responsive resin with the elastomer is relatively high and also because the temperature-responsive resin does not dissolve in water or otherwise flow out of the elastomer composition.
[0021] Therefore, the present invention solves the problem (purpose) of changing tire performance in response to temperature changes by formulating an elastomeric composition comprising a styrene elastomer and a temperature-responsive resin that changes its hydrophilicity with temperature changes, and that satisfies the above-mentioned contact angle parameters. In other words, the parameter does not define the problem (purpose), and the problem herein is to change tire performance in response to temperature changes. In order to solve this problem, the elastomeric composition is formulated to comprise a styrene elastomer and a temperature-responsive resin that changes its hydrophilicity with temperature changes, and that satisfies the above-mentioned contact angle parameters. Therefore, satisfying the above-mentioned contact angle parameters is a necessary condition.
[0022] In particular, when the temperature responsive resin shows a lower critical solution temperature (LCST) in water, the temperature responsive resin shows hydrophobicity at a temperature higher than the LCST and shows hydrophilicity at a temperature lower than the LCST.
[0023] Therefore, at high temperatures, for example, at 60° C., the temperature responsive resin is hydrophobic, and thus the compatibility with the styrene-based elastomer is improved. Therefore, good dry grip performance can be obtained.
[0024] On the other hand, at low temperatures, such as on ice, the temperature responsive resin is hydrophilic and therefore incompatible with the styrene-based elastomer; furthermore, the presence of the hydrophilic temperature responsive resin causes the elastomer surface to become hydrophilic.
[0025] The incompatibility reduces the glass transition temperature and complex elastic modulus, thus improving the grip performance on ice.
[0026] Furthermore, since the surface of the elastomer is hydrophilic (has a small contact angle), water in a water film existing on an icy road surface (also referred to as an ice road surface) can be appropriately removed, thereby improving the grip performance on ice.
[0027] In addition, at high temperatures, such as 60°C, the temperature responsive resin exhibits hydrophobicity and attracts the plasticizer to its surroundings, while at low temperatures, such as 0°C, the temperature responsive resin exhibits hydrophilicity and can easily release the plasticizer into the matrix elastomer, so that the concentration of the plasticizer in the matrix elastomer is increased, and the complex elastic modulus of the elastomer composition is reduced and the grip performance on ice is improved.
[0028] As described above, when exposed to low temperatures on icy roads, the elastomer composition shows a high water removal rate due to a small contact angle, the glass transition temperature and the complex elastic modulus of the elastomer composition decrease due to incompatibility (phase separation), and the complex elastic modulus of the elastomer composition decreases due to the release of the plasticizer into the matrix elastomer, thereby resulting in improved grip performance on ice.
[0029] Therefore, the elastomer composition provides good grip performance on ice and also has excellent comprehensive performance in terms of grip performance on ice and dry grip performance.
[0030] The elastomeric composition satisfies the following relationship at two given temperatures that differ by at least 10°C:
[0031] (Contact angle at lower temperature) / (Contact angle at higher temperature)≤0.90, and the lower temperature is less than 25°C.
[0032] Preferably, the elastomeric composition reversibly satisfies the above relationship at two different temperatures differing by at least 10° C. Herein, the phrase “reversibly satisfies the above relationship” means that the temperature dependence of the contact angle satisfies the above relationship at two different temperatures differing by at least 10° C. even when it is subjected to repeated temperature changes or is in contact with water.
[0033] Furthermore, herein, the contact angle is measured as described in the Examples.
[0034] Herein, the contact angle of the elastomer composition refers to the contact angle of the elastomer composition after vulcanization (crosslinking).
[0035] As long as the lower temperature is less than 25°C, the two given temperatures that differ by at least 10°C are not limited. The two temperatures may each be any temperature within the tire use temperature range, preferably any temperature within the range of -80°C to 80°C. The lower limit of the temperature range is more preferably -50°C or higher, more preferably -20°C or higher. The upper limit of the temperature range is more preferably 80°C or lower, more preferably 60°C or lower.
[0036] For example, the two temperatures that differ by at least 10°C may be 5°C and 60°C.
[0037] The lower temperature is less than 25°C, preferably 15°C or less, more preferably 10°C or less, another preferably 0°C or more, more preferably 1°C or more, and still more preferably 2°C or more.
[0038] The contact angle used herein generally refers to the contact angle of water, but may be the contact angle of an antifreeze liquid when measured at a temperature below 0°C.
[0039] Herein, the term "antifreeze liquid" refers to a liquid composed of methanol and water, which can be prepared by mixing water with methanol in an amount 9 times the volume of water at 25°C for 30 minutes.
[0040] The ratio of (contact angle at lower temperature) / (contact angle at higher temperature) is 0.90 or less, preferably 0.85 or less, more preferably 0.80 or less, still more preferably 0.77 or less, particularly preferably 0.75 or less, most preferably 0.70 or less, even most preferably 0.68 or less, further most preferably 0.65 or less, particularly most preferably 0.64 or less, and further most preferably 0.62 or less. The lower limit is not limited, but is preferably 0.30 or more, more preferably 0.40 or more, still more preferably 0.50 or more, and particularly preferably 0.60 or more. When the ratio is within the above range, the beneficial effect tends to be more appropriately achieved.
[0041] The contact angle (°) at a relatively low temperature is preferably 20 or more, more preferably 30 or more, still more preferably 40 or more, particularly preferably 50 or more, further preferably 80 or less, more preferably 75 or less, still more preferably 70 or less, particularly preferably 65 or less, and most preferably 60 or less. When the contact angle is within the above range, the beneficial effects tend to be more appropriately achieved.
[0042] Next, manufacturing guidelines for meeting contact angle parameters and contact angles at lower temperatures are described.
[0043] The relationship: (contact angle at lower temperature) / (contact angle at higher temperature)≤0.90 means that the contact angle of the elastomer composition at low temperature is smaller than that at high temperature (i.e., more hydrophilic at low temperature than at high temperature), and the contact angle of the elastomer composition at high temperature is larger than that at low temperature (i.e., more hydrophobic at high temperature than at low temperature). An elastomer composition having such characteristics can be achieved by including a temperature-responsive resin that changes its hydrophilicity with temperature changes.
[0044] The contact angle at a lower temperature being within the above range means that the elastomer composition has a smaller contact angle (ie, more hydrophilic). An elastomer composition having such characteristics can be achieved by including a temperature-responsive resin that changes its hydrophilicity with temperature.
[0045] Specifically, rubber having such characteristics can be produced by using a temperature-responsive resin that shows a lower critical solution temperature (LCST) in water.
[0046] Here, the contact angle (absolute value) can be adjusted by the type and amount of chemicals (especially rubber components, fillers, plasticizers, silane coupling agents) added to the composition. For example, when the amount of hydrophilic material (such as silicon dioxide) increases, the contact angle tends to decrease, and when the amount of hydrophilic material decreases, the contact angle tends to increase. In addition, when the amount of hydrophobic material increases, the contact angle tends to increase, and when the amount of hydrophobic material decreases, the contact angle tends to decrease.
[0047] Chemicals that can be used in the elastomeric composition are described below.
[0048] The elastomer composition contains a styrene-based elastomer.
[0049] Styrene elastomer can be any elastomer with a unit based on styrene.Example includes: styrene-butadiene rubber (SBR), styrene-isoprene-butadiene rubber (SIBR), styrene-based thermoplastic elastomer, styrene-isobutylene-styrene block copolymer (SIBS), styrene-isoprene-styrene block copolymer (SIS), styrene-isobutylene block copolymer (SIB), styrene-butadiene-styrene block copolymer (SBS), styrene-ethylene / butylene-styrene block copolymer (SEBS), styrene-ethylene / propylene-styrene block copolymer (SEPS), styrene-ethylene / ethylene / propylene-styrene block copolymer (SEEPS) and styrene-butadiene / butylene-styrene block copolymer (SBBS). These can be used alone or in combination with more than 2 kinds. Among these, SBR is preferred because it can more appropriately achieve beneficial effects.
[0050] Here, the elastomer component (preferably rubber component) preferably refers to a polymer (rubber) having a weight average molecular weight (Mw) of 200,000 or more, more preferably 350,000 or more. The upper limit of Mw is not limited, but is preferably 4,000,000 or less, more preferably 3,000,000 or less.
[0051] Herein, Mw and number average molecular weight (Mn) can be measured by gel permeation chromatography (GPC) calibrated with polystyrene standards (GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKGEL SUPERMULTIPORE HZ-M manufactured by Tosoh Corporation).
[0052] The amount of the diene rubber is preferably 20% by mass or more, more preferably 50% by mass or more, still more preferably 70% by mass or more, particularly preferably 80% by mass or more, most preferably 90% by mass or more, and may be 100% by mass, based on 100% by mass of the elastomer component content (preferably, based on 100% by mass of the rubber component content). When the amount is within the above range, the beneficial effects tend to be better achieved.
[0053] The elastomeric component may include an unmodified polymer or a modified polymer.
[0054] The modified polymer may be any polymer (preferably any diene rubber) having a functional group that interacts with a filler such as silica. Examples include: a chain end modified polymer obtained by modifying at least one chain end of a polymer with a compound (modifier) having the above functional group (i.e., a chain end modified polymer terminated with the above functional group); a main chain modified polymer having the above functional group in the main chain; a main chain and chain end modified polymer having the above functional group in the main chain and the chain end (e.g., a main chain and chain end modified polymer in which the main chain has the above functional group and at least one chain end is modified by the above modifier); and a chain end modified polymer in which a hydroxyl group or epoxy group is introduced by modification (coupling) with a multifunctional compound having two or more epoxy groups in the molecule.
[0055] The examples of the above functional groups include amino, amide, silyl, alkoxysilyl, isocyanate, imino, imidazole, urea, ether, carbonyl, oxycarbonyl, mercapto, sulfide group, disulfide group, sulfonyl, sulfinyl, thiocarbonyl, ammonium, imido, hydrazine, azo, diazo, carboxyl, nitrile, pyridyl, alkoxy, hydroxyl, oxy and epoxy. Here, these functional groups can be substituted. Among these, preferably amino (preferably amino with C1-C6 alkyl substituted hydrogen atom), alkoxy (preferably C1-C6 alkoxy) and alkoxysilyl (preferably C1-C6 alkoxysilyl).
[0056] Any SBR may be used. Examples include emulsion-polymerized styrene-butadiene rubber (E-SBR) and solution-polymerized styrene-butadiene rubber (S-SBR). These may be used alone or in combination of two or more.
[0057] The styrene content of SBR is preferably 5% by mass or more, more preferably 10% by mass or more, further preferably 15% by mass or more, and particularly preferably 20% by mass or more. In addition, the styrene content is preferably 60% by mass or less, more preferably 50% by mass or less, more preferably 40% by mass or less, and particularly preferably 30% by mass or less. When the styrene content is within the above range, the beneficial effect tends to be better achieved.
[0058] In this article, the styrene content of SBR can be 1 H-NMR analysis.
[0059] As the SBR, SBR products manufactured or sold by Sumitomo Chemical Co., Ltd., JSR Corporation, Asahi Kasei Corporation, Nippon Zeon Co., Ltd., and the like can be used.
[0060] The SBR may be unmodified SBR or modified SBR. Examples of the modified SBR include those into which the functional groups listed for the modified polymer have been introduced.
[0061] The amount of the styrene elastomer (preferably SBR) is preferably 10% by mass or more, more preferably 20% by mass or more, still more preferably 40% by mass or more, and particularly preferably 50% by mass or more, based on 100% by mass of the elastomer component content (preferably, based on 100% by mass of the rubber component content). The amount may be 100% by mass, but is preferably 90% by mass or less, more preferably 70% by mass or less. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0062] The elastomers that can be used other than styrene elastomers are not limited. Examples include: diene rubbers commonly used as rubber components in tire compositions, such as isoprene rubber, polybutadiene rubber (BR), ethylene-propylene-diene rubber (EPDM), chloroprene rubber (CR) and acrylonitrile-butadiene rubber (NBR); acrylic (ester) rubbers, such as butyl acrylate rubber, ethyl acrylate rubber and octyl acrylate rubber; nitrile rubber, isobutylene rubber, methyl methacrylate-butyl acrylate block copolymer, ethylene-propylene copolymer (EPR), chlorosulfonated polyethylene, silicone rubber (grindable type, room temperature vulcanization type), butyl rubber, fluororubber, olefin thermoplastic elastomer, vinyl chloride thermoplastic elastomer, polyurethane thermoplastic elastomer, polyamide thermoplastic elastomer, polyester thermoplastic elastomer and fluorine thermoplastic elastomer. These can be used alone or in combination of two or more. Among these, diene rubbers are preferred, and BR is more preferred.
[0063] Any BR can be used. Examples include high cis BR with a high cis content, BR containing syndiotactic polybutadiene crystals, and BR synthesized using a rare earth catalyst (rare earth-catalyzed BR). These can be used alone or in combination of two or more. In particular, in order to improve wear resistance, a high cis BR having a cis content of 90% by mass or more is preferred. Here, the cis content can be measured by infrared absorption spectroscopy.
[0064] Furthermore, BR may be unmodified BR or modified BR. Examples of modified BR include those into which the functional groups listed for the modified polymer have been introduced.
[0065] Examples of commercially available BR include those available from Ube Industries, Ltd., JSR Corporation, Asahi Kasei Corporation, Nippon Zeon Corporation, and the like.
[0066] The amount of BR is preferably 5% by mass or more, more preferably 8% by mass or more, still more preferably 10% by mass or more, particularly preferably 30% by mass or more, and further preferably 80% by mass or less, and more preferably 60% by mass or less, based on 100% by mass of the elastomer component content (preferably, based on 100% by mass of the rubber component content). When the amount is within the above range, the beneficial effects tend to be better achieved.
[0067] Examples of isoprene-based rubbers include natural rubber (NR), polyisoprene rubber (IR), modified NR, modified NR, and modified IR. Examples of NR include those commonly used in the tire industry, such as SIR20, RSS#3, and TSR20. Any IR can be used, including, for example, those commonly used in the tire industry, such as IR2200. Examples of modified NR include deproteinized natural rubber (DPNR) and high-purity natural rubber (UPNR). Examples of modified NR include epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), and grafted natural rubber. Examples of modified IR include epoxidized polyisoprene rubber, hydrogenated polyisoprene rubber, and grafted polyisoprene rubber. These can be used alone or in combination of two or more. Among these, NR is preferred.
[0068] The elastomeric composition includes a temperature responsive resin that changes its hydrophilicity with temperature.
[0069] The temperature-responsive resin that changes its hydrophilicity with temperature is not limited as long as it changes its hydrophilicity with temperature. Any temperature-responsive resin containing a group ("A" described later) that changes its hydrophilicity with temperature can be used.
[0070] Herein, the term "resin" refers to an organic compound that is solid at a temperature of 0° C. or higher, or specifically, an organic compound a portion of which does not follow the shape of a container different from that of the organic compound (even when the organic compound is left to stand in the container for 1 minute). In addition, the term "resin" does not include the above-mentioned styrene-based elastomer.
[0071] The temperature-responsive resin is preferably a compound including "A" and "B" bonded to each other. Here, "A" contains a group that changes its hydrophilicity with temperature changes, and "B" includes at least one selected from terpene resins, rosin resins, styrene resins, C5 resins, C9 resins, C5 / C9 resins, coumarone resins, indene resins, and olefin resins. Since "A" is bonded to "B", the dissolution of "A" (a group that changes its hydrophilicity with temperature changes) in water can be suppressed. Therefore, it can reversibly change tire performance in response to temperature changes.
[0072] First, "A" will be described.
[0073] Herein, the group that changes its hydrophilicity with temperature may be any group that changes its hydrophilicity with temperature, and preferably is a group that reversibly changes its hydrophilicity with temperature.
[0074] The group that reversibly changes its hydrophilicity with temperature changes may be a temperature-responsive polymer (temperature-responsive polymer group). In other words, "A" comprising a group that changes its hydrophilicity with temperature changes may refer to, for example, "A" comprising a group formed by a temperature-responsive polymer. Examples of such "A" include: "A" grafted with a temperature-responsive polymer, "A" comprising a temperature-responsive polymer unit in the main chain, and "A" comprising a temperature-responsive polymer block in the main chain. These may be used alone or in combination of two or more. In particular, preferably, "A" is a temperature-responsive polymer (ie, "A" comprises a temperature-responsive polymer).
[0075] The term "temperature-responsive polymer" refers to a material that undergoes a reversible change in the conformation of a polymer chain associated with hydration and dehydration in response to temperature changes in water, thereby reversibly changing its hydrophilicity and hydrophobicity with temperature changes. It is known that this reversible change is caused by a molecular structure containing a hydrophilic group capable of forming hydrogen bonds and a hydrophobic group that is difficult to be compatible with water.
[0076] Then, the present inventors found that the temperature-responsive polymer shows reversible changes in hydrophilicity and hydrophobicity with temperature changes not only in water but also in a composition containing a resin and / or an elastomer.
[0077] Known temperature-responsive polymers include polymers that exhibit a lower critical solution temperature (LCST, also called lower critical consolute temperature or lower critical dissolution temperature) in water and polymers that exhibit an upper critical solution temperature (UCST (Upper Critical Solution Temperature, also called upper critical consolute temperature or upper critical dissolution temperature) in water. These can be used alone or in combination of two or more.
[0078] At temperatures above the LCST limit, the polymer chains that exhibit the LCST become hydrophobic due to the enhanced hydrophobic interaction within or between molecules, causing the polymer chains to aggregate. On the other hand, at temperatures below the LCST, the polymer becomes hydrophilic due to the hydration of the polymer chains by binding to water molecules. Therefore, the polymer exhibits a reversible phase transition behavior near the LCST.
[0079] Conversely, a polymer showing a UCST becomes hydrophobic and insoluble at a temperature below the UCST, and becomes hydrophilic and soluble at a temperature above the UCST. Therefore, the polymer shows a reversible phase transition behavior near the UCST. The reason for showing this UCST-type behavior is believed to be that the intermolecular force can be driven by hydrogen bonds between side chains having multiple amide groups.
[0080] When the group that reversibly changes its hydrophilicity with temperature change is a polymer that exhibits LCST, the temperature change may cause the polymer to become incompatible with other ingredients in the composition so that the glass transition temperature may be changed. Thus, it may change tire performance (e.g., dry grip performance, ice grip performance) in response to temperature change.
[0081] In "A", the group whose hydrophilicity changes reversibly with temperature is preferably a polymer showing LCST. In other words, the group whose hydrophilicity changes with temperature is preferably a group showing a lower critical solution temperature in water.
[0082] Herein, a group showing a lower critical solution temperature (LCST) in water refers to a group present in "A" or in a temperature responsive resin, which shows a lower critical solution temperature in water when the group is disconnected from "A" or from the temperature responsive resin and the disconnected group (polymer) is introduced into water.
[0083] Likewise, herein, a group showing an upper critical solution temperature (UCST) in water refers to a group present in "A" or in a temperature responsive resin, which shows an upper critical solution temperature in water when the group is disconnected from "A" or from the temperature responsive resin and the disconnected group (polymer) is introduced into water.
[0084] The group (polymer) showing LCST is described below.
[0085] The group (polymer) showing LCST may include a single group (polymer) or a combination of two or more groups (polymers).
[0086] The group (polymer) showing LCST may be any group (polymer) showing LCST. Preferred is poly(N-substituted (meth)acrylamide), among which the group represented by the following formula (I) is preferred:
[0087]
Chemistry 1
[0088]
[0089] Wherein, n represents an integer from 1 to 1000; R 1 , R 2and R 3 Each independently represents a hydrogen atom or a hydrocarbon group, provided that R 1 or R 2 At least one of them is not a hydrogen atom, and R 1 and R 2 Can form a ring structure together.
[0090] Preferably, n is 3 or more, more preferably 5 or more, still more preferably 10 or more, particularly preferably 20 or more, further preferably 500 or less, more preferably 300 or less, still more preferably 150 or less, particularly preferably 80 or less, most preferably 40 or less, and further most preferably 30 or less. When n is within the above range, the beneficial effects tend to be better achieved.
[0091] For R 1 and R 2 The hydrocarbon group may have any number of carbon atoms. The number of carbon atoms is preferably 1 or more, more preferably 2 or more, and further preferably 3 or more, but is preferably 20 or less, more preferably 18 or less, further preferably 14 or less, particularly preferably 10 or less, most preferably 6 or less, and further most preferably 4 or less. When the number of carbon atoms is within the above range, the beneficial effects tend to be better achieved.
[0092] For R 1 and R 2 Examples of the hydrocarbon group include: alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, neopentyl, isopentyl and n-hexyl; cycloalkyl groups such as cyclohexyl; and aryl groups such as methylphenyl and ethylphenyl. Among them, alkyl groups and cycloalkyl groups are preferred, and alkyl groups are more preferred.
[0093] By R 1 and R 2 The number of carbon atoms in the formed ring structure is preferably 3 or more, more preferably 4 or more, and is also preferably 7 or less, more preferably 5 or less. When the number of carbon atoms is within the above range, the advantageous effects tend to be better achieved.
[0094] For R 1 and R 2 The hydrocarbon group may be branched or unbranched, preferably branched.
[0095] Preferably, R 1 and R 2 are each a hydrogen atom, an alkyl group (particularly a branched alkyl group) or a cycloalkyl group, or R 1 and R 2 More preferably, R 1 and R 2It is any combination shown in Table 1, and a combination of a hydrogen atom and an alkyl group (particularly a branched alkyl group) is more preferred, and a combination of a hydrogen atom and a propyl group (particularly an isopropyl group) is particularly preferred.
[0096] [Table 1]
[0097] Table 1: Chemical structures and LCST of preferred poly(N-substituted acrylamide)
[0098]
[0099] For R 3 The hydrocarbon group may have any number of carbon atoms. The number of carbon atoms is preferably 1 or more, and is also preferably 5 or less, more preferably 3 or less, still more preferably 2 or less, and particularly preferably 1. When the number of carbon atoms is within the above range, the beneficial effects tend to be better achieved.
[0100] For R 3 Examples of the hydrocarbon group include 1 and R 2 Among them, alkyl is preferred.
[0101] For R 3 The hydrocarbyl group may be branched or unbranched.
[0102] R 3 It is preferably a hydrogen atom or an alkyl group, and more preferably a hydrogen atom.
[0103] Examples of the group represented by formula (I) include: poly(N-alkylacrylamide) polymers such as poly(N-isopropylacrylamide), poly(N-ethylacrylamide), poly(N-n-propylacrylamide), poly(N-ethyl, N-methylacrylamide), poly(N,N-diethylacrylamide), poly(N-isopropyl, N-methylacrylamide), poly(N-cyclopropylacrylamide), poly(N-acryloylpyrrolidine) and poly(N-acryloylpiperidine); and
[0104] Poly(N-alkylmethacrylamide) polymers, such as poly(N-isopropylmethacrylamide), poly(N-ethylmethacrylamide), poly(N-n-propylmethacrylamide), poly(N-ethyl, N-methylmethacrylamide), poly(N,N-diethylmethacrylamide), poly(N-isopropyl, N-methylmethacrylamide), poly(N-cyclopropylmethacrylamide), poly(N-methacryloylpyrrolidine) and poly(N-methacryloylpiperidine). These may be used alone or in combination of two or more. Among them, poly(N-isopropylacrylamide) and poly(N,N-diethylacrylamide) are preferred, and poly(N-isopropylacrylamide) (PNIPAM) is more preferred.
[0105] PNIPAM is a thermosensitive material that exhibits large changes in surface energy in response to small changes in temperature. See, for example, N. Mori et al., Temperature Induced Changes in the Surface Wettability of SBR+PNIPA Films, 292, Macromol. Mater. Eng. 917, 917-22 (2007).
[0106] PNIPAM has a hydrophobic isopropyl group on the side chain and a hydrophilic amide bond at the base of the isopropyl group.
[0107] PNIPAM becomes soluble in water at temperatures below 32°C, where the hydrophilic amide bond moieties form hydrogen bonds with water molecules. On the other hand, at temperatures above 32°C, the hydrogen bonds are broken due to the violent molecular thermal motion, and the hydrophobic interactions within or between molecules are enhanced due to the hydrophobic isopropyl moieties on the side chains, resulting in aggregation of the polymer chains, and thus PNIPAM becomes insoluble in water.
[0108] As mentioned above, the LCST (ie, the transition temperature from the hydrophilic state to the hydrophobic state) of PNIPAM is about 32°C.
[0109] The contact angle of a water drop placed on a PNIPAM polymer film changes dramatically above and below the LCST temperature. For example, the contact angle of a water drop placed on a PINPAM film is about 60° (hydrophilic) below 32°C, and then exceeds about 93° (hydrophobic) when it is heated to a temperature above 32°C.
[0110] Temperature-responsive resins containing PNIPAM groups (PNIPAM groups dramatically change their surface properties from hydrophilic to hydrophobic at about 32°C) can change tire performance in response to temperature changes.
[0111] Although the group (polymer) showing LCST may be suitably the group as described above, it is also preferably a poly(alkyl vinyl ether), more preferably a group represented by the following formula (A). In this case, the beneficial effects tend to be more appropriately achieved. Such groups may be used alone or in combination of two or more.
[0112]
Chemistry 2
[0113]
[0114] In the formula, m represents an integer from 1 to 1000, R 4 , R 5 and R 6Each independently represents a hydrogen atom or a hydrocarbon group.
[0115] m is preferably 3 or more, more preferably 5 or more, further preferably 10 or more, particularly preferably 20 or more, and is also preferably 500 or less, more preferably 300 or less, further preferably 150 or less, particularly preferably 80 or less, most preferably 40 or less, and further most preferably 30 or less. When m is within the above range, the beneficial effects tend to be better achieved.
[0116] For R 4 The hydrocarbon group may have any number of carbon atoms. The number of carbon atoms is preferably 1 or more, more preferably 2 or more, further preferably 20 or less, more preferably 18 or less, still more preferably 14 or less, particularly preferably 10 or less, most preferably 6 or less, and further most preferably 4 or less. When the number of carbon atoms is within the above range, the beneficial effects tend to be better achieved.
[0117] For R 5 and R 6 The hydrocarbon group may have any number of carbon atoms. The number of carbon atoms is preferably 1 or more, and is also preferably 5 or less, more preferably 3 or less, still more preferably 2 or less, and particularly preferably 1. When the number of carbon atoms is within the above range, the beneficial effects tend to be better achieved.
[0118] For R 4 , R 5 and R 6 Examples of the hydrocarbon group include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, neopentyl, isopentyl and n-hexyl, cycloalkyl groups such as cyclohexyl and aryl groups such as methylphenyl and ethylphenyl. Among them, alkyl groups and cycloalkyl groups are preferred, and alkyl groups are more preferred.
[0119] Preferably, R 4 is an alkyl group, R 5 and R 6 is a hydrogen atom. More preferably, R 4 is ethyl, R 5 and R 6 It's a hydrogen atom.
[0120] Examples of the group represented by formula (A) include poly(methyl vinyl ether), poly(ethyl vinyl ether), poly(propyl vinyl ether), poly(butyl vinyl ether), poly(pentenyl ether), poly(hexyl vinyl ether), poly(heptyl vinyl ether) and poly(octyl ether). These may be used alone or in combination of two or more. Among them, poly(ethyl vinyl ether) (PEVE) is preferred. In-depth studies by the present inventors have shown that the LCST of PEVE is -20 to +5°C.
[0121] Although the group (polymer) showing LCST may be suitably a group as described above, it is also preferably a group represented by the following formula (B). In this case, a beneficial effect tends to be more appropriately achieved. Such a group may be used alone or in combination of two or more.
[0122]
Chemistry 3
[0123]
[0124] In the formula, m represents an integer from 1 to 1000, R 7 , R 8 and R 9 Each independently represents a hydrogen atom or a hydrocarbon group.
[0125] Preferably, m is 3 or more, more preferably 5 or more, further preferably 10 or more, particularly preferably 20 or more, further preferably 500 or less, more preferably 300 or less, further preferably 150 or less, particularly preferably 80 or less, most preferably 40 or less, and further most preferably 30 or less. When m is within the above range, the beneficial effects tend to be better achieved.
[0126] For R 7 The hydrocarbon group may have any number of carbon atoms. The number of carbon atoms is preferably 1 or more, more preferably 2 or more, further preferably 20 or less, more preferably 18 or less, still more preferably 14 or less, particularly preferably 10 or less, most preferably 6 or less, and further most preferably 4 or less. When the number of carbon atoms is within the above range, the beneficial effects tend to be better achieved.
[0127] For R 8 and R 9 The hydrocarbon group may have any number of carbon atoms. The number of carbon atoms is preferably 1 or more, and is also preferably 5 or less, more preferably 3 or less, still more preferably 2 or less, and particularly preferably 1. When the number of carbon atoms is within the above range, the beneficial effects tend to be better achieved.
[0128] For R 7 , R 8 and R 9 Examples of the hydrocarbon group include: alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, neopentyl, isopentyl and n-hexyl; cycloalkyl groups such as cyclohexyl; and aryl groups such as methylphenyl and ethylphenyl. Among them, alkyl groups and cycloalkyl groups are preferred, and alkyl groups are more preferred.
[0129] Preferably, R 7 is an alkyl group, R 8 and R 9 is a hydrogen atom. More preferably, R 7 is n-propyl or isopropyl, R8 and R 9 It's a hydrogen atom.
[0130] Examples of the group represented by formula (B) include poly(isopropylvinyl acrylamide) (PNIPVM, R 7 is isopropyl, R 8 and R 9 is a hydrogen atom), poly(n-propylvinyl acrylamide) (PNNPAM, R 7 is n-propyl, R 8 and R 9 is a hydrogen atom), poly(n-butyl vinyl acrylamide) (R 7 is n-butyl, R 8 and R 9 is a hydrogen atom), poly(tert-butyl vinyl acrylamide) (R 7 is tert-butyl, R 8 and R 9 is a hydrogen atom), poly(sec-butyl vinyl acrylamide) (R 7 is sec-butyl, R 8 and R 9 is a hydrogen atom), poly(methyl vinyl acrylamide) (R 7 is methyl, R 8 and R 9 is a hydrogen atom), poly(ethyl vinyl acrylamide) (R 7 is ethyl, R 8 and R 9 is a hydrogen atom), poly(n-pentyl vinyl acrylamide) (R 7 is n-pentyl, R 8 and R 9 is a hydrogen atom) and poly(isoamyl vinyl acrylamide) (R 7 is isopentyl, R 8 and R 9 is a hydrogen atom). These can be used alone or in combination of two or more. Among them, PNIPVM, PNNPAM, poly(n-butyl vinyl acrylamide), poly(tert-butyl vinyl acrylamide) are preferred, and PNIPVM or PNNPAM is more preferred. In-depth studies by the present inventors have shown that the LCST of PNIPVM is 39°C, and the LCST of PNNPAM is 32°C.
[0131] In addition to the group represented by formula (I), the group represented by formula (A) and the group represented by formula (B), examples of the group (polymer) showing LCST include: poly(N-vinyl-caprolactam) represented by the following formula (II) (LSCT: about 31°C), poly(2-alkyl-2-oxazoline) represented by the following formula (III) (LSCT: about 62°C when R is ethyl, about 36°C when R is isopropyl, and about 25°C when R is n-propyl), alkyl-substituted cellulose (e.g., methyl cellulose represented by the following formula (IV) (LSCT: about 50°C), hydroxypropyl cellulose, hydroxyethyl methyl cellulose and hydroxypropyl methyl cellulose), poly(N-ethoxyethyl acrylamide) (LSCT: about 35°C), poly(N-ethoxyethyl methacrylamide) )(LSCT: about 45°C), poly(N-tetrahydrofurfuryl acrylamide) (LSCT: about 28°C), poly(N-tetrahydrofurfuryl methacrylamide) (LSCT: about 35°C), polyvinyl methyl ether, poly[2-(dimethylamino)ethyl methacrylate], poly(3-ethyl-N-vinyl-2-pyrrolidone), hydroxybutyl chitosan, polyoxyethylene (20) sorbitan monostearate, polyoxyethylene (20) sorbitan monolaurate, polyoxyethylene (20) sorbitan monooleate, poly(ethylene glycol) methacrylate containing 2 to 6 ethylene glycol units, polyethylene glycol-co-polypropylene glycol (preferably those containing 2 to 8 ethylene glycol units and 2 to 8 polypropylene units, more preferably a compound represented by formula (A)), ethoxylated iso-C 13 H 27 -alcohol (preferably having an ethoxylation degree of 4 to 8), polyethylene glycol containing 4 to 50 (preferably 4 to 20) ethylene glycol units, polypropylene glycol containing 4 to 30 (preferably 4 to 15) propylene glycol units, monomethyl, dimethyl, monoethyl or diethyl ether of polyethylene glycol containing 4 to 50 (preferably 4 to 20) ethylene glycol units, and monomethyl, dimethyl, monoethyl or diethyl ether of polypropylene glycol containing 4 to 50 (preferably 4 to 20) propylene glycol units. These may be used alone or in combination of two or more.
[0132] (A)HO-[-CH2-CH2-O] x -[-CH(CH3)-CH2-O] y -[-CH2-CH2-O] z -H
[0133] In the formula, y is 3-10, and x and z are each 1-8, provided that y+x+z is 5-18.
[0134]
Chemistry 4
[0135]
[0136] In formulae (II) to (IV), n is as defined in formula (I). In formula (III), R is an alkyl group selected from n-propyl, isopropyl or ethyl.
[0137] Examples of groups (polymers) showing LCST other than the above groups include copolymers of N-isopropylacrylamide and butyl acrylate, block copolymers of N-isopropylacrylamide and polyethylene oxide, copolymers of N-isopropylacrylamide and fluorine-containing monomers, polymer composites of poly-N-acetylacrylamide and polyethylene oxide, polymer composites of poly-N-acetylacrylamide and polyacrylamide, polymer composites of copolymers of N-acetylacrylamide and acrylamide and polyacrylamide, copolymers of N-acryloylglycinamide and N-acetylacrylamide, copolymers of 2-methoxyethyl acrylate and N,N-dimethylacrylamide, and copolymers of the compound represented by the following formula 1 and N,N-dimethylacrylamide. copolymers of N,N-diethylacrylamide, poly(sulfopropyl-N,N-dimethyl(acrylamidepropyl)ammonium), copolymers of N,N-diethylacrylamide and maleic anhydride, copolymers of N,N-diethylacrylamide and dimethyl fumarate, copolymers of N,N-diethylacrylamide and hydroxyethyl methacrylate, copolymers of N,N-diethylacrylamide and butadiene, polymer composites of polyvinyl alcohol or polyvinyl alcohol hydrolyzate and polyacrylamide, N-acryloyl asparagine polymers, N-acryloyl glutamine polymers, N-methacryloyl asparagine polymers, copolymers of N-acryloyl glycinamide and biotin methacrylamide derivatives, copolymers of N-acryloyl glycinamide and N-acryloyl asparagine, Biotin-immobilized temperature-responsive magnetic microparticles (microparticles produced by the reaction of N-acryloylglycinamide, methacrylated magnetic microparticles and biotin monomers), poly(sulfobetainemethacrylamide), copolymers of N-vinyl-n-butylamide and maleic anhydride, copolymers of N-vinyl-n-butylamide and dimethyl fumarate, copolymers of N-vinyl-n-butylamide and hydroxyethyl methacrylate, copolymers of N-vinyl-n-butylamide and butadiene, polyester amides, polyether amides, copolymers of ethylene oxide and propylene oxide, monoamines of copolymers of ethylene oxide and propylene oxide, and polyethylene oxide-polypropylene oxide-polyethylene oxide Ethylene oxide block copolymers, polymer composites of polyethylene oxide and polyvinyl alcohol, polypropylene oxide modified by maltopentaose, poly(lactide-co-glycolide)-polyethylene oxide-polylactide triblock copolymers, copolymers of 2-methoxyethyl acrylate and acryloylmorpholine, copolymers of 2-methoxyethyl acrylate and N-vinylpyrrolidone, copolymers of 2-methoxyethyl acrylate and 2-hydroxyethyl acrylate, copolymers of 2-methoxyethyl acrylate and methoxytriethylene glycol acrylate, poly[2-(2-ethoxyethoxy)ethyl acrylate], poly(2-(2-ethoxyethoxy)ethyl acrylate-co-2-(methoxyethoxy)ethyl methacrylate), poly(2-(N,N-dimethylaminoethyl) methacrylate), copolymers of N-vinyl caprolactam and hydroxyethyl methacrylate, copolymers of methyl vinyl ether and hydroxyethyl methacrylate, N-vinyl caprolactam polymers, copolymers of N-vinyl caprolactam and maleic anhydride, copolymers of N-vinyl caprolactam and dimethyl fumarate, copolymers of N-vinyl caprolactam and butadiene, copolymers of N-vinyl caprolactam and vinyl pyrrolidine and glycidyl methacrylate, copolymers of N-vinyl caprolactam and vinyl pyrrolidine and methacrylic acid, Copolymers of N-vinyl caprolactam, vinyl pyrrolidone and α, α-dimethyl-m-isopropenyl benzyl isocyanate, copolymers of N-vinyl caprolactam, vinyl pyrrolidone and hydroxyethyl methacrylate, poly(1-ethyl-3-vinyl-2-imidazolidinone), poly(1-methyl-3-vinyl-2-imidazolidinone), poly(1-n-propyl-3-vinyl-2-imidazolidinone), poly(1-isopropyl-3-vinyl-2-imidazolidinone), poly(1-acetyl-3-vinyl-2-imidazolidinone), poly(1-propionyl-3 -vinyl-2-imidazolidinone), a copolymer represented by the following formula 2, a poly(N-vinyl-2-imidazolidinone compound), a copolymer of 2-hydroxyethyl vinyl ether and vinyl acetate, a copolymer of diethylene glycol monovinyl ether and vinyl acetate, a copolymer of methyl vinyl ether and maleic anhydride, a copolymer of methyl vinyl ether and dimethyl fumarate, a carbamylated polyamino acid, a polymer of a compound represented by the following formula 3, a polymer of a compound represented by the following formula 4, a poly(orthoester) having a [N-(2-hydroxyethyl)-L-glutamine] side group, a poly Acetal-poly[N-(2-hydroxyethyl)-L-glutamine]-polyacetal triblock copolymer, poly[N-(2-hydroxyethyl)-L-glutamine]-poly(orthoester)-poly[N-(2-hydroxyethyl)-L-glutamine] triblock copolymer, poly[N-(2-hydroxyethyl)-L-glutamine]-polyacetal diblock copolymer, amino-terminated poly[N-(2-hydroxyethyl)-L-glutamine], amino-terminated poly(orthoester), amino-terminated polyacetal, cellulose triacetate, magnetic nanoparticles, amino-containing polystyrene, and glycoluril polymer. These may be used alone or in combination of two or more. ,
[0138]
Chemistry 5
[0139]
[0140] The weight average molecular weight of the group that changes its hydrophilicity with temperature (the group formed by the temperature responsive polymer) is preferably 330 or more, more preferably 560 or more, and further preferably 1130 or more, and is further preferably 57000 or less, more preferably 34000 or less, and further preferably 17000 or less. When the weight average molecular weight is within the above range, the beneficial effect tends to be better achieved.
[0141] The phase transition temperature (lower critical solution temperature (LCST) or upper critical solution temperature (UCST)) of the temperature responsive polymer is preferably -50°C or higher, more preferably -40°C or higher, further preferably -30°C or higher, particularly preferably -20°C or higher, most preferably at least -10°C, even most preferably 0°C or higher, further most preferably 5°C or higher, further preferably 60°C or lower, more preferably 50°C or lower, still more preferably 40°C or lower, particularly preferably 35°C or lower, most preferably 30°C or lower, even most preferably 25°C or lower, further most preferably 20°C or lower. When the phase transition temperature is within the above range, the beneficial effects tend to be better achieved.
[0142] Herein, the phase transition temperature of the temperature-responsive polymer is measured using a temperature-controlled spectrophotometer. An aqueous solution of the temperature-responsive polymer adjusted to 10% by mass can be placed in a sample cell, and then the sample cell can be covered with paraffin film to prevent evaporation, and an in-cell temperature sensor can be connected to the sample cell. The experiment can be performed at a measurement wavelength of 600nm, a collection temperature of 0.1°C, and a heating rate of 0.1°C. The temperature at which the transmittance reaches 90% is defined as the phase transition temperature.
[0143] Here, the temperature responsive polymer refers to a temperature responsive polymer group (temperature responsive polymer) cleaved from a temperature responsive resin containing the temperature responsive polymer group.
[0144] Next, "B" will be described.
[0145] "B" is not limited as long as it includes at least one selected from terpene resins, rosin resins, styrene resins, C5 resins, C9 resins, C5 / C9 resins, coumarone resins, indene resins and olefin resins. Preferably, "B" is at least one selected from terpene resins, rosin resins, styrene resins, C5 resins, C9 resins, C5 / C9 resins, coumarone resins, indene resins and olefin resins. These can be used alone or as a mixture of two or more. In addition, the resin itself can be a copolymer of monomer components from different sources. "B" is more preferably a terpene resin, a styrene resin, a C9 resin, a C5 / C9 resin, a coumarone resin and / or an indene resin, and is even more preferably a styrene resin, because these resins have good compatibility with styrene elastomers, so that the beneficial effects can be more appropriately achieved.
[0146] Examples of such commercially available resins include products available from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF Corporation, Arizona Chemical Co., Ltd., Nippon Co., Ltd., Nippon Shokubai Co., Ltd., JXTG Energy Co., Ltd., Arakawa Chemical Industries, Ltd., Taoka Chemical Industries, Ltd., and the like.
[0147] The terpene resin may be any resin containing a unit derived from a terpene compound, and examples thereof include polyterpenes (resins obtained by polymerizing terpene compounds), terpene aromatic resins (resins obtained by copolymerizing terpene compounds with aromatic compounds), aromatic modified terpene resins (resins obtained by modifying terpene resins with aromatic compounds), etc. These may be used alone or in combination of two or more.
[0148] The term "terpene compound" refers to a terpene having a carbonyl group consisting of (C5H8) n The hydrocarbons of the composition represented by the formula (C) or their oxygen-containing derivatives, each of which has a terpene skeleton and is classified into, for example, monoterpenes (C 10 H 16 ), sesquiterpenes (C 15 H 24 ) or diterpenes (C 20 H 32 ). Examples of such terpene compounds include α-pinene, β-pinene, dipentene, limonene, myrcene, alloocimene, ocimene, α-phellandrene, α-terpinene, γ-terpinene, terpinolene, 1,8-cineole, 1,4-cineole, α-terpineol, β-terpineol, and γ-terpineol. These may be used alone or in combination of two or more.
[0149] The aromatic compound may be any compound having an aromatic ring. Examples include: phenol compounds, such as phenol, alkylphenol, alkoxyphenol, and phenol containing an unsaturated hydrocarbon group; naphthol compounds, such as naphthol, alkylnaphthol, alkoxynaphthol, and naphthol containing an unsaturated hydrocarbon group; styrene and styrene derivatives, such as alkylstyrene, alkoxystyrene, and styrene containing an unsaturated hydrocarbon group. These may be used alone or in combination of two or more. Among these, styrene is preferred.
[0150] Examples of the above-mentioned terpene compounds also include resin acids (rosin acids), such as abietic acid, neoabietic acid, palustric acid, levopimaric acid, pimaric acid and isopimaric acid. Herein, terpene resins mainly (50% by mass or more, preferably 80% by mass or more) formed from abietic acid obtained by processing pine resin are considered to be rosin resins.
[0151] Here, examples of rosin-based resins include natural rosin resins (polymerized rosins), such as gum rosin, wood rosin, and tall oil rosin; modified rosin resins, such as maleic acid-modified rosin resins, rosin-modified phenolic resins; rosin esters, such as rosin glycerol esters; and disproportionated rosin resins obtained by disproportionating rosin resins. These may be used alone or in combination of two or more.
[0152] The above-mentioned styrene resin refers to a polymer formed by a styrene monomer as a structural monomer, and examples thereof include polymers polymerized by styrene monomers as a main component (more than 50% by mass, preferably more than 80% by mass). Specific examples include: homopolymers obtained by polymerization of a single styrene monomer (such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, p-methoxystyrene, p-tert-butylstyrene, p-phenylstyrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene), copolymers obtained by copolymerization of two or more styrene monomers, and copolymers of styrene monomers and other monomers copolymerizable therewith. These can be used alone or in combination of more than two. Among them, copolymers of styrene monomers and other monomers copolymerizable therewith are preferred, and styrene monomers are more preferred.
[0153] Examples of other monomers include: acrylonitriles, such as acrylonitrile and methacrylonitrile; unsaturated carboxylic acids, such as acrylic acid and methacrylic acid; unsaturated carboxylic acid esters, such as methyl acrylate and methyl methacrylate; dienes, such as chloroprene, butadiene, and isoprene; olefins, such as 1-butene and 1-pentene; α,β-unsaturated carboxylic acids and their anhydrides, such as maleic anhydride. These may be used alone or in combination of two or more. Among them, unsaturated carboxylic acids are preferred, and acrylic acid or methacrylic acid is more preferred.
[0154] Among styrene-based resins, styrene homopolymers and α-methylstyrene-based resins (eg α-methylstyrene homopolymers and copolymers of α-methylstyrene and styrene) are preferred, styrene homopolymers or α-methylstyrene homopolymers are more preferred, and styrene homopolymers are more preferred.
[0155] Examples of C5 resins include aliphatic petroleum resins containing olefins or diolefins from the C5 fraction obtained by naphtha cracking as the main component (more than 50% by mass, preferably more than 80% by mass). Examples of C9 resins include aromatic petroleum resins containing vinyltoluene from the C9 fraction obtained by naphtha cracking as the main component (more than 50% by mass, preferably more than 80% by mass). Examples of C5 / C9 resins include resins containing olefins or diolefins from the C5 fraction and vinyltoluene from the C9 fraction as the main component (more than 50% by mass, preferably more than 80% by mass). These resins may be resins copolymerized with the above-mentioned other monomers. These may be used alone or in combination of two or more.
[0156] Examples of benzofuran resins include resins containing benzofuran as a main component (50% by mass or more, preferably 80% by mass or more). Examples of indene resins include resins containing indene or methylindene as a main component (50% by mass or more, preferably 80% by mass or more). These resins may be resins copolymerized with the above-mentioned other monomers. These may be used alone or in combination of two or more. Here, benzofuran resins and indene resins include benzofuran-indene resins.
[0157] Examples of olefin resins include polyethylene resins such as polyethylene, ethylene-propylene copolymers, ethylene-propylene-non-conjugated diene copolymers, ethylene-butene copolymers, ethylene-hexene copolymers, ethylene-octene copolymers, ethylene-vinyl acetate copolymers, ethylene-vinyl alcohol copolymers, ethylene-ethyl acrylate copolymers, and chlorinated polyethylene; polypropylene resins such as polypropylene, propylene-ethylene random copolymers, propylene-ethylene block copolymers, and chlorinated polypropylene; polybutene, polyisobutylene, polymethylpentene, and copolymers of cycloolefins. These may be used alone or in combination of two or more.
[0158] "A" and "B" can be combined with each other by any method. Those skilled in the art can combine them. For example, a monomer capable of forming "A" can be first polymerized to form an "A" block, and then a monomer capable of forming "B" can be added to the reaction system to form a "B" block after the "A" block, thereby making a compound including "A" and "B" combined with each other. Specifically, a temperature-responsive resin can be manufactured, for example, as described in JP2019-83761A.
[0159] The ratio (mass %) of "A" to "B" in the temperature responsive resin ("A":"B") is preferably 50:50 to 98:2. The lower limit is preferably 60:40, and more preferably 65:35. The upper limit is preferably 95:5, and more preferably 90:10. When the ratio is within the above range, the beneficial effects tend to be better achieved.
[0160] The ratio of "A" to "B" can be determined by NMR.
[0161] The temperature-responsive resin is preferably a block copolymer, more preferably a block copolymer having a block formed by "A" and a block formed by "B", further preferably a block copolymer having a block formed by "A" at one end and a block formed by "B" at the other end, and particularly preferably a diblock copolymer formed by a block formed by "A" and a block formed by "B".
[0162] The temperature responsive resin is preferably a compound including "A" and "B" bonded to each other.
[0163] "A" is preferably a group that changes its hydrophilicity with temperature, more preferably a temperature-responsive polymer, and even more preferably a polymer that shows a lower critical solution temperature in water. It is particularly preferably a poly(N-substituted (methyl)acrylamide) or a group represented by formula (B), and most preferably a group represented by formula (I) or a group represented by formula (B).
[0164] Here, "B" is preferably a terpene resin, a styrene resin, a C9 resin, a C5 / C9 resin, a coumarone resin and / or an indene resin, and more preferably a styrene resin.
[0165] The weight average molecular weight (Mw) of the temperature responsive resin is preferably 500 or more, more preferably 1,000 or more, further preferably 5,000 or more, particularly preferably 10,000 or more, most preferably 20,000 or more, further most preferably 30,000 or more, and further preferably 80,000 or less, more preferably 75,000 or less. When Mw is within the above range, the beneficial effects tend to be better achieved.
[0166] The amount of the temperature responsive resin is preferably 1 part by mass or more, more preferably 5 parts by mass or more, still more preferably 10 parts by mass or more, particularly preferably 15 parts by mass or more, and further preferably 60 parts by mass or less, more preferably 50 parts by mass or less, further preferably 40 parts by mass or less, particularly preferably 30 parts by mass or less, relative to 100 parts by mass of the elastomer component content (preferably, relative to 100 parts by mass of the rubber component content). When the amount is within the above range, the beneficial effects tend to be better achieved.
[0167] In order to make the temperature-responsive resin change its hydrophilicity more appropriately with the change in temperature, water is preferably present. Therefore, the elastomer composition preferably contains at least one water-absorbent material, such as a water-absorbent fiber, a water-absorbent elastomer and / or a water-absorbent resin. In this case, the elastomer composition may be appropriately blended with water so that the temperature-responsive resin can change its hydrophilicity more appropriately with the change in temperature. These materials may be used alone or in combination of two or more.
[0168] Examples of such water-absorbing materials include heteroatom-containing materials (fibers, elastomers, resins).
[0169] The term "heteroatom" refers to an atom other than a carbon atom and a hydrogen atom, and may be any heteroatom capable of forming a reversible molecular bond such as a hydrogen bond or an ionic bond with water. The heteroatom is preferably at least one atom selected from an oxygen atom, a nitrogen atom, a silicon atom, a sulfur atom, a phosphorus atom and a halogen atom, more preferably an oxygen atom, a nitrogen atom or a silicon atom, and still more preferably an oxygen atom.
[0170] Examples of the structure or group containing an oxygen atom include an ether group, an ester group, a carboxyl group, a carbonyl group, an alkoxy group, and a hydroxyl group. Among them, an ether group is preferred, and an oxyalkylene group is more preferred.
[0171] Examples of the structure or group containing a nitrogen atom include an amino group (primary amino group, secondary amino group or tertiary amino group), an amide group, a cyano group and a nitro group. Among them, an amino group is preferred, and a tertiary amino group is more preferred.
[0172] Examples of the structure or group containing a silicon atom include a silyl group, an alkoxysilyl group, and a silanol group. Among them, a silyl group is preferred, and an alkoxysilyl group is more preferred.
[0173] Examples of the structure or group containing a sulfur atom include a sulfide group, a sulfate group, a sulfate ester, and a sulfone group.
[0174] Examples of the structure or group containing a phosphorus atom include a phosphate group and a phosphate ester.
[0175] Examples of the structure or group containing a halogen atom include halogenated groups such as fluoro, chloro, bromo and iodo groups.
[0176] Examples of water-absorbent fibers include cellulose fibers containing hydroxyl groups.
[0177] Among the cellulose fibers, cellulose microfibrils are preferred. Any cellulose microfibrils from naturally occurring materials can be used. Examples include those from the following materials: resource biomass such as fruits, grains, and root vegetables; wood, bamboo, hemp, jute, kenaf, and pulp, paper, or cloth made from these; waste biomass such as agricultural waste, food waste, and urban sludge; unused biomass such as straw, wheat straw, and thinnings; cellulose produced by sea squirts, acetic acid bacteria, or other organisms. These may be used alone or in combination of two or more.
[0178] Examples of the water-absorbing elastomer include elastomers containing oxyalkylene groups, and examples thereof include epoxide / allyl glycidyl ether copolymers, amine / allyl glycidyl ether copolymers, and silyl / allyl glycidyl ether copolymers. These may be used alone or in combination of two or more.
[0179] Examples of the water-absorbent resin include polyvinyl alcohol, polyethylene glycol, sodium polyacrylate, polyurethane, polyvinyl acetate, epoxy resin, and cellulose resin. These may be used alone or in combination of two or more.
[0180] The amount of the water-absorbent fiber, water-absorbent elastomer and / or water-absorbent resin is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and further preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and further preferably 20 parts by mass or less, relative to 100 parts by mass of the elastomer component content (preferably, relative to 100 parts by mass of the rubber component content). When the amount is within the above range, the beneficial effects tend to be better achieved.
[0181] Here, when two or more types of water-absorbent fibers, water-absorbent elastomers and / or water-absorbent resins are combined, the above amount means the total amount thereof.
[0182] The composition preferably contains silica as a filler (reinforcing filler). Since silica is a hydrophilic material containing hydroxyl groups, water can be appropriately incorporated into the elastomer composition so that the temperature-responsive resin can more appropriately change its hydrophilicity with temperature changes.
[0183] Any silica can be used, and examples thereof include dry silica (anhydrous silicic acid) and wet silica (hydrous silicic acid). These can be used alone or in combination of two or more. Among them, wet silica is preferred because it has a large number of silanol groups.
[0184] Examples of commercially available silica include products from Degussa, Rhodia, Tosoh Silica Corporation, Solvay Japan Co., Ltd., Tokuyama Co., Ltd., and the like.
[0185] The nitrogen adsorption specific surface area (N2SA) of silicon dioxide is preferably 70 m 2 / g or more, more preferably 140m 2 / g or more. In addition, the N2SA is preferably 300m 2 / g or less, more preferably 250m 2 When N2SA is within the above range, the beneficial effects tend to be better achieved.
[0186] Here, the N2SA of silica can be measured according to ASTM D3037-81.
[0187] The amount of silica is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, further preferably 15 parts by mass or more, particularly preferably 20 parts by mass or more, most preferably 30 parts by mass or more, further most preferably 50 parts by mass or more, and further preferably 200 parts by mass or less, more preferably 180 parts by mass or less, still more preferably 150 parts by mass or less, particularly preferably 120 parts by mass or less, and most preferably 100 parts by mass or less, relative to 100 parts by mass of the elastomer component content (preferably, relative to 100 parts by mass of the rubber component content). When the amount is within the above range, the beneficial effects tend to be better achieved.
[0188] When the above composition contains silica, it preferably contains a silane coupling agent together with the silica.
[0189] Any silane coupling agent may be used. Examples include sulfide-based silane coupling agents such as bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide. disulfide, bis(3-triethoxysilylpropyl) disulfide, bis(2-triethoxysilylethyl) disulfide, bis(4-triethoxysilylbutyl) disulfide, bis(3-trimethoxysilylpropyl) disulfide, bis(2-trimethoxysilylethyl) disulfide, bis(4-trimethoxysilylbutyl) disulfide, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide , 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide and 3-triethoxysilylpropyl methacrylate monosulfide; mercapto-based silane coupling agents, such as 3-mercaptopropyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, NXT and NXT-Z purchased from Momentive; vinyl-based silane coupling agents, such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based Silane coupling agents, such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy silane coupling agents, such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro silane coupling agents, such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; chlorine (substituted) silane coupling agents, such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. These can be used alone or in combination of two or more. Among them, sulfide silane coupling agents are preferred.
[0190] Examples of commercially available silane coupling agents include products from Degussa, Momentive, Shin-Etsu Silicone, Tokyo Chemical Industry, AZmax, Dow Corning Toray, and the like.
[0191] If a silane coupling agent is present, the amount of the silane coupling agent is preferably 0.1 parts by mass or more, more preferably 3 parts by mass or more, and even more preferably 6 parts by mass or more relative to 100 parts by mass of the silica content. In addition, the amount is preferably 20 parts by mass or less, more preferably 16 parts by mass or less, even more preferably 12 parts by mass or less, and particularly preferably 10 parts by mass or less. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0192] The above composition preferably contains carbon black.
[0193] Examples of carbon black include N134, N110, N220, N234, N219, N339, N330, N326, N351, N550, and N762. These may be used alone or in combination of two or more.
[0194] The nitrogen adsorption specific surface area (N2SA) of carbon black is preferably 5 m 2 / g or more, more preferably 30m 2 / g or more, and more preferably 60 m 2 / g or more, particularly preferably 80m 2 / g or more, most preferably 100m 2 / g or more. In addition, the N2SA is preferably 300m 2 / g or less, more preferably 200m 2 / g or less, and more preferably 150m 2 When N2SA is within the above range, the beneficial effects tend to be better achieved.
[0195] Here, the nitrogen adsorption specific surface area of carbon black can be measured in accordance with JIS K 6217-2:2001.
[0196] The dibutyl phthalate oil absorption (DBP) of carbon black is preferably 5 ml / 100 g or more, more preferably 70 ml / 100 g or more, and even more preferably 90 ml / 100 g or more. In addition, the DBP is preferably 300 ml / 100 g or less, more preferably 200 ml / 100 g or less, even more preferably 160 ml / 100 g or less, and particularly preferably 120 ml / 100 g or less. When the DBP is within the above range, the beneficial effects tend to be better achieved.
[0197] Here, the DBP of carbon black can be measured in accordance with JIS K 6217-4:2001.
[0198] Examples of commercially available carbon black include products from Asahi Carbon Co., Ltd., Cabot Japan KK, Tokai Carbon Co., Ltd., Mitsubishi Chemical Corporation, Lion Corporation, NSCC Carbon Co., Ltd., Columbia Carbon Co., Ltd., and the like.
[0199] The amount of carbon black is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, still more preferably 3 parts by mass or more, particularly preferably 5 parts by mass or more, relative to 100 parts by mass of the elastomer component content (preferably, relative to 100 parts by mass of the rubber component content), and is also preferably 100 parts by mass or less, more preferably 50 parts by mass or less, still more preferably 30 parts by mass or less, particularly preferably 20 parts by mass or less, and most preferably 10 parts by mass or less. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0200] The above composition preferably contains sulfur.
[0201] Examples of sulfur include those commonly used in the rubber industry, such as powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, and soluble sulfur. These may be used alone or in combination of two or more.
[0202] Examples of commercially available sulfur include products from Tsurumi Chemical Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexsys, Inc., Nippon Senryu Kogyo Co., Ltd., Hosoi Chemical Co., Ltd., and the like.
[0203] The amount of sulfur is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, relative to 100 parts by mass of the elastomer component content (preferably, relative to 100 parts by mass of the rubber component content). In addition, the amount is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, even more preferably 8 parts by mass or less, and particularly preferably 5 parts by mass or less. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0204] The above composition preferably contains a vulcanization accelerator.
[0205] Examples of vulcanization accelerators include: thiazole vulcanization accelerators, such as 2-mercaptobenzothiazole and di-2-benzothiazolyl disulfide; thiuram vulcanization accelerators, such as tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD), tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); sulfenamide vulcanization accelerators, such as N-cyclohexyl-2-benzothiazolyl sulfenamide, N-tert-butyl-2-benzothiazolyl sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, N,N'-diisopropyl-2-benzothiazole sulfenamide; guanidine vulcanization accelerators, such as diphenylguanidine, di-o-tolylguanidine, o-tolylbiguanide. These may be used alone or in combination of two or more.
[0206] Examples of commercially available vulcanization accelerators include products from Kawaguchi Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., Rhein Chemie Co., Ltd., and the like.
[0207] The amount of the vulcanization accelerator is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, relative to 100 parts by mass of the elastomer component content (preferably, relative to 100 parts by mass of the rubber component content). In addition, the amount is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, even more preferably 8 parts by mass or less, and particularly preferably 5 parts by mass or less. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0208] The above composition preferably contains stearic acid.
[0209] Conventionally known stearic acid can be used, including, for example, products available from NOF Corporation, Kao Corporation, Fujifilm Co., Ltd., Wako Pure Chemical Industries, Ltd., Chiba Fatty Acid Co., Ltd., and the like.
[0210] The amount of stearic acid is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, relative to 100 parts by mass of the elastomer component content (preferably, relative to 100 parts by mass of the rubber component content). In addition, the amount is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, even more preferably 8 parts by mass or less, and particularly preferably 5 parts by mass or less. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0211] The above composition may comprise zinc oxide.
[0212] Conventionally known zinc oxide can be used, including, for example, products available from Mitsui Mining and Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Shodo Chemical Industry Co., Ltd., Sakai Chemical Industry Co., Ltd., and the like.
[0213] The amount of zinc oxide is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, relative to 100 parts by mass of the elastomer component content (preferably, relative to 100 parts by mass of the rubber component content). In addition, the amount is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, even more preferably 8 parts by mass or less, and particularly preferably 5 parts by mass or less. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0214] The above composition may contain an antioxidant.
[0215] Examples of antioxidants include naphthylamine antioxidants such as phenyl-α-naphthylamine; diphenylamine antioxidants such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; p-phenylenediamine antioxidants such as N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and N,N'-di-2-naphthyl-p-phenylenediamine; quinoline antioxidants such as 2,2,4-trimethyl-1,2-dihydroquinoline polymers; monophenol antioxidants such as 2,6-di-tert-butyl-4-methylphenol and styrenated phenol; and bisphenol, triphenol or polyphenol antioxidants such as tetrakis[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]methane. These may be used alone or in combination of two or more. Among them, p-phenylenediamine antioxidants and quinoline antioxidants are preferred, and p-phenylenediamine antioxidants are more preferred.
[0216] Examples of commercially available antioxidants include products from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., Flexsys Corporation, and the like.
[0217] The amount of the antioxidant is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more relative to 100 parts by mass of the elastomer component content (preferably, relative to 100 parts by mass of the rubber component content). In addition, the amount is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, even more preferably 8 parts by mass or less, and particularly preferably 5 parts by mass or less. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0218] The above composition may contain a wax.
[0219] Any wax may be used, and examples thereof include: petroleum waxes such as paraffin wax, microcrystalline wax; naturally occurring waxes such as plant waxes and animal waxes; and synthetic waxes such as polymers of ethylene, propylene or other similar monomers. These may be used alone or in combination of two or more.
[0220] Examples of commercially available waxes include products from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., Seiko Chemical Co., Ltd., and the like.
[0221] The amount of the wax is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, relative to 100 parts by mass of the elastomer component content (preferably, relative to 100 parts by mass of the rubber component content). In addition, the amount is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, further preferably 8 parts by mass or less, and particularly preferably 5 parts by mass or less. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0222] The rubber composition preferably contains a liquid plasticizer.
[0223] Herein, the term "plasticizer" refers to an organic compound that imparts plasticity to rubber. The term "liquid plasticizer" refers to a plasticizer that is liquid at a temperature of 0°C or higher, or specifically, refers to an organic compound that, when left to stand in a container for 1 minute, has a shape that is similar to that of a container that is different from its shape. Such liquid plasticizers may be used alone or in combination of two or more.
[0224] Specific examples of liquid plasticizers include oils, ester plasticizers, and liquid resins (also collectively referred to as oils, etc.). These can be used alone or in combination of two or more. Among them, oils are preferred.
[0225] The amount of the liquid plasticizer is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, relative to 100 parts by mass of the elastomer component content (preferably, relative to 100 parts by mass of the rubber component content). In addition, the amount is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 30 parts by mass or less. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0226] Any oil can be used, and examples thereof include conventional oils, including: process oils such as paraffinic process oils, aromatic process oils, and naphthenic process oils; low polycyclic aromatic (PCA) process oils such as TDAE and MES; vegetable oils and fats; and mixtures of the foregoing. These can be used alone or in combination of two or more. Among them, aromatic process oils are preferred. Specific examples of the above-mentioned aromatic process oils include DianaProcess Oil AH series available from Idemitsu Kosan Co., Ltd.
[0227] Examples of commercially available oils include products available from Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., Nippon Energy Co., Ltd., Olisoy Co., Ltd., H&R Co., Ltd., Toyokuni Oil Refining Co., Ltd., Showa Shell Sekiyu Co., Ltd., Fuji Kosan Co., Ltd., and the like.
[0228] Examples of ester plasticizers include: the above-mentioned vegetable oils; synthetic plasticizers and processed vegetable oils, such as glycerol fatty acid monoesters, glycerol fatty acid diesters, and glycerol fatty acid triesters; and phosphate esters (e.g., phosphate ester plasticizers and mixtures thereof). These may be used alone or in combination of two or more.
[0229] Suitable examples of the ester plasticizer include fatty acid esters represented by the following formula:
[0230]
[0231] In the formula, R 11 represents a C1-C8 straight chain or branched alkyl group, a C1-C8 straight chain or branched alkenyl group, or a C2-C6 straight chain or branched alkyl group substituted with 1 to 5 hydroxyl groups; R 12 It represents a C11-C21 alkyl or alkenyl group.
[0232] R 11 Examples of R include methyl, ethyl, 2-ethylhexyl, isopropyl and octyl, and groups obtained by substituting these groups with 1 to 5 hydroxyl groups. 12 Examples of include straight-chain or branched alkyl or alkenyl groups such as lauryl, myristyl, palmityl, stearyl and oleyl groups.
[0233] Examples of fatty acid esters include oleic acid alkyl esters, stearic acid alkyl esters, linoleic acid alkyl esters, and palmitic acid alkyl esters. Among them, oleic acid alkyl esters (methyl oleate, ethyl oleate, oleic acid-2-ethylhexyl ester, isopropyl oleate, octyl oleate, etc.) are preferred. In this case, the amount of oleic acid alkyl ester is preferably 80% by mass or more based on the amount of fatty acid ester as 100% by mass.
[0234] Other examples of fatty acid esters include fatty acid monoesters or fatty acid diesters formed by fatty acids (e.g., oleic acid, stearic acid, linoleic acid, palmitic acid) and alcohols (e.g., ethylene glycol, glycerine, trimethylolpropane, pentaerythritol, erythritol, xylitol, sorbitol, galactitol, mannitol, inositol). Among them, oleic acid monoesters are preferred. In this case, the total amount of fatty acid monoesters and fatty acid diesters is 100% by mass, and the amount of oleic acid monoesters is preferably more than 80% by mass.
[0235] Phosphoric acid esters can be suitably used as ester plasticizers.
[0236] Preferred phosphates include C12-C30 compounds, wherein C12-C30 trialkyl phosphates are suitable. Here, the carbon number of trialkyl phosphates refers to the total number of carbon atoms in 3 alkyl groups. The 3 alkyl groups may be the same or different groups. Examples of alkyl groups include straight or branched chain alkyl groups, which may contain heteroatoms (such as oxygen atoms) or may be substituted by halogen atoms (such as fluorine, chlorine, bromine or iodine).
[0237] Other examples of phosphate esters include well-known phosphate ester plasticizers, such as: monoesters, diesters or triesters of phosphoric acid and C1-C12 monohydric alcohols or their (poly)oxyalkylene adducts; and compounds obtained by replacing one or two alkyl groups in the above trialkyl phosphates with phenyl groups. Specific examples include tri(2-ethylhexyl) phosphate, trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, triphenyl phosphate, tricresol phosphate, tri(xylene) phosphate, diphenyl cresol phosphate, 2-ethylhexyl diphenyl phosphate, and tri(2-butoxyethyl) phosphate.
[0238] Examples of liquid resins include terpene resins, rosin resins, styrene resins, C5 resins, C9 resins, C5 / C9 resins, coumarone resins, indene resins, olefin resins, polyurethane resins, acrylic resins, p-tert-butylphenol acetylene resins, dicyclopentadiene resins (DCPD resins), and other resins that are liquid at 0°C. These can be used alone or as a mixture of two or more. In addition, the resin itself can be a copolymer of monomer components from different sources.
[0239] In addition, examples of other liquid resins include: liquid (meaning liquid at 0° C., the same below) farnesene-based polymers, such as liquid farnesene homopolymers, liquid farnesene-styrene copolymers, liquid farnesene-butadiene copolymers, liquid farnesene-styrene-butadiene copolymers, liquid farnesene-isoprene copolymers, and liquid farnesene-styrene-isoprene copolymers; liquid myrcene-based polymers, such as liquid myrcene homopolymers, liquid myrcene-styrene copolymers, liquid myrcene-butadiene copolymers, liquid myrcene-styrene-butadiene copolymers, liquid myrcene-isoprene copolymers, and liquid myrcene-styrene-isoprene copolymers; liquid diene Liquid olefin polymers, such as liquid styrene-butadiene copolymers (liquid SBR), liquid polybutadiene polymers (liquid BR), liquid polyisoprene polymers (liquid IR), liquid styrene-isoprene copolymers (liquid SIR), liquid styrene-butadiene-styrene block copolymers (liquid SBS block polymers) and liquid styrene-isoprene-styrene block copolymers (liquid SIS block polymers); liquid olefin polymers containing olefin resins (such as polyethylene, polypropylene) as hard segments (hard phases) and rubber components as soft segments (soft phases); and liquid ester polymers containing polyesters as hard segments and polyethers, polyesters, etc. as soft segments. These can be modified with polar groups at the chain ends or skeletons. These can be used alone or in combination of two or more.
[0240] Examples of commercially available liquid resins include products available from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF Corporation, Arizona Chemical Co., Ltd., Nippon Paint Chemicals Co., Ltd., Nippon Shokubai Co., Ltd., JXTG Energy Co., Ltd., Arakawa Chemical Industries, Ltd., Taoka Chemical Industries, Ltd., Sartomer Co., Ltd., Kuraray Co., Ltd., and the like.
[0241] In addition to the above components, the above composition may contain additives commonly used in the tire industry, such as vulcanizing agents other than sulfur (e.g., organic crosslinking agents, organic peroxides), calcium carbonate, mica (e.g., sericite), aluminum hydroxide, magnesium oxide, magnesium hydroxide, clay, talc, alumina, and titanium oxide. The amount of these components is preferably 0.1 parts by mass or more, and preferably 200 parts by mass or less, relative to 100 parts by mass of the elastomer component content (preferably the rubber component content).
[0242] The above composition can be prepared, for example, by kneading the above-mentioned respective components using a rubber kneading device such as an open roll mill or a Banbury mixer, and then vulcanizing the kneaded mixture.
[0243] The kneading conditions are as follows. In the basic kneading process of kneading additives other than the crosslinking agent (vulcanizing agent) and the vulcanization accelerator, the kneading temperature is usually 100 to 180°C, preferably 120 to 170°C. In the final kneading process of kneading the vulcanizing agent and the vulcanization accelerator, the kneading temperature is usually 120°C or less, preferably 80 to 110°C. Then, the composition obtained after kneading the vulcanizing agent and the vulcanization accelerator is usually vulcanized by, for example, press vulcanization. The vulcanization temperature is usually 140 to 190°C, preferably 150 to 185°C.
[0244] The above composition can be used for tire components (used as a rubber composition for tires), such as tread (track tread), sidewall, tread base, undertread, clinch, bead apex, breaker cushion rubber, carcass cord topping rubber, insulation, chafer and inner liner, and side reinforcement layer of run-flat tire. The above composition can be suitably used for outer layer components of tires, such as tread (track tread), sidewall, clinch and inner liner, and can be more suitably used for tread (track tread).
[0245] The tire of the present invention can be manufactured from the above composition by conventional methods. Specifically, the tire can be produced by extruding an unvulcanized composition containing various additives as required into the shape of a tire component (especially an outer layer component of the tire, such as a tread (tread running surface)), then forming it in a conventional manner on a tire molding machine and assembling it with other tire components to form an unvulcanized tire, and then heating and pressurizing the unvulcanized tire in a vulcanizer.
[0246] The tire may be any type of tire, including pneumatic tires, solid tires and non-pneumatic tires. Among them, pneumatic tires are preferred.
[0247] The tires can be suitable for use as passenger car tires, large passenger car tires, large SUV tires, truck and bus tires, or two-wheeled vehicle tires, or as racing tires, winter tires (studless winter tires, snow tires, studded tires), all-season tires, run-flat tires, aircraft tires, mining tires, etc. Among them, the tires can be more suitable for use as winter tires (studless winter tires, snow tires, studded tires) or all-season tires.
[0248] Preferably, the tire includes a temperature responsive component comprising the elastomer composition, and the maximum thickness of the temperature responsive component is 1 mm or more.
[0249] The maximum thickness of the temperature responsive component is preferably 1 mm or more, more preferably 3 mm or more, and further preferably 5 mm or more. There is no upper limit, but it is preferably 20 mm or less, more preferably 15 mm or less, and even more preferably 10 mm or less. When the maximum thickness is within the above range, the beneficial effect tends to be better achieved.
[0250] Here, the temperature responsive member is preferably an outer layer member as described above, and more preferably a tread (cap tread).
[0251] Preferably, the tire includes at least one adjacent component adjacent to the temperature responsive component and formed of a material different from the elastomer composition, and the difference in hardness between the adjacent component and the temperature responsive component at 25° C. is 15 or less.
[0252] The hardness difference is more preferably 13 or less, still more preferably 10 or less, particularly preferably 8 or less, most preferably 5 or less, even most preferably 2 or less, and further most preferably 0. When the difference is within the above range, the advantageous effects tend to be better achieved.
[0253] The hardness of the temperature responsive member at 25° C. is preferably 55 or more, more preferably 60 or more, and is also preferably 80 or less, more preferably 75 or less. When the hardness is within the above range, the advantageous effects tend to be more effectively achieved.
[0254] Here, preferably, the temperature responsive component is a tread (cap tread), and the adjacent component is a base tread.
[0255] Furthermore, for example, the formulation of the adjacent member may be a formulation of the elastomer composition from which the temperature responsive resin is omitted.
[0256] Herein, hardness refers to JIS-A hardness measured using a type A durometer in accordance with JIS K 6253-3 (2012) "Rubber, vulcanized or thermoplastic rubber - Determination of hardness - Part 3: Durometer method".
[0257] Example
[0258] The present invention is specifically described with reference to the following examples, but is not limited to the following examples.
[0259] Hereinafter, various chemicals used in the following Examples and Comparative Examples are listed.
[0260] SBR: Nipol 1502 (E-SBR, styrene content: 23.5% by mass, vinyl content: less than 20%) purchased from Zeon Co., Ltd., Japan
[0261] BR: BR150B purchased from Ube Industries, Ltd. (cis content: 98 mass %)
[0262] NR: TSR20 (natural rubber)
[0263] Carbon black: Seast N220 (N2SA: 111m 2 / g, DBP: 115ml / 100g)
[0264] Silicon dioxide: ULTRASIL VN3 (N2SA: 175m 2 / g)
[0265] Silane coupling agent: Si266 (bis(3-triethoxysilylpropyl) disulfide) purchased from Evonik Degussa
[0266] Wax: Ozoace wax purchased from Nippon Seira Co., Ltd.
[0267] Antioxidant: NOCRAC 6C (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine) purchased from Ouchi Shinko Chemical Industry Co., Ltd.
[0268] Oil: PS-32 purchased from Idemitsu Kosan Co., Ltd.
[0269] PNIPAM-b-Sty (1): N-isopropylacrylamide-styrene diblock copolymer synthesized according to the polymerization method described in JP 2019-83761A (Mw: 70,000, NIPAM:Sty=90:10 (mass %))
[0270] PNIPAM-b-Sty (2): N-isopropylacrylamide-styrene diblock copolymer synthesized according to the polymerization method described in JP 2019-83761A (Mw: 50,000, NIPAM:Sty = 70:30 (mass %))
[0271] PNIPVM-b-Sty (1): PNIPVM-styrene diblock copolymer synthesized according to the polymerization method described in JP 2019-83761A (Mw: 70,000, NIPVM:Sty = 90:10 (mass %))
[0272] PNIPVM-b-Sty (2): PNIPVM-styrene diblock copolymer synthesized according to the polymerization method described in JP 2019-83761A (Mw: 50,000, NIPVM:Sty = 70:30 (mass %))
[0273] PNIPAM-b-AMS: N-isopropylacrylamide-α-methylstyrene diblock copolymer synthesized according to the polymerization method described in JP 2019-83761A (Mw: 70,000, NIPAM:AMS=90:10 (mass %))
[0274] Epoxide / allyl glycidyl ether copolymer: Epoxide / allyl glycidyl ether copolymer described in Preparation Example 2 of WO2020 / 022325
[0275] Cellulose fiber: Biomass nanofiber purchased from Sugino Machine Co., Ltd. (trade name "BiNFi-scellulose", microfibrillated cellulose fiber)
[0276] Stearic acid: purchased from NOF Corporation
[0277] Zinc oxide: Zinc oxide #2 purchased from Mitsui Mining and Smelting Co., Ltd.
[0278] Sulfur: Powdered sulfur purchased from Tsurumi Chemical Industry Co., Ltd.
[0279] Vulcanization accelerator: NOCCELER NS (N-tert-butyl-2-benzothiazolylsulfenamide) purchased from Ouchi Shinko Chemical Industry Co., Ltd.
[0280] (Examples and Comparative Examples)
[0281] According to the formulation shown in Table 2 or Table 3, chemicals other than sulfur and a vulcanization accelerator were kneaded at 150° C. for 5 minutes using a 1.7 L Banbury mixer (Kobe Steel, Ltd.) to obtain a kneaded mixture. Then, sulfur and a vulcanization accelerator were added to the kneaded mixture, and they were kneaded at 80° C. in an open roll mill for 5 minutes to obtain an unvulcanized rubber composition.
[0282] The unvulcanized rubber composition was press-vulcanized at 170° C. for 12 minutes to produce a vulcanized rubber composition sheet having a thickness of 2 mm.
[0283] In addition, the unvulcanized rubber composition prepared as above was formed into a cap tread shape and assembled with other tire components to prepare an unvulcanized tire according to Table 4. The unvulcanized tire was vulcanized at 170° C. for 15 minutes to prepare a test tire (size: 195 / 65R15).
[0284] Here, the formulation of the base tread rubber was the same as that of Comparative Example 1, but the oil content and filler content were appropriately adjusted to change the hardness.
[0285] Furthermore, the tire is prepared so that the base tread is adjacent to the cap tread in the tire radial direction.
[0286] The vulcanized rubber composition and the test tire prepared as described above were stored in a dark place at room temperature for 3 months, and then the following evaluations were performed. Tables 2 to 4 show the results.
[0287] (Measurement of water contact angle)
[0288] The water contact angle was measured on each 2 mm thick sheet of the vulcanized rubber composition.
[0289] Specifically, a vulcanized rubber composition sheet having a thickness of 2 mm was kept at the measurement temperature for 10 minutes, and then a 20 μL drop of water was dropped on the surface of the sheet. After 15 seconds, the contact angle of the drop was measured using a contact angle meter.
[0290] Here, the measurement is first carried out at a measurement temperature of 5°C, and then at a measurement temperature of 60°C. The measurement result is taken as the first measurement result. After the first measurement, the vulcanized rubber composition sheet after the measurement is immersed in water for 1 hour so that the measurement surface is in contact with water. After being immersed in water, the vulcanized rubber composition sheet is dried at 60°C for 24 hours. Then, the dried vulcanized rubber composition sheet is cooled to room temperature. Thereafter, the second measurement is carried out at a measurement temperature of 5°C, and then at a measurement temperature of 60°C. The measurement result is taken as the second measurement result. Tables 2 and 3 show the second measurement results.
[0291] (Rubber hardness, Hs)
[0292] The hardness of the rubber sample cut out from the tread and base tread of each test tire was measured. Specifically, the hardness of the sample (JIS-A hardness) was measured using a type A durometer according to JIS K 6253-3 (2012) "Rubber, vulcanized or thermoplastic - Determination of hardness - Part 3: Durometer method". The measurement was performed at 25°C.
[0293] (Ice grip performance)
[0294] A set of test tires were mounted on a 2000cc front-engine rear-wheel drive car made in Japan. The car was driven on ice to evaluate the grip performance on ice. Specifically, in order to evaluate the grip performance on ice, the stopping distance (ice braking stopping distance) required for the car traveling on ice at a speed of 30 km / h to stop after applying the locking brake was measured. The distance was expressed as an index (ice grip performance index) relative to Comparative Example 5 (value 100). A higher index indicates better braking performance on ice (ice grip performance).
[0295] (Dry grip performance)
[0296] The test tires were mounted on each wheel of a car (a 2000cc front-engine front-wheel drive car made in Japan). The braking distance of the car on a dry asphalt road surface was measured at an initial speed of 100 km / h. The distance was expressed as an index (dry grip performance index) relative to Comparative Example 5 (value 100). A higher index indicates a shorter braking distance and better dry grip performance.
[0297] [Table 2]
[0298]
[0299] [Table 3]
[0300]
[0301] [Table 4]
[0302]
[0303] Tables 2 and 3 reveal the following. The elastomer compositions of the examples contain a styrene-based elastomer and a temperature-responsive resin that changes its hydrophilicity with temperature, and also satisfy the following relationship at two given temperatures that differ by at least 10° C.: (contact angle at the lower temperature) / (contact angle at the higher temperature) ≤ 0.90, wherein the lower temperature is less than 25° C. These elastomer compositions can change tire performance in response to temperature changes because the hydrophilicity (contact angle) can be changed with temperature changes to change the compatibility with other components in the composition.
[0304] In addition, Table 4 also shows that the tire of the embodiment has excellent comprehensive performance in terms of ice grip performance and dry grip performance (expressed as the sum of the two indexes of ice grip performance and dry grip performance).
[0305] In addition, comparison between Comparative Example 2 and Examples shows that since the styrene-based elastomer is more oleophilic than natural rubber and is more compatible with a material having an LCST at a temperature above the LCST and is less compatible with the material at a temperature below the LCST, it promotes changes in tire performance between low and high temperatures.
[0306] Exemplary embodiments of the present invention include:
[0307] Embodiment 1. An elastomer composition comprising:
[0308] Styrenic elastomers; and
[0309] Temperature-responsive resins that change their hydrophilicity as the temperature changes.
[0310] The elastomeric composition satisfies the following relationship at two given temperatures that differ by at least 10°C:
[0311] (Contact angle at lower temperature) / (Contact angle at higher temperature)≤0.90,
[0312] The lower temperature is less than 25°C.
[0313] Embodiment 2. The elastomer composition according to embodiment 1,
[0314] Wherein, the elastomer composition satisfies the following relationship at two given temperatures that differ by at least 10°C:
[0315] (Contact angle at lower temperature) / (contact angle at higher temperature)≤0.85.
[0316] Embodiment 3. The elastomer composition according to embodiment 1,
[0317] Wherein, the elastomer composition satisfies the following relationship at two given temperatures that differ by at least 10°C:
[0318] (Contact angle at lower temperature) / (contact angle at higher temperature)≤0.80.
[0319] Embodiment 4. The elastomer composition according to any one of embodiments 1 to 3,
[0320] Wherein, the elastomer composition satisfies the following relationship at two given temperatures that differ by at least 10°C:
[0321] (Contact angle at lower temperature) / (contact angle at higher temperature)≥0.30.
[0322] Embodiment 5. The elastomer composition according to any one of embodiments 1 to 3,
[0323] Wherein, the elastomer composition satisfies the following relationship at two given temperatures that differ by at least 10°C:
[0324] (Contact angle at lower temperature) / (contact angle at higher temperature)≥0.40.
[0325] Embodiment 6. The elastomer composition according to any one of embodiments 1 to 5,
[0326] The temperature-responsive resin is a compound comprising "A" and "B" bonded to each other.
[0327] "A" contains groups that change their hydrophilicity with temperature, and
[0328] “B” includes at least one selected from terpene resins, rosin resins, styrene resins, C5 resins, C9 resins, C5 / C9 resins, coumarone resins, indene resins, and olefin resins.
[0329] Embodiment 7. The elastomer composition according to embodiment 6,
[0330] Therein, the group exhibits a lower critical solution temperature in water.
[0331] Embodiment 8. The elastomer composition according to any one of embodiments 1 to 7,
[0332] The temperature responsive resin is a block copolymer.
[0333] Embodiment 9. The elastomer composition according to embodiment 6,
[0334] The ratio (mass %) of "A" to "B" in the temperature responsive resin is 50:50 to 98:2.
[0335] Embodiment 10. The elastomer composition according to any one of embodiments 1 to 9,
[0336] The weight average molecular weight of the temperature responsive resin is 500 or more and 80,000 or less.
[0337] Embodiment 11. The elastomer composition according to any one of embodiments 1 to 10,
[0338] The elastomer composition further comprises at least one of water-absorbent fibers, elastomers or resins.
[0339] Embodiment 12. A tire comprising a temperature-responsive component, wherein the temperature-responsive component is formed from the elastomer composition according to any one of Embodiments 1 to 11.
[0340] The maximum thickness of the temperature responsive member is 1 mm or more.
[0341] Embodiment 13. The tire according to embodiment 12,
[0342] The temperature responsive component is an outer layer component of the tire.
[0343] Embodiment 14. The tire according to embodiment 12 or 13,
[0344] wherein the tire comprises at least one adjacent component adjacent to the temperature responsive component and formed of a material different from the elastomer composition, and
[0345] The difference in hardness between the adjacent member and the temperature responsive member at 25° C. is 15 or less.
Claims
1. An elastomer composition comprising: Styrenic elastomers; and A temperature-responsive resin that changes its hydrophilicity as the temperature changes, wherein The elastomeric composition satisfies the following relationship at two given temperatures that differ by at least 10°C: (Contact angle at lower temperature) / (Contact angle at higher temperature) ≤ 0.90, The lower temperature is less than 25°C, The temperature-responsive resin is a compound comprising "A" and "B" bonded to each other. "A" contains groups that change their hydrophilicity with temperature, "B" includes at least one selected from terpene resins, rosin resins, styrene resins, C5 resins, C9 resins, C5 / C9 resins, coumarone resins, indene resins and olefin resins.
2. The elastomer composition according to claim 1, in, The elastomeric composition satisfies the following relationship at two given temperatures that differ by at least 10°C: (Contact angle at lower temperature) / (Contact angle at higher temperature) ≤ 0.
85.
3. The elastomer composition according to claim 1, in, The elastomeric composition satisfies the following relationship at two given temperatures that differ by at least 10°C: (Contact angle at lower temperature) / (Contact angle at higher temperature) ≤ 0.
80.
4. The elastomer composition according to any one of claims 1 to 3, in, The elastomeric composition satisfies the following relationship at two given temperatures that differ by at least 10°C: (Contact angle at lower temperature) / (Contact angle at higher temperature) ≥ 0.
30.
5. The elastomer composition according to any one of claims 1 to 3, in, The elastomeric composition satisfies the following relationship at two given temperatures that differ by at least 10°C: (Contact angle at lower temperature) / (Contact angle at higher temperature) ≥ 0.
40.
6. The elastomer composition according to claim 1, in, The group exhibits a lower critical solution temperature in water.
7. The elastomer composition according to any one of claims 1 to 3, in, The temperature responsive resin is a block copolymer.
8. The elastomer composition according to claim 1, in, The ratio of "A" to "B" in the temperature responsive resin is 50:50 to 98:2 in mass %.
9. The elastomer composition according to any one of claims 1 to 3, in, The weight average molecular weight of the temperature responsive resin is 500 or more and 80,000 or less.
10. The elastomer composition according to any one of claims 1 to 3, in, The elastomeric composition further comprises at least one of a water-absorbent fiber, an elastomer, or a resin.
11. A tire comprising a temperature-responsive component, wherein the temperature-responsive component is formed from the elastomer composition according to any one of claims 1 to 10, The maximum thickness of the temperature responsive member is 1 mm or more.
12. The tire according to claim 11, in, The temperature responsive component is an outer layer component of the tire.
13. The tire according to claim 11 or 12, in, The tire comprises at least one adjacent component adjacent to the temperature responsive component and formed of a material different from the elastomer composition, The difference in hardness between the adjacent member and the temperature responsive member at 25° C. is 15 or less.